Electrochemical process for recovering platinum group metals (PGM) from solid residues
By using an electrochemical method of using a low eutectic solvent and aqueous chloride solution in a single reactor, selective recovery of platinum group metals from solid residues is achieved, and the problems of low recovery and high cost in the prior art are solved, which is suitable for industrialization application.
Patent Information
- Application Number
- CN202380024745.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-08
- Filing Date
- 2023-03-07
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art is difficult to effectively recover platinum group metals (PGM) from solid residues, especially failed automotive catalysts, and the recovery rate is low, unable to meet European needs, and there are environmental and economic costs problems.
Electric leaching and electrodeposition in a single reactor using eutectic solvent (DES) and aqueous chloride ions-containing solution. Selective recovery of PGM is achieved through the combination of hydrogen bond acceptor and hydrogen bond donor, and the main impurities are left in In solution or solid, avoid co-deposition.
It improves the recovery rate and selectivity of PGM, reduces costs, is suitable for industrial-scale applications, and is carried out under mild conditions, without the need for external oxidants, simplifies the process, and is suitable for recycling of Pd, Pt and Rh from failed automotive catalysts.
Smart Images

Figure CN118891400A_ABST
Abstract
Description
[0001] This application claims the benefit of European patent application EP22382212.3 filed on March 3, 2022. Technical Field
[0002] The present invention relates to the field of recovery of metals from solid residues. More particularly, the present invention relates to an electrochemical process for recovery of platinum group metals (PGMs) from solid residues such as spent automobile catalysts. Background Art
[0003] Platinum Group Metals (PGMs), namely platinum (Pt), palladium (Pd), ruthenium (Ru), rhodium (Rh), iridium (Ir) and osmium (Os), are classified as critical raw materials (CRMs) by the European Commission (EC). PGMs are used in a wide range of industrial applications and often have no substitutes.
[0004] The main use of PGM is in the automotive, chemical manufacturing and petroleum refining industries due to its catalytic properties. The PGM market was in deficit in 2019 and its prices hit a record high in 2020. In this context, Europe is the world's largest consumer of PGM for industrial applications, with roughly constant demand each year, especially for the preparation of automotive catalysts. However, in the EU, the main production of PGM is negligible, with about 84% of the main supply coming from South Africa and Russia, two countries with suboptimal geopolitical stability.
[0005] It is estimated that the recycling input rate for end-of-life (EOL) products containing PGMs in Europe is only 14%, which is far from enough to meet the EU demand.
[0006] Therefore, there is still huge untapped potential in improving the above recovery percentages, especially by increasing current recovery rates. EOL products containing PGMs, such as spent automotive catalysts, are considered promising platinum group metal (PGM) resources. These secondary resources of PGMs contain PGM concentrations much higher than their corresponding ores. Recycling EOL products containing PGMs has attractive advantages, especially in terms of protecting primary resource reserves and reducing negative environmental impacts caused by mining.
[0007] PCT application WO2008155464 generally describes a method for recovering metals from a spent catalyst composition comprising organic contaminants on a catalyst support and a catalytically active metal. In the method, leaching of metallic cobalt, nickel, molybdenum, rhenium or a precious metal from the spent catalyst composition is achieved by adding an ionic liquid comprising an ammonium compound and a hydrogen bond donor capable of forming hydrogen bonds with the ammonium compound.
[0008] Therefore, there is still a need to find an environmentally friendly, low-cost and efficient method for recovering PGMs from solid residues, especially from spent automotive catalysts, and to overcome the problems of the prior art. SUMMARY OF THE INVENTION
[0010] The present invention has developed an electrochemical process for the recovery of platinum group metals (PGMs), in particular Pd, Pt and Rh, from solid residues, such as from end-of-life (EOL) products containing PGMs, in particular from spent automotive catalysts, in one single reactor, using a specific electrolyte comprising a deep eutectic solvent (DES). Advantageously, the process allows the simultaneous recovery of PGMs via their selective electrodeposition, while the main metallic impurities remain in solution, thus limiting the co-deposition of impurities with the recovered PGMs. Thus, the present invention provides a versatile and efficient process for the recovery of PGMs from solid residues, which is compact in design and easily automated.
[0011] The present invention therefore relates to an electrochemical process for recovering platinum group metals (PGMs) from a solid residue containing platinum group metals (PGMs), the process comprising the following steps:
[0012] a) electro-leaching the solid residue to leach PGM from the solid residue and simultaneously electrodepositing the leached PGM to a cathode; wherein the electro-leaching and the electrodeposition are performed in an electrolyte comprising a deep eutectic solvent (DES) and an aqueous solution containing chloride ions and having a pH value of <7; and
[0013] b) recovering the electrodeposited PGM;
[0014] DES is composed of a mixture of the following substances:
[0015] (i) a hydrogen bond acceptor (HBA) compound (A) which is choline chloride; and
[0016] (ii) a hydrogen bond donor (HBD) compound (B) selected from (C 1 To C 12 ) alcohol, (C 1 To C 12 )aldehyde, (C 1 To C 18 ) carboxylic acid, (C 1 To C 6 )urea, (C 1 To C 12 )amide, (C 1 To C 12 ) nitrogen-containing compounds, (C 1 To C 12 ) amino acids and (C 1 To C 12 )sugar;
[0017] The molar ratio of (A) to (B) is 1:10 to 10:1.
[0018] Although the use of some DES for the recovery of PGMs contained in some solid residues such as spent automobile catalysts by leaching is known, the use of DES in combination with an aqueous solution of chloride ions at pH < 7 (such as aqueous NaCl solution in the presence of HCl) for simultaneous electro-leaching and electrodeposition of PGMs from such residues has not been suggested.
[0019] The combination of electro-leaching and electrodeposition under the conditions defined above allows the recovery of platinum group metals (PGMs) in a single reactor. Surprisingly, as shown in the examples, this method allows a selective and increased recovery of PGMs contained in the solid residue compared to the methods of the prior art, in particular compared to the conventional methods using DES leaching.
[0020] The solid residue containing PGMs contains other metallic impurities such as Al, Fe, La, Ce, Pb and Nd. The process of the present invention allows recovery of the electrodeposited PGMs, while other metallic impurities such as Al, Fe, La, Ce and Nd either remain in the solid residue or remain in the solution after electroleaching.
