Joining structure

By using the intermetallic compound layer formed by Sn and the Ni conductive film formed by Sn in the bonding structure between the electronic components and the wiring substrate, the formation of the Kirkendal void is suppressed, the diffusion problem caused by the low melting point of Sn is solved, and the stability of the bonding is improved and reliability.

CN118891964APending Publication Date: 2024-11-01TDK CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380027650.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-17
Filing Date
2023-03-14
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

During the bonding process between electronic components and wiring substrates, the low melting point of Sn causes the diffusion of intermetallic compound elements, forming a Kirkendal void, affecting the stability and reliability of the bonding.

Method used

The bonding structure of the first metal layer, the intermetallic compound layer and the second metal layer formed by Sn sequentially composed of the electronic component side, wherein the thickness of the second metal layer is the first metal layer and the intermetallic compound. The total layer is less than 50% or less, and the intermetallic compound layer may be present on the wiring substrate terminals, and a Ni conductive film is formed on the wiring substrate terminals to suppress diffusion.

Benefits of technology

The diffusion driving force concentration gradient of intermetallic compound elements is effectively reduced, the formation of Kirkendal voids is inhibited, and the stability and reliability of bonding are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891964A_ABST
    Figure CN118891964A_ABST
Patent Text Reader

Abstract

This bonding structure is obtained by bonding an electronic component and a wiring substrate, and is provided with, in order from the electronic component side, a first metal layer containing a metal that forms an intermetallic compound with Sn, an intermetallic compound layer comprising an intermetallic compound containing Sn, and a second metal layer containing Sn. The thickness of the second metal layer is 50% or less of the total thickness of the first metal layer, the intermetallic compound layer, and the second metal layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a joint structure. Background Art

[0002] In recent years, along with the development of electronics, the development of technology for mounting electronic components on substrates is being promoted. For example, with regard to the assembly of fine electronic components, the terminals of the electronic components have previously been made of gold, and Sn is plated or thin-filmed on the opposite side of the wiring substrate, and joined by soldering or diffusion bonding. When the electronic components are joined to the wiring substrate by Au plating and Sn plating, there is a tendency for intermetallic compounds of Au and Sn to form at the bonding interface through eutectic reaction. As one of the problems of Sn-Au solder, the brittleness of Sn-Au based intermetallic compounds can be cited. As a method for overcoming its brittleness, a technology for dispersing intermetallic compounds at a ratio of 5 to 50% in terms of the area fraction of the bonding cross section is disclosed (for example, Patent Document 1). Prior art literature Patent Literature

[0003] Patent Document 1: Japanese Patent Application Publication No. 2003-286531 Summary of the invention [Problems to be solved by the invention]

[0004] However, Sn has a low melting point, so the metallic element tends to diffuse easily in the alloy containing Sn. Therefore, the structure in which the intermetallic compound is dispersed has the following problems: the element forming the intermetallic compound with Sn diffuses in the alloy containing Sn, and Kirkendall voids are generated at the position where the element forming the intermetallic compound with Sn exists.

[0005] An object of the present invention is to provide a joining structure capable of suppressing Kirkendall voids. [Technical means to solve the problem]

[0006] The bonding structure of the present invention is formed by bonding an electronic component to a wiring substrate, and comprises, in order from the electronic component side: a first metal layer comprising a metal that forms an intermetallic compound with Sn, an intermetallic compound layer composed of an intermetallic compound comprising Sn, and a second metal layer comprising Sn, wherein the thickness of the second metal layer is less than 50% of the total thickness of the first metal layer, the intermetallic compound layer and the second metal layer.

[0007] In the bonding structure of the present invention, the thickness of the second metal layer is less than 50% of the total thickness of the first metal layer, the intermetallic compound layer and the second metal layer. This means that in the initial state of bonding, the metal element that forms the intermetallic compound with Sn exists in a wider range than the central part of the bonding structure. In this case, the concentration gradient of the metal element that forms the intermetallic compound with Sn, which becomes the driving force for diffusion, can be reduced, and Kirkendall voids can be suppressed.

[0008] The first metal layer may include Au. Au easily forms an intermetallic compound with Sn, and Au easily diffuses into a layer including Sn, so it is a metal element that easily forms Kirkendall voids. In contrast, by adopting the structure of the present invention, even when Au is used, Kirkendall voids can be suppressed.

[0009] The intermetallic compound layer may exist on the terminals of the wiring substrate. Since the intermetallic compound layer containing Sn exists on the terminals of the wiring substrate, the concentration gradient of the metal element forming the intermetallic compound with Sn is low, and diffusion is not easy to occur, so Kirkendall voids can be suppressed.

