Ultrahigh-tensile-strength copper foil additive, manufacturing method thereof and electrolytic copper foil
The prior art was solved by using composite additives of collagen, hydroxyethyl cellulose, sodium polydithiodipropane sulfonate, sodium thiazolinyldithiopropane sulfonate and MDT-100 in electrolytic copper foils. Due to the poor mechanical properties of 6μm copper foil, electrolytic copper foil with high tensile strength and low roughness has been prepared, which improves the stability and safety of lithium batteries.
Patent Information
- Application Number
- CN202411129954.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-01
AI Technical Summary
The electrolytic additives used in the existing 6μm copper foil lead to poor mechanical properties of copper foil, especially in terms of tensile strength and crack resistance, which affects the stability and safety of lithium batteries.
Using an ultra-high tensile strength copper foil additive, including collagen, hydroxyethyl cellulose, sodium polydithiodipropane sulfonate, sodium thiazolinyldithiopropane sulfonate and MDT-100, Mixed with the electrolyte solution and electrolyzed to prepare an electrolytic copper foil with high tensile strength and low roughness.
Effectively control the growth of electrolytic copper foil grains, obtain uniform and fine grains, with high tensile strength and excellent fracture resistance, meet the demand of the lithium battery industry for ultra-thin electrolytic copper foil, and the tensile strength is no less than 800MPa. The elongation rate is not less than 2%.
Smart Images

Figure CN118880403A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrolytic copper foil, and in particular to an ultra-high tensile strength copper foil additive, a manufacturing method thereof and an electrolytic copper foil. Background Art
[0002] With the rapid development of the lithium battery industry, the technical level of lithium batteries has gradually developed from the middle and low end to the high end. In the technological development, high tensile strength and ultra-thin electrolytic copper foil for lithium batteries is the mainstream direction of future research and development.
[0003] At present, the main research and development direction of electric vehicles is to improve the endurance and intelligence. In order to improve the endurance, high energy density lithium batteries are the main research direction. There are many ways to improve the energy density of lithium batteries, and the fastest and lowest cost method is to reduce the thickness of the negative electrode carrier (thickness of the electrolytic copper foil), thereby increasing the amount of energy storage slurry coating to achieve the purpose of improving the energy density of lithium batteries; the reduction of the thickness of the electrolytic copper foil will also reduce its tensile strength, which will directly affect the crack resistance of the copper foil. During the charging and discharging process of the lithium battery, the lithium battery will release heat. Due to thermal expansion and contraction, the battery volume will change, which may cause the electrolytic copper foil to break, and lithium battery short circuit fire and other safety problems; therefore, the tensile strength performance of the electrolytic copper foil will directly affect the stability, safety and service life of the lithium battery. Therefore, improving the tensile strength performance of the electrolytic copper foil has become an urgent problem to be solved in the lithium battery industry.
[0004] As we all know, in the production process of electrolytic copper foil, different types of copper foil will be obtained by using different electroplating additive processes. The research and development of additive formulas has always been an important direction for the research and development of copper foil products. How to develop an additive formula to effectively improve the tensile strength of ultra-thin electrolytic copper foil to meet the needs of the lithium battery industry is an urgent problem that the industry needs to solve.
[0005] China's invention patent publication number CN118223083A discloses a high-strength, high-precision, ultra-thin electrolytic copper foil additive for lithium batteries. The mass composition of each component of the additive is: polyethylene glycol 3-12 mg / L, hydroxyethyl cellulose 5-12 mg / L, collagen 15-40 mg / L, polydisulfide dipropane sulfonate sodium 1-10 mg / L, cycloethanol 6-15 mg / L, hydrochloric acid 6-15 mg / L. The grain structure of the copper foil is equiaxed grains, and the average grain size is 3-10 nm, the tensile strength is greater than 460 MPa, the surface roughness is less than 54.0 nm, and it does not fade when heated at 150 ° C / 8 min. The problem of poor mechanical properties of copper foil is solved through the synergistic effect between specific components.
[0006] China invention patent authorization announcement number CN113445081B discloses an additive for electrolytic copper foil, an electrolyte for electrolytic copper foil, copper foil and a preparation method thereof. The additive for electrolytic copper foil includes: sodium polydisulfide propane sulfonate, sodium alcoholthiopropane sulfonate, polymer glue, polyethylene glycol and hydroxyethyl cellulose; wherein the mass ratio of sodium polydisulfide propane sulfonate, sodium alcoholthiopropane sulfonate, polymer glue, polyethylene glycol and hydroxyethyl cellulose is (3-30): (1-15): (5-50): (1-20): (1-10). Through the synergistic effect between specific components, the problem of poor mechanical properties of copper foil is solved.
