Method for manufacturing non-aqueous electrolyte battery
By forming a combination of lithium-aluminum alloy layer and carbon layer on the negative electrode surface, the problems of expansion at high temperature and reduced discharge characteristics at low temperature in non-aqueous electrolyte batteries are solved, achieving excellent battery characteristics over a wide temperature range.
Patent Information
- Application Number
- CN202411235627.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2019-06-10
- Filing Date
- 2020-06-05
- Publication Date
- 2024-11-05
AI Technical Summary
Existing non-aqueous electrolyte batteries tend to expand when stored at high temperatures and their discharge characteristics decrease at low temperatures, making it difficult to maintain excellent battery characteristics over a wide temperature range.
A lithium-aluminum alloy layer is formed on the surface of the negative electrode, and a carbon layer is further formed on it. The lithium-aluminum alloy layer is formed through the reaction between the lithium layer and the aluminum layer. The carbon layer is combined to suppress battery expansion during high-temperature storage and improve discharge performance at low temperatures.
It effectively suppressed battery expansion during high-temperature storage, improved discharge performance at low temperatures, especially exhibited excellent load characteristics at -40℃, and reduced the decrease in discharge voltage after high-temperature storage.
Smart Images

Figure CN118899459A_ABST
Abstract
Description
[0001] The present invention is a divisional application of the invention application with application number 2020800419061, application date June 5, 2020, and invention name “Non-aqueous electrolyte battery and its manufacturing method”. Technical Field
[0002] The present invention relates to a non-aqueous electrolyte battery having excellent high-temperature storage characteristics and low-temperature load characteristics and a method for producing the same. Background Art
[0003] Currently, non-aqueous electrolyte batteries such as lithium primary batteries and lithium ion secondary batteries having non-aqueous electrolytes are used in various fields, such as power sources for portable devices, and are exposed to high temperatures and large vibrations, such as power sources for pressure sensors inside tires. In order to cope with the expansion of such uses, attempts have been made to improve various characteristics.
[0004] However, when batteries are stored at high temperatures, a reaction between the electrolyte and the electrodes occurs, causing problems such as battery expansion. Therefore, for applications where batteries are used in high temperature environments, measures to suppress the reaction between the electrolyte and the electrodes are required.
[0005] In contrast, sulfur compounds such as propane sultone are known as additives that can suppress reaction with an electrolyte solution and suppress battery expansion during high-temperature storage by forming a coating on the surface of a positive electrode or a negative electrode (Patent Document 1).
[0006] In addition, Patent Document 2 discloses that by using a non-aqueous electrolyte containing lithium bis(oxalatoborate) [LiB(C2O4)2] and LiBF4 in a molar ratio of 2:8 to 5:5, an increase in internal resistance caused by water released from the positive electrode active material into the electrolyte at high temperatures and an increase in internal pressure caused by decomposition of the electrolyte can be prevented, thereby forming a battery that can obtain excellent characteristics at both low and high temperatures.
[0007] However, when additives such as propane sultone and lithium bis(oxalatoborate) are contained in the electrolyte to produce sufficient effects, for example, a film formed on the negative electrode surface inhibits the discharge reaction and increases the internal resistance of the battery, which easily causes a problem of reduced discharge characteristics after high-temperature storage.
[0008] On the other hand, Patent Documents 3 and 4 propose forming a layer containing carbon on the surface of a negative electrode as a method of replacing the above-mentioned additives.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Application Publication No. 2004-47413
[0012] Patent Document 2: Japanese Patent Application Publication No. 2006-269173
[0013] Patent Document 3: Japanese Patent Application Publication No. 2010-257828
[0014] Patent Document 4: Japanese Patent Application Publication No. 2011-091034 Summary of the invention
[0015] Problems to be solved by the invention
[0016] However, non-aqueous electrolyte batteries are required to have battery characteristics that can be used in a wide range of temperature environments including low temperatures, not only at high temperatures. Further research is needed to achieve both storage characteristics at high temperatures and load characteristics at low temperatures.
[0017] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a non-aqueous electrolyte battery having excellent high-temperature storage characteristics and low-temperature load characteristics, and a method for manufacturing the same.
[0018] Methods for solving problems
[0019] The nonaqueous electrolyte battery of the present invention is characterized in that it comprises a positive electrode, a negative electrode, a separator and a nonaqueous electrolyte, wherein the negative electrode has a lithium layer with a lithium-aluminum alloy layer formed on the surface, and further has a carbon layer on the lithium-aluminum alloy layer.
