Catalytic material based on group VIB and group IVB elements for hydrogen production by electrolysis of water
By using Group VIB and Group IVB metal composites in the form of sulfide in the electrochemical reduction reaction, combined with doping elements, the cost and scarcity of platinum catalysts are solved, the electrocatalytic performance of MoS2 catalysts is improved, and the electrolysis is achieved High-efficiency catalytic effect in water hydrogen production process.
Patent Information
- Application Number
- CN202380028346.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-18
- Filing Date
- 2023-03-08
- Publication Date
- 2024-11-05
AI Technical Summary
In the prior art, catalysts such as platinum for electrochemical reduction reactions have problems in terms of cost and scarcity, and the MoS2-based catalysts are not as catalytic as platinum, especially in the process of electrolyzing hydrogen production, with low efficiency and lack of Effectively dopant materials to enhance their inherent properties.
Catalytic materials containing Group VIB metals (such as molybdenum and tungsten) and Group IVB metals (such as titanium, zirconium, hafnium) in the form of sulfides are deposited on the conductive support through specific preparation methods to form titanium-molybdenum and zirconium -Molybdenum and other composite materials combine doping of boron, phosphorus and silicon to improve catalytic performance.
A catalytic performance similar to existing platinum catalysts is achieved, reducing production costs, and showing excellent electrocatalytic activity in the electrolytic water hydrogen production process, especially in cathode applications.
Abstract
Description
Prior art
[0002] Molecular hydrogen is now an important energy carrier in the energy transition. For current industrial applications (refineries, ammonia production, hydrogenation or reduction processes), molecular hydrogen must be produced with low greenhouse gas emissions. For example, it can be used in mobile applications (automobiles, heavy transport, railways, aviation) to replace methane in furnaces (the combustion of H2 actually only produces water) or to store intermittent solar or wind energy. One of the technologies for producing decarbonized hydrogen is the electrolysis of water. In a water electrolyzer, the hydrogen evolution reaction (HER) occurs at the cathode and the oxygen evolution reaction (OER) occurs at the anode. The overall reaction is:
[0003] H2O→H2+1 / 2 O2
[0004] The potential of the electrochemical proton reduction reaction is 0V / NHE, NHE is a standard hydrogen electrode, a reference electrode. This potential represents the thermodynamic energy required for reduction. However, the overpotential associated with the activation of the reaction by the material at the interface between electrons and protons (and where gas can be formed) must be added to this minimum thermodynamic energy. At present, the most widely used material for this electrocatalyst work, and in the case of proton exchange membrane (PEM) electrolyzers, is platinum. Although the electrocatalytic properties are excellent, platinum is expensive and scarce. In order to replace platinum with more abundant and cheaper materials but with the same or even better catalytic properties, a large amount of research work is currently underway.
[0005] Catalysts based on metals from column VIB of the periodic table, including MoS2, are of interest for electroreduction reactions, in particular for the production of H2. Patent applications US2022 / 0018033 and US2022 / 010439 disclose various methods for preparing catalysts using at least one active phase precursor based on a metal of group VIB and optionally at least one active phase precursor of a metal of group VIII.
[0006] MoS2-based materials have a layered structure to exhibit electrocatalytic properties in the HER. The active phase can be used in bulk form (when the electron conduction from the cathode is sufficient), or in a supported state, which then acts as a support of different properties. In the latter case, the support must have specific properties:
[0007] - High specific surface area to facilitate the dispersion of active phase;
[0008] -Excellent electronic conductivity;
[0009] -Chemical and electrochemical stability under water electrolysis conditions.
[0010] Carbon is the most commonly used support for PEM electrolyzers.
[0011] However, for the reaction of interest, MoS2 alone is still not as effective as platinum. For example, Y.Zhao et al., Sc.Reports, 5,8722 reported an overpotential of 50mV for platinum and an overpotential of 220mV for MoS2 in the form of nanosheets on graphene sheets. Several strategies can be developed to reduce the overpotential of catalysts based on MoS2. For example, it is recognized that catalysts showing high catalytic potential are characterized by the fact that the relevant active phases are perfectly dispersed on the support surface and show a high active phase content. However, once the catalyst is perfectly dispersed, its electrocatalytic properties are limited by its inherent properties.
[0012] In order to improve its intrinsic properties, MoS2 can be enhanced by various dopants. Document CN111847513 discloses dopants such as vanadium, chromium, manganese, rhenium, iridium, platinum or gold or metalloids such as fluorine, oxygen, selenium, tellurium, nitrogen, phosphorus, carbon or boron. Similarly, document CN110479311 includes MoS2 / graphene composites, in which MoS2 is doped with at least one of the following elements: vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, ruthenium, rhodium, palladium, silver, cadmium, platinum or gold. Other prior art documents are more specific to adding only one or two heteroatoms to dope molybdenum sulfide or form composites with it:
[0013] - Cobalt: CN107881529 discloses a catalyst comprising a cobalt disulfide phase, CN110026210 discloses a CN / Co4S3 / MoS2 catalyst, CN109046409 relates to a catalyst having cobalt phosphide-molybdenum sulfide nanosheets on carbon nanotubes, CN113668008 describes a Co-MoS2 catalyst on carbon nanotubes, CN113061928 discloses a catalyst based on molybdenum sulfide nanosheets and cobalt sulfide nanoparticles, CN107904620 describes a catalyst on a 3D support (with graphene and carbon nanotubes) and a molybdenum sulfide / cobalt sulfide composite, and CN109796044 discloses a catalyst based on cobalt-molybdenum sulfide supported on palladium.
[0014] - Nickel: CN108517534 discloses nickel-doped molybdenum sulfide, CN108441879 describes a composite material of molybdenum sulfide, nanoporous nickel and graphene, CN105655140 proposes a molybdenum sulfide-nickel sulfide-graphene composite material in the form of flakes, CN111992227 discloses a nickel-cobalt-molybdenum sulfide composite material, and CN110327946 discloses a molybdenum sulfide-nickel selenide composite material,
[0015] - Vanadium: CN109939699 proposes a flower-shaped vanadium-doped molybdenum sulfide catalyst, and CN107574454 describes a tungsten-doped vanadium dioxide nanotube / molybdenum sulfide composite material.
[0016] - Iron: US2021 / 170384 describes molybdenum sulfide nanosheets with dispersed iron phosphide nanoparticles,
[0017] - Gold: CN108654647 discloses molybdenum sulfide with gold nanoparticles,
[0018] -Cadmium: CN111229260 discloses a catalyst based on molybdenum sulfide and cadmium sulfide,
[0019] - Nitrogen, which can be used to dope the carbon support as described above, but can also form nitrides with molybdenum sulfide. For example, CN109161919 and CN113846347 disclose catalysts formed from carbonitride-molybdenum sulfide binary compounds and carbon / molybdenum sulfide-molybdenum nitride, respectively.
