Method for improving infiltration of ion battery pole piece

Through pre-charging and discharging, pre-charging and three-time liquid injection methods, the problems of complex and poor infiltration of lithium-ion battery electrodes are solved, which improves the battery's wetting ability and production efficiency, simplifies the process and reduces costs.

CN118888992APending Publication Date: 2024-11-01VISION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410975642.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing lithium-ion battery electrode plate infiltration process is complicated, poor effect, low production efficiency and high cost.

Method used

The methods of pre-charge and discharge, pre-charge and three injections are adopted, including pre-charge and discharge after one injection, pre-charge after the second injection, and then three injections under vacuum conditions to improve the impregnation of the electrode by the electrolyte. sex.

Benefits of technology

The infiltration process is simplified, the time is shortened, the liquid retention capacity of the battery is improved, the production energy consumption is reduced, and the electrode wetting and the battery circulation performance is significantly improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a method for improving infiltration of an ion battery pole piece, which comprises the following steps: S01, performing primary liquid injection on a to-be-infiltrated ion battery, and then performing pre-charging and pre-discharging to obtain a pre-charging and pre-discharging ion battery; s02, performing secondary liquid injection on the pre-charge-discharge ion battery in the step S01, and then performing pre-charge to obtain a pre-charge ion battery; and S03, under a vacuum condition, performing third liquid injection on the pre-charged ion battery in the step S02 to obtain an infiltrated ion battery. The electrolyte infiltrates the electrode through high-temperature pre-charging and pre-discharging, normal-temperature pre-charging and three times of liquid injection, and the wettability of the electrolyte to the electrode can be effectively improved. According to the invention, the traditional long-time high-temperature shelving process is canceled, the operation is simple, the whole process can be controlled within 24 hours, the production efficiency is greatly improved, the production energy consumption is reduced, and the infiltration of the electrolyte on the pole piece can be greatly improved, so that the electrolyte retention capacity of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries, and in particular relates to a method for improving the wetting of ion battery pole pieces. Background Art

[0002] With the continuous development of the application field of lithium-ion batteries, people have higher and higher requirements for the volume energy density and capacity of batteries. Lithium-ion batteries mainly include positive electrodes, electrolytes, diaphragms and negative electrodes. Among them, energy generation and transmission are generally carried out in the electrode (positive and negative) area. Therefore, the performance of the electrode directly determines the performance of the battery. In order to improve the energy density of the battery, the compaction density of lithium battery pole pieces is getting higher and higher, and the larger compaction density will lead to a decrease in the porosity of the pole pieces, which makes it difficult for the electrolyte to infiltrate into the gaps in the pole pieces, and ultimately leads to a decrease in the wettability of the pole pieces and a decrease in the overall liquid retention of the battery. If the wettability of the pole piece is poor, the electrode polarization internal resistance of the battery will increase during the charge and discharge process, the risk of lithium precipitation will increase, the energy efficiency will decrease, and the battery cycle performance will be poor due to insufficient electrolyte.

[0003] Patent application CN109065826A discloses a method for impregnating a high-capacity and high-pressure negative-electrode lithium-ion battery. Based on high-temperature infiltration, the application uses a total of six stages of vacuum injection, high-temperature storage, pre-formation, high-temperature storage, secondary injection and sealing, and subsequent formation to infiltrate the battery. The infiltration process is complicated and time-consuming, which greatly reduces production efficiency.

[0004] Patent application CN110649265A discloses a hollow conductive microsphere material that can provide electrolyte storage space for the pole piece, improve battery capacity and cycle performance. However, the hollow conductive microsphere material used in this application is only in point contact with the active material in the pole piece, which cannot prevent the problem of conductive network destruction caused by gaps caused by pole piece expansion, and there are also problems such as high production costs. In addition, there are also methods of optimizing the electrolyte to improve the wettability of the electrode, such as adding electrolyte additives, selecting solvents with lower viscosity, or reducing the concentration of lithium salts. Although these methods can improve the wettability of the electrode to a certain extent, the room for improvement is always limited. Summary of the invention

[0005] The embodiment of the present invention provides a method for improving the wetting of an ion battery pole piece, aiming to solve the problems of the existing ion battery wetting process being complicated, poor wetting effect, low production efficiency, and high wetting cost.