[0021] Another advantage of the process of the invention is that it can be carried out under very mild conditions, in particular using a mixture of DES and aqueous NaCl solution with HCl as an additive. DES can be prepared from naturally occurring precursors, and the aqueous NaCl solution required to form the electrolyte mixture can be obtained from seawater, which has advantages in terms of availability and cost.
[0022] Importantly, by performing the electroleaching step, strong oxidants such as hydroxyl radicals (·OH), hydrogen peroxide (H 2 O 2 ) or both, so that no external oxidant such as H is added 2 O 2 or concentrated strong acid.
[0023] All these features make this method particularly suitable for use on an industrial scale.
[0024] BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The mechanism of direct recovery of PGM from solid residue (R) in a single electrochemical reactor according to the method of the present invention is shown. A: anode; K: cathode.
[0026] Figure 2The flow chart of the electroleaching experiment is shown, including the leaching and polarization steps. a) Electroleaching as in Example 1 (choline chloride (ChCl) / formic acid DES solution + HCl + NaCl aqueous solution (0.5M), 64 mA / cm 2 ; t=3; WE=boron-doped diamond (BDD); G: PGM deposited on graphite; L: leached; b) switched polarization, aqueous NaCl solution (0.5 M) (1 V; ~30 min; WE=graphite), i: initial, f: final; c) first filtration (5 μm pores), P 1 : The first filtered precipitate, L 1 : First extract; d) Second filtration (0.45 μm pores), L 2 : The second extract, P 2 : Filtered precipitate.
[0027] Figure 3 Shown is a chronoamperometric test (current (mA) versus time (min)) with 1 V applied; after 5 minutes, the current drops to almost zero, a sign of PGM detachment. DETAILED DESCRIPTION OF THE INVENTION
[0029] Unless otherwise specified, all terms used in this application should be understood to have the common meaning known in the art. Other more specific definitions of specific terms used in this application are described below and are intended to be uniformly applied throughout the specification and claims, unless a definition explicitly listed otherwise provides a broader definition.
[0030] The term "platinum group metals (PGM)" refers to the group of platinum (Pt), palladium (Pd), ruthenium (Ru), rhodium (Rh), iridium (Ir) and osmium (Os). For the purposes of the present invention, Pd, Pt and Rh are of particular interest. For example, these three platinum group metals are present in spent catalysts.
[0031] As used herein, the term "electroleaching" refers to the process of separating or extracting a solute (in the context of the present invention, a PGM as defined above) from a solid initial product by a solvent (in the context of the present invention, a specific DES as defined herein), wherein a chemical reaction on the target substance is carried out by electrons in an electrochemical reaction. Specifically, a chemical reagent such as an oxidant can be generated at an electrode.
[0032] As used herein, the term "leachate" refers to the liquid containing the extracted or leached metals originally contained in the solid starting product.
[0033] As used herein, the term "electrodeposition" refers to a process in which metal ions present in an electrolyte are reduced at a cathode to form a metal deposit.
[0034] As used herein, the term "room temperature" refers to a temperature of 15°C to 35°C, specifically a temperature of 20°C to 25°C.
[0035] As used herein, the term "wt%" (weight percent) of a component refers to the amount of a single component relative to the total weight of the composition, or, if specifically mentioned, relative to the amount of another component.
[0036] The term "about" or "approximately" as used herein refers to a numerical range of ±10% of a particular value. For example, the expression "about 10" or "approximately 10" includes ±10% of 10, i.e., 9 to 11.
[0037] As used herein, when there is no quantifier before an element, it means "at least one" or "one or more than one". Unless otherwise specified, "said" and "the" used in this document also include "more than one".
[0038] As described above, the present invention relates to an electrochemical process for recovering platinum group metals (PGMs) from a PGM-containing solid residue by subjecting the solid residue to simultaneous electroleaching and electrodeposition processes in a single reactor using an electrolyte comprising a specific deep eutectic solvent (DES) and an aqueous solution containing chloride ions and having a pH <7.
[0039] The solid residue containing PGMs is typically an EOL product containing PGMs. For the purpose of the present invention, the term "end-of-life" (EOL) product refers to a product containing PGMs, especially PGMs in the form of metals, oxides or alloys, which have reached the end of their life cycle.
[0040] Therefore, in an embodiment of the method of the present invention, the solid residue containing PGMs can be a secondary source of PGMs, especially Pd, Pt and Rh, to be recovered and recycled, such as spent automobile catalysts, tailings, electronic waste, waste membrane residues, catalytic converters, spent petroleum refining catalysts, spent proton exchange membrane fuel cells (PEMFCs), spent catalysts used in the chemical industry, and any other EOL materials containing PGMs. Specifically, the solid residue containing PGMs is a spent automobile catalyst and a waste membrane residue containing Pd. Preferably, the solid residue containing PGMs is in the form of a powder obtained by a conventional grinding process.
[0041] The terms "vehicle catalyst," "autocatalyst," "automotive catalytic converter," "vehicle catalytic converter (VCC)," or simply "converter" are used interchangeably herein.
[0042] In another embodiment, optionally in combination with one or more features of the various embodiments described above and below, the aqueous solution containing chloride ions is an aqueous solution comprising water-soluble chloride salts such as KCl and NaCl. 2 SO4 ), hydrochloric acid (HCl) and nitric acid (HNO 3 ), more specifically HCl, a pH < 7, ie an acidic medium, can be obtained.
[0043] In another embodiment, optionally in combination with one or more features of the various embodiments described above and below, the acid is added in a weight ratio of solid residue to inorganic acid of 1:0.5 to 1:2, in particular about 1:1. Specifically, the inorganic acid is added in the form of an aqueous solution with a concentration of 1M to 4M, for example 2M.
[0044] In another embodiment, optionally in combination with one or more features of the various embodiments described above and below, the aqueous solution containing chloride ions and pH <7 is a mixture of water and HCl as an additive, wherein the water contains NaCl in a concentration of 0M to 2.5M, and the HCl as an additive is, for example, HCl in the form of an aqueous solution. In a specific embodiment, the aqueous solution containing chloride ions and pH <7 is water in the presence of HCl as an additive, for example, in the form of an aqueous solution. In another specific embodiment, the aqueous solution containing chloride ions and pH <7 is an aqueous NaCl solution in the presence of HCl as an additive, for example, in the form of an aqueous solution. In particular, the concentration of NaCl in the aqueous solution is 0.3M to 2.5M, or 0.5M to 2.0M, or 0.5M to 1.5M, or 0.5M to 1M, for example 0.5M or 0.6M.