[0010] The terminal of the wiring substrate may have a conductive film containing Ni formed on the surface. The conductive film containing Ni can suppress the reaction of the metal element forming an intermetallic compound with Sn inside the terminal of the wiring substrate. As a result, the diffusion distance extension of the metal element forming an intermetallic compound with Sn can be suppressed, and Kirkendall voids can be suppressed.

[0011] The volume ratio of the second metal layer may be 50% or less of the total volume of the first metal layer, the intermetallic compound layer, and the second metal layer. This makes it difficult for the metal element that forms the intermetallic compound with Sn to diffuse, and Kirkendall voids can be suppressed.

[0012] The volume ratio of the first metal layer may be less than 50% of the total volume of the first metal layer, the intermetallic compound layer, and the second metal layer. By reducing the volume of the first metal layer including the metal element that forms an intermetallic compound with Sn, the element that diffuses can be reduced, thereby suppressing Kirkendall voids.

[0013] The bonding structure of the present invention is formed by bonding an electronic component to a wiring substrate, and comprises, in order from the electronic component side: a first metal layer containing a metal that forms an intermetallic compound with Sn, and an intermetallic compound layer composed of an intermetallic compound containing Sn, wherein the intermetallic compound layer exists on a terminal of the wiring substrate.

[0014] The bonding structure of the present invention is a laminated structure of a first metal layer including a metal that forms an intermetallic compound with Sn and an intermetallic compound including Sn, rather than a eutectic structure. In addition, the intermetallic compound layer reaches the terminal of the wiring substrate. Therefore, the concentration gradient of the metal element that forms an intermetallic compound with Sn, which serves as a driving force for diffusion, can be reduced, and Kirkendall voids can be suppressed.

[0015] The terminal of the wiring substrate may have a conductive film containing Ni formed on the surface. The conductive film containing Ni can suppress the reaction of the metal element forming an intermetallic compound with Sn inside the terminal of the wiring substrate. As a result, the diffusion distance of the metal element forming an intermetallic compound with Sn can be suppressed, and Kirkendall voids can be suppressed.

[0016] The bonding structure of the present invention is formed by bonding an electronic component to a wiring substrate, and comprises: a first metal layer including a metal that forms an intermetallic compound with Sn, an intermetallic compound layer composed of an intermetallic compound including Sn, and a second metal layer including Sn, wherein the volume ratio of the second metal layer can be less than 50% of the total volume of the first metal layer, the intermetallic compound layer and the second metal layer.

[0017] In the bonding structure of the present invention, the volume ratio of the second metal layer is less than 50% of the total volume of the first metal layer, the intermetallic compound layer and the second metal layer. This means that in the initial state of bonding, the metal element that forms the intermetallic compound with Sn exists in a wider range than the central part of the bonding structure. In this case, the concentration gradient of the metal element that forms the intermetallic compound with Sn, which becomes the driving force for diffusion, can be reduced, and Kirkendall voids can be suppressed. [Effects of the Invention]

[0018] According to the present invention, a joining structure capable of suppressing Kirkendall voids can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a schematic cross-sectional view showing a mounting substrate having a bonding structure according to an embodiment of the present invention. Figure 2 It is a schematic cross-sectional view of a wiring board showing a bonding structure according to an embodiment of the present invention. Figure 3 It is a schematic cross-sectional view showing an example of a laminated structure of a joint structure. Figure 4 It is a schematic cross-sectional view showing an example of a laminated structure of a joint structure. Figure 5 This is a diagram showing an example of a SEM (Scanning Electron Microscope) image. Figure 6 A diagram for explaining a method of bonding an electronic component to a wiring board. Figure 7 This is a table showing the measurement results of Examples and Comparative Examples. Figure 8 It is a schematic cross-sectional view showing an example of a laminated structure of a joint structure. DETAILED DESCRIPTION

[0020] Reference Figure 1 and Figure 2 , a joining structure 100 according to an embodiment of the present invention will be described. Figure 1 1 is a schematic cross-sectional view showing a mounting substrate 1 including a bonding structure 100 according to an embodiment of the present invention. Figure 2 1 is a schematic cross-sectional view of a wiring board 3 showing a junction structure 100 according to an embodiment of the present invention.

[0021] like Figure 1 As shown, the mounting substrate 1 includes an electronic component 2 and a wiring substrate 3. The mounting substrate 1 is configured by mounting the electronic component 2 on the wiring substrate 3 via a bonding layer 40 .