[0006] In order to achieve the above object, an embodiment of the present invention provides a method for improving the wetting of an ion battery electrode, comprising the following steps:

[0007] S01, pre-charging and discharging the ion battery to be impregnated after once injecting liquid to obtain a pre-charged and discharged ion battery;

[0008] S02, pre-charging the pre-charged ion battery in step S01 after secondary injection to obtain a pre-charged ion battery;

[0009] S03, under vacuum conditions, inject liquid three times into the pre-charged ion battery in step S02 to obtain a soaked ion battery.

[0010] As a preferred embodiment, in step S01,

[0011] The ion battery to be impregnated is a square lithium-ion battery.

[0012] The total injection volume of the ion battery to be infiltrated is greater than or equal to 1.4 times the capacity of the ion battery to be infiltrated.

[0013] The injection volume of the one-time injection is 70% to 80% of the total injection volume. During the one-time injection, vacuum injection is not required.

[0014] The pre-charge and discharge are achieved by the following method: first charge at 0.01C to 0.1C to 2.5V to 2.8V, and then discharge at 0.01C to 0.05C to 2.5V; the discharge current is smaller than the charge current.

[0015] The temperature of the pre-charge and discharge is 35° C. to 50° C.; the pressure of the pre-charge and discharge is -0.8 MPa to -0.9 MPa.

[0016] The voltage of the pre-charged and discharged ion battery is 2.5V to 2.8V.

[0017] As a preferred embodiment, in step S02,

[0018] The injection volume of the secondary injection is 10% to 15% of the total injection volume. During the secondary injection, vacuum injection is not required.

[0019] The pre-charging temperature is 20°C to 30°C; the pre-charging current is 0.05C to 0.2C; and the pre-charging and discharging pressure is -0.8Mpa to -0.9Mpa.

[0020] The pre-charging is achieved by the following method: first charging to 2.8V to 3.0V at 0.05C to 0.1C, then charging to 3.2V at 0.1C to 0.2C, and finally charging to 3.3V to 3.5V at 0.15C to 0.2C.

[0021] The pre-charging is achieved by the following method: first charging to 2.8V to 3.0V at 0.05C to 0.1C, and then charging to 3.3V to 3.5V at 0.1C to 0.2C.

[0022] The charging capacity of the pre-charged ion battery is 30% to 80% of the total capacity of the ion battery to be infiltrated; the voltage of the pre-charged ion battery is 3.0V to 3.5V.

[0023] As a preferred implementation, in step S03,

[0024] The vacuum condition is achieved by vacuuming 2 to 3 times.

[0025] The injection amount of the three injections is 5% to 20% of the total injection amount. During the three injections, vacuum injection is required.

[0026] The method for improving the wettability of the ion battery pole piece is carried out in an environment with a humidity of 0% to 5%.

[0027] Compared with the prior art, the present invention has the following advantages:

[0028] This application realizes the infiltration of the electrolyte into the electrode through high-temperature pre-charge and discharge, room-temperature pre-charge and three injections, which can effectively improve the wettability of the electrolyte into the electrode. Compared with the traditional long-term high-temperature storage process of 48 to 64 hours, this application cancels the traditional long-term high-temperature storage process, is simple to operate, and the entire process can be controlled within 24 hours, which greatly improves production efficiency, reduces production energy consumption, and can significantly improve the infiltration of the electrolyte into the electrode, thereby increasing the battery's liquid retention. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back, top, bottom...), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.

[0031] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0032] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be an intermediate element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be an intermediate element at the same time.

[0033] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or suggesting their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0034] In the embodiments of the present application, the dosage of each component and the specific ingredients of each component can be selected and matched according to actual needs, and the solution of the present application can be implemented as long as it is within the dosage range and ingredient requirements required above.

[0035] Specifically, the embodiment of the present application provides a method for improving the wettability of an ion battery electrode, comprising the following steps:

[0036] S01, pre-charging and discharging the ion battery to be impregnated after once injecting liquid to obtain a pre-charged and discharged ion battery;

[0037] S02, pre-charging the pre-charged ion battery in step S01 after secondary injection to obtain a pre-charged ion battery;

[0038] S03, under vacuum conditions (the vacuum degree can be set according to actual needs, as long as there is a vacuum degree), the pre-charged ion battery of step S02 is injected with liquid three times to obtain an impregnated ion battery.

[0039] As a preferred embodiment, in step S01,

[0040] The ion battery to be impregnated is a square lithium-ion battery.

[0041] The square lithium-ion battery is one of a lithium cobalt oxide (LCO) battery, a lithium manganese oxide (LMO) battery, a lithium iron phosphate (LFP) battery, a ternary lithium battery or a polymer lithium-ion battery. The type of square lithium-ion battery can be selected according to actual needs.