[0020] Catalysts based on molybdenum sulfide containing elements of Group IVB of the periodic table are rarely studied. Catalysts with molybdenum sulfide and the presence of titanium are only described in the literature. Typically, titanium is present in a substrate as described below: M.Medina et al., J.Braz.Chem.Soc.302210, E.Girel et al., Catalyst Today 292,154, A.Jagminas et al., Metals 10,1251 and A.Tahira et al., ACS Appl.Energy Mater.3,2053, and is the subject of the following patent applications: CN109097790 (wherein titanium wire is used as a carrier of carbon fiber), CN102849798 (wherein the substrate can be carbon, molybdenum, tungsten, silver, copper or titanium) and CN113755827 (wherein molybdenum sulfide crystals are based on titanium mesh). It can also form a composite material with molybdenum sulfide. KM Alaqad et al., 47, 2366, Y. Kim et al., Advanced Functional Materials, 271701825 and J. Liang et al., ACS Appl. Mater. Interfaces 10, 6084 studied the catalytic properties of TiO2 / MoS2 composites with various microstructures. Composite materials of the same family are also the subject of patent application CN110252345. The composite materials here are formed of graphene, molybdenum sulfide and titanium dioxide in an accordion structure. Finally, J. Liu et al., Applied Catalyst B: Environmental 241, 89 describe MoS2 / Ti3C2T with very good electrocatalytic activity. x Hybrid.
[0021] Finally, there are no catalysts described in the literature having MoS2 doped with titanium or another element of group IVB or another metal of column VIB of the periodic table.
[0022] The applicant company has developed a new method for preparing a catalytic material, making it possible to obtain an electrode usable in an electrolytic cell for carrying out an electrochemical reduction reaction, and more particularly making it possible to obtain a cathode usable in an electrolytic cell for producing hydrogen by electrolysis of water. In particular, the applicant has surprisingly found that the deposition of at least one metal of group VIB on a conductive support in the presence of at least one metal of group IVB makes it possible to obtain a catalytic material having catalytic properties at least as good as or better than those obtained with catalytic materials according to the prior art, in particular when it is used as the catalytic phase of an electrode for electrochemical reduction reactions, and even more particularly when the catalytic material is used as the catalytic phase of a cathode for producing hydrogen by electrolysis of water.
[0023] Subject matter of the invention
[0024] A first subject according to the invention relates to a catalytic material comprising an active phase and a conductive support, wherein the active phase comprises at least one Group VIB metal at least partially in the form of a sulfide, at least one Group IVB metal at least partially in the form of a sulfide, wherein the Group VIB metal is selected from molybdenum and / or tungsten, and the Group IVB metal is selected from titanium, zirconium and / or hafnium.
[0025] According to one or more embodiments, when the Group VIB metal is molybdenum, the molybdenum content is from 4 wt % to 60 wt % of the molybdenum element relative to the weight of the catalytic material.
[0026] According to one or more embodiments, when the Group VIB metal is tungsten, the tungsten content is 7 wt % to 70 wt % of tungsten element relative to the weight of the catalytic material.
[0027] According to one or more embodiments, the content of Group IVB metals is advantageously between 0.1% and 25% by weight of Group IVB elements relative to the total weight of the catalytic material.
[0028] According to one or more embodiments, the active phase is selected from the following element combinations: titanium-molybdenum, zirconium-molybdenum, hafnium-molybdenum, titanium-zirconium-molybdenum, titanium-hafnium-molybdenum, zirconium-hafnium-molybdenum, titanium-tungsten, zirconium-tungsten, hafnium-tungsten, titanium-zirconium-tungsten, titanium-hafnium-tungsten, zirconium-hafnium-tungsten, titanium-molybdenum-tungsten, zirconium-molybdenum-tungsten and hafnium-molybdenum-tungsten.
[0029] According to one or more embodiments, the catalytic material further comprises at least one doping material selected from the group consisting of boron, phosphorus and silicon.
[0030] According to one or more embodiments, the conductive support is selected from:
[0031] -Carbon black, graphite, carbon nanotubes and graphene;
[0032] - Nickel, gold, copper, silver, titanium and silicon;
[0033] -Fluorine-doped tin dioxide and indium tin oxide.
[0034] According to one or more embodiments, the support of the catalytic material has a thickness greater than 75 m 2 / g specific surface area.
[0035] Another subject matter according to the invention relates to a method for preparing a catalytic material according to the invention, said method comprising at least the following steps:
[0036] a) a step of contacting the support with at least one solution containing at least one precursor of at least one Group VIB metal;
[0037] b) a step of contacting said support with at least one solution containing at least one precursor of at least one Group IVB metal;
[0038] Steps a) and b) are performed in any order or simultaneously;
[0039] c) a drying step at a temperature below 250° C. at the end of the sequence of steps a) and b) or b) and a), without a subsequent calcination step;
[0040] d) a step of vulcanizing the material obtained at the end of step c) at a temperature between 100°C and 600°C.
[0041] According to one or more embodiments, the precursor of at least one Group VIB metal is selected from:
[0042] Corresponding to the formula (H h X x M m O y ) q- a polyoxometalate of 5,6,7,8,9,10,11,12 or 18, wherein H is hydrogen, X is an element selected from phosphorus (P), silicon (Si) and boron (B), said element being taken alone, M is one or more elements selected from molybdenum (Mo) and tungsten (W), O is oxygen, h is an integer between 0 and 12, x is an integer between 0 and 4, m is an integer equal to 5, 6, 7, 8, 9, 10, 11, 12 or 18, y is an integer between 17 and 72 and q is an integer between 1 and 20;
[0043] Salts of precursors of Group VIB elements; and
[0044] Mo- or W-based organic or inorganic precursors.
[0045] According to one or more embodiments, the precursor of at least one Group IVB metal is selected from zirconium, hafnium and titanium alkoxides, zirconium hydroxide, hafnium hydroxide, hafnium oxalate, hafnium nitrate and hafnium sulfate.
[0046] According to one or more embodiments, after step a) and / or b) and before step c), a maturation step is carried out at a temperature between 10°C and 50°C for a time of less than 48 hours.
[0047] According to one or more embodiments, the drying step c) is carried out at a temperature between 70°C and 180°C.
[0048] Another subject matter according to the present invention relates to a method for preparing an electrode, comprising at least the following steps:
[0049] 1) dissolving at least one ion-conducting polymer binder in a solvent or a solvent mixture;
[0050] 2) adding at least one catalytic material according to the present invention or a catalytic material obtained by the preparation method according to the present invention in the form of powder to the solution obtained in step 1) to obtain a mixture;
[0051] Steps 1) and 2) are performed in any order or simultaneously;
[0052] 3) depositing the mixture obtained in step 2) on a metal conductive support or a current collector.
[0053] Another subject matter according to the invention relates to an electrolysis device comprising an anode, a cathode and an electrolyte, said device being characterized in that at least one of the anode or the cathode is an electrode obtained by the preparation method according to the invention.
[0054] Another subject matter according to the invention relates to the use of the electrolysis device according to the invention in an electrochemical reaction, wherein the device is used as:
[0055] - water electrolysis plants for producing a gas mixture of hydrogen and oxygen and / or for producing hydrogen alone;
[0056] - Carbon dioxide electrolysis plant for the production of formic acid;
[0057] - Nitrogen electrolysis plants for the production of ammonia;
[0058] - A fuel cell device for generating electricity from hydrogen and oxygen. DETAILED DESCRIPTION OF THE INVENTION
[0060] definition
[0061] In the following, the groups of chemical elements are given according to the CAS classification (CRC Handbook of Chemistry and Physics, published by CRC Press, ed. DRLide, 81st edition, 2000-2001). For example, Group IVB according to the CAS classification corresponds to metals (e.g., Ti, Zr, and Hf) in the 4th column according to the new IUPAC classification, and Group VIII (or VIIIB) according to the CAS classification corresponds to metals in the 8th, 9th, and 10th columns according to the new IUPAC classification.