[0020] The non-aqueous electrolyte battery of the present invention is manufactured by a manufacturing method (manufacturing method of the non-aqueous electrolyte battery of the present invention) having the following steps, namely: a step of stacking an aluminum layer on the surface of a lithium layer; a step of further forming a carbon layer on the surface of the above-mentioned aluminum layer; and a step of causing the above-mentioned lithium layer to react with the above-mentioned aluminum layer to form a lithium-aluminum alloy layer on the surface of the lithium layer.
[0021] Effects of the Invention
[0022] According to the present invention, a nonaqueous electrolyte battery having excellent high-temperature storage characteristics and load characteristics at low temperatures and a method for producing the same can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a longitudinal cross-sectional view schematically showing an example of the nonaqueous electrolyte battery of the present invention.
[0024] Figure 2 This is a graph showing the measurement results of the discharge voltage of the non-aqueous electrolyte battery of the example. DETAILED DESCRIPTION
[0025] The non-aqueous electrolyte battery of the present invention comprises a negative electrode having a lithium layer with a lithium-aluminum alloy layer formed on the surface, and further having a carbon layer on the lithium-aluminum alloy layer. The reason is not clear, but by using the above-mentioned negative electrode, it is possible to suppress the reduction of battery characteristics during high-temperature storage, and improve the load characteristics of the non-aqueous electrolyte battery after high-temperature storage at low temperatures (for example, load characteristics at low temperatures of -40°C).
[0026] The lithium-aluminum alloy layer possessed by the negative electrode can be formed, for example, as follows: an aluminum layer composed of aluminum foil or aluminum alloy foil is arranged on the surface of a lithium layer composed of lithium foil or lithium alloy foil to form a stack, and a carbon layer is further formed on the surface of the aluminum layer of the stack (the surface on the opposite side to the lithium layer) to obtain a stack for the negative electrode, and the stack for the negative electrode is brought into contact with a non-aqueous electrolyte to cause the lithium layer and the aluminum layer to react.
[0027] When the above-mentioned negative electrode laminate is contacted with a non-aqueous electrolyte to form a lithium-aluminum alloy layer, it can also be implemented before the battery is assembled. In this case, the negative electrode obtained by changing the aluminum layer of the above-mentioned negative electrode laminate to a lithium-aluminum alloy layer is used for the assembly of a non-aqueous electrolyte battery. On the other hand, the battery can also be assembled using the above-mentioned negative electrode laminate instead of the negative electrode, and the above-mentioned negative electrode laminate is contacted with a non-aqueous electrolyte during its assembly, and a lithium-aluminum alloy layer is formed in the same manner as above to obtain a negative electrode. In this case, the negative electrode manufacturing process before the battery assembly can be simplified, so it is preferred from the perspective of being able to further improve the productivity of the battery.
[0028] As lithium foil or lithium alloy foil for forming a lithium layer, there can be listed foil (lithium foil) composed of Li (and inevitable impurities); foil (lithium alloy foil) composed of a Li alloy containing Fe, Ni, Co, Mn, Cr, V, Ti, Zr, Nb, Mo, etc. as alloy components in an amount of less than 40 mass %, preferably less than 10 mass %, more preferably less than 5 mass %, and the rest being Li and inevitable impurities; etc.
[0029] The thickness of the lithium foil or lithium alloy foil constituting the lithium layer is preferably 0.1 to 1.5 mm.
[0030] Examples of the aluminum foil or aluminum alloy foil used to constitute the aluminum layer include a foil (aluminum foil) composed of Al (and inevitable impurities); a foil (aluminum alloy foil) composed of an Al alloy containing Fe, Ni, Co, Mn, Cr, V, Ti, Zr, Nb, Mo, etc. as alloy components and the remainder being Al and inevitable impurities (the content of the above alloy components is, for example, 50 mass % or less in total, preferably 10 mass % or less, and more preferably 5 mass % or less); and the like.
[0031] In order to clearly demonstrate the effects of the present invention by forming the lithium-aluminum alloy layer, the thickness of the aluminum foil or aluminum alloy foil constituting the aluminum layer is preferably 1 μm or more, more preferably 3 μm or more, and particularly preferably 5 μm or more.
[0032] On the other hand, if the ratio of the lithium-aluminum alloy layer to the lithium layer is too much, the capacity of the negative electrode will be reduced. In addition, due to the volume expansion of the aluminum layer when alloying with lithium, the aluminum layer (aluminum alloy layer) will cause cracks, but if the thickness of the aluminum layer becomes thicker, the above cracks will occur deep inside the negative electrode, and there is a risk of a part of the aluminum alloy layer falling off when subjected to large vibrations. Therefore, in order to make the thickness of the lithium-aluminum alloy layer formed below a certain value, the thickness of the aluminum foil and the aluminum alloy foil is preferably set to 20 μm or less, and more preferably set to 15 μm or less.
