Nickel-preplated battery shell steel belt and manufacturing method thereof

By precisely controlling the chemical composition and manufacturing process of the pre-nickel-plated battery casing steel strip, the problems of weak nickel layer adhesion and insufficient corrosion resistance were solved, enabling the production of high-strength and deep-drawing performance battery casing steel strips to meet the high requirements of battery casings.

CN118880189AInactive Publication Date: 2024-11-01МААНЬШАНЬ АЙРОН ЭНД СТИЛ КО ЛТД

Patent Information

Application Number
CN202410857913.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing post-nickel plating process for battery casing steel results in a thin nickel layer, weak adhesion, and easy peeling, and cannot meet the requirements of high-speed stamping and corrosion resistance. The existing pre-nickel plating process uses steel with unreasonable composition, high cost, or poor production plate shape.

Method used

By precisely controlling the chemical composition and manufacturing process of the pre-nickel-plated battery casing steel strip, including steps such as molten iron pretreatment, low-temperature annealing, and nickel electroplating, an alloy layer is formed to ensure coating adhesion and corrosion resistance, meeting the requirements for high strength and deep drawing performance.

Benefits of technology

The production of ultra-low carbon steel strips with excellent coating adhesion, corrosion resistance and high strength meets the high-speed stamping requirements of battery casings, improving the overall performance of materials and processing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880189A_ABST
    Figure CN118880189A_ABST
Patent Text Reader

Abstract

The invention discloses a pre-nickel-plated battery case steel belt and a manufacturing method thereof. The pre-nickel-plated battery case steel belt comprises the following chemical components in percentage by weight: 0.002%-0.005% of C, less than or equal to 0.030% of Si, 0.10%-0.30% of Mn, less than or equal to 0.008% and less than or equal to 0.015% of P, less than or equal to 0.012% of S, 0.035%-0.055% of Ti, 0.03%-0.08% of Cr, 0.015%-0.035% of Ca and the balance of Fe and inevitable impurities. By optimizing the chemical components and the content of the chemical components in steel, the pre-nickel-plated plate for the battery shell is prepared, wherein the yield strength of the pre-nickel-plated plate is 230-280 MPa, the tensile strength of the pre-nickel-plated plate is 350-400 MPa, the elongation is larger than or equal to 35%, HV0.3 is larger than or equal to 130 and smaller than or equal to 155, the r value is larger than or equal to 1.2, Ra is larger than or equal to 0.5 micrometer and smaller than or equal to 1.0 micrometer, RPC is larger than or equal to 120, nickel-plated layers of 1-10 micrometers are arranged on the two faces respectively, the thickness of an alloy layer is larger than or equal to (0.5 * d) micrometers, d is the thickness of the nickel-plated layers, and the surface iron exposure rate is smaller than or equal to 5%. The plate is good in adhesive force when being stamped into a plating layer subsequently, and has high-speed stamping capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of manufacturing and using power battery shell steel, and in particular to a pre-nickel-plated battery shell steel strip and a manufacturing method thereof. Background Art

[0002] In recent years, with the rapid development of the energy storage market, cylindrical batteries have been widely used in power tools, laptops, and electric vehicles due to their mature technology, high degree of automated production, good pressure resistance, and good product consistency. However, most of the battery shells on the market currently use a post-nickel plating process, that is, stamping first and then electroplating. Since the post-nickel-plated battery shell is a blind hole battery, the thickness of the nickel layer at the bottom of the battery shell is thin or even leaks, resulting in weak corrosion resistance at the bottom. In addition, since there is no chemical reaction between the nickel plating layer and the iron matrix of the post-plating method, the bonding force is weak, and nickel powder is prone to fall off during the use of the battery, resulting in a self-discharge reaction inside the battery. In order to solve the above problems, the pre-nickel plating process is currently used instead of the existing post-nickel plating process, that is, the nickel layer is plated on the steel plate in the steel plate production process, and an alloying reaction occurs to improve its coating adhesion.