[0062] The BET specific surface area is understood to mean the specific surface area determined by nitrogen adsorption according to standard ASTM D 3663-78 drawn up by the Brunauer-Emmett-Teller method described in The Journal of the American Chemical Society, 60, 309 (1938).
[0063] Preparation method
[0064] A method for preparing a catalytic material for an electrode for an electrochemical reduction reaction, the material comprising an active phase based on at least one Group VIB metal, at least one Group IVB metal and a conductive support, the method comprising at least the following steps:
[0065] a) a step of contacting the support with at least one solution containing at least one precursor of at least one Group VIB metal;
[0066] b) a step of contacting said support with at least one solution containing at least one precursor of at least one Group IVB metal;
[0067] Steps a) and b) are performed in any order or simultaneously;
[0068] c) a drying step at a temperature below 250° C. at the end of the sequence of steps a) and b) or b) and a), without a subsequent calcination step;
[0069] d) a step of vulcanizing the material obtained at the end of step c) at a temperature between 100°C and 600°C.
[0070] Step a)
[0071] According to step a) of the preparation method of the present invention, at least one step of contacting the support with at least one solution is carried out, the solution containing at least one precursor of an active phase containing at least one metal of Group VIB. Advantageously, according to the implementation of step a), the step of contacting the support with at least one precursor of an active phase containing at least one metal of Group VIB can be carried out by dry impregnation or excess impregnation, or can also be carried out by deposition-precipitation according to methods known to those skilled in the art. Preferably, step a) is carried out by dry impregnation, which comprises contacting the support with a solution containing at least one precursor containing Group VIB, wherein the volume of the solution is 0.25 to 1.5 times the pore volume of the support to be impregnated.
[0072] Precursor comprising at least one Group VIB metal
[0073] Precursors comprising at least one Group VIB metal may be selected from all Group VIB element precursors known to those skilled in the art. They may be selected from polyoxometalates (POMs) or salts of precursors of Group VIB elements, such as molybdates, thiomolybdates, tungstates or thiotungstates. They may be selected from Group VIB oxides. They may be selected from organic or inorganic precursors, such as MoCl5 or WCl4 or WCl6, or alkoxides of Mo or W, for example Mo(OEt)5 or W(OEt)5.
[0074] In the context of the present invention, polyoxometalates (POM) are understood to be salts corresponding to the formula (H h X x M m O y ) q- A compound wherein H is hydrogen, X is an element selected from phosphorus (P), silicon (Si) and boron (B), the element being used alone, M is one or more elements selected from molybdenum (Mo) and / or tungsten (W), O is oxygen, h is an integer between 0 and 12, x is an integer between 0 and 4, m is an integer equal to 5, 6, 7, 8, 9, 10, 11, 12 or 18, y is an integer between 17 and 72 and q is an integer between 1 and 20.
[0075] The polyoxometallates defined according to the present invention comprise two classes of compounds: isopolyanions and heteropolyanions. These two classes of compounds are defined in the paper Heteropoly and Isopoly Oxometallates, Pope, 1983, published by Springer-Verlag.
[0076] The polyanions useful in the present invention are of the general formula (H h X x M m Oy ) q- wherein x=0 and the other elements have the meanings mentioned above.
[0077] Preferably, the m atoms M of the homopolyanion are all molybdenum atoms, or are all tungsten atoms, or are a mixture of molybdenum and tungsten atoms.
[0078] Preferably, in the case where the element M is molybdenum (Mo), m is equal to 7 or 12. Also preferably, in the case where the element M is tungsten (W), m is equal to 12.
[0079] Same polyanion Mo7O 24 6- and H2W 12 O 40 6- In the context of the present invention it is advantageously used as an active phase precursor.
[0080] The heteropolyanion that can be used in the present invention is of the formula (H h X x M m O y ) q- wherein x=1, 2, 3 or 4 and the other elements have the meanings mentioned above.
[0081] Heteropolyanions generally exhibit a structure in which the element X is the “central” atom and the element M is a metal atom to which X different from M is coordinated almost systematically in an octahedral manner.
[0082] Preferably, the m atoms M are all molybdenum atoms, or are all tungsten atoms, or are a mixture of tungsten and molybdenum atoms.
[0083] Preferably, the element X is at least one phosphorus atom.
[0084] Heteropolyanions are negatively charged polyoxometalate species. In order to compensate for these negative charges, counterions and more particularly cations must be introduced. These cations can advantageously be protons H + or any other NH4 + type of cation, or metal cation.
[0085] In the case where the counterion is a proton, the molecular structure comprising a heteropolyanion and at least one proton constitutes a heteropolyacid. The heteropolyacid that can be used as an active phase precursor in the present invention can be, for example, phosphomolybdic acid (3H + ,PMo 12 O 40 3- ) or phosphotungstic acid (3H + ,PW 12 O 40 3-).
[0086] In the case where the counterion is not a proton, the heteropolyanion salt is mentioned to indicate this molecular structure. It is then advantageously possible to utilize a combination of a metal M and its promoter, i.e. elemental titanium and / or elemental zirconium and / or elemental hafnium, in the same molecular structure by using a heteropolyanion salt, which promoter may replace at least one atom M of molybdenum and / or tungsten in the structure of the heteropolyanion at a position X or partially in the structure of the heteropolyanion, or in the counterion position.
[0087] Preferably, the polyoxometalate used according to the invention is a polyoxometalate corresponding to the formula (H h X x M m O y ) q- A compound wherein H is hydrogen, X is an element selected from phosphorus (P), silicon (Si) and boron (B), the element being used alone, M is one or more elements selected from molybdenum (Mo) and / or tungsten (W), O is oxygen, h is an integer between 0 and 6, x is an integer that may be equal to 0, 1 or 2, m is an integer equal to 5, 6, 7, 9, 10, 11 and 12, y is an integer between 17 and 48 and q is an integer between 3 and 12.
[0088] More preferably, the polyoxometalate used according to the present invention is a polyoxometalate corresponding to the formula (H h X x M m O y ) q- A compound wherein h is an integer equal to 0, 1, 4 or 6, x is an integer equal to 0, 1 or 2, m is an integer equal to 5, 6, 10 or 12, y is an integer equal to 23, 24, 38 or 40 and q is an integer equal to 3, 4, 6 and 7, H, X, M and O having the meanings mentioned above.
[0089] Preferred polyoxometalates used according to the invention are advantageously selected from the group consisting of the formula PMo 12 O 40 3- , PW 12 O 40 3- 、SiMo 12 O 40 4- 、SiW 12 O 40 3- or P2Mo5O 23 6- Polyoxometallates, used alone or as a mixture.