[0042] The total injection volume of the ion battery to be infiltrated is greater than or equal to 1.4 times the capacity of the ion battery to be infiltrated.

[0043] The injection volume of the one-time injection is 70% to 80% of the total injection volume (depending on the actual use requirements, it can be 70%, or 75%, or 80%, etc.). During the one-time injection, there is no need to use vacuum injection. By controlling the injection volume of the one-time injection, the polarization of the electrode during the pre-charge and discharge of the ion battery can be reduced as much as possible.

[0044] The pre-charge and discharge are achieved by the following method: first charge at 0.01C~0.1C (depending on the actual use needs, it can be 0.01C, or 0.05C, or 0.1C, etc.) to 2.5V~2.8V (depending on the actual use needs, it can be 2.5V, or 2.6V, or 2.8V, etc.), and then discharge at 0.01C~0.05C (depending on the actual use needs, it can be 0.01C, or 0.03C, or 0.05C, etc.) to 2.5V; the discharge current is less than the charging current.

[0045] The pre-charge and discharge temperature is 35°C to 50°C (depending on the actual use requirements, it can be 35°C, 45°C, 50°C, etc.); the pre-charge and discharge pressure is -0.8Mpa to -0.9Mpa (depending on the actual use requirements, it can be -0.8Mpa, -0.85Mpa, -0.9Mpa, etc.). By controlling the pre-charge and discharge temperature and pressure, the infiltration of the electrolyte into the electrode can be effectively accelerated, and the polarization of the current to the electrode can be effectively reduced.

[0046] The voltage of the pre-charged and discharged ion battery is 2.5V to 2.8V (depending on actual use requirements, it can be 2.5V, or 2.6V, or 2.8V, etc.).

[0047] During the charging process of the ion battery, the metal ions will bring the solvent molecules close to the negative electrode. Conversely, during the discharge process, the metal ions will escape from the negative electrode and return to the positive electrode. Therefore, through pre-charging and discharging, the wettability of the electrolyte to the electrode can be effectively improved, so that after the pre-charging and discharging is completed, the secondary injection can be carried out directly without high temperature storage.

[0048] As a preferred embodiment, in step S02,

[0049] The injection volume of the secondary injection is 10% to 15% of the total injection volume (depending on actual use requirements, it can be 10%, or 12%, or 15%, etc.) During the secondary injection, vacuum injection is not required.

[0050] The pre-charging temperature is 20℃~30℃ (depending on the actual use requirements, it can be 20℃, 25℃, 30℃, etc.); the pre-charging current is 0.05C~0.2C (depending on the actual use requirements, it can be 0.05C, 0.1C, 0.2C, etc.); the pre-charging and discharging pressure is -0.8Mpa~-0.9Mpa (depending on the actual use requirements, it can be -0.8Mpa, -0.85Mpa, -0.9Mpa, etc.).

[0051] The pre-charging is achieved by the following method: first charge to 2.8V-3.0V at 0.05C-0.1C, then charge to 3.2V at 0.1C-0.2C, and finally charge to 3.3V-3.5V at 0.15C-0.2C (depending on actual use needs, it can be 3.3V, 3.45V, 3.5V, etc.).

[0052] The pre-charging is achieved by the following method: first charging to 2.8V-3.0V at 0.05C-0.1C, and then charging to 3.3V-3.5V at 0.1C-0.2C (depending on actual use requirements, it can be 3.3V, or 3.45V, or 3.5V, etc.).

[0053] The pre-charging current adopts 2 to 3 gradients and controls the current size of each gradient for charging, which can effectively promote the formation of a stable SEI film at the negative electrode.

[0054] The charging capacity of the pre-charged ion battery is 30% to 80% of the total capacity of the ion battery to be impregnated (depending on actual use needs, it can be 30%, 55%, 80%, etc.); the voltage of the pre-charged ion battery is 3.0V to 3.5V (depending on actual use needs, it can be 3.0V, 3.3V, 3.5V, etc.).

[0055] As a preferred implementation, in step S03,

[0056] The vacuum condition is achieved by vacuuming 2 to 3 times (depending on actual use requirements, it can be 2 times, or 3 times, etc.).

[0057] The injection volume of the three injections is 5% to 20% of the total injection volume (5%, 15%, 20%, etc., depending on actual use needs). During the three injections, vacuum injection is required to ensure that the gas inside the battery can be completely discharged.

[0058] The method for improving the wettability of the ion battery pole piece is carried out in an environment with a humidity of 0% to 5% (depending on the actual use requirements, it can be 1%, 2%, 5%, etc.). The wetted battery obtained can be directly sealed by the method of the present application.