[0003] Domestic patent publication number CN115852243A "A high corrosion-resistant and heat-resistant pre-nickel-plated battery shell steel and its manufacturing method" discloses a high corrosion-resistant and heat-resistant pre-nickel-plated battery shell steel, which includes a substrate and a Fe-Ni alloy layer covering the surface of the substrate. The weight percentage of the chemical composition of the substrate is: C: 0.02~0.065%, 0<Si≤0.03%, Mn: 0.1~0.32%, 0<S≤0.01%, Cu: 0.005~0.03%, Ni: 0.005~0.035%, Cr: 0.015~0.065%, 0<Ti≤0.002%, and the remainder is Fe. The patent composition is ordinary aluminum-killed steel, which cannot meet the requirements of high-speed stamping.

[0004] The domestic patent publication number CN117448673A "An Ultra-low Carbon Pre-nickel Plated Steel Strip and Its Preparation Method" discloses an ultra-low carbon pre-nickel plated steel strip and its preparation method. The chemical composition weight percentage of the battery shell steel is as follows: C: 0.005-0.010%, Si≤0.03%, Mn: 0.30-0.60%, P: 0.008-0.015%, S≤0.008%, Alt: 0.03-0.07%, Cr: 0.03-0.06% N: ≤0.003%, Ti: 0.0050-0.020%, Nb: 0.01-0.02%, B: 0.0003-0.0008%, [O]≤0.002% The rest is Fe and unavoidable impurities. The patent adds a higher Nb element, the cost is higher, and due to the high annealing temperature, the surface exposed iron rate is difficult to control. In addition, neither of the above two solutions adopts a low-temperature annealing process. When producing thin-gauge pre-nickel-plated battery shell steel, it is very easy to have poor plate shape and poor coating adhesion. Summary of the invention

[0005] In view of the above problems, the present invention proposes a pre-nickel-plated battery shell steel strip and a manufacturing method thereof. The present invention focuses on the innovative design and manufacturing process of the pre-nickel-plated battery shell steel strip, aiming to produce an ultra-low carbon steel strip with excellent deep drawing performance, high strength, high corrosion resistance and good coating adhesion through fine composition control and strict manufacturing process, so as to meet the stringent requirements of battery shells for materials.

[0006] In order to solve the above technical problems, the present invention is implemented by the following technical solutions:

[0007] The present invention proposes a pre-nickel-plated battery shell steel strip, comprising a substrate and a nickel-plated layer attached to the surface of the substrate, wherein an alloy layer is formed between the nickel-plated layer and the substrate; the chemical composition of the substrate is as follows by weight percentage: C: 0.002% to 0.005%, Si≤0.030%, Mn: 0.10% to 0.30%, 0.008%≤P≤0.015%, S≤0.012%, Ti: 0.035% to 0.055%, Cr: 0.03% to 0.08%, Ca: 0.015% to 0.035%, and the rest is Fe and unavoidable impurities.

[0008] Preferably, the thickness d of the nickel plating layer is 1-10 μm, and the thickness of the alloy layer is ≥ (0.5*d) μm.

[0009] Preferably, the pre-nickel-plated battery shell steel strip meets the following properties: yield strength of 230MPa-280MPa, tensile strength of 350MPa-400MPa, elongation ≥34%, 130≤HV 0.3 ≤155, r value ≥1.2, 0.5μm ≤ Ra ≤ 1.0μm, RPC ≥120, surface exposed iron rate ≤5%.

[0010] The present invention also provides a method for manufacturing a pre-nickel-plated battery shell steel strip, comprising the following steps: molten iron pretreatment → converter → alloy fine-tuning station → RH → continuous casting → flame cleaning → hot rolling → curling → pickling → cold rolling → low-temperature annealing → nickel electroplating → high-temperature annealing → flattening → finished product.

[0011] Preferably, during smelting and continuous casting: pre-slag removal and post-slag removal measures are adopted during molten iron pretreatment to adjust the S element; self-circulating scrap steel is added in the early and middle stages of decarburization to modify the ladle top slag.

