Ni-Co-S material for electrochemically recovering PET waste plastic hydrolysate into formate

By growing Co-MOF and Ni-Co-S nanoarray materials on foam nickel, the problems of low Faraday efficiency and high cost of precious metal catalysts are solved, and the PET hydrolysate is efficiently converted into formate salts. Reduced costs.

CN118909265AActive Publication Date: 2024-11-08CHENGDU UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410946968.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

In the prior art, in the electrochemical oxidation and recovery process of PET plastics, Faraday efficiency is low and the cost of using precious metal catalysts is high, making it difficult to achieve efficient conversion to formate.

Method used

Using non-precious metal organic framework compound Co-MOF and its derivative Ni-Co-S nanoarray material, the nanosheet array is grown on foam nickel by hydrothermal method, and as an electrocatalyst, the contact area between the active material and the electrolyte is improved and the contact area between the active material and the electrolyte is achieved to achieve high efficiency. The PET hydrolysate was converted to formate.

Benefits of technology

Achieving over 90% formate Faraday efficiency at 1.5V applied potential and maintaining good catalytic performance at high current density reduces costs while improving electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909265A_ABST
    Figure CN118909265A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a metal organic framework compound (Co-MOF NSAs) and a derivative (Ni-Co-S NSAs) electro-catalytic material taking foamed nickel as a substrate and an electro-catalytic application of the Co-MOF NSAs and the derivative (Ni-Co-S NSAs) electro-catalytic material. The preparation method of the material comprises the following steps: (1) cleaning foamed nickel; and (2) preparing Co-MOF NSAs: adding cobalt nitrate hexahydrate and 2-methylimidazole into deionized water, stirring, putting the mixture and foamed nickel into a 100mL hot autoclave, carrying out hydrothermal reaction at 70 DEG C for 4 hours, taking out, cleaning and drying, thereby obtaining the Co-MOF NSAs. And (3) preparation of Ni-Co-S NSAs: taking the Co-MOF NSAs as a precursor, adding thioacetamide into deionized water, performing ultrasonic mixing, putting the mixture into a 100mL hot autoclave, performing hydrothermal reaction at 120 DEG C for 4 hours, taking out, cleaning, and drying, thereby obtaining the Ni-Co-S NSAs. The electro-catalytic material is applied to electro-catalytic oxidation of polyethylene glycol terephthalate (PET) hydrolysate ethylene glycol (EG), the current density of about 130 mA cm <-2 > can be generated at the positive electrode end, and formate Faraday efficiency exceeding 90% is achieved under the external potential of 1.5 V vs RHE.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of new energy materials, and specifically relates to the preparation of a non-precious metal electrocatalytic material and the application research of the material in electrochemically oxidizing PET hydrolysis products to formate. Background Art

[0002] Plastics are increasingly used in our daily lives. Among them, polyethylene terephthalate (PET), as an important plastic, has been widely used in industries such as packaging, automobiles and textiles due to its excellent properties. However, PET plastic products are often discarded, resulting in a large amount of plastic waste every year. Due to slow natural degradation, a large amount of PET waste plastic accumulates in the environment, erodes and breaks into smaller plastic particles, posing a serious threat to the ecosystem.

[0003] Therefore, from both economic and environmental perspectives, it is of great significance to upgrade PET plastics into valuable chemicals. At present, typical methods for processing plastics include separation and degradation. Plastic separation technologies involve adsorption, coagulation / flocculation and filtration, while plastic degradation technologies mainly include biodegradation, advanced oxidation degradation, electrochemical degradation and photocatalytic degradation. Among them, separation technology is difficult to completely remove microplastics, and degradation technology has high energy consumption and is prone to produce by-products, which cannot be recycled and there is a secondary pollution problem.

[0004] In contrast, electrochemical plastic reforming is expected to provide a green, convenient and efficient way to recycle plastics. In recent years, there has been an increasing amount of research on the electrochemical upgrading of PET. The method is based on the catalytic hydrolysis of PET, followed by electrochemical oxidation of ethylene glycol (EG) and purified terephthalic acid (PTA) in aqueous solution. Further electrochemical catalytic oxidation of ethylene glycol (EG oxidation reaction, EGOR) can produce valuable chemicals, formic acid, glycolic acid and green hydrogen energy.

[0005] This scheme provides a sustainable and attractive route for direct upgrading of PET-derived EG to high-value chemicals under alkaline conditions. On the one hand, the reaction conditions are relatively mild and the experimental conditions are simple. On the other hand, the high-value-added chemicals produced by plastic upgrading on the anode can be carried out simultaneously with hydrogen production (hydrogen evolution reaction, HER) on the cathode. This method is a very promising recycling strategy by converting PET into PTA and other easily separated valuable products (such as formic acid).