[0090] Other preferred polyoxometalates which can be advantageously used in the process according to the invention are of the general formula XM 12 O 40 q- The "Keggin" heteropolyanion has an m / x ratio of 12 and a general formula of XM 11 O 39 q- "Lacunary Keggin" heteropolyanions, whose m / x ratio is equal to 11 and in which the elements X and M and the charge q have the meanings mentioned above. X is therefore an element chosen from phosphorus (P), silicon (Si) and boron (B), said element being taken alone, M is one or more elements chosen from molybdenum (Mo) and / or tungsten (W), and q is an integer between 1 and 20, and preferably between 3 and 12.
[0091] The Keggin species are advantageously obtained in a pH range that can be varied according to the publication by A. Griboval, P. Blanchard, E. Payen, M. Fournier and JL Dubois and the production route described in Chemistry Letters, 1997, vol. 26, no. 12, 1259-1260.
[0092] Salts of heteropolyanions of the Keggin or lacunar Keggin type can also be advantageously used according to the invention.
[0093] Another preferred polyoxometalate which can be advantageously used as a precursor in the process according to the invention is of the formula H h P2Mo5O 23 (6-h)- The Strandberg heteropolyanion has h equal to 0, 1 or 2 and its m / x ratio is equal to 5 / 2.
[0094] The Strandberg heteropolyanions are described in the paper by WC. Cheng and NP Luthra, J. Catal., 1988, 109, 163, in particular the compounds of the formula H h P2Mo5O 23 (6-h)- Preparation of heteropolyanions.
[0095] The precursor comprising at least one Group VIB metal is at least partially soluble in an aqueous phase or an organic phase. The solvent used is typically water, an alcohol (preferably ethanol), an ether, a ketone, a chlorinated compound or an aromatic compound. Water, acidified water, toluene, benzene, methylene chloride, tetrahydrofuran, cyclohexane, normal hexane, ethanol, methanol and acetone are preferably used. When the Group VIB metal is introduced in the form of an alkoxide or in the form of an organic precursor, the solvent is preferably selected from toluene, benzene, methylene chloride, tetrahydrofuran, cyclohexane and normal hexane.
[0096] Thus, using various preparation methods, a large number of polyoxometalates and their related salts are available. Generally speaking, all of these polyoxometalates and their related salts can be advantageously used in the electrolysis process carried out in the method according to the invention. However, the above list is not exhaustive and other combinations can be considered.
[0097] Step b)
[0098] According to step b) of the preparation method of the present invention, at least one step of contacting the support with at least one solution containing at least one precursor of an active phase containing at least one metal of Group IVB is carried out. Advantageously, according to the implementation of step b), the step of contacting the support with at least one precursor of an active phase containing at least one metal of Group IVB can be carried out by dry impregnation or excess impregnation, or by deposition-precipitation according to methods known to those skilled in the art. Preferably, said step b) is carried out by dry impregnation, which comprises contacting the support with a solution containing at least one precursor containing Group IVB, wherein the volume of said solution is from 0.25 to 1.5 times the pore volume of the support to be impregnated.
[0099] Precursors comprising at least one Group IVB metal
[0100] The precursor comprising at least one Group IVB metal may be chosen from all Group IVB element precursors known to those skilled in the art.
[0101] Preferred Group IVB elements are non-noble elements: they are selected from titanium (Ti), zirconium (Zr) and hafnium (Hf). Group IVB metals can be introduced in the form of salts, chelate compounds, alkoxides or glycoxides. The sources of Group IVB elements that can be advantageously used in the form of salts are well known to those skilled in the art. They are selected from nitrates, sulfates, hydroxides, phosphates, carbonates and halides selected from chlorides, bromides and fluorides.
[0102] The Group IVB elements can also be introduced in the form of oxides, in which case the precursors can be dissolved using an acid solution (nitric acid, phosphoric acid, hydrochloric acid, hydrofluoric acid, sulfuric acid, H2O2, etc.) before impregnation of the support.
[0103] The precursor containing at least one Group IVB metal is partially soluble in an aqueous phase or an organic phase. The solvent used is typically water, an alkane, an alcohol, an ether, a ketone, a chlorinated compound or an aromatic compound. Preferably, an acid aqueous solution, toluene, benzene, dichloromethane, tetrahydrofuran, cyclohexane, n-hexane, ethanol, methanol and acetone are used. When an organic solvent is used, the Group IVB metal is preferably introduced in the form of an alkoxide.
[0104] Preferably, in aqueous solution, the Zr precursor is zirconium hydroxide (Zr(OH)4), and the Hf precursor is hafnium hydroxide, hafnium oxalate, hafnium nitrate or hafnium sulfate.
[0105] In one embodiment, the precursors of zirconium, hafnium and titanium are selected from alkoxides of zirconium, hafnium and titanium.
[0106] Implementation of steps a) and b)
[0107] According to one embodiment of the present invention, the precursor comprising at least one Group IVB metal:
[0108] i) prior to the contacting step a), introduced in a "pre-impregnation" step using a solution comprising at least one precursor comprising at least one Group IVB metal;
[0109] ii) during the contacting step a), introduced in a co-impregnation with said solution comprising at least one precursor comprising at least one metal of Group VIB;
[0110] iii) after the contacting step a), introduction in a "post-impregnation" step using a solution containing at least one precursor comprising at least one Group IVB metal.
[0111] Each of steps a) and b) of contacting the support with at least one solution containing at least one precursor of an active phase comprising at least one metal of Group VIB (step a) and contacting the support with at least one solution containing at least one precursor of an active phase comprising at least one metal of Group IVB (step b) is carried out at least once and can advantageously be carried out several times, all possible combinations of the implementation of steps a) and b) being included within the scope of the present invention.
[0112] After each contacting step, an intermediate drying step may preferably be carried out. The intermediate drying step is carried out at a temperature below 250°C, preferably between 15°C and 240°C, more preferably between 30°C and 220°C, even more preferably between 50°C and 200°C, and even more preferably between 70°C and 180°C.
[0113] Advantageously, after each contacting step, optionally before an intermediate drying step, the impregnated support may be allowed to mature. The maturation allows the solution to be evenly distributed within the support. When a maturation step is carried out, it is advantageously carried out at atmospheric pressure, under an inert atmosphere or under an oxygen-containing atmosphere or under an atmosphere containing water or the impregnation solvent and at a temperature between 10° C. and 50° C., and preferably at ambient temperature. Typically, a maturation time of less than 48 hours, and preferably between 5 minutes and 12 hours, is sufficient.
[0114] Advantageously, when steps a) and b) are not carried out simultaneously, each contacting step may preferably be followed by an intermediate drying step and then an intermediate vulcanization step, as described above.
[0115] The intermediate sulphurization step can advantageously be carried out using a H2S / H2 or H2S / N2 gas mixture containing at least 5% by volume of H2S in the mixture or under a pure H2S stream at a temperature between 100°C and 600°C, at a total pressure equal to or greater than 0.1 MPa for at least 2 hours. Preferably, the sulphurization temperature is between 350°C and 550°C.