[0012] Preferably, during hot rolling and coiling: the heating temperature is 1200°C to 1250°C, the final rolling temperature is 850°C to 950°C, and the coiling temperature is 680°C to 730°C.

[0013] Preferably, in the pickling and cold rolling: the pickling rolling adopts five-stand continuous rolling, the pickling rolling reduction rate is ≥85%, the end stand adopts smooth roller rolling, the roughness is ≤0.5μm, and RPc≥220.

[0014] Preferably, in the low-temperature annealing, the soaking temperature is 400° C. to 500° C., and the soaking time is 30 s to 100 s.

[0015] Preferably, in high temperature annealing: the annealing temperature is 680°C to 740°C, the speed of the strip in the furnace is 250mpm to 300mpm, the cooling speed in the rapid cooling section is 30°C / s to 50°C / s, and the temperature is cooled from 680°C to 350°C.

[0016] Preferably, the flattening elongation is 0.6-1.2%, the board surface roughness is 0.5 μm≤Ra≤1.0 μm, and RPc≥120.

[0017] The role of the alloying elements in the steel grades in the present invention is mainly based on the following principles:

[0018] 1) Carbon (C): As the C element decreases, the strength of the steel plate decreases, the elongation, n value and r value increase, and the deep drawing performance of the steel plate will gradually improve. Therefore, ultra-low carbon is a prerequisite for the production of battery shell steel. At the same time, trace amounts of C elements help to improve the strength and hardness of the steel and ensure that the battery shell is not easily deformed. Therefore, the present invention adopts an ultra-low carbon component design to control C: 0.002% to 0.005%.

[0019] 2) Silicon (Si): If the Si content is too high, the iron oxide scale on the surface of the steel plate is difficult to remove, and micro cracks are easily formed on the surface due to the intrusion of oxides. During the high-speed deep drawing process of the steel strip, the micro cracks can serve as crack sources and cause the steel plate to crack. In addition, the excessive content of Si element affects the electroplating performance of the steel plate, so in the present invention, Si≤0.030%.

[0020] 3) Manganese (Mn): Mn can reduce the phase transition temperature of austenite → ferrite (which can compensate for the increase in the phase transition temperature of austenite → ferrite caused by the reduction of C element content), expand the hot working temperature range, and is beneficial to refine the ferrite grain size; but if the Mn content is too high, it will be detrimental to the plasticity, stamping performance, and fatigue performance. Considering comprehensively, the Mn percentage control range in the present invention is 0.10% to 0.30%.

[0021] 4) Phosphorus (P): A certain amount of P content in steel has a certain corrosion resistance effect, but excessive P is easy to form segregation in steel, which is not good for the formability of steel plates. Therefore, the content of P element in the present invention is controlled in the range of 0.008% to 0.015%.

[0022] 5) Sulfur (S): The sulfur element is a harmful element in battery shell steel, which makes the steel hot brittle, reduces the ductility and toughness of the steel, and easily causes cracks during rolling. In addition, sulfur is not good for welding performance and reduces corrosion resistance. Therefore, the present invention tries to control the sulfur content in the steel within the range of S≤0.012%.

[0023] 6) Chromium (Cr): A small amount of Cr element in steel improves the corrosion resistance of the steel, and Cr element also helps to improve the adhesion of the nickel layer. When Cr element is added to the steel at the same time, the electrochemical reaction in the steel is inhibited, which helps to improve the corrosion resistance of the battery shell. However, Cr element can significantly improve the strength and hardness of steel and deteriorate the stamping performance of the steel plate. Therefore, the Cr element is controlled in the range of 0.03-0.08%.

[0024] 7) Calcium (Ca): A small amount of Ca element has a certain improvement effect on improving the surface quality of the steel plate, and can effectively improve the adhesion of the nickel layer, thereby improving the corrosion resistance of the steel plate. Therefore, the control range of Ca element is 0.015~0.035%.

