Lithium niobate film ridge waveguide for optical electric field sensor and preparation method thereof
By using lithium niobate thin film spinal waveguide in optical electric field sensors and using ionic etching technology to form a ridge structure, the problem of insufficient light constraint ability of waveguides in the prior art is solved, and higher sensitivity and smaller the optical mode field area.
Patent Information
- Application Number
- CN202410813100.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-23
- Publication Date
- 2024-11-01
AI Technical Summary
The existing integrated optical electric field sensors use diffusion waveguides to have weak constraining ability on light, resulting in increased sensitivity and bandwidth, and the long distance of the electrode leads to a large half-wave voltage and poor sensitivity.
The lithium niobate film spinal waveguide and its preparation method include forming a ridge-shaped raised film layer on the substrate and buffer layer, and coating photoresist, electron beam exposure and ionic etching on the lithium niobate film The etching technology forms a ridge waveguide, retaining part of the unetched area, removing the photoresist layer, and obtaining a lithium niobate film ridge waveguide.
The optical mode field area is significantly reduced, and the electro-optical modulation efficiency and sensitivity are improved. Compared with the bulk lithium niobate diffusion waveguide, the optical mode field size is reduced by two orders of magnitude, and the sensitivity is greatly improved.
Smart Images

Figure CN118884604A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optical electric field measurement, and in particular relates to a lithium niobate thin film ridge waveguide for an optical electric field sensor and a preparation method thereof. Background Art
[0002] Electric field measurement is an indispensable measurement indicator of the power system. As the energy Internet evolves towards digitalization, the demand for electric field sensors is developing towards high sensitivity and wide bandwidth.
[0003] Compared with traditional electric field sensors, integrated optical electric field sensors have the advantages of high spatial resolution, wide measurement range, and little interference with the original field. However, the diffuse waveguide currently used has weak light confinement ability, resulting in the need to improve its sensitivity and bandwidth.
[0004] Lithium niobate (LiNbO3, LN) is an optical material with excellent electro-optical properties. For decades, lithium niobate has been recognized as an ideal material for integrated optical electric field sensors due to its excellent linear electro-optical effect, large linear electro-optical coefficient and stable chemical properties.
[0005] However, since lithium niobate waveguides are difficult to etch, existing integrated optical electric field sensors are basically diffuse waveguides prepared by annealing proton exchange or titanium diffusion process. The refractive index distribution of this waveguide from the core to the cladding is basically gradual, the refractive index difference is small, and the ability to confine light is weak. In order to reduce the metal's absorption loss of light, the electrodes must be placed outside the light field as much as possible. Since the waveguide has a weak ability to confine light, the area of the light field distribution will be larger and the distance between the electrodes will be farther, resulting in a larger half-wave voltage of the sensor and poorer sensitivity. Summary of the invention
[0006] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.
[0007] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a lithium niobate thin film ridge waveguide for an optical electric field sensor and a preparation method thereof.
[0008] To solve the above technical problems, the present invention provides the following technical solutions: including, a lithium niobate thin film ridge waveguide for an optical electric field sensor, including, a composite layer, including a substrate, a buffer layer arranged on the substrate and a thin film layer arranged on the buffer layer; wherein, a ridge-shaped protrusion is arranged on the thin film layer.
[0009] As a preferred solution of the lithium niobate thin film ridge waveguide for optical electric field sensor described in the present invention, the material of the substrate is single crystal silicon, and the thickness of the substrate is 500 μm.
[0010] As a preferred solution of the lithium niobate thin film ridge waveguide for optical electric field sensor described in the present invention, the material of the buffer layer is silicon dioxide with a thickness of 2 μm.
[0011] As a preferred solution of the lithium niobate thin film ridge waveguide for optical electric field sensor described in the present invention, wherein: the thin film layer is lithium niobate with a thickness of 600 nm.