[0007] The above two patents use different combinations of additive components to improve the mechanical properties of copper foil, but the copper foil thicknesses they target are different. For example, the copper foil thickness of Examples 1-10 in China Invention Patent Publication No. CN118223083A is 5 μm, and the copper foil thicknesses of Examples 1-5 in China Invention Patent Authorization Announcement No. CN113445081B are 7.23 μm, 7.06 μm, 7.63 μm, 6.53 μm, and 6.84 μm. Copper foils of different thicknesses will affect the mechanical properties of the copper foil. The mechanical property evaluation of a single thickness, such as 6 μm copper foil, is missing, and the research on large-scale production of copper foils of the same actual thickness is of little significance. Summary of the invention
[0008] The problem to be solved by the present invention is that the electrolytic additives used in the existing 6μm copper foil cause the copper foil to have poor mechanical properties. To this end, an ultra-high tensile strength copper foil additive applied to 6μm copper foil and a manufacturing method thereof and an electrolytic copper foil are provided.
[0009] The technical solution of the present invention is: an ultra-high tensile strength copper foil additive, comprising: 1 mg / L-10 mg / L of collagen, 1 mg / L-10 mg / L of hydroxyethyl cellulose, 1 mg / L-10 mg / L of sodium polydisulfide propane sulfonate, 20 mg / L-70 mg / L of sodium thiazoline disulfide propane sulfonate and 1 mg / L-20 mg / L of MDT-100.
[0010] The mass ratio of sodium thiazolyl dithiopropane sulfonate to MDT-100 in the above scheme is (2.5-12.5):(1.8-5).
[0011] The mass ratio of the collagen, hydroxyethyl cellulose and sodium polydisulfide propane sulfonate is 1:1:1.
[0012] A method for preparing an ultra-high tensile strength electrolytic copper foil comprises the following steps: mixing the additive as described above with an electrolyte, and electrolyzing to obtain the electrolytic copper foil.
[0013] The electrolyte in the above scheme contains 90g / L-95g / L Cu2+ 100g / L-110g / LH 2 SO 4 and 20mg / L-25mg / L Cl - .
[0014] The flow rate of the electrolyte in the above scheme is 40m 3 / h-70m 3 / h, and the additive is added to the electrolyte in an amount of 100mL / min-800mL / min.
[0015] An ultra-high tensile strength electrolytic copper foil is prepared by the above-mentioned method for preparing an ultra-high tensile strength electrolytic copper foil.
[0016] The smooth surface Ra of the electrolytic copper foil in the above scheme is not higher than 0.3 μm, Rz is not higher than 3.0 μm, the tensile strength is not lower than 800 MPa, and the elongation is not lower than 2%.
[0017] The invention has the beneficial effects of being composed of a composite of collagen, hydroxyethyl cellulose, sodium polydisulfide propane sulfonate, sodium thiazoline disulfide propane sulfonate and MDT-100, which can effectively control the growth of electrolytic copper foil grains, thereby obtaining an electrolytic copper foil with uniform and fine grains, high tensile strength and ultra-thinness, meeting the requirements of the rapid development of the lithium battery industry. The 6μm electrolytic copper foil prepared by using the additive of the invention has low roughness, high tensile strength and excellent fracture resistance, wherein the smooth surface roughness is not higher than 0.3μm, the roughness of the matte surface is not higher than 3.0μm, the tensile strength is not lower than 800Mpa, and the elongation is not lower than 2%. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 EBSD pattern quality characterization diagram of the preferred example copper foil of the present invention;
[0019] Figure 2 is an EBSD grain distribution diagram of a preferred example copper foil of the present invention;
[0020] Figure 3 This is an EBSD orientation distribution chart of a preferred example copper foil of the present invention. DETAILED DESCRIPTION
[0021] The following is an explanation of the embodiments of the present invention by specific specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. Before further describing the specific embodiments of the present invention, it should be understood that the scope of protection of the present invention is not limited to the specific specific embodiments described below; it should also be understood that the terms used in the embodiments of the present invention are to describe specific specific embodiments, rather than to limit the scope of protection of the present invention. When the embodiments give a numerical range, it should be understood that, unless otherwise specified in the present invention, the two endpoints of each numerical range and any value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by ordinary technicians in the technical field to which the present invention belongs.
[0022] The present invention does not limit the source of the raw materials used. Unless otherwise specified, the raw materials used in the present invention are all common commercial products in the field of this technology. Unless otherwise specified, the solvents used in the solution of this application are all water, preferably pure water, wherein the molecular weight of collagen is 1000-5000; hydroxyethyl cellulose, CAS: 9004-62-0, purchased from Wuhan Zhuochuang Yuanhang; sodium thiazolyl disulfide propane sulfonate, CAS: 8106-00-1; sodium polydisulfide propane sulfonate was purchased from Wuhan Shuer, CAS: 27206-35-5; MDT-100 was purchased from Jiangsu Mengde. It should be noted that the specific model used in this embodiment does not have a substantial impact on the performance of the product and should not be regarded as a limitation on the scope of protection.