[0025] 8) Titanium (Ti): Ti is a strong carbide, sulfide and nitride forming element. This type of compound is not easily soluble in austenite at high temperatures, which hinders the growth of austenite grains, refines grains, and improves the deep drawing performance of steel sheets. However, too much second phase precipitates will also affect the deep drawing performance of steel sheets. Therefore, the present invention controls the Ti element in the steel to be within the range of 0.035% to 0.055%.

[0026] The manufacturing method of the cold-rolled sheet for the ultra-low carbon battery shell requires the following steps: molten iron smelting, slab continuous casting, flame cleaning, soaking in a soaking furnace, hot continuous rolling controlled rolling and controlled cooling, coiling, pickling, cold rolling, and continuous annealing. The process features are as follows:

[0027] (1) Smelting and continuous casting: In the process of molten iron pretreatment, taking measures such as pre-slag removal and post-slag removal to adjust the [S] element can reduce harmful elements in molten steel. Adding self-circulating scrap steel in the early and middle stages of decarburization to modify the ladle top slag can help reduce impurity elements in molten steel.

[0028] (2) Hot rolling and coiling: The heating temperature is controlled at 1200℃~1250℃. At high temperature, the second phase particles are dissolved in the steel and are beneficial to rolling. Fine particles are reprecipitated during the coiling process, which is beneficial to improving the stamping performance and corrosion resistance of the material. The final rolling temperature is controlled at 850℃~950℃, which can ensure that the final rolling temperature is controlled above the austenite temperature to avoid the mixed crystal phenomenon caused by rolling in the two-phase region. The coiling temperature is set at 680℃~730℃.

[0029] (3) Pickling and rolling: Pickling rolling adopts five-stand continuous rolling, and the reduction rate of pickling rolling is ≥85%. A large reduction rate can increase the grain distortion energy in the steel, reduce the recrystallization temperature, and is conducive to grain refinement and improving the deep drawing performance of the steel plate. The last stand adopts smooth roller rolling, and the roughness is controlled to be ≤0.5μm and RPc≥220. This measure can effectively improve the surface quality of the finished plate and improve the adhesion of the steel plate.

[0030] (4) Low temperature annealing: The soaking temperature is controlled at 400℃~500℃ and the soaking time is 30s~100s. The cleaning and drying sections of this process can remove the oil stains on the surface of the hard rolled coil. The straightening and flattening processes can correct the plate shape. Heating can increase the activity of the grains on the surface of the substrate and reduce the strength of the hard rolled coil, thereby improving the electroplating adhesion of the steel plate.

[0031] (5) Nickel electroplating: The chemical electroplating method is used to plate a nickel layer of 1μm to 10μm on both sides of the steel coil, and the coating is smooth and delicate.

[0032] (6) High temperature annealing: annealing temperature 680℃~740℃, strip furnace speed: 250mpm~300mpm, rapid cooling section temperature cooling speed: 30℃ / s~50℃ / s, cooling from 680℃ to 350℃. This process can achieve ultra-low carbon yield strength range of: 230MPa~280MPa.

[0033] (7) Smoothing: Laser texturing roller is used for smoothing, and the smoothing elongation is controlled at 0.6-1.2%. A smoothing roller with Ra of 1.6 μm is used to ensure that the plate surface roughness is 0.5 μm ≤ Ra ≤ 1.0 μm, and RPc ≥ 120. This roughness is conducive to the smooth surface of the battery shell after stamping.

[0034] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0035] The present invention mainly produces a low-carbon cold-rolled plate for deep-drawing battery shell by precisely controlling the components in the steel and through hot rolling, acid rolling, low-temperature annealing, nickel plating, high-temperature annealing and flattening processes.