[0006] According to previous reports, some electrocatalysts have shown remarkable performance in the ethylene glycol oxidation reaction (EGOR). For example, Wang et al. demonstrated the use of CuO nanowires for the oxidation of PET hydrolysate, with a Faradaic efficiency (FE) of 86.5% for the selective conversion of EG to formate. In a similar study, a nickel-modified cobalt phosphide (CoNi 0.25 Pd) can electrochemically convert PET-derived ethylene glycol into formic acid and acetic acid with a FE exceeding 80%, but the selectivity for formic acid is relatively low. Recently, Liu et al. demonstrated that PET-derived ethylene glycol can be efficiently converted into acetic acid in Pd-Ni(OH)2 at 300 mA cm -2 The selectivity exceeds 90% at a current density of 2.5 Å. However, the use of Pd reduces the cost-effectiveness of the process. In general, the development of efficient non-precious metal electrocatalysts that can achieve high formate selectivity at high current density is a major research direction.

[0007] Therefore, we utilized a simple hydrothermal method to prepare non-precious metal organic framework (Co-MOF) and its derivative (Ni-Co-S) materials with nanosheet arrays (NSAs) that can convert PET hydrolysis products into formate at the cathode. As a preferred catalyst, Ni-Co-S can produce about 130 mA cm -2 A high-format Faradaic efficiency of over 90% was achieved at an applied potential of 1.5 V vs RHE. Summary of the invention

[0008] Aiming at the problem of low Faraday efficiency in converting electrocatalytic PET waste plastics into formate and high cost of electrocatalytic materials based on precious metals, the present invention provides a non-precious metal organic framework compound (Co-MOF NSAs) and its derivative (Ni-Co-S NSAs) electrocatalytic material and its preparation method and application. The electrocatalytic material is directly grown on nickel foam (NF) in situ, which is beneficial to the contact area between the active material and the charged substance, thereby reducing the charge transfer path and improving the electrochemical performance.

[0009] To achieve the above purpose, the technical solution adopted by the present invention to solve the technical problem is:

[0010] (1) Nickel foam treatment: The nickel foam was continuously sonicated in a hydrochloric acid solution, anhydrous ethanol and deionized water, and then dried in a vacuum drying oven at 60°C to obtain a blank NF.

[0011] (2) Preparation of Co-MOF NSAs: Cobalt nitrate hexahydrate and 2-methylimidazole were dissolved in 40 mL of deionized water and stirred. After complete dissolution, they were added together with the treated nickel foam into a stainless steel autoclave and then heated in an electric oven at 70°C for 4 hours. After cooling, the mixture was taken out, rinsed with anhydrous ethanol and deionized water, and then dried in a vacuum drying oven at 60°C for 4 hours to obtain Co-MOF NSAs material.

[0012] (3) Preparation of Ni-Co-S NSAs: Using Co-MOF NSAs as precursors, thioacetamide (TAA) was dissolved in 60 mL of deionized water and stirred. After complete dissolution by ultrasound, they were added together with the precursor into a stainless steel autoclave and then heated in an electric oven at 120°C for 4 hours. After cooling, the mixture was taken out, rinsed with anhydrous ethanol and deionized water, and then dried in a vacuum drying oven at 60°C for 4 hours to obtain Ni-Co-S NSAs.

[0013] Preferably, in step (1), the size of the nickel foam is 2cm*4cm, the concentration of hydrochloric acid is 3mol / L aqueous solution, and the concentration of anhydrous ethanol is 95%.

[0014] In the step (2), the mass of cobalt nitrate hexahydrate in solution 1 is 291.5 mg, the amount of deionized water is 40 mL, and the stirring time is 10 minutes. The mass of 2-methylimidazole in solution 2 is 1250.3 mg, the amount of deionized water is 40 mL, and the stirring time is 10 minutes.

[0015] Preferably, in step (2), the hydrothermal reaction temperature is 70° C. and the reaction time is 4 hours.

[0016] Preferably, in step (3), TAA is 202.3 mg, the total amount of deionized water is 60 mL, the ultrasonic time is 5 min, the hydrothermal reaction temperature is 120° C., and the reaction time is 4 hours.