[0033] It should be noted that the aluminum alloy layer may not be formed on the entire surface of the lithium layer, and may be formed on a portion of the lithium layer surface. However, the more the area ratio of the aluminum alloy layer is formed, the easier it is to produce the effect of the present invention, so the area ratio of the aluminum alloy layer formed on the lithium layer surface is preferably 40% or more, more preferably 70% or more, and most preferably 100%, that is, the aluminum alloy layer is formed on the entire surface of the lithium layer.
[0034] The aluminum layer can be formed on one or both sides of the lithium layer depending on the shape of the battery. For example, in a battery with positive electrodes arranged on both sides of the negative lithium layer, aluminum layers can be provided on both sides of the lithium layer to form a lithium-aluminum alloy layer.
[0035] The laminate having the lithium layer and the aluminum layer can be formed by laminating and pressing a lithium foil or a lithium alloy foil for constituting the lithium layer and an aluminum foil or an aluminum alloy foil for constituting the aluminum layer.
[0036] The carbon layer of the negative electrode may be composed of carbon (particles thereof) alone, or may contain both carbon and a binder.
[0037] Examples of carbon constituting the carbon layer include carbon black such as furnace black, channel black, acetylene black, and thermal black; graphites such as natural graphite (such as flaky graphite) and artificial graphite; and the like. Only one of these may be used, or two or more of them may be used in combination.
[0038] In addition, as binders that can be used in the carbon layer, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), polyvinyl pyrrolidone, etc. In particular, compounds having a five-membered ring lactam structure such as polyvinyl pyrrolidone can well disperse tiny carbon materials such as carbon black when dissolved in a solvent, and are therefore preferably used.
[0039] The content of the binder in the carbon layer is preferably 2% by mass or less, more preferably 1% by mass or less, and particularly preferably 0.5% by mass or less.
[0040] From the viewpoint of ensuring the above-mentioned effect well by forming the carbon layer, the weight per unit area of the carbon layer in the negative electrode is preferably 0.15 mg / cm 2 More preferably 0.3 mg / cm 2 Above, particularly preferably 0.5 mg / cm 2 However, even if the carbon layer is thickened, the effect will be saturated. In addition, the overall thickness of the negative electrode will decrease, for example, the amount of positive electrode active material that can be introduced into the battery will decrease, which may cause a risk of reducing the battery capacity. Therefore, from the perspective of increasing the battery capacity, the unit area weight of the carbon layer in the negative electrode is preferably 1.5 mg / cm 2 Below, more preferably 1.0 mg / cm 2 the following.
[0041] It should be noted that the carbon layer may not be formed on the entire surface of the aluminum alloy layer, and the carbon layer may be formed on a portion of the surface of the aluminum alloy layer. That is, a portion of the aluminum alloy layer may not be covered by the carbon layer and may be exposed on the surface of the negative electrode. For example, when a lithium-aluminum alloy layer is formed, its surface may become concave-convex, and the convex portion may be exposed on the surface of the negative electrode. In addition, a portion of the surface of the lithium layer may also have a portion where the carbon layer is directly formed without forming the aluminum alloy layer.
[0042] However, the larger the area ratio of the portion where the aluminum alloy layer and the carbon layer are formed on the lithium layer becomes, the easier it is to produce the effect of the present invention. Therefore, the area ratio of the carbon layer formed on the surface of the aluminum alloy layer is preferably 40% or more, more preferably 70% or more, and particularly preferably 100%, that is, the carbon layer is formed on the entire surface of the aluminum alloy layer.
[0043] Furthermore, it is most preferred that the aluminum alloy layer is formed on the entire surface of the lithium layer, and the carbon layer is formed on the entire surface of the aluminum alloy layer.
[0044] The carbon layer can be formed, for example, by applying a carbon layer forming composition (a liquid composition such as a paste or slurry) prepared by dispersing carbon and a binder added as needed in an organic solvent (the binder may also be soluble) to the surface of the aluminum layer in a stack having a lithium layer and an aluminum layer and drying it.