[0059] Example 1

[0060] A method for improving the wettability of an ion battery electrode comprises the following steps:

[0061] S01, pre-charging and discharging the ion battery to be impregnated after once injecting liquid to obtain a pre-charged and discharged ion battery;

[0062] S02, pre-charging the pre-charged and discharged ion battery in step S01 after secondary injection to obtain a pre-charged ion battery;

[0063] S03, under vacuum conditions, injecting liquid three times into the pre-charged ion battery in step S02 to obtain a soaked ion battery.

[0064] In step S01,

[0065] The ion battery to be impregnated is a 100Ah square lithium iron phosphate battery, and the total liquid injection volume of the battery is 413g.

[0066] The total injection volume of the ion battery to be infiltrated is greater than or equal to 1.4 times the capacity of the ion battery to be infiltrated.

[0067] The injection amount of the one-time injection is 290 g. During the one-time injection, there is no need to use vacuum injection.

[0068] The pre-charge and discharge (pre-charge and discharge are repeated 3 times) are achieved by the following method: first charge to 2.8V at 0.02C constant current, and then discharge to 2.5V at 0.01C constant current; the discharge current is smaller than the charging current.

[0069] The temperature of the pre-charge and discharge is 40±2°C; the pressure of the pre-charge and discharge is -0.8Mpa.

[0070] In step S02,

[0071] The injection amount of the secondary injection is 50g. During the secondary injection, there is no need to use vacuum injection.

[0072] The pre-charging temperature is 25° C., which is a normal temperature; and the pre-charging and discharging pressure is -0.85 MPa.

[0073] The pre-charging is achieved by the following method: first charging to 2.8V at 0.05C, then charging to 3.2V at 0.1C, and finally charging to 3.3V at 0.15C.

[0074] In step S03,

[0075] The vacuum condition is achieved by evacuating the air twice.

[0076] The injection amount of the three injections is 73 g. During the three injections, vacuum injection is required.

[0077] The method for improving the wettability of the ion battery pole piece is carried out in an environment with a humidity of 2%.

[0078] Example 2

[0079] A method for improving the wettability of an ion battery electrode comprises the following steps:

[0080] S01, pre-charging and discharging the ion battery to be impregnated after once injecting liquid to obtain a pre-charged and discharged ion battery;

[0081] S02, pre-charging the pre-charged ion battery in step S01 after secondary injection to obtain a pre-charged ion battery;

[0082] S03, under vacuum conditions, inject liquid three times into the pre-charged ion battery in step S02 to obtain a soaked ion battery.

[0083] In step S01,

[0084] The ion battery to be impregnated is a 100Ah square lithium iron phosphate battery, and the total injection volume of the battery is 420g. The injection volume of the first injection is 336g.

[0085] The pre-charge and discharge (pre-charge and discharge are repeated 3 times) are achieved by the following method: first charge to 2.8V at 0.015C constant current, and then discharge to 2.5V at 0.01C constant current; the discharge current is smaller than the charging current.

[0086] The temperature of the pre-charge and discharge is 45±2°C; the pressure of the pre-charge and discharge is -0.8Mpa.

[0087] In step S02,

[0088] The injection amount of the secondary injection is 50g. During the secondary injection, there is no need to use vacuum injection.

[0089] The pre-charging temperature is 25° C., which is a normal temperature; and the pre-charging and discharging pressure is -0.85 MPa.

[0090] The pre-charging is achieved by the following method: first charging to 2.8V at 0.05C, then charging to 3.2V at 0.1C, and finally charging to 3.3V at 0.2C.

[0091] In step S03,

[0092] The vacuum condition was achieved by evacuating the air three times.

[0093] The injection amount of the three injections is 34 g. During the three injections, vacuum injection is required.

[0094] The method for improving the wettability of the ion battery pole piece is carried out in an environment with a humidity of 5%.

[0095] Example 3

[0096] A method for improving the wettability of an ion battery electrode comprises the following steps:

[0097] S01, pre-charging and discharging the ion battery to be impregnated after once injecting liquid to obtain a pre-charged and discharged ion battery;

[0098] S02, pre-charging the pre-charged ion battery in step S01 after secondary injection to obtain a pre-charged ion battery;

[0099] S03, under vacuum conditions, inject liquid three times into the pre-charged ion battery in step S02 to obtain a soaked ion battery.