[0012] In order to solve the above technical problems, the present invention also provides the following technical solutions: a preparation method, comprising coating a photoresist on a lithium niobate film and performing a soft baking process to form a photoresist layer; performing electron beam exposure on the photoresist layer and then developing it; using plasma etching technology to partially etch the developed lithium niobate film, wherein the etching process does not completely penetrate the lithium niobate film to retain some unetched areas; removing the photoresist layer and cleaning it to obtain a lithium niobate film ridge waveguide.
[0013] As a preferred embodiment of the preparation method of the present invention, the lithium niobate film is divided into three layers, the top layer is an x-cut lithium niobate film layer with a thickness of 600nm, the middle layer is a silicon dioxide buffer layer with a thickness of 2μm, and the bottom layer is a silicon substrate with a thickness of 500μm.
[0014] As a preferred embodiment of the preparation method described in the present invention, the photoresist coating and soft baking treatment include: thermally cleaning the lithium niobate film, placing the sample on a hot plate at 130°C for 1 minute; spin coating the photoresist on the surface of the lithium niobate film; placing the lithium niobate film with the photoresist spin-coated on it into a coating machine for coating, and placing the coated lithium niobate film on a hot plate for pre-baking to solidify the photoresist.
[0015] As a preferred embodiment of the preparation method described in the present invention, the plasma etching step includes using argon as etching gas, the upper electrode of the etcher generates plasma, and the lower electrode forms an electric field perpendicular to the sample surface so that the plasma reacts with the surface of the lithium niobate film.
[0016] As a preferred embodiment of the preparation method described in the present invention, the cleaning step includes using a mixed solution of sulfuric acid and hydrogen peroxide to remove residual photoresist on the waveguide pattern of the lithium niobate film; using a mixed solution of hydrogen peroxide, ammonia water and water to remove heavy deposition on the surface of the sample, and further drying the lithium niobate film.
[0017] Beneficial effects of the present invention: Compared with bulk lithium titanium niobate diffused waveguides, the size of the waveguide optical mode field on the lithium niobate film is reduced by more than an order of magnitude. Fabricating a waveguide on the lithium niobate film can greatly reduce the optical mode field area, thereby improving the electro-optical modulation efficiency.
[0018] Compared with lithium niobate thin film titanium diffused waveguide, lithium niobate thin film ridge waveguide has greatly improved the refractive index difference, thereby greatly reducing the mode field diameter, and the optical mode field size is reduced by more than three times. Compared with the bulk lithium niobate titanium diffused waveguide, the optical mode field size of lithium niobate thin film ridge waveguide is reduced by two orders of magnitude; lithium niobate thin film ridge waveguide has the smallest optical mode field, and the use of lithium niobate thin film ridge waveguide can make the sensor have the greatest sensitivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0020] Figure 1 A structural comparison of the traditional diffuse waveguide (left) and the ridge waveguide (right).
[0021] Figure 2 Structural diagrams of (a) planar waveguide, (b) diffused waveguide, (c) rectangular waveguide, and (d) ridge waveguide.
[0022] Figure 3 Flow chart of the waveguide fabrication process using a photoresist mask.
[0023] Figure 4 A typical etch pattern of a ridge waveguide with photoresist as mask.
[0024] Figure 5 This is the structure diagram of the Mach-Zehnder intensity modulator.
[0025] Figure 6 This is a local etching diagram of the Mach-Zehnder intensity modulator structure.
[0026] Figure 7 Image of the grating structure made for the lithium niobate thin film ridge waveguide.
[0027] Figure 8 Waveguide morphology at different etching times.
[0028] Fig. 9 is the TE fundamental mode mode field diameter of the bulk lithium titanium niobate diffused waveguide.
[0029] Fig.10 is the TE fundamental mode mode field diameter of the lithium niobate thin film titanium diffused waveguide.
[0030] Fig.11 is the mode field diameter of the TE fundamental mode of the lithium niobate film ridge waveguide. DETAILED DESCRIPTION
[0031] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the accompanying drawings.