[0017] The above-mentioned NF, Co-MOF, and Ni-Co-S NSAs electrocatalytic materials are used as working electrodes. In summary, the Ni-Co-S NSAs nanosheet array with spherical particles was formed in situ on nickel foam by a two-step hydrothermal generation method, which has good EGOR performance and can oxidize ethylene glycol and increase its added value to generate formic acid. Using PET alkaline hydrolysis product as electrolyte, its positive terminal can reach 130mA cm at an applied voltage of 1.5V vs RHE. -2 The highly selective conversion of formic acid FE (>90%) was achieved at a current density of 1.5 Å. This study reveals the synthesis strategy of transition metal sulfides and provides a new efficient and sustainable route for the value-added conversion of PET. DETAILED DESCRIPTION

[0018] For the convenience of comparison and analysis, the present invention uses the following three examples to illustrate the advantages of Ni-Co-S NSAs in detail:

[0019] Example 1. A method for preparing a blank NF catalytic material comprises the following steps: continuously ultrasonicating nickel foam in a hydrochloric acid solution, anhydrous ethanol and deionized water, and then drying in a vacuum drying oven at 60° C. to obtain a blank NF.

[0020] Example 2. A method for preparing a Co-MOF NSAs catalytic material comprises the following steps: dissolving cobalt nitrate hexahydrate and 2-methylimidazole in 40 mL of deionized water respectively and stirring. After complete dissolution, they are added together with the treated nickel foam (Example 1) into a stainless steel autoclave, and then heated in an electric oven at 70°C for 4 hours. After cooling, take out, rinse with anhydrous ethanol and deionized water, and then dry in a vacuum drying oven at 60°C for 4 hours to obtain Ni-Co NSAs.

[0021] Example 3. A method for preparing a Ni-Co-S NSAs catalytic material comprises the following steps: using Co-MOF NSAs (Example 2) as a precursor, dissolving thioacetamide (TAA) in 60 mL of deionized water and stirring. After complete dissolution by ultrasound, add them together with the precursor into a stainless steel autoclave, and then heat them in an electric oven at 120°C for 4 hours. After cooling, take them out, rinse with anhydrous ethanol and deionized water, and then dry them in a vacuum drying oven at 60°C for 4 hours to obtain Ni-Co-SNSAs.

[0022] The NF, Co-MOF NSAs and Ni-Co-S NSAs materials obtained in steps (1), (2) and (3) were first analyzed for their microstructure and morphology.

[0023] Figure 1 The preparation flow chart of the present invention is shown in FIG. A nickel and cobalt salt and a piece of treated NF are added to an autoclave by a simple hydrothermal method, placed at 70°C for 4 hours, and then washed and dried to obtain a precursor. The precursor is then hydrothermally treated with TAA at 120°C, and then washed and dried to obtain Ni-Co-S NSAs.

[0024] Figure 2It is the XRD diagram of the present invention. As shown in the figure, in addition to the three diffraction peaks of the nickel foam substrate, the XRD spectrum of Ni-Co NSAs shows four obvious diffraction peaks at (12.5°, 16°, 18° and 27.5°), and its diffraction peak position is the same as the CO-MOF reported in the literature, indicating that Ni-Co NSAs is successfully synthesized on nickel foam. After sulfurization, we can see that the sulfurized catalyst has diffraction peaks at (29°, 31°, 41° and 48°), which are basically consistent with the diffraction peak position of the Co9S8 standard card, corresponding to (311)(222)(420)(511) crystal planes respectively. The results show that Co9S8 is successfully grown on nickel foam.

[0025] Figure 3 2 and 3 are SEM images of the present invention. Figure 3 As shown in a, the nanosheet arrays are uniformly grown on the nickel foam skeleton. Figure 3 As shown in (b), the nanosheet arrays gradually become thinner and nanospheres are attached to the surface of the nanosheets. This Ni-Co-S NSAs / NF morphology exposes a larger contact area, thereby increasing the number of electrochemically active sites and the absorbency of the electrolyte.

[0026] Figure 4 : -EDS diagram of Example 2 and Example 3 of the present invention. Figure 4 As shown in a, Ni and Co elements exist in the Ni-Co NSAs sample; Figure 4 As shown in (b), Ni, Co and S exist in the Ni-Co-S NSAs sample, and the element atomic ratios are 15.68%, 44.38% and 36.54%, respectively.

[0027] Taking the electrocatalytic materials of Examples 1, 2 and 3 as examples, performance tests were conducted. The test process was as follows: electrochemical tests were conducted on the electrocatalytic materials using a three-electrode system in 1M KOH and 1M KOH+1M EG electrolytes prepared with deionized water.

[0028] The specific operation of the electrochemical test is as follows: take an appropriate amount of 1M KOH and 1M KOH+1M EG electrolyte prepared with deionized water into the electrolytic cell, use NF, Co-MOF NSAs and Ni-Co-SNSAs electrocatalytic materials as working electrodes, saturated Hg / HgO electrode as reference electrode, platinum wire as counter electrode, and use Coster electrochemical workstation to perform electrochemical testing on the electrocatalytic materials at room temperature.

