Organic coating composition for oxidized surface of aluminum alloy, coating, preparation process and aluminum alloy part
By spraying an organic coating composition composed of methyl siloxane, acrylic modified silicone resin and silicon sol on the aluminum alloy, the problem of corrosion of alumina film in an alkaline environment is solved, and alkali corrosion resistance is achieved and enhance gloss, suitable for kitchen appliances and other applications.
Patent Information
- Application Number
- CN202411150853.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The aluminum oxide film after aluminum alloy anodization is easily corroded in an alkaline environment, resulting in adverse effects such as decolorization when applied to kitchen appliances.
Using an organic coating composition, including methylsiloxane, acrylic modified silicone resin, silicon sol and solvent, a film layer that resists alkali corrosion by spraying and high temperature curing, has the characteristics of hydrophobic and oleophobicity and glossiness. .
It forms a film that is resistant to alkali corrosion, flat and glossy, which improves the durability and appearance of aluminum alloy parts, and is suitable for kitchen appliances and other environments.
Smart Images

Figure CN118909540A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aluminum alloy surface treatment, and specifically relates to an organic coating composition, a coating, a preparation process, and an aluminum alloy part for an oxidized surface of an aluminum alloy. Background Art
[0002] Aluminum alloy anodizing is an electrochemical surface treatment process, mainly used for aluminum and its alloy materials to improve their corrosion resistance, wear resistance, insulation, decorative and other properties. The principle of this process is to use aluminum or aluminum alloy as anode, place it in an acidic electrolyte (usually sulfuric acid), and form an aluminum oxide film on the aluminum surface through electrolysis.
[0003] However, in actual application, although there is an aluminum oxide film on the surface treated aluminum alloy, it is easily corroded by alkaline substances. This is because aluminum oxide reacts with hydroxide in an alkaline environment. Therefore, when the anodized aluminum alloy workpieces used in kitchen appliances encounter alkaline cleaners (such as Green Umbrella, Viman, etc.), the aluminum oxide film layer will be destroyed, causing discoloration and other adverse effects. Summary of the invention
[0004] In order to solve the above technical problems, the present application improves the formulation of the coating composition in order to obtain an aluminum alloy part resistant to alkali corrosion. One of the purposes of the present invention is to provide an organic coating composition for aluminum alloy parts, the second purpose is to provide a corresponding coating, the third purpose is to provide a corresponding preparation process, and the fourth purpose is to provide a corresponding aluminum alloy part.
[0005] The specific technical solution is described below:
[0006] An organic coating composition for an aluminum alloy part comprises the following components by mass fraction:
[0007] Methylsiloxane, 20-35 parts;
[0008] Acrylic acid modified silicone resin, 15-25 parts;
[0009] Silica sol, 5-10 parts;
[0010] Solvent, 27-58 parts;
[0011] Leveling agent, 2 to 3 parts.
[0012] In the above technical solution:
[0013] The main component that resists alkali corrosion is silica sol;
[0014] During the preparation process, methylsiloxane and acrylic modified silicone resin are cross-linked to form a film layer;
[0015] Among them, methylsiloxane provides methyl side chains, which form microscopic synaptic structures, making the film layer have certain hydrophobicity and oleophobicity at the same time;
[0016] Acrylic modified silicone resin can improve the glossiness and film-forming properties of the film layer;
[0017] The solvent provides a homogeneous environment;
[0018] Leveling agents can reduce the surface tension of the liquid phase, thereby forming a smoother and flatter film layer.
[0019] In a preferred technical solution, the methylsiloxane is polydimethylsiloxane and / or methylhydrogensiloxane, the acrylic modified silicone resin is methyl silicone resin, the solvent is one or a combination of ethylene glycol butyl ether, ethyl acetate, and isopropanol, and the leveling agent is polyacrylate or propylene glycol methyl ether.