[0045] As an organic solvent used in the composition for forming the carbon layer, it is preferred to use a solvent used in the non-aqueous electrolyte possessed by the battery. As specific examples thereof, cyclic carbonates such as ethylene carbonate, propylene carbonate (PC), butylene carbonate, and vinylene carbonate can be cited; chain carbonates such as dimethyl carbonate, diethyl carbonate, and methyl ethyl carbonate; ethers such as 1,2-dimethoxyethane (DME), diethylene glycol dimethyl ether (diethylene glycol dimethyl ether), triethylene glycol dimethyl ether (triethylene glycol dimethyl ether), tetraethylene glycol dimethyl ether (tetraethylene glycol dimethyl ether), methoxyethoxyethane, 1,2-diethoxyethane, and tetrahydrofuran; cyclic esters such as γ-butyrolactone; nitrile; etc., one or two of them can be used, and carbonates such as propylene carbonate react with lithium to form lithium carbonate, which has the risk of reducing the reactivity of the negative electrode surface, so from the viewpoint of making it easier to exert the effect of the present invention, it is preferred to use a solvent other than a carbonate, more preferably an ether, and further preferably DME.
[0046] In addition, as the organic solvent used in the carbon layer forming composition, the solvent used when forming a coating such as a slurry having a positive electrode active material can also be used. In the case of using a tiny carbon material such as carbon black, since compounds having a five-membered ring lactam structure such as 2-pyrrolidone and N-methyl-2-pyrrolidone (NMP) can disperse the above-mentioned carbon material well, it is preferably used. The above-mentioned compound having a five-membered ring lactam structure can also be mixed with the solvent used in the above-mentioned non-aqueous electrolyte for use.
[0047] The negative electrode may be composed only of a lithium layer, a lithium-aluminum alloy layer, and a carbon layer, and may further include a current collector as necessary.
[0048] As the negative electrode current collector, there can be cited negative electrode current collectors made of copper, nickel, iron, and stainless steel as raw materials, and as its form, there can be cited flat woven metal mesh, expanded metal mesh, lath mesh, stamped metal, metal foam, foil (plate), etc. The thickness of the current collector is preferably 5 to 100 μm, for example. It is also preferred to apply a paste-like conductive material such as carbon paste or silver paste on the surface of such a current collector in advance.
[0049] The positive electrode involved in the non-aqueous electrolyte battery can, for example, use a formed body formed by forming a mixture containing a positive electrode active material, a conductive aid, a binder, etc. (positive electrode mixture) into particles, or a positive electrode having a layer (positive electrode mixture layer) composed of the above-mentioned positive electrode mixture on one or both sides of the collector.
[0050] As the positive electrode active material, manganese dioxide, lithium-containing manganese oxides [e.g., LiMn3O6, composite oxides having the same crystal structure as manganese dioxide (β-type, γ-type, or a structure in which β-type and γ-type are mixed, etc.), Li content of 3.5 mass % or less, preferably 2 mass % or less, more preferably 1.5 mass % or less, particularly preferably 1 mass % or less, etc.], Li a Ti 5 / 3 O4 (4 / 3≦a<7 / 3) and other lithium-containing composite oxides; vanadium oxides; niobium oxides; titanium oxides; sulfides such as iron disulfide; graphite fluoride; etc.
[0051] Examples of the conductive additive used in the positive electrode mixture include flake graphite, acetylene black, Ketjen black, and carbon black. These may be used alone or in combination of two or more.
[0052] Furthermore, examples of the binder in the positive electrode mixture include fluororesins such as PVDF, PTFE, and hexafluoropropylene polymers, and these may be used alone or in combination of two or more.
[0053] In the case of a positive electrode mixture molded body, the positive electrode can be produced by, for example, press-molding a positive electrode mixture prepared by mixing a positive electrode active material, a conductive aid, a binder, and the like into a predetermined shape.
[0054] In addition, in the case of a positive electrode having a positive electrode mixture layer and a current collector, it can be manufactured, for example, through the following steps, namely: the positive electrode active material, conductive aid and binder are dispersed in water or an organic solvent such as N-methyl-2-pyrrolidone (NMP) to prepare a composition (slurry, paste, etc.) containing the positive electrode mixture (the binder can also be dissolved in the solvent), apply it on the collector and dry it, and perform a pressing treatment such as calendering as needed.
[0055] However, the positive electrode is not limited to the positive electrode manufactured by the above-mentioned methods, and may be a positive electrode manufactured by other methods.
[0056] As the composition of the positive electrode mixture for the positive electrode, the amount of the positive electrode active material is preferably 80 to 90% by mass, the content of the conductive aid is preferably 1.5 to 10% by mass, and the content of the binder is preferably 0.3 to 10% by mass.