[0029] Figure 5a is the LSV polarization curve of the electrocatalytic materials of Examples 1, 2 and 3 of the present invention in an alkaline environment. It can be seen from the figure that at the same current density, the OER overpotential of the Ni-Co-S NSAs catalyst is much lower than that of the Co-MOF NSAs and NF catalysts, and the catalyst performance is significantly improved after sulfurization. Figure 5 b It can be seen that the Ni-Co-S NSAs catalyst exhibits the best electrocatalytic performance after adding 1MEG. Figure 5 c, at 50 and 100 mA cm -2 The overpotential of Ni-Co-S NSAs is lower than that of other catalysts at a current density of 100 mA cm -2 When quenched, the overpotential of Ni-Co-S NSAs (1.28 V) is much lower than that of Co-MOF NSAs (1.33 V) and NF (1.42 V).

[0030] Figure 6 The present invention is a schematic flow diagram of the hydrolysis of PET under alkaline conditions. The polyester structure of PET is easily hydrolyzed into PTA and EG in an alkaline aqueous solution, so the EG monomer is obtained by heating in an alkaline environment. Under experimental conditions, PET powders of different masses are hydrolyzed in 100 mL of 1M KOH solution at 60° C. for 24 hours to obtain different amounts of ethylene glycol monomers.

[0031] Figure 7 The figure shows the hydrolysis effect of PET of different masses in 100 mL 1 M KOH solution of the present invention. Figure 7 a and Figure 7 b are the EG detection curve of the standard solution in liquid chromatography and the standard curve drawn with different concentrations of ethylene glycol, the purpose is to facilitate the study of the EG yield after PET hydrolysis. Figure 7 As can be seen in c, the curve shows a clear peak at 15.8min, which is consistent with the peak of standard ethylene glycol, indicating that PET produces a large amount of EG under alkaline hydrolysis. In order to study the relationship between the amount of PET used and the amount of EG hydrolysis, PET of different masses was hydrolyzed under the same conditions, and then the amount of EG hydrolysis was calculated according to the standard curve. Figure 7 d It can be seen that in 100 mL of 1 M KOH, about 1.0 g PET can be hydrolyzed to 0.35 M EG.

[0032] Figure 8 The electrochemical performance test of Example 3 of the present invention was carried out in an alkaline environment and 1.0 g of PET hydrolyzate. Figure 8 In a, we can see that at the same current density (10 mA cm -2), it takes 1.34 V to drive OER in an alkaline environment, while only 1.24 V is required in a PET hydrolyzate environment, which indicates that in the presence of EG, the starting voltage of Ni-Co-SNSAs / NF is much lower than the starting voltage required to drive OER, which can simultaneously promote more efficient hydrogen production at the cathode. In addition, Figure 8 b The optimal EG concentration of the catalyst was also explored. Figure 8 As shown in Fig. 2b, the anodic oxidation potential gradually decreases with the increase of EG concentration. When 1 M EG is added to the aqueous electrolyte solution, the oxidation potential is only 1.33 V and the current density is 100 mA cm -2 However, as the EG concentration further increased, the oxidation potential slowly moved toward the negative direction. Therefore, the optimal EGOH concentration was 1 M. Figure 8 As shown in Figure c, the catalytic performance of Ni-Co-SNSAs / NF catalyst when the EG concentration of PET hydrolyzate is 1.0 g is very close to the catalytic performance at the optimal EG concentration.

[0033] Fig. 9 This is the stability test of Example 3 under the hydrolysis condition of 1.0g PET. Fig. 9 As shown in a, the initial current density can reach 130 mA cm -2 About, after 24 hours of CA testing, the current density can be maintained above half. Fig. 9 b is the analysis after stability testing. After IC testing, the product is basically formic acid, and the Faraday efficiency is calculated to be about 91%.

[0034] The experimental results show that PET is hydrolyzed to produce ethylene glycol under alkaline conditions, and the catalytic performance of the catalyst is well enhanced in the presence of PET hydrolysis products, generating valuable formic acid and promoting hydrogen evolution. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a flow chart of the product obtained in Example 3 of the present invention;

[0036] Figure 2 is the XRD diagram of the materials in Examples 2 and 3 of the present invention;

[0037] Figure 3 It is the SEM image of the materials in Examples 2 and 3 of the present invention;

[0038] Figure 4 It is the EDS graph of the materials in Examples 2 and 3 of the present invention;

[0039] Figure 5a is the LSV polarization curve of Examples 1, 2, and 3 of the present invention in an alkaline environment; b is the LSV polarization curve of Examples 1, 2, and 3 in an ethylene glycol environment; c is the LSV polarization curve of Examples 1, 2, and 3 in an alkaline medium containing ethylene glycol and excluding ethylene glycol while maintaining 50 and 100 mA cm -2 Comparison of the potential required for current density.