[0032] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0033] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0034] Unless otherwise specified, the raw materials used in the present invention are all commercially available in the art.
[0035] Example 1
[0036] The present invention provides a lithium niobate thin film ridge waveguide for an optical electric field sensor:
[0037] The composite layer comprises a substrate, a buffer layer arranged on the substrate and a film layer arranged on the buffer layer; wherein the film layer is provided with ridge-shaped protrusions.
[0038] Preferably, the material of the substrate is single crystal silicon, and the thickness of the substrate is 500 μm.
[0039] Preferably, the buffer layer is made of silicon dioxide with a thickness of 2 μm.
[0040] Preferably, the thin film layer is lithium niobate with a thickness of 600 nm.
[0041] Example 2
[0042] The present invention provides a method for preparing a lithium niobate thin film ridge waveguide of an optical electric field sensor:
[0043] coating a photoresist on the lithium niobate film and performing a soft baking process to form a photoresist layer;
[0044] electron beam exposure of the photoresist layer followed by development;
[0045] Partially etching the developed lithium niobate film using a plasma etching technique, wherein the etching process does not completely penetrate the lithium niobate film to retain a portion of the unetched area;
[0046] The photoresist layer is removed and cleaned to obtain a lithium niobate thin film ridge waveguide.
[0047] Preferably, the lithium niobate film is divided into three layers, the top layer is an x-cut lithium niobate film layer with a thickness of 600 nm, the middle layer is a silicon dioxide buffer layer with a thickness of 2 μm, and the bottom layer is a silicon substrate with a thickness of 500 μm.
[0048] Preferably, coating the photoresist and performing a soft baking treatment includes thermally cleaning the lithium niobate film, placing the sample on a hot plate at 130° C. for 1 minute; spin coating the photoresist on the surface of the lithium niobate film; placing the lithium niobate film with the spin-coated photoresist in a coating machine for coating, and placing the coated lithium niobate film on a hot plate for pre-baking to solidify the photoresist.
[0049] Preferably, the plasma etching step includes using argon as etching gas, the upper electrode of the etcher generates plasma, and the lower electrode forms an electric field perpendicular to the sample surface so that the plasma interacts with the surface of the lithium niobate film.
[0050] Preferably, the cleaning step includes using a mixed solution of sulfuric acid and hydrogen peroxide to remove residual photoresist on the lithium niobate film waveguide pattern; using a mixed solution of hydrogen peroxide, ammonia and water to remove heavy deposits on the sample surface, and further drying the lithium niobate film.
[0051] Compared with lithium niobate thin film titanium diffused waveguide, lithium niobate thin film ridge waveguide has greatly improved the refractive index difference, thereby greatly reducing the mode field diameter, and the optical mode field size is reduced by more than three times. Compared with the bulk lithium niobate titanium diffused waveguide, the optical mode field size of lithium niobate thin film ridge waveguide is reduced by two orders of magnitude; lithium niobate thin film ridge waveguide has the smallest optical mode field, and the use of lithium niobate thin film ridge waveguide can make the sensor have the greatest sensitivity.
[0052] In terms of sensitivity, the film field diameter is defined as the point where the field intensity drops to 1 / e of the maximum value. Because the smaller the optical film field, the greater the electric field difference per unit area, and under the same applied electric field, the larger the output signal, that is, the higher the sensitivity.
[0053] Compared with the bulk lithium niobate titanium diffused waveguide, the size of the waveguide optical mode field on the lithium niobate film is reduced by more than an order of magnitude. The reason is that on the one hand, the lithium niobate film itself is small in size, and the optical mode field is naturally small. On the other hand, the lithium niobate film can naturally form a large refractive index difference with the surrounding medium, and has a strong ability to bind light. The refractive index of the titanium diffusion area of the bulk lithium niobate titanium diffused waveguide changes slowly, and has a poor ability to bind light. The size of the optical mode field of the lithium niobate film ridge waveguide is more than three times smaller than that of the lithium niobate film titanium diffused waveguide. The reason is that the ridge waveguide can also form a large refractive index difference with the surrounding medium in the x-axis direction, which greatly reduces the mode field diameter in the x-axis direction, and naturally reduces the mode field area.