[0057] In the case of a positive electrode mixture molded body, the thickness is preferably 0.15 to 4 mm. On the other hand, in the case of a positive electrode having a positive electrode mixture layer and a current collector, the thickness of the positive electrode mixture layer (thickness per side of the current collector) is preferably 30 to 300 μm.
[0058] When a current collector is used in the positive electrode, as the current collector, for example, a current collector made of stainless steel such as SUS316, SUS430, SUS444, etc. can be cited, and as its form, a plain woven metal mesh, an expanded metal mesh, a lath mesh, a stamped metal, a metal foam, a foil (plate), etc. can be exemplified. The thickness of the current collector is preferably 0.05 to 0.2 mm, for example. It is also preferred to apply a paste-like conductive material such as a carbon paste or a silver paste on the surface of such a current collector in advance.
[0059] The non-aqueous electrolyte battery of the present invention is assembled using a laminated body (laminated electrode body) formed by laminating the above-mentioned negative electrode and the above-mentioned positive electrode through a separator, a wound body (wound electrode body) formed by spirally winding the laminated body, and further forming the wound body into a flat wound body (flat wound electrode body) with a flat cross-section. In addition, the non-aqueous electrolyte battery of the present invention can also be assembled using a positive electrode composed of a formed body of a positive electrode mixture and the above-mentioned negative electrode, with a separator interposed between them and housed in a flat battery case.
[0060] Alternatively, a battery may be assembled using the negative electrode laminate instead of the negative electrode, and the negative electrode may be formed during the assembly.
[0061] The diaphragm uses nonwoven fabrics and microporous membranes (microporous membranes). As its raw materials, polyolefins such as polyethylene (PE), polypropylene (PP), and ethylene-propylene copolymers can be used. In addition, in the case of requiring heat resistance due to the relationship with battery use, fluororesins such as tetrafluoroethylene-perfluoroalkoxyethylene copolymers (PFA), polyphenylene sulfide (PPS), polyetheretherketone (PEEK), polybutylene terephthalate (PBT), polymethylpentene, polyamide, polyimide, aromatic polyamide, cellulose, etc. can also be used. The raw materials of nonwoven fabrics and microporous membranes can use only one of the raw materials exemplified above, or two or more can be used. In addition, the nonwoven fabrics and microporous membranes forming the diaphragm can also use nonwoven fabrics and microporous membranes of a laminated structure formed by laminating multiple nonwoven fabrics and microporous membranes composed of different raw materials, in addition to the nonwoven fabrics and microporous membranes of the monolayer structure formed by the raw materials exemplified above.
[0062] From the viewpoint of suppressing the reduction of the energy density of the battery, the thickness of the separator can be, for example, 500 μm or less, preferably 450 μm or less, and more preferably 300 μm or less. However, if the separator is too thin, there is a risk of reducing the function of preventing short circuits, so when a non-woven fabric is used, the thickness can be, for example, 30 μm or more, preferably 100 μm or more, and more preferably 150 μm or more. In addition, when a microporous membrane is used, it is preferably 10 μm or more, and more preferably 15 μm or more.
[0063] As the non-aqueous electrolyte of the non-aqueous electrolyte battery, there can be listed non-aqueous electrolytes prepared by dissolving LiPF6, LiBF4, LiClO4, LiCF3SO3, etc. as electrolytes in organic solvents. As the organic solvent, there can be listed cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, and vinylene carbonate; chain carbonates such as dimethyl carbonate, diethyl carbonate, and methyl ethyl carbonate; ethers such as 1,2-dimethoxyethane, diethylene glycol dimethyl ether (diethylene glycol dimethyl ether), triethylene glycol dimethyl ether (triethylene glycol dimethyl ether), tetraethylene glycol dimethyl ether (tetraethylene glycol dimethyl ether), methoxyethoxyethane, 1,2-diethoxyethane, and tetrahydrofuran; cyclic esters such as γ-butyrolactone; mononitriles such as acetonitrile and propionitrile; etc., and one or more of them can be used. It is particularly preferred to use the above-mentioned carbonates and ethers in combination.
[0064] When carbonate and ether are used together as the nonaqueous electrolyte solvent, the amount ratio (mixing ratio) of carbonate and ether in the total solvent is preferably carbonate:ether=30:70 to 70:30 in terms of volume ratio.
[0065] The concentration of the electrolyte in the non-aqueous electrolyte is preferably 0.3 to 1.5 mol / l.