[0020] In the preferred technical solution, the mass ratio of the methylsiloxane to the acrylic modified silicone resin is in the range of 0.8 to 2.33. Relatively speaking, if the ratio is too low, the hydrophobicity and oleophobicity of the film layer will be significantly reduced, and if the ratio is too high, the glossiness of the film layer will be significantly reduced.
[0021] In a further preferred technical solution, the mass ratio of the methylsiloxane to the acrylic modified silicone resin is in the range of 1.25 to 1.67. The ratio of the methylsiloxane to the acrylic modified silicone resin within this range has relatively balanced hydrophobicity and oleophobicity and glossiness, and also has good film-forming properties.
[0022] In a further preferred technical solution, the mass ratio of the sum of the mass of the methylsiloxane and the acrylic modified silicone resin to the mass of the silica sol is in the range of 4.3 to 12. If the ratio is too low, it is difficult to form a continuous film layer. If the ratio is too low, the alkali corrosion resistance of the coating is insufficient.
[0023] The coating is prepared from the organic coating composition described in any of the above technical solutions.
[0024] The coating preparation process of the organic coating composition described in any of the above technical solutions comprises the following steps:
[0025] ① Degreasing: wipe the anodized and sealed aluminum alloy parts with an organic solution to remove oil and other impurities on the surface, and dry them at room temperature for 10 to 20 minutes;
[0026] ② Spraying: Mix the organic coating composition and spray it on the aluminum alloy part, with a spraying thickness of 3 to 10 μm;
[0027] ③Curing: Curing is carried out at a temperature of 120°C to 150°C, and then an aluminum alloy part with an organic coating is obtained.
[0028] Aluminum alloy parts are prepared by the above coating preparation process.
[0029] In summary, the technical solution of the present invention has the following main beneficial effects:
[0030] Compared with the prior art, the technical solution of the present invention can form a film layer that is resistant to alkali corrosion and has hydrophobic and oleophobic properties;
[0031] Furthermore, the technical solution of the invention can also form a smooth and glossy film layer.
[0032] Further or more detailed beneficial effects will be described in detail in conjunction with specific examples in the specific implementation manner. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 is a diagram for judging the appearance effect of the aluminum alloy part described in the embodiment; DETAILED DESCRIPTION
[0034] The present invention is further explained with reference to the following embodiments:
[0035] The core technical problem faced by the technical solution of the embodiment of the present application comes from the inventor's accurate understanding of the prior art. Therefore, how to obtain an aluminum alloy part that is resistant to alkali corrosion is a technical problem that the inventor urgently needs to solve.
[0036] At the same time, how to make the coating hydrophobic, oleophobic, smooth and glossy is also a technical problem that the inventors want to solve simultaneously.
[0037] It should be noted that the embodiments do not constitute a limitation on the protection scope of the claims of the present invention. According to the technical concepts provided / proven by the embodiments, all technical solutions that can be reasonably anticipated by technicians in the relevant technical field should be included in the protection scope of the claims of the present invention.
[0038] The embodiments are described in detail as follows:
[0039] The preparation process of aluminum alloy parts with organic coating is as follows:
[0040] (S1): Degreasing: Wipe the anodized and sealed aluminum alloy parts with an alcohol solution of ≥50% concentration to remove oil and other impurities on the surface, and dry the surface at room temperature of 20-40℃ for 10-20min;
[0041] (S2): After mixing the organic coating composition, the organic coating composition is sprayed on the aluminum alloy part by using an electrostatic cup spraying machine, and the spraying thickness is 5 μm;
[0042] (S3): Curing the aluminum alloy part with an organic coating at 120°C to 150°C for 15 minutes in a high temperature tunnel furnace.
[0043] in:
[0044] The organic coating composition in (S2) is composed of the following components by mass fraction:
[0045] At least one of polydimethylsiloxane and methyl hydrogensiloxane, 20 to 35 parts;
[0046] Methyl silicone resin, 15-25 parts;
[0047] Silica sol, 5-10 parts;
[0048] 27-58 parts of one or more of ethylene glycol butyl ether, ethyl acetate, and isopropanol;
[0049] Polyacrylate or propylene glycol methyl ether, 2 to 3 parts.