[0023] Example 1: An additive for improving the tensile strength of electrolytic copper foil, comprising 1 mg / L collagen, 1 mg / L hydroxyethyl cellulose, 20 mg / L sodium thiazolyl disulfide propane sulfonate, 1 mg / L sodium polydisulfide propane sulfonate and 1 mg / L MDT-100.
[0024] The preparation method of the additive comprises the following steps:
[0025] (1) Weighing: Weigh collagen, sodium thiazoline disulfide propane sulfonate, hydroxyethyl cellulose, sodium polydisulfide propane sulfonate and MDT-100 in sequence;
[0026] (2) Dissolution: The collagen, sodium thiazolyl disulfide propane sulfonate, hydroxyethyl cellulose, sodium polydisulfide propane sulfonate and MDT-100 weighed in step (1) are placed in a 100 L tank for dissolution, and then diluted with water. The volume of the additive mixed solution is 100 L to obtain the additive.
[0027] The electrolytic copper foil is prepared by using the above additives, and the specific preparation method is as follows:
[0028] The above-mentioned additives are added to the lower liquid pipe of the high-level tank to mix with the electrolyte flowing downward, and copper foil is electrolyzed on the rough foil electrolytic cell. The obtained copper foil is the electrolytic copper foil. The amount of additive added in the process is 500mL / min, the copper content in the electrolyte is 92g / L; the sulfuric acid content is 105g / L; the chloride ion content is 20mg / L, and the machine flow rate is 50m 3 / h, the current density during electrolysis on the foil electrolytic cell is 60A / dm 2 .
[0029] Example 2: An additive for improving the tensile strength of electrolytic copper foil, comprising 3 mg / L collagen, 3 mg / L hydroxyethyl cellulose, 3 mg / L sodium polydisulfide propane sulfonate, 30 mg / L sodium thiazolyl disulfide propane sulfonate and 3 mg / L MDT-100.
[0030] The preparation method of the additive is the same as that of Example 1;
[0031] The preparation method of the electrolytic copper foil is the same as that of Example 1.
[0032] Example 3: An additive for improving the tensile strength of electrolytic copper foil, comprising 5 mg / L collagen, 5 mg / L hydroxyethyl cellulose, 40 mg / L sodium thiazolyl disulfide propane sulfonate, 5 mg / L sodium polydisulfide propane sulfonate, and 5 mg / L MDT-100.
[0033] The preparation method of the additive is the same as that of Example 1;
[0034] The preparation method of the electrolytic copper foil is the same as that of Example 1.
[0035] Example 4: An additive for improving the tensile strength of electrolytic copper foil, comprising 8 mg / L collagen, 8 mg / L hydroxyethyl cellulose, 50 mg / L sodium thiazolyl disulfide propane sulfonate, 8 mg / L sodium polydisulfide propane sulfonate, and 10 mg / L MDT-100.
[0036] The preparation method of the additive is the same as that of Example 1;
[0037] The preparation method of the electrolytic copper foil is the same as that of Example 1.
[0038] Example 5: An additive for improving the tensile strength of electrolytic copper foil, comprising 10 mg / L collagen, 10 mg / L hydroxyethyl cellulose, 60 mg / L sodium thiazolyl disulfide propane sulfonate, 10 mg / L sodium polydisulfide propane sulfonate, and 20 mg / L MDT-100.
[0039] The preparation method of the additive is the same as that of Example 1;
[0040] The preparation method of the electrolytic copper foil is the same as that of Example 1.
[0041] Example 6: An additive for improving the tensile strength of electrolytic copper foil, comprising 5 mg / L collagen, 5 mg / L hydroxyethyl cellulose, 70 mg / L sodium thiazolyl disulfide propane sulfonate, 5 mg / L sodium polydisulfide propane sulfonate, and 20 mg / L MDT-100.
[0042] The preparation method of the additive is the same as that of Example 1;
[0043] The preparation method of the electrolytic copper foil is the same as that of Example 1.
[0044] Example 7: An additive for improving the tensile strength of electrolytic copper foil, comprising 10 mg / L collagen, 1 mg / L hydroxyethyl cellulose, 50 mg / L sodium thiazolyl disulfide propane sulfonate, 2 mg / L sodium polydisulfide propane sulfonate, and 20 mg / L MDT-100.