[0036] Fine control of chemical composition: Ultra-low carbon (C: 0.002% ~ 0.005%) ensures the high ductility and deep drawing performance of the material, while the presence of trace carbon enhances the basic strength of the material. Silicon (Si ≤ 0.030%) and sulfur (S ≤ 0.012%) strictly control the content of these two elements to reduce surface defects and hot brittleness and optimize electroplating performance. Manganese (Mn: 0.10% ~ 0.30%) and titanium (Ti: 0.035% ~ 0.055%) synergistically act on the transformation from austenite to ferrite, refine the grains, and improve the comprehensive mechanical properties of the material. The addition of phosphorus (0.008% ≤ P ≤ 0.015%), chromium (Cr: 0.03% ~ 0.08%), and calcium (Ca: 0.015% ~ 0.035%) enhances corrosion resistance, improves the adhesion of nickel plating, and optimizes surface quality, while maintaining good stamping performance.

[0037] Optimization of production process: Smelting and continuous casting: Through fine molten iron pretreatment and ladle top slag modification, the purity of the material is guaranteed, laying a solid foundation for subsequent processing. Hot rolling and curling: High temperature heating and controlled final rolling temperature ensure uniform organizational structure, and the solid solution and re-precipitation of second phase particles at high temperature enhance the mechanical properties and corrosion resistance of the material. Pickling and cold rolling: The combination of high pressure reduction rate pickling and continuous rolling and smooth roller final finishing rolling effectively refines the grains, improves the surface quality and electroplating adhesion. Low temperature annealing and high temperature annealing: Low temperature annealing improves the activity of the grains on the substrate surface, and high temperature annealing further stabilizes the microstructure of the material, ensuring the final mechanical properties and coating quality. Nickel electroplating and leveling: The precision electroplating process combined with laser roughening and leveling forms a uniform and dense nickel plating layer and suitable surface roughness, ensuring the firm bonding of the coating and the adaptability of subsequent processing.

[0038] The cold-rolled steel sheet produced by the method of the present invention has a yield strength of 230MPa-280MPa, a tensile strength of 350MPa-400MPa, an elongation of ≥34%, and 130≤HV 0.3 ≤155, r value ≥1.2, 0.5μm ≤ Ra ≤ 1.0μm, RP C ≥120, 1-10μm nickel-plated layer on both sides, and alloy layer thickness ≥(0.5*d)μm, d is the thickness of the nickel-plated layer, and surface iron exposure rate ≤5% pre-nickel-plated plate for battery shell. The plate has good adhesion to the subsequent stamping of the plating layer and has the ability of high-speed stamping.

[0039] In summary, the present invention successfully solves the challenge of achieving excellent corrosion resistance, plate shape and coating adhesion while maintaining high strength and deep drawing properties of ultra-low carbon materials through highly coordinated chemical composition design and multi-step precision processing technology. The proposed pre-nickel-plated battery shell steel strip not only meets the high requirements of battery shells for material properties, but also improves the overall performance and processing efficiency of the material through a unique alloy element ratio and optimized manufacturing process, bringing significant technological progress to the field of battery shell materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is the distribution diagram of iron elements on the surface of the coated steel strip in Example 4.

[0041] Figure 2 This is the nickel element distribution diagram on the surface of the coated steel strip in Example 4. DETAILED DESCRIPTION

[0042] In order to enable those skilled in the art to better understand the technical solution of the present invention, the preferred implementation scheme of the present invention is described below in conjunction with specific embodiments, but it should not be understood as limiting the present invention and is only used as an example.

[0043] The experimental methods or test methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials are obtained from conventional commercial channels or prepared by conventional methods unless otherwise specified.

[0044] The present invention is further described in detail below in conjunction with specific embodiments.

[0045] The chemical composition and content of the molten steel of Examples 1-6 of the present invention and Comparative Examples 1-7 are shown in Table 1, and the rest are Fe and unavoidable impurity elements.

[0046] The production processes of molten steel of Examples 1-6 of the present invention and Comparative Examples 1 to 7 are shown in Table 2, wherein Comparative Examples 1 to 7 are not smelted completely according to the production process of the present invention.