[0050] The alkali resistance test method in the embodiment is as follows:
[0051] 1. Prepare a sodium hydroxide aqueous solution with a pH of 8 and immerse the aluminum alloy parts in it for 24 hours at room temperature;
[0052] 2. Spray the strong kitchen stain remover (Green Umbrella) on the aluminum alloy parts, and wipe with a rag at a force of 10N for 30s;
[0053] The test results of the above methods 1 and 2 show no cracking or peeling of the coating, which is qualified; otherwise, it is unqualified.
[0054] The test method for hydrophobicity and oleophobicity is as follows:
[0055] The water contact angle is ≥90°, which is qualified, otherwise it is unqualified;
[0056] When the water contact angle is ≥90°, it means that the surface energy is very low, so it is both hydrophobic and oleophobic.
[0057] The method for judging the appearance effect is shown in the appendix of the manual. Figure 1 :
[0058] Attached Figure 1 In the figure, the left side shows a good appearance effect, the middle side shows a slightly discolored appearance effect, and the right side shows a low gloss appearance effect.
[0059] The test method for thermal shock is as follows:
[0060] Keep the aluminum alloy parts in an environment of 150℃±3℃ for 30 minutes, take them out and keep them at room temperature for 10 minutes, and then keep the samples in an environment of -30℃±3℃ for 30 minutes as one cycle. Continue for 15 cycles. If the coating has no cracking or falling off, it is qualified. Continue for 18 cycles. If the coating has no cracking or falling off, it is excellent.
[0061] The formulations in Examples 1 to 5 and Comparative Examples 1 to 2 are as follows: polydimethylsiloxane, methyl silicone resin, silica sol, ethyl acetate and polyacrylate.
[0062] The formulas of the organic coating compositions described in Examples 1 to 5 and Comparative Examples 1 to 2 are shown in Table 1 below:
[0063] Table 1 Formulation and curing temperature of the organic coating composition described in Examples 1 to 5 and Comparative Examples 1 to 2
[0064]
[0065] The performance test results of the coatings in Examples 1 to 5 and Comparative Examples 1 to 2 are shown in Table 2 below:
[0066] Table 2 Performance test results of the organic coatings described in Examples 1 to 5 and Comparative Examples 1 to 2
[0067]
[0068] It can be seen from Table 1 and Table 2 that the curing temperature has a great influence on the appearance effect. The curing temperature of Comparative Example 1 is relatively high, which is 160°C, resulting in a slight discoloration of its appearance. The curing temperature of Comparative Example 2 is relatively low, which is 110°C, resulting in a low glossiness of its appearance and failure to pass the alkali resistance test.
[0069] In Examples 1, 2 and 5, the ratio of methylsiloxane to acrylic modified silicone resin is between 1.25 and 1.67, and they have excellent resistance to thermal shock. In Examples 3 and 5, the ratio of methylsiloxane to acrylic modified silicone resin is 2 and 0.8 respectively, which are outside the range of 1.25 to 1.67, and they still have qualified thermal shock resistance. In kitchen appliances, temperature shocks are often encountered. Therefore, the coatings corresponding to Examples 1, 2 and 5 are more suitable for the working environment with temperature shocks in the kitchen.
[0070] The only difference between Comparative Examples 1 and 2 and Example 1 is the curing temperature. However, their thermal shock performance is not excellent. It can be seen that selecting a suitable curing temperature has a proper influence on the thermal shock performance of the film layer.
[0071] Comparative Example 3:
[0072] The only difference from Example 3 is that the ratio of polydimethylsiloxane to methyl silicone resin is about 2.46.
[0073] Comparative Example 4:
[0074] The only difference from Example 4 is that the ratio of polydimethylsiloxane to methyl silicone resin is about 0.7.