[0045] In another embodiment, optionally in combination with one or more features of the various embodiments described above and below, the amount of DES is 75% to 90% by weight, in particular 80% by weight, relative to the total weight of DES and water, optionally containing NaCl. In particular, the water contains NaCl in a concentration of 0.3M to 0.6M. In an example, the concentration of the NaCl aqueous solution is 0.5M, and the amount of DES is 80% by weight relative to the total weight of the DES and NaCl aqueous solution. More specifically, seawater can be used as the aqueous solution of NaCl.
[0046] In another embodiment, optionally in combination with one or more features of the various embodiments described above and below, the weight ratio of solid residue to electrolyte is 1:5 to 1:15, specifically 1:5, 1:9, 1:10 or 1:15, more specifically 1:9.
[0047] The electrochemical method of the present invention can be carried out in a reactor comprising a working electrode, a counter electrode and a reference electrode.
[0048] In an embodiment, optionally in combination with one or more features of the various embodiments described above and below, the simultaneous electro-leaching and electro-deposition process (step a) is carried out in a reactor comprising a counter electrode, such as a carbon-based or metal-based material, carbon paper or nickel plate, in particular a graphite plate; a reference electrode such as an Ag / AgCl electrode, a calomel electrode or a hydrogen reference electrode, in particular Ag / AgCl; and a working electrode selected from boron-doped diamond (BDD) and boron-doped reduced graphene oxide-based graphite (BRGO). Advantageously, BDD and BRGO are non-sacrificial anodes, unlike the sacrificial anodes used in prior art methods.
[0049] The simultaneous electroleaching and electrodeposition in step a) can be achieved by applying an electric potential or a current density. The applied electric potential can be adjusted to obtain the desired current density and leaching efficiency. Specifically, a potential of 2.5V to 3V, more specifically 2.5V to 3V, can be applied, or alternatively, 45mA / cm 2 Up to 64mA / cm 2 , for example 64mA / cm 2 of current density.
[0050] For this purpose, the three-electrode device can be electrically connected to a voltage or current supply, such as a potentiostat, which can be used in a potentiostatic mode or a galvanostatic mode.
[0051] Applying a potential or current density to a three-electrode device using the electrolyte causes water and chloride ions contained in the electrolyte to undergo an oxidation reaction and form several strong oxidants such as hydroxyl radicals (·OH), hydrogen peroxide (H 2 O 2 ) and Cl 2 .
[0052] Advantageously, the process of the present invention can be carried out directly using the PGM residue without adding any additional PGM salts or any external oxidizing agents.
[0053] The reaction can be carried out at a temperature significantly below 100° C., in particular at a temperature between 20° C. and 100° C., for example 80° C. This therefore represents an advantage over other prior art methods for recovering PGMs from solid residues by DES leaching, or by electroleaching and electrodeposition in other electrolytes such as ionic liquids, which require temperatures close to 100° C.
[0054] As known to those skilled in the art, the reaction time may vary depending on several factors, such as the specific conditions, the nature of the solid residue containing PGMs, the specific DES used in the electrolyte, the amount of PGMs to be electrodeposited and the solid residue containing PGMs. However, the reaction time of the method of the present invention is significantly reduced compared to the reaction time required to recover PGMs via the methods of the prior art.
[0055] To facilitate the electroleaching of the metal, the method can be carried out under stirring.
[0056] The process of the present invention can use a homogeneous solid residue containing PGMs, in particular in the form of a powder, such as particles with an average particle size of less than 2 mm, to further improve the efficiency of the process. Therefore, if necessary, the solid residue containing PGMs can be conveniently pre-treated by methods well known in the art, such as pre-treatments aimed at size reduction, homogenization, surface cleaning, etc.
[0057] Conventional physical pretreatment steps usually involve, first, disassembling the converter to separate the precious metal-containing support material from the precious metal-free steel shell, either by removing the shell in the case of ceramic converters or by crushing in the case of metal converters. This step is usually followed by a comminution step, such as crushing or grinding. Other pretreatments may also be performed, such as oxidation / reduction steps or calcination. For example, if the waste platinum-containing material contains platinum or palladium in the form of oxides (e.g., PtO 2 、PtO、PdO、PdO 2 ), a pre-reduction step, for example with formic acid, may be beneficial.
[0058] In one embodiment, optionally in combination with one or more features of the various embodiments described above and below, the electroleaching and electrodeposition processes (step a) are carried out simultaneously for 1 hour to 6 hours, such as 2 hours, 3 hours or 4 hours.
[0059] Deep eutectic solvents
[0060] As described above, the deep eutectic solvent used in the electrochemical method of the present disclosure is composed of a mixture of a hydrogen bond acceptor (HBA) compound (A) and a hydrogen bond donor (HBD) compound (B), wherein the hydrogen bond acceptor compound (A) is choline chloride, and the hydrogen bond donor compound (B) is selected from (C 1 To C 12 ) alcohol, (C 1 To C 12 )aldehyde, (C 1 To C 18 ) carboxylic acid, (C1 to C 6 )urea, (C 1 To C 12 )amide, (C 1 To C 12 ) nitrogen-containing compounds, (C 2 To C 12 ) amino acids and (C 1 To C 12 )sugar.