[0022] The electronic component 2 includes a main body 6 and a pair of terminals 7. The main body 6 is a member for performing the function of the electronic component 2. The terminal 7 is a metal portion formed on the main surface of the main body 6. The electronic component 2 is composed of, for example, a micro LED (Light Emitting Diode). The micro LED is a component that emits light based on the input from the wiring substrate 3.

[0023] The wiring substrate 3 includes a substrate 8, a wall 9, and a pair of terminals 10. The substrate 8 is a flat plate-shaped main body of the wiring substrate 3. The wall 9 is a member formed of an insulator formed on the upper surface of the substrate 8. The material of the wall 9 is, for example, a resin material such as epoxy resin, acrylic resin, phenolic resin, melamine resin, urea-formaldehyde resin, and alkyd resin. It is particularly preferred that the material of the wall 9 is epoxy resin or acrylic resin. The terminal 10 is a metal portion formed on the main surface of the substrate 8. The material of the terminal 10 is Ni, Cu, Ti, Cr, Al, Mo, Pt, Au, or an alloy of at least two selected from these. The terminal 10 has a conductive film 12 formed on the surface. The material of the conductive film 12 is a film of Ti, Cu, Ni, Al, Mo, Cr, Ag, etc., or a film formed by mixing metal particles and an adhesive, etc.

[0024] The Sn layer 20 is a layer containing Sn that joins the terminal 7 of the electronic component 2 and the terminal 10 of the wiring substrate 3. Before assembly, the wiring substrate 3 has a bonding material 4A (see Figure 2The bonding material 4A functions as solder. During assembly, the terminal 10, the conductive film 12, the bonding material 4A, and the terminal 7 are stacked and then soldered.

[0025] A recess 11 is formed in the wall 9. The recess 11 is formed by a through hole penetrating the wall 9. Thus, the upper surface of the substrate 8 is exposed at the bottom side of the recess 11. The recess 11 is rectangular when viewed from the thickness direction of the wiring substrate 3. The terminal 7, the terminal 10, the conductive film 12, and the Sn layer 20 are arranged in the recess 11 formed in the wall 9, and are thus surrounded by the wall 9. A small gap is formed between the terminal 7, the terminal 10, the conductive film 12, and the Sn layer 20 and the inner side surfaces of the four sides of the recess 11 (i.e., the inner side surfaces of the wall 9).

[0026] The constituent material 30 is disposed in the recess 11 between the electronic component 2 and the Sn layer 20 and the wall 9. Thus, the electronic component 2 is supported by the constituent material 50, so that it is not easy to peel off from the wiring substrate 3. In addition, the force applied to the electronic component 2, the Sn layer 20 or the terminals 7 and 10 can be alleviated, thereby improving reliability. The material of the constituent material 50 is, for example, epoxy resin, acrylic resin, phenolic resin, melamine resin, urea resin, alkyd resin or a mixture of these, or a resin material and SiO X , ceramics, etc. It is preferable that the material of the constituent member 50 is epoxy resin or acrylic resin.

[0027] Then, refer to Figure 3 and Figure 4 The joining structure 100 of this embodiment will be described in more detail. Figure 3 In the example of (a), the bonding structure 100 includes, in order from the electronic component 2 side: a terminal 7, an intermetallic compound layer 25, a bonding material 4, a conductive film 12, and a terminal 10. The bonding structure 100 includes, in order from the electronic component 2 side: a first metal layer 21 including a first metal that forms an intermetallic compound with Sn, an intermetallic compound layer 25 composed of an intermetallic compound containing Sn, and a second metal layer 22 composed of a second metal containing Sn. Here, the terminal 7 of the electronic component 2 corresponds to the first metal layer 21, and the bonding material 4 corresponds to the second metal layer 22. The intermetallic compound layer 25 is provided between the terminal 7 and the bonding material 4, and is composed of a bonding material containing Sn and an intermetallic compound with the first metal.

[0028] In the following description, the stacked structure composed of the terminal 7 containing Au and the Sn layer 20 may be referred to as a bonding layer 40 .

[0029] The second metal of the bonding material 4 may contain Sn or may be composed of an alloy containing Sn. In addition to Sn, the second metal may contain an element that lowers the melting point of Sn. Examples of the element that lowers the melting point of Sn include Bi.

[0030] The first metal of the terminal 7 is any one of Au, Cu, Ni, Ag, and Pd, or an alloy of at least two selected from these. The first metal may be a metal containing at least Au.