[0075] Comparative Example 5:
[0076] The only difference from Example 3 is that the ratio of the mass of polydimethylsiloxane to the mass of methyl silicone resin to the mass of silica sol is 4.
[0077] Comparative Example 6:
[0078] The only difference from Example 5 is that the ratio of the mass of polydimethylsiloxane to the mass of methyl silicone resin to the mass of silica sol is about 13.
[0079] The formulas of the organic coating compositions described in Comparative Examples 3 to 6 are shown in Table 3 below:
[0080] Table 3 Formulation of the organic coating composition described in Comparative Examples 3 to 6
[0081]
[0082] The performance test results of the coatings in Comparative Examples 3 to 6 are shown in Table 4 below:
[0083] Table 4 Performance test results of the organic coatings described in Comparative Examples 3 to 6
[0084]
[0085] From Table 3 and Table 4, we can see that:
[0086] Comparative Example 3 has a lower gloss than Example 3;
[0087] Compared with Example 4, the hydrophobicity and oleophobicity of Comparative Example 4 are unqualified;
[0088] Compared with Example 3, it is difficult to form a complete film layer in Comparative Example 5;
[0089] Compared with Example 5, the alkali resistance of Comparative Example 6 is unqualified.
[0090] In the description of this specification, the description with reference to the terms "embodiment", "basic embodiment", "preferred embodiment", "other embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0091] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0092] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. An organic coating composition for aluminum alloy parts, characterized in that: According to mass fraction, it contains the following components: Methylsiloxane, 20-35 parts; Acrylic acid modified silicone resin, 15-25 parts; Silica sol, 5-10 parts; Solvent, 27-58 parts; Leveling agent, 2 to 3 parts.
2. The organic coating composition according to claim 1, characterized in that: The methylsiloxane is polydimethylsiloxane and / or methylhydrogensiloxane.
3. The organic coating composition according to claim 2, characterized in that: The acrylic modified silicone resin is a methyl silicone resin.
4. The organic coating composition according to claim 3, characterized in that: The solvent is one or a combination of ethylene glycol butyl ether, ethyl acetate and isopropanol.
5. The organic coating composition according to any one of claims 1 to 4, characterized in that: The leveling agent is polyacrylate or propylene glycol methyl ether.
6. The organic coating composition according to claim 3, characterized in that: The mass ratio of the methylsiloxane to the acrylic modified silicone resin is in the range of 0.8 to 2.
33.
7. The organic coating composition according to claim 6, characterized in that: The mass ratio of the methylsiloxane to the acrylic modified silicone resin is in the range of 1.25 to 1.
67.
8. The organic coating composition according to claim 7, characterized in that: The mass ratio of the sum of the mass of the methylsiloxane and the acrylic modified silicone resin to the mass of the silica sol is in the range of 4.3 to 12.
9. A coating, characterized in that: The organic coating composition is prepared from any one of claims 1 to 8.
10. The coating preparation process of the organic coating composition according to any one of claims 1 to 8, characterized in that: The steps include: ① Degreasing: wipe the anodized and sealed aluminum alloy parts with a cleaning agent to remove the oil on the surface, and dry it at room temperature; ② Spraying: Mix the organic coating composition and spray it on the aluminum alloy part, with a spraying thickness of 3 to 10 μm; ③Curing: Curing is carried out at a temperature of 120°C to 150°C, and then an aluminum alloy part with an organic coating is obtained.
11. Aluminum alloy parts, characterized in that: The coating is prepared by the coating preparation process described in claim 10.
Citation Information
Patent Citations
Composite coating on surface of anti-alkali anti-corrosion aluminum alloy and technology
CN104962974A
Anti-aging nano water-based ceramic coating and preparation method thereof
CN114426783A
Resinous composition for foul releasing coat and coated articles
CN1186090A
Aqueos coating composition
US20070106008A1
Surface coating composition
WO2006049368A1