[0066] Furthermore, in order to improve the storage characteristics at high temperatures, the non-aqueous electrolyte may contain additives as needed. Examples of additives that can be used include saturated sultone compounds such as 1,3-propane sultone and 1,4-butane sultone; unsaturated sultone compounds such as 1,3-propylene sultone; acid anhydrides such as maleic anhydride and phthalic anhydride; organic boron lithium salts such as LiB(C2O4)2; dinitriles such as malononitrile, succinonitrile, glutaronitrile, and adiponitrile; etc., and one or more of them can be used.
[0067] The content of the above-mentioned additive in the nonaqueous electrolyte is, for example, preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and particularly preferably 0.5% by mass or more. On the other hand, if the content of the additive is too much, there is a risk that the internal resistance of the battery increases and the discharge characteristics decrease, so the content of the additive in the nonaqueous electrolyte is preferably 3% by mass or less, more preferably 2% by mass or less, and particularly preferably 1.5% by mass or less.
[0068] There is no particular limitation on the form of the non-aqueous electrolyte battery, and the non-aqueous electrolyte battery may be in various forms, such as a flat form (including a coin form and a button form), a laminated form, a cylindrical form [cylindrical form, a square form (square cylindrical form)], etc. In addition, as an outer package (battery case) that contains the negative electrode, the positive electrode, the separator, and the non-aqueous electrolyte inside, a metal can (outer package can) and a lid (sealing can) having an opening may be used in combination, or a metal laminate film may be used.
[0069] Specifically, a flat or cylindrical battery can be made by riveting the outer can and the sealing can with a gasket, or by welding the outer can and the sealing can to seal them. A laminated battery can be made by overlapping two sheets of metal laminate films, or by bending a sheet of metal laminate film and sealing it around.
[0070] It should be noted that, in the case of an outer body in the form of riveting and sealing, the raw material of the gasket between the outer tank and the sealing tank can be PP, nylon, etc., and in the case of requiring particularly high heat resistance due to the relationship with the battery use, fluororesins such as PFA, polyphenylene ether (PEE), polysulfone (PSF), polyarylate (PAR), polyethersulfone (PES), PPS, PEEK and other heat-resistant resins with a melting point or thermal decomposition temperature of 200°C or above can also be used. In addition, when the battery is used for applications requiring heat resistance, its seal can also be sealed with glass vacuum.
[0071] Example
[0072] Hereinafter, the present invention will be described in detail based on examples. However, the following examples do not limit the present invention.
[0073] (Example 1)
[0074] <Production of positive electrode>
[0075] A positive electrode mixture prepared by mixing manganese dioxide as a positive electrode active material, carbon black as a conductive aid, and PTFE as a binder in a mass ratio of 90:5:5 was molded to obtain a positive electrode (positive electrode mixture molded body) having a diameter of 16 mm and a thickness of 1.8 mm.
[0076] <Production of negative electrode laminate>
[0077] A 9 μm-thick aluminum foil was pressed onto one side of a 1.2 mm-thick lithium foil, and the foil was punched into a circular shape with a diameter of 16 mm to obtain a laminate of a lithium layer and an aluminum layer.
[0078] Next, acetylene black was dispersed in propylene carbonate to prepare a composition (slurry) for forming a carbon layer, and the slurry was applied to the aluminum layer of the laminate and dried to prepare a negative electrode laminate having a carbon layer composed of acetylene black formed on the entire surface of the aluminum layer of the laminate. The unit area weight of the carbon layer was 0.5 mg / cm 2 .
[0079] <Preparation of non-aqueous electrolyte>
[0080] LiClO4 was dissolved at a concentration of 0.5 mol / l in a mixed solvent of propylene carbonate and 1,2-dimethoxyethane at a volume ratio of 1:1, and 1,3-propane sultone was further added at 2 mass % to prepare a non-aqueous electrolyte.
[0081] <Battery Assembly>
[0082] The positive electrode, the negative electrode laminate and the non-aqueous electrolyte were used, and a non-woven fabric made of polymethylpentene (thickness: 320 μm) was used as the separator. Figure 1 The structure shown is a coin-shaped non-aqueous electrolyte primary battery with a diameter of 20 mm and a height of 3.2 mm.
[0083] By bringing the negative electrode laminate into contact with the nonaqueous electrolyte, a negative electrode is constructed in the battery in which a lithium-aluminum alloy layer is formed on the surface of the lithium layer and a carbon layer is further provided on the lithium-aluminum alloy layer.
[0084] (Example 2)
[0085] The weight per unit area of the carbon layer on the surface of the negative electrode laminate was set to 0.02 mg / cm 2 , a coin-shaped nonaqueous electrolyte primary battery was assembled in the same manner as in Example 1 except for the above.