[0047] Table 1 Chemical composition, wt%

[0048]

[0049]

[0050] All production processes were trial-produced according to Table 2, and the finished product thickness specification was 0.30 mm.

[0051] Table 2 Production process

[0052]

[0053] Table 3 Detection performance values

[0054] category direction <![CDATA[R p0.2 / MPa]]> <![CDATA[R m / MPa]]> <![CDATA[A 50 / %]]> r-value <![CDATA[HV 0.3 ]]> Iron exposure rate Electroplating Adhesion Example 1 0° 233 356 40 1.42 131 4.75% OK Example 2 0° 276 392 35 1.26 153 4.36% OK Example 3 0° 243 376 37 1.44 139 3.95% OK Example 4 0° 268 386 36 1.25 147 4.18% OK Example 5 0° 272 392 35 1.21 156 4.59% OK Example 6 0° 243 369 38 1.36 142 4.96% OK Comparative Example 1 0° 226 345 42 1.45 118 6.12% No Comparative Example 2 0° 175 337 44 1.52 106 7.15% No Comparative Example 3 0° 263 406 32 1.05 164 4.12% No Comparative Example 4 0° 193 354 38 1.38 115 4.69% No Comparative Example 5 0° 286 404 33 0.75 163 4.12% No Comparative Example 6 0° 234 361 40 0.85 118 5.13% No Comparative Example 7 0° 275 385 34 0.73 153 5.36% No

[0055] The mechanical property values ​​of the final product and the electroplating adhesion test are shown in Table 3. The electroplating adhesion test method is to bend the electroplated battery shell 180°, stick it tightly with 3M tape, and then tear it off to check whether nickel powder falls off. Then, bend it 360° in the opposite direction according to the bending mark, stick it tightly with 3M tape, and then tear it off to check whether nickel powder falls off. If the nickel powder does not fall off, it is OK, otherwise it is No.

[0056] The performance of Examples 1 to 6 can meet the requirements. Figure 1 and Figure 2 It can be seen that the surface iron exposure rate of the steel plate in Example 4 of the present invention is 4.18%, which has good corrosion resistance. In Comparative Example 1, due to the lack of addition of Cr and Ca elements, the Rpc value is lower than 120, the yield strength is lower than 230MPa, and the adhesion is poor, and nickel powder falls off. It cannot meet the requirements of high-speed stamping of battery shell steel. Comparative Example 2 adopts an ordinary IF steel component system, resulting in low yield strength, low hardness, and poor adhesion of nickel powder. In Comparative Example 3, the Cr element exceeds the standard, resulting in ultra-high tensile performance and low r value, which cannot meet the stamping requirements of battery shell steel. Comparative Example 4 has a large number of orange peel defects and low hardness, which cannot meet the requirements of the finished product. Comparative Examples 1 to 7 all use the low-temperature annealing process of this patent, resulting in poor adhesion of the nickel plating layer and the phenomenon of nickel powder removal. Among them, the yield strength, tensile strength and hardness of Comparative Example 3 are lower than the requirements of this patent. Comparative Example 6 does not add Cr elements. Although the yield strength, tensile strength and elongation meet the requirements, the microhardness is low and the nickel powder adhesion is poor, which cannot meet the requirements. Comparative Examples 5 to 7 all use aluminum-killed steel components, and the r value is significantly reduced, which cannot meet the high-speed stamping of cylindrical batteries. In addition, if the annealing temperature is greater than 730°C and the annealing speed is less than 250mpm, the exposed iron rate of the coating will be greater than 5%, as shown in Comparative Examples 1, 2, 6, and 7.

[0057] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A pre-nickel-plated battery shell steel strip, comprising a substrate and a nickel-plated layer attached to the surface of the substrate, wherein an alloy layer is formed between the nickel-plated layer and the substrate; characterized in that: The chemical composition of the substrate is calculated by weight percentage as follows: C: 0.002% to 0.005%, Si≤0.030%, Mn: 0.10% to 0.30%, 0.008%≤P≤0.015%, S≤0.012%, Ti: 0.035% to 0.055%, Cr: 0.03% to 0.08%, Ca: 0.015% to 0.035%, and the rest is Fe and unavoidable impurities.