[0116] Other co-catalysts
[0117] The solutions used in the various impregnation or successive impregnation steps may optionally contain a precursor of at least one doping element selected from boron, phosphorus and silicon. Precursors of doping elements selected from boron, phosphorus and silicon may also advantageously be added alone or as a mixture to an impregnation solution that does not contain a precursor of at least one metal selected from Group IVB metals and Group VIB metals. Preferably, the doping element is phosphorus.
[0118] The solutions used in the various impregnation or successive impregnation steps may optionally contain at least one organic compound. The organic compound may be chosen from all organic compounds known to the person skilled in the art and in particular from chelating agents, non-chelating agents, reducing agents or non-reducing agents. It may also be chosen from optionally etherified mono-, di- or polyols, carboxylic acids, sugars, non-cyclic mono-, disaccharides or polysaccharides, such as glucose, fructose, maltose, lactose or sucrose, esters, ethers, crown ethers, cyclodextrins and sulphur- or nitrogen-containing compounds, such as nitriloacetic acid, ethylenediaminetetraacetic acid or diethylenetriamine, alone or as a mixture.
[0119] The precursors of the Group IVB and Group VIB metals, precursors of the doping elements and organic compounds are advantageously introduced into the impregnation solution(s) in amounts such that the contents of the Group IVB elements, Group VIB elements, doping elements and organic additives on the final catalyst are as defined below.
[0120] Drying step c)
[0121] The drying step is carried out at a temperature below 250°C, preferably between 15°C and 240°C, more preferably between 30°C and 220°C, even more preferably between 50°C and 200°C, and even more preferably between 70°C and 180°C. Very preferably, the drying is carried out under reduced pressure at a temperature not exceeding 80°C. The drying time is between 30 minutes and 24 hours, preferably between 30 minutes and 16 hours. Preferably, the drying time does not exceed 4 hours.
[0122] The drying step can be carried out by any technique known to the person skilled in the art. It is advantageously carried out under an inert atmosphere or under an oxygen-containing atmosphere. It is advantageously carried out under atmospheric pressure or under reduced pressure.
[0123] Vulcanization step d)
[0124] The sulphidation carried out during step d) is aimed at at least partially sulphiding the metal of Group VIB and, optionally, at least partially sulphiding the metal of Group IVB.
[0125] The sulphurization step d) can advantageously be carried out using a H2S / H2 or H2S / N2 gas mixture containing at least 5% by volume of H2S in the mixture or under a pure H2S stream at a temperature between 100°C and 600°C, at a total pressure equal to or greater than 0.1 MPa, for at least 2 hours.
[0126] Preferably, the vulcanization temperature is between 250°C and 450°C.
[0127] Catalytic materials
[0128] The activity of the catalytic material for the electrolysis of water to produce hydrogen is ensured by the inclusion of, preferably consisting of, at least one Group VIB metal at least partially in the form of a sulfide and at least one Group IVB metal at least partially in the form of a sulfide. Advantageously, the active phase is selected from the following element combinations: titanium-molybdenum or zirconium-molybdenum or hafnium-molybdenum or titanium-zirconium-molybdenum or titanium-hafnium-molybdenum or zirconium-hafnium-molybdenum or titanium-tungsten or zirconium-tungsten or hafnium-tungsten or titanium-zirconium-tungsten or titanium-hafnium-tungsten or zirconium-hafnium-tungsten or titanium-molybdenum-tungsten or zirconium-molybdenum-tungsten or hafnium-molybdenum-tungsten.
[0129] When the Group VIB metal is molybdenum, the molybdenum (Mo) content is 4 to 60 wt% of Mo element relative to the weight of the final catalytic material, and preferably 7 to 50 wt% relative to the weight of the final catalytic material obtained after the last preparation step, i.e. sulfidation.
[0130] When the Group VIB metal is tungsten, the tungsten (W) content is 7 to 70 wt% of W element relative to the weight of the final catalytic material, and preferably 12 to 60 wt% relative to the weight of the final catalytic material obtained after the last preparation step, i.e., sulfidation.
[0131] The surface density, which corresponds to the amount of molybdenum Mo atoms and / or tungsten W atoms deposited per unit surface area of the support, will advantageously be between 0.5 and 20 Mo atoms and / or W atoms / square nanometer support and preferably between 2 and 15 Mo and / or W atoms / square nanometer support.
[0132] The content of group IVB metals is advantageously between 0.1% and 25% by weight, preferably between 0.5% and 20% by weight, of group IVB elements relative to the total weight of the final catalytic material obtained after the last preparation step, ie sulphurization.
[0133] Catalytic material carrier
[0134] The support of the catalytic material is a support comprising at least one electrically conductive material, preferably a support consisting of at least one electrically conductive material.
[0135] In one embodiment according to the present invention, the support of the catalytic material comprises at least one material selected from carbon structures, preferably carbon black, graphite, carbon nanotubes or graphene.
[0136] In one embodiment according to the present invention, the support of the catalytic material comprises at least one material selected from nickel, gold, copper, silver, titanium or silicon.
[0137] In one embodiment according to the present invention, the support of the catalytic material comprises a material selected from fluorine-doped tin oxide (FTO), indium tin oxide (ITO) and any other transparent conductive support.
[0138] Porous and non-conductive materials can be made conductive by depositing conductive materials on their surface; mention may be made, for example, of refractory oxides, such as alumina, inside which graphitic carbon is deposited.
[0139] The support of the catalytic material advantageously exhibits a 2 / g, preferably greater than 100m 2 / g, very preferably greater than 130m 2 BET specific surface area (S BET ).
[0140] electrode
[0141] The catalytic material obtainable by the preparation method according to the present invention can be used as an electrode catalytic material that can be used for electrochemical reactions, and in particular for water electrolysis in a liquid electrolytic medium.
[0142] Advantageously, the electrode comprises the catalytic material obtained by the preparation method according to the invention and a binder.
[0143] The binder is preferably a polymeric binder selected for its ability to be deposited in the form of a layer of variable thickness and for its ability in aqueous media in terms of ion conduction and diffusion of dissolved gases. The layer of variable thickness, advantageously between 1 and 500 μm, in particular about 10 to 100 μm, can in particular be a gel or a membrane.
[0144] Advantageously, the ion-conducting polymer binder is:
[0145] * anion-conducting groups, in particular hydroxyl groups, and in particular selected from:
[0146] - polymers stable in aqueous medium, which may be perfluorinated, partially fluorinated or non-fluorinated and which have cationic groups of quaternary ammonium, guanidinium, imidazolium, phosphonium, pyridinium or sulfide type so as to be able to conduct hydroxide anions;
[0147] - ungrafted polybenzimidazole;
[0148] - chitosan; and
[0149] a polymer mixture comprising at least one of the various polymers mentioned above, said mixture having anion-conducting properties;
[0150] * or a cationic conductive group so as to be able to conduct protons and is particularly selected from:
[0151] - polymers that are stable in aqueous media, which may be perfluorinated, partially fluorinated or non-fluorinated and have anionic groups so as to be able to conduct protons;
[0152] - Grafted polybenzimidazole;
[0153] - chitosan; and
[0154] A polymer mixture comprising at least one of the various polymers mentioned above, said mixture having cation-conducting properties.