[0086] (Example 3)
[0087] The weight per unit area of the carbon layer on the surface of the negative electrode laminate was set to 0.2 mg / cm 2 , a coin-shaped nonaqueous electrolyte primary battery was assembled in the same manner as in Example 1 except for the above.
[0088] (Example 4)
[0089] The weight per unit area of the carbon layer on the surface of the negative electrode laminate was set to 1 mg / cm 2 , a coin-shaped nonaqueous electrolyte primary battery was assembled in the same manner as in Example 1 except for the above.
[0090] (Example 5)
[0091] A coin-shaped nonaqueous electrolyte primary battery was assembled in the same manner as in Example 1 except that acetylene black was dispersed in 1,2-dimethoxyethane to prepare a slurry, and the carbon layer was formed using the slurry.
[0092] (Example 6)
[0093] The weight per unit area of the carbon layer on the surface of the negative electrode laminate was set to 0.02 mg / cm 2 , a coin-shaped nonaqueous electrolyte primary battery was assembled in the same manner as in Example 5 except for the above.
[0094] (Example 7)
[0095] The weight per unit area of the carbon layer on the surface of the negative electrode laminate was set to 0.2 mg / cm 2 , a coin-shaped nonaqueous electrolyte primary battery was assembled in the same manner as in Example 5 except for the above.
[0096] (Example 8)
[0097] The weight per unit area of the carbon layer on the surface of the negative electrode laminate was set to 1 mg / cm 2 , a coin-shaped nonaqueous electrolyte primary battery was assembled in the same manner as in Example 5 except for the above.
[0098] (Comparative Example 1)
[0099] The slurry prepared in Example 1 was applied to one side of a lithium foil having a thickness of 1.2 mm and dried to prepare a laminate of a lithium layer and a carbon layer having a carbon layer formed entirely on one side of the lithium layer. The unit area weight of the carbon layer was 0.5 mg / cm 2 A coin-shaped nonaqueous electrolyte primary battery was assembled in the same manner as in Example 1 except that the above-mentioned laminate was used instead of the negative electrode laminate of Example 1.
[0100] (Comparative Example 2)
[0101] Formation of the Carbon Layer A coin-shaped nonaqueous electrolyte primary battery was assembled in the same manner as in Comparative Example 1 except that the slurry prepared in Example 5 was used.
[0102] (Comparative Example 3)
[0103] A coin-shaped nonaqueous electrolyte primary battery was assembled in the same manner as in Example 1 except that the surface of the stack of lithium layers and aluminum layers was not coated with the carbon layer-forming composition and the stack was used directly for battery assembly.
[0104] Each battery of Examples 1 to 8 and Comparative Examples 1 to 3 was kept in a thermostatic chamber at -40°C. After the battery temperature dropped, it was discharged at a current value of 10 mA, and the battery discharge voltage (CCV) was measured 8 msec after the start of discharge to evaluate the load characteristics at low temperature before storage.
[0105] Separately from the above evaluation, each battery of Examples 1 to 8 and Comparative Examples 1 to 3 was stored in a high temperature environment of 120°C for 500 hours, and then the discharge voltage of the battery was measured in the same manner as above to evaluate the load characteristics at low temperature after high temperature storage. The respective measurement results are shown in Tables 1 and Figure 2 middle.
[0106] [Table 1]
[0107]
[0108] like Figure 2 As shown in the results, in the batteries of Examples 1 to 4 and Examples 5 to 8 in which a lithium-aluminum alloy layer is formed on the surface of the lithium layer of the negative electrode and a carbon layer is further formed on the above-mentioned lithium-aluminum alloy layer, in either case before storage or after high-temperature storage, the greater the unit area weight of the carbon layer, the higher the discharge voltage of the battery, and the more the load characteristics at low temperatures can be improved.
[0109] In addition, the batteries of Examples 5 to 8 using DME as a solvent for the carbon layer forming composition can improve the discharge voltage of the battery compared to the batteries of Examples 1 to 4 using PC, and can further suppress the reduction of the discharge voltage caused by high-temperature storage. This is believed to be because the carbon dispersion in the carbon layer forming composition using DME as a solvent is better, and a uniform carbon layer can be formed, and problems such as lithium carbonate generation when using PC as a solvent do not occur.
[0110] On the other hand, in the batteries of Comparative Examples 1 and 2 in which the carbon layer was directly formed on the surface of the lithium layer, even if the weight per unit area of the carbon layer was increased to 0.5 mg / cm 2 , the discharge voltage drop caused by high temperature storage also increased to about 1 V. In addition, for the battery of Comparative Example 3 in which a lithium-aluminum alloy layer is formed on the surface of the lithium layer but a carbon layer is not formed thereon, the discharge voltage drop caused by high temperature storage also increased to about 1 V.