[0061] Non-limiting examples of HBD include (C1 To C 6 ) urea, such as urea, 1-(trifluoromethyl)urea, 1-methylurea, allylurea, 1,3-dimethylurea, 1,1-dimethylurea, thiourea, tetramethylurea; (C 1 To C 12 ) amides, such as N-methylacetamide, acetamide, benzamide, 2,2,2-trifluoroacetamide, salicylamide; (C 1 To C 12 ) alcohols, for example ethylene glycol, 9-anthracene methanol, ethanol, propan-2-ol, mannitol, 8-hydroxyquinoline, methyl and phenyl salicylate, triethanolamine, 2-chloroethanol, 4-hydroxy-3-methoxybenzaldehyde (vanillin), p-hydroxybenzaldehyde, benzyl alcohol, phenol, p-cresol, o-cresol, m-cresol, p-chlorophenol, p-aminophenol, xylenol, glycerol, ethylene glycol, triethylene glycol, 1,4-butanediol, 1,6-hexanediol; (C 1 To C 12 ) aldehydes such as benzaldehyde; (C 2 To C 12 ) amino acids such as glycine, alanine, lysine, and phenylalanine; (C 1 To C 12 ) Sugars such as fructose, lactose, saccharin, glucose, xylitol, sorbitol;
[0062] (C 1 -C 18 ) carboxylic acids such as trifluoroacetic acid, glycolic acid, trichloroacetic acid, glyoxylic acid, benzoic acid, citric acid, mandelic acid, valeric acid, tartaric acid, glutaric acid, m-nitrobenzoic acid, p-hydroxybenzoic acid, glutamic acid, m-aminobenzoic acid, malonic acid, oxalic acid, benzoic acid, phenylacetic acid, phenylpropionic acid, itaconic acid, levulinic acid, propane-1,2,3-tricarboxylic acid (tricarballylic acid), salicylic acid, trans-cinnamic acid, 3,5-dinitrobenzoic acid, nicotinic acid, stearic acid, hippuric acid, oleic acid, terephthalic acid, adipic acid, malic acid, succinic acid, acetic acid and lactic acid; and (C 1 To C 12 ) Nitrogen-containing compounds such as aniline, imidazole, hydroxylamine hydrochloride, diaminoethane, 1,2-diaminopropane, pyridine, benzylamine, triethylamine.
[0063] In a specific embodiment, optionally in combination with one or more features of the various embodiments described above and below, the hydrogen bond donor (B) is selected from (C 1 To C 12 ) alcohol, (C 1 To C 12 )aldehyde, (C 1 To C 18 ) carboxylic acid, (C 1 To C 12 )amide, (C1 To C 12 ) nitrogen-containing compounds, (C 2 To C 12 ) amino acids and (C 1 To C 12 ) sugars, more specifically selected from (C 1 To C 12 ) alcohol, (C 1 To C 12 )aldehyde, (C 1 To C 18 ) carboxylic acid and (C 1 To C 12 )amide.
[0064] In another embodiment, optionally in combination with one or more features of the various embodiments described above or below, the hydrogen bond donor (B) is (C 1 To C 6 More specifically, the hydrogen bond donor is selected from urea, 1-(trifluoromethyl)urea, 1-methylurea, allylurea, 1,3-dimethylurea, 1,1-dimethylurea, thiourea and tetramethylurea (C 1 To C 6 ) urea; even more specifically urea.
[0065] In another specific embodiment, optionally in combination with one or more features of the various embodiments described above and below, the hydrogen bond donor (B) is (C 1 To C 18 ) carboxylic acid. Specifically, the hydrogen bond donor is (C 1 To C 18 ) carboxylic acid selected from trifluoroacetic acid, glycolic acid, trichloroacetic acid, glyoxylic acid, benzoic acid, citric acid, mandelic acid, valeric acid, tartaric acid, glutaric acid, m-nitrobenzoic acid, p-hydroxybenzoic acid, glutamic acid, m-aminobenzoic acid, malonic acid, oxalic acid, benzoic acid, phenylacetic acid, phenylpropionic acid, itaconic acid, levulinic acid, propane-1,2,3-tricarboxylic acid (tricarballylic acid), salicylic acid, trans-cinnamic acid, 3,5-dinitrobenzoic acid, nicotinic acid, stearic acid, hippuric acid, oleic acid, terephthalic acid, adipic acid, malic acid, succinic acid, acetic acid and lactic acid. More specifically, the hydrogen bond donor is (C 1 To C 9 ) carboxylic acid, in particular selected from oxalic acid, formic acid, glycolic acid or lactic acid (C 1 To C 9 ) carboxylic acid, more specifically oxalic acid or formic acid.
[0066] Typically, in the deep eutectic solvent, the hydrogen bond acceptor compound (A) and the hydrogen bond donor (HBD) compound (B) have a molar ratio of (A) to (B) of 1:10 to 10:1. In a specific embodiment, optionally in combination with one or more features of the various embodiments described above and below, the hydrogen bond acceptor compound (A) and the hydrogen bond donor (HBD) compound (B) have a molar ratio of (A) to (B) of 1:5 to 5:1, more specifically 1:4 to 4:1, even more specifically 1:1 to 1:5. Specifically, the hydrogen bond acceptor compound (A) and the hydrogen bond donor (HBD) compound (B) have a molar ratio of (A) to (B) of 1:1, 1:2, 1:3, 1:4 or 1:5, more specifically 1:2.
[0067] The deep eutectic solvent used in the method of the present invention may also contain a second hydrogen bond donor (HBD) compound, thereby forming a ternary deep eutectic solvent. This component may be the same as or different from the HBD of the binary DES consisting of a mixture of a hydrogen bond acceptor compound (A) and a hydrogen bond donor (HBD) compound (B) as defined above.
[0068] In a specific embodiment, optionally in combination with one or more than one feature of the various embodiments described above and below, the second hydrogen bond donor of the ternary DES is (C 1 To C 18 ) carboxylic acid. More specifically, the hydrogen bond donor is (C 1 To C 18 ) carboxylic acid selected from the group consisting of trifluoroacetic acid, glycolic acid, trichloroacetic acid, glyoxylic acid, benzoic acid, citric acid, mandelic acid, valeric acid, tartaric acid, glutaric acid, m-nitrobenzoic acid, p-hydroxybenzoic acid, glutamic acid, m-aminobenzoic acid, malonic acid, oxalic acid, benzoic acid, phenylacetic acid, phenylpropionic acid, itaconic acid, levulinic acid, propane-1,2,3-tricarboxylic acid (tricarballylic acid), salicylic acid, trans-cinnamic acid, 3,5-dinitrobenzoic acid, nicotinic acid, stearic acid, hippuric acid, oleic acid, terephthalic acid, adipic acid, malic acid, succinic acid, acetic acid and lactic acid. Even more specifically, the second hydrogen bond donor of the ternary DES is (C 1 To C 9 ) carboxylic acid, even more particularly citric acid or malonic acid, and even more particularly citric acid.