[0155] Among the polymers that are stable in aqueous media and that have cationic groups so as to be able to conduct anions, mention may in particular be made of polymer chains of the perfluorinated type, such as polytetrafluoroethylene (PTFE), of the partially fluorinated type, such as polyvinylidene fluoride (PVDF), or of the non-fluorinated type, such as polyethylene, which will be grafted with anion-conducting molecular groups.
[0156] Among polymers that are stable in aqueous media and have anionic groups that can conduct protons, groups such as -SO3 - 、-COO - 、-PO3 2- 、-PO3H - or -C6H4O - Any polymer chain which is stable in an aqueous medium. Particular mention may be made of Sulfonated and phosphinated polybenzimidazole (PBI), sulfonated or phosphinated polyetheretherketone (PEEK).
[0157] According to the invention, any mixture comprising at least two polymers, at least one of which is selected from the polymers mentioned above, can be used, as long as the final mixture is ionically conductive in an aqueous medium. Thus, a mixture comprising a polymer that is stable in an alkaline medium and has cationic groups so as to be able to conduct hydroxide anions and a polyethylene to which anion-conducting molecular groups are not grafted can be mentioned as an example, as long as this final mixture is anionically conductive in an alkaline medium. A mixture of a polymer that is stable in an acidic or alkaline medium and has anionic or cationic groups so as to be able to conduct protons or hydroxide and grafted or ungrafted polybenzimidazole can also be mentioned as an example.
[0158] Advantageously, polybenzimidazole (PBI) is used as a binder in the present invention. It is not an intrinsically good ionic conductor but in alkaline or acidic media, it proves to be an excellent polyelectrolyte with very good anionic or cationic conducting properties, respectively. PBI is usually used in grafted form as PBI is a polymer used in the manufacture of proton-conducting membranes for fuel cells, for membrane-electrode assemblies and for PEM electrolyzers. In these applications, PBI is usually functionalized / grafted, for example by sulfonation, to make it proton-conducting. The role of PBI in this type of system is therefore different from the role it has in the manufacture of electrodes according to the invention, where it is used only as a binder and has no direct role in the electrochemical reaction.
[0159] Even though its long-term stability in concentrated acid media is limited, chitosan, which can be used as an anionic or cationic conducting polymer, is a polysaccharide that exhibits ionic conducting properties similar to PBI in alkaline media (G. Couture, A. Alaaeddine, F. Boschet and B. Ameduri, Progress in Polymer Science, 36 (2011), 1521-1557).
[0160] Advantageously, the electrode according to the invention is formulated by a process further comprising a step of removing the solvent simultaneously with or after step 3). The removal of the solvent can be carried out by any technique known to a person skilled in the art, in particular by evaporation or phase inversion.
[0161] In the case of evaporation, the solvent is an organic or inorganic solvent whose evaporation temperature is below the decomposition temperature of the polymer binder used. As examples, dimethyl sulfoxide (DMSO) or acetic acid or propanol can be mentioned. Those skilled in the art can select an organic or inorganic solvent that is suitable for the polymer or polymer mixture used as a binder and that can be evaporated.
[0162] According to a preferred embodiment of the invention, the electrode can be used for the electrolysis of water in an alkaline liquid electrolyte medium and the polymer binder is then a conductor of anions, in particular hydroxide, in the alkaline liquid electrolyte medium.
[0163] Within the meaning of the present invention, an alkaline liquid electrolyte medium is understood to mean a medium having a pH greater than 7, advantageously greater than 10.
[0164] The binder is advantageously capable of conducting hydroxide in an alkaline medium. It is chemically stable in the electrolytic cell and has OH groups that will participate in the electrochemical reaction. - The ability of the particle surface that ions diffuse and / or are transported to the site of the redox reaction that is used to produce H2 and O2 gas. Therefore, the surface that is not in direct contact with the electrolyte still participates in the electrolytic reaction, which is the key point of the effectiveness of the system. The molding of the selected binder and electrode does not hinder the diffusion of the formed gas and limits their adsorption, so that they can be discharged. According to another preferred embodiment of the present invention, this electrode can be used for water electrolysis in an acidic liquid electrolyte medium, and the polymer binder is a cation conductor in an acidic liquid electrolyte medium, and can conduct protons in particular.
[0165] Within the meaning of the present invention, an acidic medium is understood to mean a medium having a pH of less than 7, advantageously less than 2.
[0166] A person skilled in the art will be able to define the amounts of the various components of the electrode according to their general knowledge. The particle density of the catalytic materials must be sufficient to reach their electro-percolation threshold.
[0167] According to a preferred embodiment of the present invention, the polymer binder / catalytic material weight ratio is between 5 / 95 and 95 / 5, preferably between 10 / 90 and 90 / 10, and more preferably between 60 / 40 and 40 / 60.
[0168] Electrode preparation method
[0169] The electrode can be prepared according to techniques known to those skilled in the art. More particularly, the electrode is prepared by a preparation method comprising the following steps:
[0170] 1) dissolving at least one ion-conducting polymer binder in a solvent or a solvent mixture;
[0171] 2) adding at least one catalytic material prepared according to the present invention in powder form to the solution obtained in step 1) to obtain a mixture;
[0172] Steps 1) and 2) are performed in any order or simultaneously;
[0173] 3) depositing the mixture obtained in step 2) on a metal or metal-type conductive carrier or current collector.
[0174] Within the meaning of the present invention, a catalytic material powder is understood to mean a powder consisting of micron-, submicron- or nanometer-sized particles. The powder can be prepared by techniques known to a person skilled in the art.
[0175] In the meaning of the present invention, a metallic carrier or current collector is understood to refer to any conductive material having the same conductive properties as a metal, such as graphite or certain conductive polymers, such as polyaniline and polythiophene. The mixture obtained (between the binder and the catalytic material) can be deposited on the carrier by any method particularly selected from dip coating, printing, induction, pressing, coating, spin coating, filtering, vacuum deposition, spray deposition, casting, extrusion or lamination. The carrier or the current collector can be solid or perforated. As an example of a carrier, a grid (perforated carrier) or a plate or sheet (solid carrier) of stainless steel (such as 304L or 316L) can be mentioned.
[0176] An advantage of the mixture according to the invention is that it can be deposited on a solid or perforated current collector by commonly available deposition techniques capable of being deposited in the form of a layer of variable thickness, ideally between about 10 and 100 μm.
[0177] According to the invention, the mixture can be prepared by any technique known to a person skilled in the art, in particular by mixing a binder and at least one catalytic material in powder form in a solvent or solvent mixture suitable for obtaining a mixture having rheological properties that allow the electrode material to be deposited in the form of a film of controlled thickness on an electronically conductive substrate. The use of catalytic materials in powder form enables the surface area formed by the electrode to be maximized and the associated performance qualities to be enhanced. A person skilled in the art will be able to select the various formulation parameters according to their general knowledge and the physicochemical characteristics of the mixture.
[0178] How to operate
[0179] Another subject matter according to the invention relates to an electrolysis device comprising an anode, a cathode and an electrolyte, wherein at least one of the anode or the cathode is an electrode according to the invention.