[0054] Example 3
[0055] Using simulation calculations, the mode field diameter is defined as the point where the field intensity drops to 1 / e of the maximum value. In order to simply calculate the mode field size, the points where the electric field maximum value decays to 1 / e along the two coordinate axes are found respectively.
[0056] Table 1
[0057]
[0058] See also Figure 9-11 It can be seen that the waveguide optical mode field size on the lithium niobate film is reduced by more than an order of magnitude compared to the bulk lithium niobate titanium diffused waveguide. The reason is that the lithium niobate film itself is small in size, so the optical mode field is naturally small. On the other hand, the lithium niobate film can naturally form a large refractive index difference with the surrounding medium, and has a strong ability to bind light. The refractive index of the titanium diffusion area of the bulk lithium niobate titanium diffused waveguide changes slowly, and has a poor ability to bind light.
[0059] The optical mode field size of the lithium niobate thin film ridge waveguide is more than three times smaller than that of the lithium niobate thin film titanium diffused waveguide. The reason is that the ridge waveguide can also form a large refractive index difference with the surrounding medium in the x-axis direction, which greatly reduces the mode field diameter in the x-axis direction, and naturally reduces the mode field area.
[0060] Example 4
[0061] The prepared lithium niobate thin film ridge waveguide is used in a typical Mach-Zehnder intensity modulator structure.
[0062] It mainly includes three parts: electrode, modulation voltage and optical waveguide. The optical waveguide is the application position of lithium niobate thin film ridge waveguide.
[0063] Example 5
[0064] The prepared lithium niobate thin film ridge waveguide is used to make a traditional grating structure.
[0065] Example 6
[0066] In different optical electric field sensors, ridge waveguides with inverted T-shaped, right T-shaped and other structures may be required.
[0067] See also Figure 7 During the etching process, under the bombardment of argon plasma, the molecules on the surface of the lithium niobate substrate will be blown away. Most of these blown-away molecules will be carried away by the argon gas flow, but the lithium niobate molecules near the mask are easily bombarded onto the mask and accumulated at the root of the mask to form lithium niobate heavy deposition. In the early stage of etching, the etching rate is relatively slow, and the heavy deposition will act as a mask to protect the waveguide from being etched. From the two pictures of etching for 3 minutes, it can be seen that due to the protection of the heavy deposition, the inclination angle of the waveguide side wall in the early stage of etching is only 20 to 30 degrees.
[0068] As etching proceeds, the etching rate increases, the speed of heavy deposition is lower than the speed of consumption, and the heavy deposition is not enough to serve as a mask on both sides of the waveguide, so the outermost part of the waveguide is exposed. This part of the waveguide is etched away faster, the steepness of the waveguide side wall increases, and the inclination angle of the waveguide side wall increases to about 45°.
[0069] As the etching rate reaches the maximum value and remains stable, the formation and consumption of heavy deposition also remain stable, and the sidewall steepness no longer increases. The final sidewall steepness is determined by the angle formed by the heavy deposition accumulation and the angle of the argon plasma bombarding the waveguide sidewall, and the sidewall roughness is determined by the roughness of the mask sidewall and the roughness inherited from the heavy deposition.
[0070] Therefore, by combining different etching times, waveguides with different sidewall inclinations can be obtained for optical electric field sensors with different performances.