[0069] In a specific embodiment, optionally in combination with one or more features of the various embodiments described above and below, the second HBD is present in the ternary DES in an amount of 1 wt % to 40 wt %, more specifically 5 wt % to 20 wt %, even more specifically 10 wt % to 15 wt %, relative to the total weight of the DES.
[0070] In another specific embodiment, optionally in combination with one or more features of the various embodiments described above or below, the DES used in the method of the present invention is selected from choline chloride: oxalic acid; choline chloride: formic acid, choline chloride: lactic acid, choline chloride: lactic acid and citric acid, choline chloride: lactic acid and malonic acid.
[0071] In another specific embodiment, optionally in combination with one or more features of the various embodiments described above and below, the DES used in the method of the present invention is selected from:
[0072] - 100 wt / wt% of choline chloride:lactic acid in a molar ratio of 1:2,
[0073] - 85 wt / wt% of choline chloride:lactic acid in a molar ratio of 1:1 + 15 wt / wt% of citric acid,
[0074] - 85% w / w of choline chloride:lactic acid in a molar ratio of 1:2 + 15% w / w of citric acid,
[0075] - 85% w / w of choline chloride:lactic acid in a molar ratio of 1:3 + 15% w / w of citric acid,
[0076] - 90% w / w of choline chloride:lactic acid in a molar ratio of 1:2 + 10% w / w of malonic acid,
[0077] -Choline chloride:formic acid (1:3), and
[0078] -Choline chloride:oxalic acid (1:1).
[0079] In another specific embodiment, optionally in combination with one or more features of the various embodiments described above and below, the DES used in the method of the present invention is a mixture of choline chloride and a carboxylic acid selected from oxalic acid, formic acid, glycolic acid and lactic acid, in particular selected from oxalic acid and formic acid. More specifically, the DES is selected from choline chloride:formic acid (1:3); and choline chloride:oxalic acid (1:1).
[0080] DES is usually obtained by mixing the required amounts of a hydrogen bond acceptor (HBA) compound (A) as defined above and a hydrogen bond donor (HBD) compound (B) as defined above (e.g. an alcohol, amine or carboxylic acid), preferably by heating at a suitable temperature, e.g. room temperature to 100° C., for a suitable period of time, e.g. 6 minutes to 1 hour.
[0081] Without wishing to be bound by theory, it is believed that the electroleaching and electrodeposition processes can be carried out simultaneously because, by applying the above-mentioned potential or current density, in addition to the oxidation of the PGM contained in the solid residue, the following reactions also occur:
[0082] Anode reaction
[0083] Electrode type: Boron-doped diamond (BDD) ( electrodes, CONDIAS) or boron-doped reduced graphene oxide-based graphite (BRGO) (prepared as described below).
[0084] The anode reaction occurring on BDD or BRGO is described as follows:
[0085] H 2 O→OH˙ (自由基) +H + +e - (1)
[0086] 2Cl - (水溶液) →Cl 2(气体) +2e - (2)
[0087]
[0088] 2OH˙ (自由基) →H 2 O 2 (1)
[0089] The BDD electrode and BRGO electrode are favorable for the formation of weakly adsorbed hydroxyl radicals, such as BDD (OH · )(1), which is a very strong oxidant (E 0 =2.8V), and is prone to forming oxidation products or free radicals. In the electrolyte, chloride exists in the aqueous solution of NaCl and is easily reacted with BDD (OH · ) is oxidized to form chlorine gas (2), which can then dissolve to form hypochlorite and hydrochloric acid (3). The electrically generated hydroxyl radicals can also react with each other to form hydrogen peroxide near the electrode surface (4).
[0090] Cathode reaction
[0091] Electrode Type: Graphite
[0092]
[0093] [PtCl 6 ] 2- +H 2 →[PtCl 4 ] 2+ +2H + +2Cl - (6)
[0094] [PtCl 4 ] 2- +H2 →Pt 0 +2H + +4Cl - (7)
[0095] [PdCl 4 ] 2- +H 2 →Pd 0 +2H + +4Cl - (8)
[0096] 2[RhCl 6 ] 3- +3H 2 →2Rh 0 +6H + +12Cl - (9)
[0097] It can be seen from the above reaction that when a mixture of a low eutectic solvent containing HCl and an aqueous NaCl solution is used as the electrolyte, PGM first dissolves in the form of chlorine metal salts and then is electrochemically generated by H 2 (Reaction 5) reduction (Reaction 6, Reaction 7, Reaction 8, Reaction 9), and deposition to the cathode.
[0098] exist Figure 1 A schematic diagram of the complete process can be seen in .
[0099] As mentioned above, the method of the present invention also includes the step of recovering the PGM electrodeposited on the cathode. Electrochemical polarity switching of the electrodes can be applied to recover the PGM as a precipitate. The recovered metals can be used for concentrate preparation and sale.
[0100] In an embodiment, optionally in combination with one or more features of the various embodiments described above and below, the recovery step b) can be performed by switching the polarity of the reaction so as to separate the PGM from the cathode, wherein the separated PGM forms a precipitate; and filtering the PGM precipitate. More specifically, the recovery of the electrodeposited PGM can be performed by:
[0101] i) immersing the cathode electrodeposited with PGM in a 0.25M to 1M NaCl aqueous solution, for example a 0.5M NaCl aqueous solution, and
[0102] ii) Applying a fixed potential of 0.5V to 1V, for example 1V.
[0103] This process can be carried out at room temperature for a desired period of time until substantially all of the deposited PGMs have been separated from the cathode. The separated PGMs form a precipitate that can be recovered by filtration. Figure 3A chronoamperometric test with 1 V applied is shown, and after 5 minutes the current drops to almost zero, a sign of PGM detachment.
[0104] After the simultaneous electro-leaching and electrodeposition processes and recovery of the leached PGM from the electrolyte, the DES can be recovered and recycled for the next batch of leaching.
[0105] Throughout the specification and claims, the word "comprise" and its variants are not intended to exclude other technical features, additives, components or steps. In addition, the word "comprise" includes the case of "consisting of..."