[0180] The electrolysis device can be used as a water electrolysis device for producing a gas mixture of hydrogen and oxygen and / or producing hydrogen alone, comprising an anode, a cathode and an electrolyte, the device being characterized in that at least one of the cathode or the anode is an electrode according to the present invention, preferably a cathode. The electrolysis device consists of two electrodes (anode and cathode, which are electronic conductors), which are connected to a DC generator and separated by an electrolyte (ion conductive medium). The anode is the site of water oxidation. The cathode is the site of proton reduction and hydrogen formation.
[0181] Electrolytes can be:
[0182] - Acidic (H2SO4 or HCl, etc.) or alkaline (KOH) aqueous solution;
[0183] - or a proton exchange polymer membrane which ensures the transfer of protons from the anode to the cathode and is able to separate the anodic compartment from the cathodic compartment, which prevents the species reduced at the cathode from being reoxidized at the anode and vice versa;
[0184] - or a ceramic membrane that can conduct O2- ions. Reference is then made to solid oxide electrolysis (SOEC or solid oxide electrolysis cell).
[0185] The minimum water supply for the electrolysis device is 0.8l / Sm 3 Hydrogen. In practice, the actual value is closer to 1l / Sm 3 The incoming water must be as pure as possible, since impurities remain in the equipment and accumulate during the electrolysis process, ultimately interfering with the electrolysis reaction by:
[0186] - sludge formation; and
[0187] - Effect of chloride on electrodes.
[0188] An important specification regarding water relates to its ionic conductivity (which must be less than a few μS / cm).
[0189] There are a number of suppliers offering very diverse technologies, particularly in terms of the nature of the electrolyte and the associated technologies, ranging from possible upstream coupling to a renewable electricity supply (photovoltaic or wind) to a direct final supply of pressurized hydrogen.
[0190] The reaction has a standard potential of -1.23V, which means that it ideally requires a potential difference of 1.23V between the anode and cathode. Standard batteries typically operate at a potential difference of 1.5V and at room temperature. Some systems can operate at higher temperatures. This is because high temperature electrolysis (HTE) has been shown to be more efficient than water electrolysis at room temperature, partly because part of the energy required for the reaction can be provided by heat (cheaper than electricity), and partly because the activation of the reaction is more efficient at high temperatures. HTE systems typically operate between 100°C and 850°C.
[0191] The electrolysis device can be used as a nitrogen electrolysis device for producing ammonia, comprising an anode, a cathode and an electrolyte, the device being characterized in that at least one of the cathode or the anode is an electrode according to the present invention, preferably the cathode.
[0192] The electrolysis device consists of two electrodes (anode and cathode, which are electron conductors) connected to a DC generator and separated by an electrolyte (ion-conducting medium). The anode is the site of water oxidation. The cathode is the site of nitrogen reduction and ammonia formation. Nitrogen is continuously injected into the cathode compartment.
[0193] The nitrogen reduction reaction is:
[0194] N2+6H + +6e - →2NH3
[0195] Electrolytes can be:
[0196] - an aqueous solution (Na2SO4 or HCl), preferably saturated with nitrogen;
[0197] - or a proton exchange polymer membrane which ensures the transfer of protons from the anode to the cathode and is able to separate the anodic compartment from the cathodic compartment, which prevents the species reduced at the cathode from being reoxidized at the anode and vice versa.
[0198] The electrolysis device can be used as a carbon dioxide electrolysis device for producing formic acid, comprising an anode, a cathode and an electrolyte, the device being characterized in that at least one of the cathode or the anode is an electrode according to the invention. Examples of anodes and electrolytes that can be used in such a device are described in detail in document FR 3007427.
[0199] The electrolysis device can be used as a fuel cell device for generating electricity from hydrogen and oxygen, comprising an anode, a cathode and an electrolyte (liquid or solid), said device being characterized in that at least one of the cathode or the anode is an electrode according to the present invention.
[0200] The fuel cell device consists of two electrodes (anode and cathode, which are electronic conductors) connected to a charge C for delivering the generated current and separated by an electrolyte (ion-conducting medium). The anode is the site of hydrogen oxidation. The cathode is the site of oxygen reduction.
[0201] Electrolytes can be:
[0202] - Acidic (H2SO4 or HCl, etc.) or alkaline (KOH) aqueous solution;
[0203] - or a proton exchange polymer membrane which ensures the transfer of protons from the anode to the cathode and is able to separate the anodic compartment from the cathodic compartment, which prevents the species reduced at the cathode from being reoxidized at the anode and vice versa;
[0204] - or can conduct O2 - Ceramic membranes for the removal of ions. Reference is then made to solid oxide fuel cells (SOFCs).
[0205] The following examples illustrate the invention without limiting its scope.The following examples relate to the electrolysis of water in a liquid electrolyte medium to produce hydrogen. Example
[0206] Example 1: H3PMo 12O 40 , Zr(OH)4 and H3PO4 to prepare catalytic material C1 (according to the present invention)
[0207] By dry impregnation of 10 g of a commercial carbon-based support ( 1400m 2 / g), to prepare the catalytic material C1 (according to the present invention). The solution was prepared by 12 O 40 The catalyst is obtained by dissolving in water (at a concentration of 2.6 mol / l), Zr(OH)4 (so that the Zr / Mo ratio = 0.2) and H3PO4 (so that the P / Mo ratio = 0.65). The preparation of the catalyst continues with a maturation step in which the impregnated solid is kept in a closed chamber (whose atmosphere is saturated with water) for 12 hours, followed by a drying step under an inert atmosphere and under reduced pressure (while evacuating) at 60°C (oil bath). The precatalyst is sulfided under a pressure of 0.1 MPa in pure H2S at a temperature of 350°C for 2 hours.
[0208] On the final catalyst, the amount of Mo corresponds to 7 atoms / nm 2 The surface density of Zr and P is: Ni / Mo=0.2 and P / Mo=0.65 respectively.
[0209] Example 2: H3PMo 12 O 40 , Ni(OH)2 and citric acid to prepare catalytic material C2 (not according to the present invention)
[0210] By dry impregnation of 10 g of a commercial carbon-based support ( 1400m 2 / g) to prepare catalytic material C2 (not according to the present invention). The solution was prepared by 12 O 40 The material is obtained by dissolving in water Ni (at a concentration of 2.6 mol / l), Ni(OH)2 (so that the Ni / Mo ratio = 0.2) and citric acid (so that the "citric acid / Mo" ratio = 0.5). The preparation of the material continues with a maturation step in which the impregnated solid is kept in a closed chamber (whose atmosphere is saturated with water) for 12 hours, followed by a drying step at 60°C (oil bath) under an inert atmosphere and under reduced pressure (while evacuating). The catalytic material precursor is sulfided in pure H2S at a temperature of 350°C for 2 hours at a pressure of 0.1 MPa.
[0211] On the final catalyst, the amount of Mo corresponds to 7 atoms / nm 2 The surface density of the alloy is 0.01 and the ratios of Ni and P are Ni / Mo=0.2 and P / Mo=0.08 respectively.
[0212] Example 3: Description of a Commercial Pt Catalyst (Catalyst C3)
[0213] Material C3 comes from Alfa It contains S BET =27m 2 / g of platinum particles.