[0071] Importantly, it should be noted that the construction and arrangement of the present application shown in a plurality of different exemplary embodiments are only exemplary. Although only a few embodiments are described in detail in this disclosure, it should be readily understood by those who refer to this disclosure that many modifications are possible (e.g., the size, scale, structure, shape and proportion of various elements, and parameter values (e.g., temperature, pressure, etc.), installation arrangement, use of materials, color, directional changes, etc.) without substantially departing from the novel teachings and advantages of the subject matter described in the application. For example, the element shown as integrally formed can be composed of multiple parts or elements, the position of the element can be inverted or otherwise changed, and the nature or number or position of the discrete element can be changed or changed. Therefore, all such modifications are intended to be included in the scope of the present invention. The order or sequence of any process or method steps can be changed or reordered according to alternative embodiments. In the claims, any "device plus function" clause is intended to cover the structure of performing the function described herein, and is not only structurally equivalent but also equivalent structure. Without departing from the scope of the present invention, other replacements, modifications, changes and omissions can be made in the design, operating conditions and arrangement of the exemplary embodiments. Therefore, the invention is not limited to a specific embodiment, but extends to numerous modifications still falling within the scope of the appended claims.
[0072] Additionally, in order to provide a concise description of exemplary embodiments, all features of an actual embodiment (ie, those features that are not relevant to the best mode presently contemplated for carrying out the invention or those that are not relevant to implementing the invention) may not be described.
[0073] It will be appreciated that in the development of any actual implementation, as in any engineering or design project, numerous implementation-specific decisions may be made. Such a development effort may be complex and time-consuming, but will be a routine task of design, fabrication, and production for those of ordinary skill having the benefit of this disclosure without undue experimentation.
[0074] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.
Claims
1. A lithium niobate thin film ridge waveguide for optical electric field sensor, characterized in that: include, A composite layer comprising a substrate, a buffer layer disposed on the substrate, and a thin film layer disposed on the buffer layer; Wherein, the film layer is provided with ridge-shaped protrusions.
2. The lithium niobate thin film ridge waveguide for optical electric field sensor according to claim 1, characterized in that: The substrate is made of single crystal silicon and has a thickness of 500 μm.
3. The lithium niobate thin film ridge waveguide for optical electric field sensor according to claim 2, characterized in that: The buffer layer is made of silicon dioxide with a thickness of 2 μm.
4. The lithium niobate thin film ridge waveguide for optical electric field sensor according to claim 3, characterized in that: The thin film layer is lithium niobate with a thickness of 600 nm.
5. The method for preparing a lithium niobate thin film ridge waveguide according to any one of claims 1 to 4, characterized in that: include, coating a photoresist on the lithium niobate film and performing a soft baking process to form a photoresist layer; electron beam exposure of the photoresist layer followed by development; Partially etching the developed lithium niobate film using a plasma etching technique, wherein the etching process does not completely penetrate the lithium niobate film to retain a portion of the unetched area; The photoresist layer is removed and cleaned to obtain a lithium niobate thin film ridge waveguide.
6. The preparation method according to claim 5, characterized in that: The lithium niobate film is divided into three layers, the top layer is an x-cut lithium niobate film layer with a thickness of 600nm, the middle layer is a silicon dioxide buffer layer with a thickness of 2μm, and the bottom layer is a silicon substrate with a thickness of 500μm.
7. The preparation method according to claim 5, characterized in that: The photoresist coating and soft baking process included thermal cleaning of the lithium niobate film and placing the sample on a hot plate at 130°C for 1 minute; Spin coating photoresist on the surface of lithium niobate film; The lithium niobate film with the spin-coated photoresist is placed in a coating machine for coating, and the coated lithium niobate film is placed on a hot plate for pre-baking to solidify the photoresist.
8. The preparation method according to claim 5, characterized in that: The plasma etching step includes using argon as etching gas, the upper electrode of the etcher generates plasma, and the lower electrode forms an electric field perpendicular to the sample surface so that the plasma acts on the surface of the lithium niobate film.
9. The preparation method according to claim 5, characterized in that: The cleaning step includes using a mixed solution of sulfuric acid and hydrogen peroxide to remove the residual photoresist on the waveguide pattern of the lithium niobate film; using a mixed solution of hydrogen peroxide, ammonia and water to remove heavy deposition on the surface of the sample, and further drying the lithium niobate film.