[0106] The following examples and figures are provided by way of illustration and are not intended to limit the present invention. In addition, the present invention covers all possible combinations of the specific and preferred embodiments described herein. Example
[0107] Preparation of electrolyte
[0108] The electrolyte used was made by mixing 80% deep eutectic solvent (DES) and 20% aqueous NaCl solution (0.5 M). DES was prepared by heating and stirring a mixture of choline chloride (ChCl, 98% Sigma-Aldrich) and formic acid (FA, 98% Sigma-Aldrich) in a molar ratio of 1:3 at 80°C until a homogeneous liquid was formed. Another DES was prepared in exactly the same way as ChCl / formic acid (1:3), but oxalic acid was used instead of formic acid, and a mixture of ChCl and oxalic acid (OA, 98% Sigma-Aldrich) in a molar ratio of 1:1 was used.
[0109] Electrochemical Reactor
[0110] The electrochemical reactor consisted of a custom-made borosilicate bottle (liquid volume 100 mL) containing an anode working electrode, a counter electrode, and a reference electrode. The anode was made of boron-doped diamond (BDD) ( The other two electrodes were a non-leaking 3.4 M KCl saturated Ag / AgCl reference electrode (Innovative Instruments Ltd) and a graphite rod (as cathode).
[0111] BRGO electrodes were prepared according to the following protocol. Commercial graphene oxide (GO) dispersion (4 mg / mL) provided by Graphenea (average particles <10 μm; carbon: 49% to 56%; oxygen: 41% to 50%; nitrogen: 0% to 1%) and boric acid were purchased from Sigma Aldrich. 6 g of boric acid was dissolved in 4 g / L of GO solution and loaded into a stainless steel autoclave lined with polytetrafluoroethylene and heated at 180°C for 16 hours. The synthesized material was washed three times with deionized water and frozen at -80°C for 24 hours. It was then freeze-dried at -10°C, 63 Pa for 12 hours. Boron-doped reduced graphene oxide (BRGO) electrodes were prepared by blending the synthesized graphene material with polyvinyl alcohol and ethanol. The blend was ultrasonically stirred for only 8 hours to ensure its homogeneity. The BRGO slurry was deposited on a graphite plate acting as a current collector and dried in an oven at 60°C to remove the organic solvent to obtain a planar electrode. 3.5×2=7cm 2 Both sides of the electrodes are exposed to the liquid, so the total surface area of the electroleaching reactor is 14 cm 2 Before the electroleaching experiment, the electrode was immersed in 0.1 mol / L NaCl solution for no less than 24 h to wet the pores of the electrode. Finally, it was assembled in the electroleaching reactor.
[0112] General method for electrochemical recovery of PGMs from solid residues.
[0113] The electrochemical reactor was operated in batch mode at 80 °C with constant stirring (300 rpm) for 1 h, 3 h, or 6 h. Chronoamperometry (900 mA / cm 2 or 64mA / cm 2 The PGM-containing starting materials were ground spent automotive catalysts containing the metal elements shown in Table 1 and ground Pd-rich spent membrane solid residues (Table 2).
[0114] Table 1
[0115] element unit sample R mg / kg 349 Pd mg / kg 1681 Pt mg / kg 975 Ce mg / kg 44095 La mg / kg 4542 Mg mg / kg 52643 Al mg / kg 186377 Si mg / kg 166797 K mg / kg 1936 Ca mg / kg 5788 Ti mg / kg 4479 Fe mg / kg 6908 Cu mg / kg 178 Pb mg / kg 616
[0116] Table 2
[0117] element unit sample Pd mg / kg 89142 Ag mg / kg 4965 Al mg / kg 1713 Fe mg / kg 72 Ni mg / kg 3 Zr mg / kg 41
[0118] The PGM-containing residue was contacted with an electrolyte at 80°C under magnetic stirring. The specific weight / weight (solid / liquid) ratio was 1:9. HCl (2M) was added as an additive at a ratio of solid residue / HCl = 1:1. The chemical composition of the starting material, leachate and precipitate was analyzed by inductively coupled plasma mass spectrometry (ICP-MS).
[0119] The above contents i) and ii) can be measured by using inductively coupled plasma mass spectrometry (ICP-MS), which is a well-known technique in the art. Those skilled in the art will know how to perform the above measurements. For example, these measurements can be performed using an ICP-MS spectrometer, such as an Agilent 7900 ICP / MS device, under the following conditions:
[0120]
[0121] Calibration parameters
[0122] Curve fitting: linear, correlation coefficient limit: 0.9998%.
[0123] Origin: Blank offset
[0124] For each element, the standard concentrations used for the calibration curve were: 0 μg / L, 1 μg / L, 5 μg / L, 20 μg / L, 100 μg / L, 500 μg / L, 2000 μg / L, and 10000 μg / L. These standards were made from individually certified standards at a concentration of 1000 mg / L.
[0125] For the digestion of the solid residue, microwave-assisted acid digestion was performed using Milestone Ethos Up. In the first step, approximately 0.1 g of a representative sample was digested using microwave heating in 2 mL of concentrated nitric acid (65%), 6 mL of hydrochloric acid (37%), and 2 mL of hydrofluoric acid (48%). The mixture of sample and acid was placed in an inert PTFE-sealed microwave container. The temperature profile was set to reach 230 ± 10 ° C within 20 minutes and maintained at 230 ± 10 ° C for 15 minutes. After that, a second step was performed, adding 25 mL of 4% boric acid to complex the excess HF. The temperature profile was set to reach 180 ± 10 ° C within 20 minutes and maintained at 180 ± 10 ° C for 15 minutes. After cooling, the container contents were diluted to 50 mL and analyzed by ICP-MS. The metals deposited on the graphite electrode were dissolved in aqua regia.
[0126] Comparative Example (control, i.e. conventional leaching, no potential applied)
[0127] The results recovered after conventional leaching, i.e. without applying any potential or current, were used as comparative examples (controls). They were carried out under the same experimental conditions as the examples, but without applying any potential or current under open circuit conditions.
[0128] Experimental Results
[0129] In all examples, the leaching recoveries of different elements were calculated by two methods:
[0130] i) based on the metals remaining in the solid residue (the difference between the initial amount of each metal and the final amount in the solid residue is considered to be the amount that has leached); and / or
[0131] ii) Based on the sum of the amount detected in the leachate and the amount deposited to the cathode.
[0132] The recovery of the control was calculated according to method ii), ie from the total amount of the leached material and the cathode.