[0045] The preparation method of the additive is the same as that of Example 1;
[0046] The preparation method of the electrolytic copper foil is the same as that of Example 1.
[0047] Example 8: An additive for improving the tensile strength of electrolytic copper foil, comprising 10 mg / L collagen, 2 mg / L hydroxyethyl cellulose, 60 mg / L sodium thiazolyl disulfide propane sulfonate, 3 mg / L sodium polydisulfide propane sulfonate, and 20 mg / L MDT-100.
[0048] The preparation method of the additive is the same as that of Example 1;
[0049] The preparation method of the electrolytic copper foil is the same as that of Example 1.
[0050] Comparative Example 1: This comparative example is used as a blank comparative example. No additives are added, that is, no additives are added to the lower liquid pipe of the high-level tank, and normal electroplating is directly performed to obtain electrolytic copper foil, wherein the copper content in the electrolyte is 92g / L; the sulfuric acid content is 105g / L; the chloride ion content is 20mg / L, and the machine flow rate is 50m 3 / h, the current density during electrolysis on the foil electrolytic cell is 60A / dm 2 .
[0051] Performance test of electrolytic copper foil:
[0052] The properties of the electrolytic copper foils prepared in the examples and comparative examples are shown in Table 1, wherein the roughness test refers to IPC-TM-650 2.4.17, the tensile strength test refers to IPC-TM-650 2.4.18, and the elongation test refers to IPC-TM-650 2.4.18.
[0053] It can be seen from Table 1 that the electrolytic copper foil prepared by the present invention has lower roughness and higher tensile strength, has excellent fracture resistance, and can be used for 6 μm thick electrolytic copper foil of lithium batteries.
[0054] Meanwhile, it can be seen from Examples 7 and 8 that at this additive ratio concentration, the tensile strength of 6 μm electrolytic copper foil is not less than 800 MPa, and the elongation is not less than 2%. Therefore, Examples 7 and 8 are preferred examples of the present invention.
[0055] Table 1 Properties of electrolytic copper foil prepared in Examples and Comparative Examples
[0056]
[0057] like Figure 1-2 As shown, it can be seen from the EBSD pattern quality map and the EBSD grain distribution map that the copper foil grain size is very small, and the smaller the grain size, the greater the tensile strength, indicating that the 6μm electrolytic copper foil prepared by the present invention has high tensile strength, which is consistent with the example data; Figure 3 It can be seen from the EBSD orientation distribution table that ∑3 accounts for 82.1% and ∑9 accounts for 9.1%. The ultra-high tensile strength of the electrolytic copper foil benefits from the ultra-high proportion of ∑3.
[0058] As described above, the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments can still be modified, or some of the technical features can be replaced by equivalents, and these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. An ultra-high tensile strength copper foil additive, characterized in that: include: 1mg / L-10mg / L collagen, 1mg / L-10mg / L hydroxyethyl cellulose, 1mg / L-10mg / L sodium polydisulfide propane sulfonate, 20mg / L-70mg / L sodium thiazolyl disulfide propane sulfonate and 1mg / L-20mg / L MDT-100.
2. The ultra-high tensile strength copper foil additive according to claim 1, characterized in that: The mass ratio of the sodium thiazolyl dithiopropane sulfonate to MDT-100 is (2.5-12.5):(1.8-5).
3. The ultra-high tensile strength copper foil additive according to claim 1, characterized in that: The mass ratio of the collagen, hydroxyethyl cellulose and sodium polydisulfide propane sulfonate is 1:1:
1.
4. A method for preparing an ultra-high tensile strength electrolytic copper foil, characterized in that: The method comprises the following steps: mixing the additive described in any one of claims 1 to 2 with an electrolyte, and performing electrolysis to obtain an electrolytic copper foil.
5. The method for preparing an ultra-high tensile strength electrolytic copper foil according to claim 4, characterized in that: The electrolyte contains 90g / L-95g / L Cu 2+ , 100g / L-110g / L H2SO4 and 20mg / L-25mg / LCl-.
6. The method for preparing an ultra-high tensile strength electrolytic copper foil according to claim 4, characterized in that: The flow rate of the electrolyte is 40m 3 / h-70m 3 / h, and the additive is added to the electrolyte in an amount of 100mL / min-800mL / min.
7. An ultra-high tensile strength electrolytic copper foil, characterized by: The invention is prepared by the method for preparing an ultra-high tensile strength electrolytic copper foil as described in claim 4 or 5.
8. The ultra-high tensile strength electrolytic copper foil according to claim 7, characterized in that: The light surface Ra of the electrolytic copper foil is not higher than 0.3 μm, Rz is not higher than 3.0 μm, the tensile strength is not lower than 800 Mpa, and the elongation is not lower than 2%.