[0100] In step S01,

[0101] The ion battery to be impregnated is a 100Ah square lithium iron phosphate battery, and the total injection volume of the battery is 450g. The injection volume of the first injection is 315g. During the first injection, vacuum injection is not required.

[0102] The pre-charge and discharge (pre-charge and discharge are repeated twice) are achieved by the following method: first charge to 2.6V at a constant current of 0.012C, and then discharge to 2.5V at a constant current of 0.01C; the discharge current is smaller than the charge current.

[0103] The temperature of the pre-charge and discharge is 45±2°C; the pressure of the pre-charge and discharge is -0.85Mpa.

[0104] In step S02,

[0105] The injection amount of the secondary injection is 60g. During the secondary injection, vacuum injection is not required.

[0106] The pre-charging temperature is 25° C., which is a normal temperature; and the pre-charging and discharging pressure is -0.85 MPa.

[0107] The pre-charging is achieved by the following method: first charging to 3.0V at 0.1C constant current, and then charging to 3.3V at 0.2C constant current.

[0108] In step S03,

[0109] The vacuum condition was achieved by evacuating the air three times.

[0110] The injection amount of the three injections is 75g. During the three injections, vacuum injection is required.

[0111] The method for improving the wettability of the ion battery pole piece is carried out in an environment with a humidity of 3%.

[0112] In the description of this specification, the description with reference to the terms "an embodiment", "example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example.

[0113] In addition, it should be understood that although this specification is described according to implementation methods, not every implementation method contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.

[0114] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for improving the wettability of an ion battery electrode, characterized in that: The steps include: S01, pre-charging and discharging the ion battery to be impregnated after once injecting liquid to obtain a pre-charged and discharged ion battery; S02, pre-charging the pre-charged and discharged ion battery in step S01 after secondary injection to obtain a pre-charged ion battery; S03, under vacuum conditions, injecting liquid three times into the pre-charged ion battery in step S02 to obtain a soaked ion battery.

2. The method for improving the wettability of an ion battery pole piece according to claim 1, characterized in that: In step S01, the ion battery to be soaked is a square lithium-ion battery.

3. The method for improving the wettability of an ion battery pole piece according to claim 1, characterized in that: In step S01, the total injection volume of the ion battery to be infiltrated is greater than or equal to 1.4 times the capacity of the ion battery to be infiltrated.

4. The method for improving the wettability of an ion battery pole piece according to claim 1, characterized in that: In step S01, the injection volume of the single injection is 70% to 80% of the total injection volume; The pre-charge and discharge are achieved by the following method: first charge at 0.01C to 0.1C to 2.5V to 2.8V, and then discharge at 0.01C to 0.05C to 2.5V; the discharge current is smaller than the charge current.

5. The method for improving the wettability of an ion battery pole piece according to claim 1, characterized in that: In step S01, the pre-charge and discharge temperature is 35°C to 50°C; the pre-charge and discharge pressure is -0.8Mpa to -0.9Mpa; The voltage of the pre-charged and discharged ion battery is 2.5V to 2.8V.

6. The method for improving the wettability of an ion battery pole piece according to claim 1, characterized in that: In step S02, the injection volume of the secondary injection is 10% to 15% of the total injection volume; The pre-charging temperature is 20°C to 30°C; the pre-charging current is 0.05C to 0.2C; and the pre-charging and discharging pressure is -0.8Mpa to -0.9Mpa.

7. The method for improving the wettability of an ion battery pole piece according to claim 1, characterized in that: In step S02, the pre-charging is achieved by the following method: first charging at 0.05C to 0.1C to 2.8V to 3.0V, then charging at 0.1C to 0.2C to 3.2V, and finally charging at 0.15C to 0.2C to 3.3V to 3.5V.

8. The method for improving the wettability of an ion battery pole piece according to claim 1, characterized in that: In step S02, the pre-charging is achieved by the following method: first charging at 0.05C to 0.1C to 2.8V to 3.0V, and then charging at 0.1C to 0.2C to 3.3V to 3.5V.

9. The method for improving the wettability of an ion battery pole piece according to claim 1, characterized in that: In step S02, the charging capacity of the pre-charged ion battery is 30% to 80% of the total capacity of the ion battery to be infiltrated; and the voltage of the pre-charged ion battery is 3.0V to 3.5V.

10. The method for improving the wettability of an ion battery pole piece according to claim 1, characterized in that: In step S03, the vacuum condition is achieved by vacuuming 2 to 3 times; the injection volume of the three injections is 5% to 20% of the total injection volume; The method for improving the wettability of the ion battery pole piece is carried out in an environment with a humidity of 0% to 5%.