2. The pre-nickel-plated battery shell steel strip according to claim 1, characterized in that: The thickness d of the nickel plating layer is 1-10 μm, and the thickness of the alloy layer is ≥ (0.5*d) μm.

3. The pre-nickel-plated battery shell steel strip according to claim 1, characterized in that: The pre-nickel-plated battery shell steel strip meets the following properties: yield strength of 230MPa-280MPa, tensile strength of 350MPa-400MPa, elongation ≥34%, 130≤HV 0.3 ≤155, r value ≥1.2, 0.5μm ≤ Ra ≤ 1.0μm, RP C ≥120, surface exposed iron rate ≤5%.

4. A method for manufacturing a pre-nickel-plated battery shell steel strip according to any one of claims 1 to 3, characterized in that: The process includes the following steps: molten iron pretreatment → converter → alloy fine-tuning station → RH → continuous casting → flame cleaning → hot rolling → curling → pickling → cold rolling → low temperature annealing → nickel electroplating → high temperature annealing → flattening → finished product.

5. The method for manufacturing a pre-nickel-plated battery shell steel strip according to claim 4, characterized in that: During smelting and continuous casting: in the process of molten iron pretreatment, pre-slag removal and post-slag removal measures are taken to adjust the S element; self-circulating scrap steel is added in the early and middle stages of decarburization to modify the ladle top slag.

6. The method for manufacturing a pre-nickel-plated battery shell steel strip according to claim 4, characterized in that: During hot rolling and coiling: the heating temperature is 1200℃~1250℃, the final rolling temperature is 850℃~950℃, and the coiling temperature is 680℃~730℃.

7. The method for manufacturing a pre-nickel-plated battery shell steel strip according to claim 4, characterized in that: During pickling and cold rolling: pickling rolling adopts five-stand continuous rolling, the pickling rolling reduction rate is ≥85%, the end stand adopts smooth roller rolling, the roughness is ≤0.5μm, RPc≥220.

8. The method for manufacturing a pre-nickel-plated battery shell steel strip according to claim 4, characterized in that: In low temperature annealing: the soaking temperature is 400℃~500℃, and the soaking time is 30s~100s.

9. The method for manufacturing a pre-nickel-plated battery shell steel strip according to claim 4, characterized in that: During high temperature annealing: the annealing temperature is 680℃~740℃, the speed of the strip in the furnace is 250mpm~300mpm, the cooling speed of the rapid cooling section is 30℃ / s~50℃ / s, cooling from 680℃ to 350℃.

10. The method for manufacturing a pre-nickel plated battery shell steel strip according to claim 4, characterized in that: During leveling: the leveling elongation is 0.6-1.2%, the board surface roughness is 0.5μm≤Ra≤1.0μm, RPc≥120.

Citation Information

Patent Citations

  • Thick high-toughness pipeline steel and manufacturing method thereof

    CN105463324A

  • Cold-rolled sheet for energy-storage alkaline battery shell and production method of cold-rolled sheet

    CN117604394A

  • Method, device, and computer program for processing short-term insurance product subscription

    KR1020250003289A

  • Satellite antenna with dual-band frequency switching function

    KR102841148B1

  • Nickel-plated steel, fabrication method therefor, and battery shell

    WO2024109746A1

Cited By

  • Cold-rolled sheet for energy-storage alkaline battery shell and production method of cold-rolled sheet

    CN117604394A

  • Steel for pre-nickel-plated battery shell and preparation method of steel

    CN120273006A

  • Production method of hot-rolled steel strip for new energy vehicle battery protection frame

    CN123043397A

  • High strength nickel-plated heat-treated steel sheet for battery case and manufacturing method thereof

    EP4759967A1

  • Nickel-plated steel strip and manufacturing method therefor, and battery housing formed therefrom

    WO2026189550A1