[0040] Figure 6 Schematic diagram of the electrocatalytic hydrolysis of PET to produce hydrogen and formic acid according to the present invention.

[0041] Figure 7 The present invention aims to explore the optimal hydrolysis quality of PET in 100 ml LM KOH solution. Figure 7 a is the EG detection curve of the standard solution in liquid chromatography; Figure 7 b is the standard curve drawn for different concentrations of ethylene glycol; Figure 7 c is the liquid phase detection diagram of EG produced by hydrolysis of PET of different masses under the same conditions; Figure 7 d is the actual EG concentration measured according to the standard curve.

[0042] Figure 8 a is the LSV polarization curve of Example 3 of the present invention under alkaline and PET hydrolysis environment; Figure 8 b is the LSV polarization curve of Example 3 at different EG concentrations; Figure 8 c Comparison of the catalytic performance of Example 3 in 1.0 g PET hydrolysate with different EG concentrations.

[0043] Fig. 9 a is a 24h stability test of Example 3 of the present invention at 1.0g of PET hydrolysate; Fig. 9 b IC analysis after stability test.

Claims

1. Preparation of an electrocatalytic material for producing formic acid by electrocatalytic oxidation of ethylene glycol, a hydrolysis product of PET waste plastics. Features The following steps are involved: (1) Preparation of blank nickel foam (NF): The nickel foam was treated with a hydrochloric acid solution and then continuously ultrasonically cleaned with anhydrous ethanol and deionized water, and then dried in a vacuum drying oven at 60° C. to obtain blank NF. (2) Preparation of Co-MOF NSAs: Cobalt nitrate hexahydrate and 2-methylimidazole were dissolved in 40 mL of deionized water and stirred. After complete dissolution, they were added together with the treated nickel foam into a stainless steel autoclave and then heated in an electric oven at 70°C for 4 hours. After cooling, the autoclave was taken out, rinsed with anhydrous ethanol and deionized water, and then dried in a vacuum drying oven at 60°C for 4 hours to obtain Co-MOF NSAs. (3) Preparation of Ni-Co-S NSAs: With Co-MOF NSAs as the precursor, TAA (thioacetamide) was dissolved in 60 mL of deionized water and stirred. After complete dissolution by ultrasound, they were added together with the precursor into a stainless steel autoclave and then heated in an electric oven at 120°C for 4 hours. After cooling, the mixture was taken out, rinsed with anhydrous ethanol and deionized water, and then dried in a vacuum drying oven at 60°C for 4 hours to obtain Ni-Co-S NSAs.

2. A method for preparing NF, Co-MOF NSAs, or Ni-Co-S NSAs according to claim 1, Features: In the step (1), the thickness of the nickel foam is 1 mm, the length and width are 2 cm*4 cm, the hydrochloric acid concentration is 3 mol / L aqueous solution, and the ultrasonic cleaning time is 30 minutes.

3. A method for preparing an electrocatalytic material of Co-MOF NSAs according to claim 2, Features: In the step (2), the mass of cobalt nitrate hexahydrate in solution 1 is 291.5 mg, the amount of deionized water is 40 mL, and the stirring time is 10 minutes. The mass of 2-methylimidazole in solution 2 is 1250.3 mg, the amount of deionized water is 40 mL, and the stirring time is 10 minutes.

4. A method for preparing Co-MOF NSAs according to claim 3, Features: In the step (2), the hydrothermal reaction temperature is 70° C. and the reaction time is 4 hours.

5. A method for preparing Ni-Co-S NSAs according to claim 4, Features: In the step (3), TAA is 202.3 mg, the total amount of deionized water is 60 mL, the ultrasonic time is 5 min, the hydrothermal reaction temperature is 120° C., and the reaction time is 4 hours.

Citation Information

Patent Citations

  • Sea urchin shaped cobalt sulfide catalyst loaded on foam nickle as well as preparation method thereof and application thereof as water electrolysis oxygen evolution catalyst

    CN108796551A

  • Hollow Co3S4 / RGO composite material rich in sulfur vacancies as well as preparation method and application of hollow Co3S4 / RGO composite material

    CN114613608A

  • P-n heterojunction CuCo2S4 (at) Co-MOF core-shell nanosheet array and preparation method and application thereof

    CN116813927A

  • KR20240054843A