[0111] In the battery of the present invention, as shown in Table 1, by forming a lithium-aluminum alloy layer between the lithium layer and the carbon layer, even if the weight per unit area of the carbon layer is reduced, the discharge voltage drop caused by high-temperature storage can be sufficiently suppressed.
[0112] The present invention can be implemented in any manner other than the above without departing from the scope of the present invention. The embodiments disclosed in this application are an example, and the present invention is not limited to these embodiments. Compared with the description of the above specification, the scope of the present invention is interpreted by the description of the attached claims first, and all changes within the scope equivalent to the claims are included in the claims.
[0113] Industrial Applicability
[0114] The nonaqueous electrolyte battery of the present invention is mainly in the form of a primary battery, but may also be in the form of a secondary battery, and can be applied to various uses of conventionally known nonaqueous electrolyte primary batteries and nonaqueous electrolyte secondary batteries.
[0115] Explanation of symbols
[0116] 1 Non-aqueous electrolyte battery
[0117] 2 Positive electrode
[0118] 3 Negative electrode
[0119] 4 Diaphragm
[0120] 5. External can
[0121] 6 Sealing jars
[0122] 7 Insulation gasket.
Claims
1. A method for manufacturing a non-aqueous electrolyte battery, characterized in that: The non-aqueous electrolyte battery comprises a positive electrode, a negative electrode, a separator and a non-aqueous electrolyte, wherein the negative electrode comprises a lithium layer having a lithium-aluminum alloy layer formed on the surface, and further comprises a carbon layer on the lithium-aluminum alloy layer, and the manufacturing method comprises the following steps: The process of laminating an aluminum layer on the surface of the lithium layer, a step of further forming a carbon layer on the surface of the aluminum layer, and and forming a lithium-aluminum alloy layer on a surface of the lithium layer by reacting the lithium layer with the aluminum layer.
2. The method for manufacturing a non-aqueous electrolyte battery according to claim 1, wherein the weight per unit area of the carbon layer is set to 0.15 mg / cm 2 above.
3. The method for manufacturing a non-aqueous electrolyte battery according to claim 1 or 2, wherein the weight per unit area of the carbon layer is set to 1.5 mg / cm 2 the following. 4 . The method for producing a nonaqueous electrolyte battery according to claim 1 , wherein a liquid composition obtained by dispersing carbon particles in an organic solvent is applied to the surface of the aluminum layer and dried to form the carbon layer. 5 . The method for producing a non-aqueous electrolyte battery according to claim 4 , wherein the liquid composition contains ether as the organic solvent. 6 . The method for producing a non-aqueous electrolyte battery according to claim 5 , wherein the ether is 1,2-dimethoxyethane. 7 . The method for producing a non-aqueous electrolyte battery according to claim 1 , wherein the carbon layer contains carbon black or graphite.
8. The method for manufacturing a non-aqueous electrolyte battery according to claim 1 or 2, wherein the carbon layer contains a binder.
9. The method for producing a nonaqueous electrolyte battery according to claim 1 or 2, wherein the positive electrode contains manganese dioxide or a lithium-containing manganese oxide having the same crystal structure as manganese dioxide and a Li content of 3.5 mass % or less as a positive electrode active material.
10. The method for manufacturing a non-aqueous electrolyte battery according to claim 1 or 2, wherein in the step of laminating an aluminum layer on the surface of a lithium layer, an aluminum alloy layer is laminated on the surface of the lithium layer as the aluminum layer, The area ratio of the portion on the surface of the lithium layer where the aluminum alloy layer is stacked is set to 40% or more. 11 . The method for manufacturing a non-aqueous electrolyte battery according to claim 10 , wherein the aluminum alloy layer is laminated on the entire surface of the lithium layer.
12. The method for manufacturing a non-aqueous electrolyte battery according to claim 1 or 2, wherein in the step of laminating an aluminum layer on the surface of a lithium layer, an aluminum alloy layer is laminated on the surface of the lithium layer as the aluminum layer, In the step of further forming a carbon layer on the surface of the aluminum alloy layer, an area ratio of a portion of the surface of the aluminum alloy layer where the carbon layer is formed is set to 70% or more. 13 . The method for manufacturing a non-aqueous electrolyte battery according to claim 12 , wherein the carbon layer is formed on the entire surface of the aluminum alloy layer.