[0133] In Example 1, both results are shown as examples. However, in general, except for Fe, the two values are similar. Therefore, for the following experiments, only the values corresponding to the second method (amount detected in the leachate + amount deposited to the cathode) are given.
[0134] Example 1. Electrolytic leaching at 2.5 V for 3 hours vs. conventional leaching
[0135] The electro-leaching process was carried out in a reactor under the conditions indicated below, using BDD as anode, resulting in the recovery of about 80% of Pd and Pt and about 40% of Rh. No external oxidant was added.
[0136] condition:
[0137] - 80% of a 1:3 choline chloride / formic acid DES solution + 20% of an aqueous NaCl solution (0.5 M) with HCl (2 M) as an additive (solid residue / HCl ratio = 1:1);
[0138] - Electrode fixed potential: 2.5 V at 80°C for 3 hours; and
[0139] The results are shown in Table 3.
[0140] Table 3
[0141]
[0142] It can be seen that compared with conventional leaching performed under the same conditions but without applying any current, the leaching rate of Pt increased to a maximum of about 84%, the leaching rate of Rh increased to a maximum of about 33%, and the leaching rate of Pd was about 5%.
[0143] In the same reactor, in addition to improving the leaching rate, part of the PGM is selectively and simultaneously electrodeposited to the cathode: specifically, about 90% of Pd, about 53% of Pt and about 61% of Rh are electrodeposited to the cathode (graphite). Although Pb is also deposited, the main impurities remain in the solution (Al, Fe).
[0144] Example 2. Effect of reaction time on electroleaching experiment at 2.5 V
[0145] The electroleaching process was carried out as in Example 1, but the reaction time was extended to 6 hours. The results are shown in Table 4.
[0146] Table 4
[0147]
[0148] As can be seen, the recovery did not increase significantly compared to the 3 h reaction time. Therefore, longer reaction times did not improve the extraction rate and PGM recovery. However, electrodeposition of Pd was more selective with respect to the remaining PGMs, specifically with respect to Pt (~85% Pd; ~26% Pt and ~56% Rh deposited on the cathode, compared to 90% Pd, 53% Pt and 61% Rh deposited on the cathode in Example 1).
[0149] Comparative Example 1: Effect of additives on electroleaching
[0150] The electroleaching process was carried out as in Example 1, but without the addition of the additive HCl (2M). The results are shown in Table 5.
[0151] Table 5
[0152]
[0153] It can be seen that the recovery of almost all elements decreased dramatically when HCl was not added to the reaction system compared to the reaction carried out in the presence of HCl. These results indicate that the presence of the above additives is necessary to achieve the desired leaching behavior.
[0154] Example 3. Effect of ions in aqueous solution during electroleaching
[0155] The electroleaching process was carried out as in Example 1, but using an aqueous solution without NaCl. The results are shown in Table 6.
[0156] Table 6
[0157]
[0158] It was observed that when the ion concentration used in the aqueous solution was reduced, the recovery of PGM was slightly reduced compared to the reaction carried out with an aqueous solution containing 0.5 M NaCl (see the results of Example 1, Table 2). Therefore, the presence of NaCl in the aqueous solution used for the electrolyte can be observed to improve the effect.
[0159] Example 4. Comparison of electroleaching experiments using constant current
[0160] A constant current process (fixed current) was performed to compare with the process controlled by constant potential, and the applied current density was adjusted to 64 mA / cm 2 , and keep the other leaching conditions the same as in Example 1, namely:
[0161] - 80% of a 1:3 choline chloride / formic acid DES solution + 20% of an aqueous NaCl solution (0.5 M) with HCl (2 M) as an additive (solid residue / HCl ratio = 1:1);
[0162] - At 80°C with a current density of 64 mA / cm 2 React for 3 hours; and
[0163] -BDD anode electrode.
[0164] The results are shown in Table 7.
[0165] Table 7
[0166]
[0167] It can be observed that the recovery rate is similar to that of the constant potential control (Table 3), and it is confirmed that Pd is mainly deposited on graphite, while Pt and Rh are half and half distributed in graphite and liquid (Table 6). The main impurities remain in the electrolyte, which is beneficial for the purification of the recovered PGM.
[0168] Example 5. Effect of leaching time during constant current leaching
[0169] The effect of shortening the reaction time was also investigated in the constant current process. Therefore, the electroleaching process was carried out as in Example 4, but the leaching time was reduced to 1 hour. The results are shown in Table 8.
[0170] Table 8
[0171]
[0172] It was observed that when the leaching time was reduced to 1 hour, the recovery of Pt decreased slightly (from 82% to 65%) and the electrodeposition of Pd decreased significantly (from 87% to 60%). Therefore, 3 hours is the optimal leaching time under the conditions studied so far.
[0173] Example 6. Effect of replacing the BDD anode with a boron-doped reduced graphene oxide-based graphite (BRGO) anode.
[0174] The electroleaching process was carried out as in Example 4, but using a boron doped reduced graphene oxide based graphite (BRGO) anode instead of a BDD anode. The results are shown in Table 9.
[0175] Table 9
[0176]
[0177] It was observed that the BRGO electrode was able to achieve similar Pd recoveries compared to BDD (Table 6) (82% for Pd and 75% for BDD), but for Pt and Rh, the recoveries of BRGO were not as high as those using BDD (49% for Pt and 82% for BDD; 26% for Rh and 42% for BDD). However, the results obtained showed that BRGO was also able to improve the leaching of PGMs, especially Pt (45% increase) and Rh (15% increase) and 12% increase for Pd, compared to conventional leaching (a process without any applied potential or current).
[0178] Example 7. Changing to constant potential control and using boron-doped reduced graphene oxide-based graphite (BRGO) anode Extreme influence
[0179] The electroleaching process was carried out as in Example 6, but the applied electrode potential was 3 V instead of 64 mA / cm 2 The results are shown in Table 10.
[0180] Table 10
[0181]
[0182] From the above results, it can be seen that similar recoveries were observed.
[0183] Example 8. Substituting oxalic acid for formic acid in DES
[0184] The electroleaching process was carried out as in Example 1, but oxalic acid (ChCl / oxalic acid was 1:1) was used instead of formic acid (ChCl / formic acid was 1:3) as the hydrogen bond donor for forming DES. The results are shown in Table 11.