[0031] The intermetallic compound layer 25 is formed by diffusing the first metal of the terminal 7 on the wiring substrate 3 side. The intermetallic compound layer 25 is composed of an intermetallic compound of the first metal of the terminal 7 and the second metal containing Sn of the bonding material 4. Here, the intermetallic compound layer 25 has a first layer 31 and a second layer 32. For example, the first layer 31 is composed of AuSn2. The second layer 32 is composed of AuSn4. Furthermore, on the terminal 10 (on the conductive film 12), the bonding material 4 can be formed on a part, and the intermetallic compound layer 25 can exist on a part.

[0032] exist Figure 3 In the example of (b), the bonding structure 100 includes, in order from the electronic component 2 side: a terminal 7, an intermetallic compound layer 25, a conductive film 12, and a terminal 10. In addition, a bonding material 4 is arranged on the lateral side of the terminal 7 and the intermetallic compound layer 25. The bonding structure 100 includes, in order from the electronic component 2 side: a first metal layer 21 including a first metal that forms an intermetallic compound with Sn, and an intermetallic compound layer 25 composed of an intermetallic compound including Sn. The intermetallic compound layer 25 exists on the terminal 10 of the wiring substrate 3. Here, the terminal 10 has a conductive film 12 on the upper surface, so the intermetallic compound layer 25 exists on the conductive film 12. The intermetallic compound layer 25 includes: a first layer 31, and a second layer 32. For example, the first layer 31 is composed of AuSn2. The second layer 32 is composed of AuSn4. The bonding material 4 is in a triangular shape such as reaching the terminal 7, and the shape of the bonding material 4 is not particularly limited, nor is it limited to which layer it reaches.

[0033] Furthermore, if Figure 8 As shown, the bonding material 4 may not be in contact with the terminal 7. Figure 8 In the example shown in (a), the triangular bonding material 4 is extended in a manner offset laterally relative to the terminal 7, so as to be in a positional relationship of not contacting the terminal 7. Figure 8 In the example shown in (b), the triangular bonding material 4 does not reach the terminal 7 and is therefore in a positional relationship of not contacting the terminal 7 .

[0034] exist Figure 4 In the example (a), Figure 3The bonding material 4 is entirely formed into the intermetallic compound layer 25. The bonding structure 100 includes, in order from the electronic component 2 side: a terminal 7, an intermetallic compound layer 25, a conductive film 12, and a terminal 10. The bonding structure 100 includes, in order from the electronic component 2 side: a first metal layer 21 including a first metal that forms an intermetallic compound with Sn, and an intermetallic compound layer 25 composed of an intermetallic compound including Sn. The intermetallic compound layer 25 is present on the terminal 10 of the wiring substrate 3. The intermetallic compound layer 25 includes: a first layer 31, and a second layer 32. For example, the first layer 31 is composed of AuSn2. The second layer 32 is composed of AuSn4.

[0035] exist Figure 4 In the example (b), the structure of the intermetallic compound layer 25 is similar to Figure 4 (a) Different. The junction structure 100 includes, in order from the electronic component 2 side: a terminal 7, an intermetallic compound layer 25, a conductive film 12, and a terminal 10. The junction structure 100 includes, in order from the electronic component 2 side: a first metal layer 21 including a first metal that forms an intermetallic compound with Sn, and an intermetallic compound layer 25 composed of an intermetallic compound including Sn. The intermetallic compound layer 25 is present on the terminal 10 of the wiring substrate 3. The intermetallic compound layer 25 includes a third layer 33. For example, the third layer 33 forms an AuSn-based intermetallic compound layer 25, for example, composed of AuSn4.

[0036] Next, the thickness and area of ​​each layer of the bonding structure 100 are described. The ratio of the thickness of a specific layer below represents the ratio of the thickness of the specific layer to the thickness of the entire bonding layer 40. In addition, the ratio of the volume of a specific layer represents the ratio of the thickness of the specific layer to the volume of the entire bonding layer 40.

[0037] exist Figure 3 In the bonding structure 100 shown in (a), the thickness of the bonding material 4 (second metal layer 22) is preferably 50% or less of the total thickness of the terminal 7 (first metal layer 21), the intermetallic compound layer 25, and the bonding material 4, more preferably 35% or less, and further preferably 10% or less. The lower limit is not particularly limited. Figure 4 That is, the thickness of the bonding material 4 (second metal layer 22 ) may be 0% or more of the total thickness of the terminal 7 (first metal layer 21 ), the intermetallic compound layer 25 , and the bonding material 4 .