[0214] Example 4: Catalytic test
[0215] The characterization of the catalytic activity of the catalytic material was carried out in a 3-electrode cell. This cell consists of a working electrode, a platinum counter electrode and an Ag / AgCl reference electrode. The electrolyte is a 0.5 mol / l aqueous solution of sulfuric acid (H2SO4). This medium is deoxygenated by bubbling with nitrogen and the measurement is carried out under an inert atmosphere (degassed with nitrogen).
[0216] The working electrode consists of a 5 mm diameter glassy carbon disk mounted in a Teflon tip (rotating disk electrode). The advantage of glassy carbon is that it is catalytically inactive and is an excellent electrical conductor. In order to deposit the catalyst (C1, C2, C3) on the electrode, a catalyst ink is prepared. This ink consists of 10 microliters of 15 wt% The ink was prepared by mixing 100 μl of the prepared ink with 50 μl of the prepared solution of 100 μl of the prepared ink. The ink was then deposited on the working electrode and then dried to evaporate the solvent.
[0217] Various electrochemical methods are used to determine the performance qualities of catalysts:
[0218] - Linear voltammetry: It consists in applying a potential signal that varies with time to the working electrode, ie from 0 to -0.5 V vs RHE at a rate of 2 mV / s, and measuring the Faradaic response current, ie the current due to the redox reaction occurring at the working electrode. This method is ideal for determining the catalytic power of a material for a given reaction. It is particularly capable of determining the overpotential necessary for the reduction of protons to produce H2.
[0219] - Chronopotentiometry: It consists in applying a current or current density for a predetermined time and measuring the resulting potential. This study makes it possible to determine the catalytic activity at a constant current and the stability of the system over time. 2 The current density is carried out and continued for a given time.
[0220] The catalytic performance qualities are summarized in Table 1 below. They are expressed as -10 mA / cm 2The overpotential at a current density of .
[0221] Table 1
[0222] Catalytic materials <![CDATA[Overpotential (mV) vs RHE at -10 mA / cm 2 > C1 (according to the invention) -160 C2 (not according to the invention) -190 C3 (platinum, not according to the invention) -90
[0223] At an overpotential of only -160 mV vs RHE, the Zr and P-based catalytic material C1 has a particularly improved performance compared to the optimized electrocatalyst C2 based on MoS2 (Ni, Mo, P formulation) and is relatively close to the performance of platinum. This result proves the unquestionable advantage of the material C1 according to the present invention for the development of the water electrolysis hydrogen production industry.
Claims
1. A catalytic material comprising an active phase and a conductive support, wherein the active phase comprises at least one Group VIB metal at least partially in the form of a sulfide, at least one Group IVB metal at least partially in the form of a sulfide, wherein the Group VIB metal is selected from molybdenum and / or tungsten, and the Group IVB metal is selected from titanium, zirconium and / or hafnium.
2. The catalytic material according to claim 1, characterized in that When the Group VIB metal is molybdenum, the molybdenum content is from 4 wt% to 60 wt% of the molybdenum element relative to the weight of the catalytic material.
3. The catalytic material according to claim 1, characterized in that When the Group VIB metal is tungsten, the tungsten content is 7 wt % to 70 wt % of tungsten element relative to the weight of the catalytic material.
4. The catalytic material according to any one of claims 1 to 3, characterized in that The content of the Group IVB metal is 0.1 wt% to 25 wt% of the Group IVB element relative to the total weight of the catalytic material.
5. The catalytic material according to any one of claims 1 to 4, characterized in that The active phase is selected from the following element combinations: titanium-molybdenum, zirconium-molybdenum, hafnium-molybdenum, titanium-zirconium-molybdenum, titanium-hafnium-molybdenum, zirconium-hafnium-molybdenum, titanium-tungsten, zirconium-tungsten, hafnium-tungsten, titanium-zirconium-tungsten, titanium-hafnium-tungsten, zirconium-hafnium-tungsten, titanium-molybdenum-tungsten, zirconium-molybdenum-tungsten and hafnium-molybdenum-tungsten.
6. The catalytic material according to any one of claims 1 to 5, further comprising a dopant material selected from boron, phosphorus and silicon.
7. The catalytic material according to any one of claims 1 to 6, wherein the conductive support is selected from: -Carbon black, graphite, carbon nanotubes and graphene; - Nickel, gold, copper, silver, titanium and silicon; -Fluorine-doped tin dioxide and indium tin oxide.
8. The catalytic material according to any one of claims 1 to 7, characterized in that The carrier of the catalytic material has a thickness greater than 75 m 2 / g specific surface area.
9. A method for preparing a catalytic material according to any one of claims 1 to 8, the method comprising at least the following steps: a) a step of contacting the support with at least one solution containing at least one precursor of at least one Group VIB metal; b) a step of contacting said support with at least one solution containing at least one precursor of at least one Group IVB metal; Steps a) and b) are performed in any order or simultaneously; c) a drying step at a temperature below 250° C. at the end of the sequence of steps a) and b) or b) and a), without a subsequent calcination step; d) a step of vulcanizing the material obtained at the end of step c) at a temperature between 100°C and 600°C.
10. The method according to claim 9, wherein the precursor of at least one Group VIB metal is selected from: Corresponding to the formula (H h X x M m O y ) q- a polyoxometalate of 5,6,7,8,9,10,11,12 or 18, wherein H is hydrogen, X is an element selected from phosphorus (P), silicon (Si) and boron (B), said element being taken alone, M is one or more elements selected from molybdenum (Mo) and tungsten (W), O is oxygen, h is an integer between 0 and 12, x is an integer between 0 and 4, m is an integer equal to 5, 6, 7, 8, 9, 10, 11, 12 or 18, y is an integer between 17 and 72 and q is an integer between 1 and 20; Salts of precursors of Group VIB elements; and Mo- or W-based organic or inorganic precursors.
11. The method according to claim 9 or 10, wherein the precursor of at least one Group IVB metal is selected from zirconium, hafnium and titanium alkoxides, zirconium hydroxide, hafnium hydroxide, hafnium oxalate, hafnium nitrate and hafnium sulfate.
12. Process according to any one of claims 9 to 11, wherein a maturation step is carried out after step a) and / or b) and before step c) at a temperature between 10°C and 50°C for a period of less than 48 hours.
13. A method for preparing an electrode, comprising at least the following steps: 1) dissolving at least one ion-conducting polymer binder in a solvent or a solvent mixture; 2) adding at least one catalytic material according to any one of claims 1 to 8 or a catalytic material obtained as claimed in any one of claims 9 to 12 in powder form to the solution obtained in step 1) to obtain a mixture; Steps 1) and 2) are performed in any order or simultaneously; 3) depositing the mixture obtained in step 2) on a metal conductive support or a current collector.
14. An electrolysis device comprising an anode, a cathode and an electrolyte, wherein at least one of the anode and the cathode is an electrode obtained according to the preparation method according to claim 13.
15. Use of the electrolysis device according to claim 14 in an electrochemical reaction, wherein the device is used as: - water electrolysis plants for producing a gas mixture of hydrogen and oxygen and / or for producing hydrogen alone; - Carbon dioxide electrolysis plant for the production of formic acid; - Nitrogen electrolysis plants for the production of ammonia; - A fuel cell device for generating electricity from hydrogen and oxygen.