[0185] Table 11
[0186]
[0187] It was observed that the effect of using oxalic acid instead of formic acid as a hydrogen bond donor to form a deep eutectic solvent did not significantly affect the leaching rate and recovery of PGM. The results also showed that compared with the conventional leaching experiment (control), the leaching rate of Pt was higher, up to 45%, and that of Rh was up to 18%.
[0188] Example 9. Recovery of PGM electrodeposited to the cathode
[0189] After leaching, the PGM electrodeposited to the cathode is recovered by switching the reaction polarity. The cathode (graphite with PGM deposited) is immersed in a NaCl aqueous solution (0.5M) and a fixed potential of 1V is applied for 25 minutes at room temperature. The PGM separates from the cathode to form a precipitate, which can be recovered by filtration. This is done by filtering first with a 5μm pore size filter and then with a 0.45μm pore size filter. The flow chart of the method is shown in Figure 2 In the chronoamperometry test, 1 V was applied and run for 30 minutes, and it can be seen that all PGM was released from the electrode surface in just 5 minutes (see Figure 3 ). The recovered solid contained mainly Pd (≈70%), followed by ≈8% Pt and ≈4% Rh (≈82% PGM in the solid). The only impurity in the solid was Pb, although its content (≈18%) was relatively low relative to PGM. The recovery results of the polarization process and the composition of the recovered final solid are shown in Table 12.
[0190] Table 12
[0191]
[0192] *Approximate composition of recovered solids.
[0193] Example 10. Recovering PGM electrodeposited to cathode using different starting materials, such as waste membranes containing Pd
[0194] The electroleaching process was carried out as in Example 4, but using spent membrane as the solid residue.
[0195] In Table 13, the results of the application of an electrochemical process for the recovery of platinum group metals (PGMs) from different solid residues are shown, said process highly concentrating Pd.
[0196] Table 13
[0197]
[0198] It was observed that when 64 mA / cm was applied, the 2 The solid product Pd was significantly recovered from the waste membrane at a fixed current density of 1.5 Å. This process was performed without adding any external additives such as H 2 O 2 The main advantage compared to the conventional leaching process is that Pd is first released from the spent membrane and recovered as a solid material on the electrode surface or as a precipitate.
[0199] Reference List
[0200] -WO2008155464
[0201] - Smith E.L. et al., “Deep Eutectic Solvents (DES) and Their Applications”, Chem. Rev.
[0202] 2014, 114, 11060 - 11082.
Claims
1. An electrochemical process for recovering platinum group metals (PGMs) from a solid residue containing PGMs, the process comprising the following steps: a) subjecting the solid residue to electro-leaching to leach PGM from the solid residue and, simultaneously, electrodepositing the leached PGM onto a cathode; wherein the electroleaching and the electrodeposition are carried out in an electrolyte comprising a deep eutectic solvent (DES) and an aqueous solution containing chloride ions and having a pH value less than 7; and b) recovering the electrodeposited PGM; DES is composed of a mixture of the following substances: (i) a hydrogen bond acceptor (HBA) compound (A) which is choline chloride; and (ii) a hydrogen bond donor (HBD) compound (B) selected from (C1 to C 12 ) alcohol, (C1 to C 12 )aldehyde, (C1 to C 18 ) carboxylic acid, (C1 to C6) urea, (C1 to C 12 )amide, (C1 to C 12 ) nitrogen-containing compounds, (C1 to C 12 ) amino acids and (C1 to C 12 )sugar; The molar ratio of (A) to (B) is 1:10 to 10:
1.
2. The electrochemical method according to claim 1, wherein the DES is selected from the group consisting of choline chloride: oxalic acid, choline chloride: formic acid, choline chloride: lactic acid, choline chloride: lactic acid and citric acid, choline chloride: lactic acid and malonic acid.
3. The electrochemical process according to claim 2, wherein the DES is a mixture of choline chloride and a carboxylic acid selected from oxalic acid and formic acid.
4. The electrochemical method according to claims 1 to 3, wherein the aqueous solution containing chloride ions and having a pH <7 is a mixture of water containing NaCl in a concentration of 0 M to 2.5 M and HCl as an additive.
5. The electrochemical process according to claim 4, wherein the amount of DES is 75% to 90% by weight relative to the total amount of DES and water optionally containing NaCl.
6. The electrochemical method according to claim 4 or 5, wherein the water comprises NaCl at a concentration of 0.3M to 0.6M.
7. The electrochemical method according to claims 1 to 6, wherein the weight ratio of the solid residue to the electrolyte is 1:5 to 1:
15.
8. The electrochemical process of claims 4 to 7, wherein the HCl is added in a ratio of 1:1 solid residue:HCl.
9. The electrochemical method according to claims 1 to 8, wherein the step a) is carried out in a reactor comprising a working electrode, a counter electrode and a reference electrode, wherein the working electrode is selected from boron-doped diamond (BDD) and boron-doped reduced graphene oxide-based graphite (BRGO).
10. The electrochemical method according to claims 1 to 9, wherein step a) is performed by applying a potential of 2.5 V to 3 V, or, alternatively, applying 45 mA / cm 2 Up to 64mA / cm 2 The current density is .
11. The electrochemical process according to claims 1 to 10, wherein step a) is performed at a temperature of 20°C to 100°C.
12. The electrochemical method according to claims 1 to 11, wherein step a) is performed for 1 to 6 hours.
13. The electrochemical process according to claims 1 to 12, wherein the recovery of the electrodeposited PGM is carried out by: i) immersing the cathode with the electrodeposited PGM in a 0.25M to 1M NaCl aqueous solution, and ii) A fixed potential of 0.5V to 1V is applied.
14. The electrochemical process according to claims 1 to 13, wherein the solid residue containing PGMs is selected from spent automobile catalysts, tailings, electronic waste, spent membrane residues, catalytic converters, spent petroleum refining catalysts, spent proton exchange membrane fuel cells (PEMFCs) and spent catalysts used in the chemical industry.
15. The electrochemical process according to claim 14, wherein the PGM-containing solid residue is a spent automobile catalyst.
Citation Information
Patent Citations
Polymeric ultraviolet light stabilisers containing hindered alkyl amines and polymer compositions containing them
EP0002022A1
Method for recovery
WO2008155464A1