[0038] The volume ratio of the bonding material 4 (second metal layer 22) is preferably 50% or less of the total volume of the terminal 7 (first metal layer 21), the intermetallic compound layer 25, and the bonding material 4, and more preferably 14% or less. Figure 4 As shown, the bonding material 4 may disappear.

[0039] The volume ratio of the terminal 7 (first metal layer 21) is preferably less than 50% of the total volume of the terminal 7 (first metal layer 21), the intermetallic compound layer 25, and the bonding material 4 (second metal layer 22), and more preferably less than 30%. The lower limit is not particularly limited, and the volume ratio of the terminal 7 (first metal layer 21) is preferably more than 4% of the total volume of the terminal 7 (first metal layer 21), the intermetallic compound layer 25, and the bonding material 4 (second metal layer 22).

[0040] exist Figure 3 In the bonding structure 100 shown in (b), the volume ratio of the bonding material 4 (second metal layer 22) is preferably 50% or less of the total volume of the terminal 7 (first metal layer 21), the intermetallic compound layer 25 and the bonding material 4, and more preferably 12% or less.

[0041] The volume ratio of the terminal 7 (first metal layer 21) is preferably less than 50% of the total volume of the terminal 7 (first metal layer 21), the intermetallic compound layer 25, and the bonding material 4 (second metal layer 22), and more preferably less than 27%. The lower limit is not particularly limited, and the volume ratio of the terminal 7 (first metal layer 21) is preferably more than 4% of the total volume of the terminal 7 (first metal layer 21), the intermetallic compound layer 25, and the bonding material 4 (second metal layer 22).

[0042] exist Figure 4 In the joint structure 100 shown in (a) and (b), the volume ratio of the terminal 7 (first metal layer 21) is preferably less than 50% of the total volume of the terminal 7 (first metal layer 21) and the intermetallic compound layer 25, and more preferably less than 30%. The lower limit is not particularly limited, and the volume ratio of the terminal 7 (first metal layer 21) is preferably more than 4% of the total volume of the terminal 7 (first metal layer 21) and the intermetallic compound layer 25.

[0043] Furthermore, Figure 3 and Figure 4 The layer structure is an example. For example, the number of layers of the intermetallic compound layer 25 is not particularly limited. For example, the intermetallic compound layer 25 may further include an AuSn layer.

[0044] Reference Figure 5(a) The method for measuring the thickness and area of ​​each layer of the above-mentioned bonding structure 100 is described. First, the obtained bonding structure 100 is cut perpendicularly to the wiring substrate 3 near the center, and the phase identification of each layer is performed based on the element ratio obtained by SEM-EDS measurement. The midpoint of the cross section where the terminal 7 on the side of the electronic component 2 of the cross section is connected to the main body 6 of the electronic component 2, and the midpoint of the cross section where the bonding layer 40 on the side of the wiring substrate 3 is connected to the terminal 10 (conductive film 12) are connected by a straight line L, and the length of the straight line L passing through each layer is set as the layer thickness. The ratio of the thickness of the above-mentioned bonding material 4 can be calculated based on the results of the thickness of each layer obtained.

[0045] The area of ​​each layer of the bonding structure 100 can be calculated by measuring the area of ​​each layer in the SEM image. The volume of each layer can be obtained from the area of ​​each layer, and the ratio of the volume of the bonding material 4 and the terminal 7 can be calculated.

[0046] The thickness of each layer of the bonding structure 100 can be measured by the following method: using the least squares approximation method, the boundaries of each layer are approximated as line segments, and the distance between the midpoints is measured as the layer thickness. Based on this measurement method, the thickness of the bonding material 4 (second metal layer 22) is less than 50% of the total thickness of the terminal 7 (first metal layer 21), the intermetallic compound layer 25, and the bonding material 4.

[0047] Then, refer to Figure 6 , a method for joining the electronic component 2 and the wiring substrate 3 is described. First, Figure 6 As shown in (a), the terminal 7 of the electronic component 2 is placed on the bonding material 4A of the wiring substrate 3. Here, if heating is performed for a long time (several minutes) at a temperature exceeding the melting point of Sn, the entire structure becomes a eutectic structure, and the intermetallic compound layer 25 of the bonding structure 100 is difficult to become a layered structure. Therefore, it is possible to form the structure by controlling the processing temperature, processing time, and pressure by utilizing solid-phase diffusion that does not generate a liquid phase, or by controlling the temperature gradient during the bonding process by utilizing liquid phase bonding to form a desired stacked structure. For example, the electronic component 2 side is brought into contact with the heating plate 61, and the wiring substrate 3 side is brought into contact with the cooling plate 60, so that only the contact portion between the first metal layer 21 containing the first metal and the second metal layer 22 containing the second metal is melted. Moreover, by lowering the heating temperature and increasing the cooling temperature, the melted portion is slowly moved toward the wiring substrate 3 side, thereby obtaining a stacked structure, rather than a eutectic structure ( Figure 4 (b)).

[0048] Next, the operation and effects of the joining structure 100 of the present embodiment will be described.

[0049] The bonding structure 100 of the present embodiment is formed by bonding the electronic component 2 and the wiring substrate 3, and comprises, in order from the electronic component 2 side: a first metal layer 21 including a metal that forms an intermetallic compound with Sn, an intermetallic compound layer 25 composed of an intermetallic compound including Sn, and a second metal layer 22 including Sn. The thickness of the second metal layer 22 is 50% or less of the total thickness of the first metal layer 21, the intermetallic compound layer 25, and the second metal layer 22.

[0050] In the bonding structure 100 of the present embodiment, the thickness of the second metal layer 22 is 50% or less of the total thickness of the first metal layer 21, the intermetallic compound layer 25, and the second metal layer 22. This means that in the initial bonding state, the metal element (Au) that forms an intermetallic compound with Sn exists in a wider range than the central part of the bonding structure 100. In this case, the concentration gradient of the metal element that forms an intermetallic compound with Sn, which becomes a driving force for diffusion, can be reduced, and Kirkendall voids can be suppressed.

[0051] The first metal layer 21 may include Au. Au easily forms an intermetallic compound with Sn, and Au easily diffuses into a layer including Sn, so it is a metal element that easily forms Kirkendall voids. In contrast, by adopting the structure of this embodiment, Kirkendall voids can be suppressed even when Au is used.

[0052] The intermetallic compound layer 25 may be present on the terminal 10 (conductive film 12) of the wiring substrate 3. By having the intermetallic compound layer 25 containing Sn on the terminal 10 of the wiring substrate 3, the concentration gradient of the metal element forming the intermetallic compound with Sn is low, and diffusion is not easily generated, so that Kirkendall voids can be suppressed.

[0053] The terminal 10 of the wiring substrate 3 may have a conductive film 12 containing Ni formed on the surface. The conductive film 12 containing Ni can suppress the reaction of the metal element forming the intermetallic compound with Sn inside the terminal 10 of the wiring substrate 3. As a result, the diffusion distance of the metal element forming the intermetallic compound with Sn can be suppressed, and the Kirkendall void can be suppressed.

[0054] The volume ratio of the second metal layer 22 may be 50% or less of the total volume of the first metal layer 21, the intermetallic compound layer 25, and the second metal layer 22. This makes it difficult for the metal element forming the intermetallic compound with Sn to diffuse, and Kirkendall voids can be suppressed.

[0055] The volume ratio of the first metal layer 21 may be less than 50% of the total volume of the first metal layer 21, the intermetallic compound layer 25, and the second metal layer 22. By reducing the volume of the first metal layer 21 including the metal element that forms an intermetallic compound with Sn, the diffusion of the element can be reduced, and Kirkendall voids can be suppressed.

[0056] The joining structure 100 of this embodiment joins the electronic component 2 and the wiring substrate 3, and comprises, in order from the electronic component 2 side: a first metal layer 21 including a metal that forms an intermetallic compound with Sn, and an intermetallic compound layer 25 composed of an intermetallic compound including Sn, and the intermetallic compound layer 25 is present on the terminal 10 of the wiring substrate 3.

[0057] The bonding structure 100 of the present embodiment is a laminated structure of the first metal layer 21 of the metal that forms an intermetallic compound with Sn and an intermetallic compound containing Sn, rather than a eutectic structure. In addition, the intermetallic compound layer 25 reaches the terminal 10 of the wiring substrate 3. Therefore, the concentration gradient of the metal element that forms an intermetallic compound with Sn, which serves as a driving force for diffusion, can be reduced, and the Kirkendall void can be suppressed.

[0058] The terminal 10 of the wiring substrate 3 may have a conductive film 12 containing Ni formed on the surface. The conductive film 12 containing Ni can suppress the reaction of the metal element that forms an intermetallic compound with Sn inside the terminal 10 of the wiring substrate 3. As a result, the diffusion distance of the metal element that forms an intermetallic compound with Sn can be suppressed, and the Kirkendall void can be suppressed.

[0059] The joining structure 100 of the present embodiment joins the electronic component 2 to the wiring substrate 3, and comprises: a first metal layer 21 including a metal that forms an intermetallic compound with Sn, an intermetallic compound layer 25 composed of an intermetallic compound including Sn, and a second metal layer 22 including Sn, wherein the volume ratio of the second metal layer 22 can be less than 50% of the total volume of the first metal layer 21, the intermetallic compound layer 25 and the second metal layer 22.

[0060] In the bonding structure 100 of the present embodiment, the volume ratio of the second metal layer 22 is less than 50% of the total volume of the first metal layer 21, the intermetallic compound layer 25, and the second metal layer 22. This means that in the initial state of bonding, the metal element that forms the intermetallic compound with Sn exists in a wide range in the bonding structure. In this case, the concentration gradient of the metal element that forms the intermetallic compound with Sn, which becomes the driving force for diffusion, can be reduced, and the Kirkendall void can be suppressed.

[0061] The present invention is not limited to the above-mentioned embodiments.

[0062] The arrangement, size, or number of each layer of the junction structure is not particularly limited and can be appropriately changed within the scope of the gist of the present invention.

[0063] [Example] Reference Figure 7 , Examples 1 to 8 and Comparative Examples 1 and 2 are described. However, the present invention is not limited to these examples. First, a method for manufacturing a mounting substrate 1 of the examples and comparative examples is described. An LED is prepared as an electronic component 2, and an Au terminal 7 is formed on the LED. After the electrodeposition of a Ni conductive film 12 is formed on the Cu terminal 10 on the substrate side, a Sn bonding material 4A is formed on the conductive film 12. While the Au terminal 7 of the electronic component 2 is in contact with the Sn bonding material 4A of the wiring substrate 3, a pressure of 0.05 to 0.20 MPa is applied, while the wiring substrate 3 side is in contact with a cooling plate 60 so that it is always 50°C, and the electronic component 2 side is in contact with a heating plate 61 at 300°C to 310°C. When the contact surface begins to react, the temperature of the cooling plate 60 is appropriately increased and the temperature of the heating plate 61 is decreased, and the thickness of the intermetallic compound layer 25 is controlled to obtain a bonding structure.

[0064] Regarding Examples 1 to 6 and Comparative Examples 1 and 2, they were manufactured under the same conditions except for adjusting the temperature control. Regarding Examples 7 and 8, they were formed under the same conditions except that the area of ​​the Sn bonding material 4A was electroplated to be 5 times that of Example 2, and the current during electroplating was adjusted so that the height of the bonding material 4A was the same. Regarding the thickness of each layer of the bonding layer 40, the phase identification of each layer was carried out based on the element ratio obtained by SEM-EDS measurement, and the thickness of each layer of the bonding layer 40 was measured by the above-mentioned method of measuring the thickness of each layer based on the SEM image. The ratio of the thickness of each layer to the entire bonding layer 40 is shown in Figure 7 In addition, the area of ​​each layer is measured from the SEM image, and based on this, the ratio of the volume of the first metal layer 21 and the second metal layer 22 to the volume of the entire bonding layer 40 is measured by the above method. The ratio is shown in Figure 7 Then, the mounting substrates 1 of Examples 1 to 8 and Comparative Examples 1 and 2 were put into a constant temperature and humidity test, and after a light emission test was performed on the mounting substrates 1 after the test, the substrates were cut perpendicularly to the wiring substrate 3 near the center of the bonding layer 40, and the number of KV (Kirkendall gaps) in the cross section was measured. The measurement results are shown in Figure 7 Furthermore, the SEM image of Example 1 is shown in Figure 5 (a) The SEM image of Comparative Example 2 is shown in Figure 5 (b) In Example 1, the AuSn layer 34 is formed on the lower side of the terminal 7 .

[0065] In Comparative Example 1, the intermetallic compound layer is 0%, Au and Sn are not bonded, and although it is believed that Au and Sn are in contact and emit light before the test, the contact part is separated after the test and no light is emitted. In Comparative Example 2, the diffusion of Au is insufficient, and it is believed that more KV is generated, and the bonding layer 40 is broken and no light is emitted. In Example 6, a small amount of Au diffuses into Sn before the test, and it is believed that no breakage will occur, and poor light emission is suppressed. In Examples 2 and 4, Au diffuses into Sn before the test, and it is believed that the number of KVs generated after the test is less than that in Example 6. In Examples 1, 3, and 5, more Au diffuses into Sn before the test, and it is believed that the number of KVs generated after the test is less than that in Examples 2, 4, and 6. According to Examples 7 and 8, it is believed that even if the precipitation volume of the Sn alloy increases, the effect of the present invention can be obtained as long as the thickness ratio is the same.

[0066] [Form 1] A bonding structure that bonds an electronic component to a wiring substrate, and From the electronic components side, the following are included in order: a first metal layer including a metal that forms an intermetallic compound with Sn, an intermetallic compound layer composed of an intermetallic compound containing Sn, and A second metal layer comprising Sn, The thickness of the second metal layer is 50% or less of the total thickness of the first metal layer, the intermetallic compound layer, and the second metal layer. [Form 2] The junction structure as described in aspect 1, wherein the first metal layer contains Au. [Form 3] The joining structure as described in aspect 1 or 2, wherein the intermetallic compound layer exists on the terminal of the wiring substrate. [Form 4] The junction structure described in any one of aspects 1 to 3, wherein the terminal of the wiring substrate has a conductive film containing Ni formed on the surface. [Form 5] In the joint structure described in any one of aspects 1 to 4, the volume ratio of the second metal layer is 50% or less of the total volume of the first metal layer, the intermetallic compound layer, and the second metal layer. [Form 6] In the joint structure described in any one of aspects 1 to 5, the volume ratio of the first metal layer is 50% or less of the total volume of the first metal layer, the intermetallic compound layer, and the second metal layer. [Form 7] A bonding structure is formed by bonding an electronic component to a wiring substrate, and From the electronic components side, the following are included in order: a first metal layer including a metal that forms an intermetallic compound with Sn, and an intermetallic compound layer composed of an intermetallic compound containing Sn, The intermetallic compound layer exists on the terminal of the wiring substrate. [Form 8] In the junction structure described in aspect 7, the terminal of the wiring substrate has a conductive film containing Ni formed on the surface. [Form 9] A joining structure is formed by joining an electronic component and a wiring substrate, and comprises: a first metal layer including a metal that forms an intermetallic compound with Sn, an intermetallic compound layer composed of an intermetallic compound containing Sn, and A second metal layer comprising Sn, The volume ratio of the second metal layer is 50% or less of the total volume of the first metal layer, the intermetallic compound layer, and the second metal layer.

Explanation of symbols

[0067] 2: Electronic components 3: Wiring board 10:Terminal 12: Conductive film 21: 1st metal layer 22: 2nd metal layer 25: Intermetallic compound layer 100: Joint structure.

Claims

1. A joining structure, in, It is a joint structure formed by joining electronic components to a wiring substrate. The bonding structure comprises, in order from the electronic component side: a first metal layer including a metal that forms an intermetallic compound with Sn; an intermetallic compound layer composed of an intermetallic compound including Sn; and A second metal layer comprising Sn, The thickness of the second metal layer is 50% or less of the total thickness of the first metal layer, the intermetallic compound layer, and the second metal layer.

2. The joining structure according to claim 1, in, The first metal layer includes Au.

3. The joining structure according to claim 1, in, The intermetallic compound layer exists on a terminal of the wiring substrate.

4. The joining structure according to claim 1, in, The terminal of the wiring substrate has a conductive film containing Ni formed on the surface.

5. The joining structure according to claim 1, in, The volume ratio of the second metal layer is 50% or less of the total volume of the first metal layer, the intermetallic compound layer, and the second metal layer.

6. The joining structure according to claim 1, in, The volume ratio of the first metal layer is 50% or less of the total volume of the first metal layer, the intermetallic compound layer, and the second metal layer.

7. A joint structure, in, It is a joint structure formed by joining electronic components to a wiring substrate. The electronic components are provided in order: a first metal layer including a metal that forms an intermetallic compound with Sn; and an intermetallic compound layer composed of an intermetallic compound containing Sn, The intermetallic compound layer exists on a terminal of the wiring substrate.

8. The joining structure according to claim 7, in, The terminal of the wiring substrate has a conductive film containing Ni formed on the surface.

9. A joint structure, in, It is a joint structure formed by joining electronic components to a wiring substrate. have: a first metal layer including a metal that forms an intermetallic compound with Sn; an intermetallic compound layer composed of an intermetallic compound including Sn; and A second metal layer comprising Sn, The volume ratio of the second metal layer is 50% or less of the total volume of the first metal layer, the intermetallic compound layer, and the second metal layer.

Citation Information

Patent Citations

  • Solder-joint layer

    JP2003286531A