Negative pole piece of lithium metal battery, lithium metal battery and activation method of lithium metal battery
By using gradient-distributed lithium-philic elements and doped carbon materials in the negative electrode sheet of lithium metal battery to form a dense SEI film, the side reaction problem between lithium and electrolyte during recycling of lithium metal batteries is solved, and the efficiency of Coulomb and Lifespan and increase charge and discharge rate.
Patent Information
- Application Number
- CN202410950837.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
During the recycling process of lithium metal batteries, the side reaction between lithium metal and electrolyte results in uneven active lithium loss and SEI, resulting in shortening of Coulomb efficiency and life, and slow charging and discharge rate.
A lithium metal battery negative electrode sheet including first, second and third active materials are used. The first and second active materials contain lithium-philic elements Ag, Zn, Sn, and Al, and the lithium-philic element atomic content gradient distribution, and the third active material is The material does not contain lithium-philic elements, and the carbon material is doped with elements N, P, S, and O. The carbon layer is coated to reduce the contact between lithium and the electrolyte to form a dense SEI film.
It improves the shuttle rate of lithium ions, reduces side reactions, extends the Coulomb efficiency and service life of lithium metal batteries, and improves the charge and discharge rate and safety.
Smart Images

Figure CN118919656A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium batteries, and in particular relates to a lithium metal battery negative electrode sheet, a lithium metal battery and an activation method thereof. Background Art
[0002] Lithium metal batteries can use metallic lithium as the negative electrode, or use a high-capacity carbon material as the negative electrode. When a high-capacity carbon material is used as the negative electrode, lithium metal will be deposited on the negative electrode during the charge and discharge process, and the metallic lithium can participate in the subsequent charge and discharge process. With the popularity of consumer electronic products such as laptops, mobile phones, handheld game consoles, tablets, mobile power supplies, and drones, people have increasingly stringent requirements for electrochemical devices (e.g., batteries). For example, people not only want batteries to be lighter, but also want them to have shorter charging times and longer working lives. In this context, among many batteries, lithium metal batteries have attracted much attention in the field of research and development because of their highest energy density.
[0003] The gram capacity of lithium metal as the negative electrode can reach 3860mAh / g, which is more than ten times higher than the current theoretical gram capacity of graphite of 372mAh / g. However, lithium metal has the lowest chemical potential (-3.04V) and very high reactivity. Although the energy density of lithium metal as the negative electrode material of the battery can be greatly improved, the cycle life will be sharply shortened. On the one hand, during the recycling of lithium metal batteries, the lithium metal negative electrode and the electrolyte will have a strong side reaction, resulting in a large amount of active lithium loss during the reaction process; on the other hand, because lithium metal is used as the negative electrode, the SEI (solid electrolyte layer) formed is not uniform and stable enough. At the same time, since the negative electrode has no lithium-bearing structure, lithium metal will produce a huge volume effect (that is, volume expansion) during the cycle. The huge volume effect will not only destroy the already formed SEI, expose fresh lithium metal, thereby producing uncontrollable lithium dendrites, but also repeatedly consume active lithium to form SEI.
[0004] To solve the above problems, patent CN112447949A discloses a carbon hollow sphere, wherein the inner wall of the carbon hollow sphere contains lithium-philic precious metal nanoparticles, and the shell material of the carbon hollow sphere is a nitrogen-doped carbon material. It utilizes the synergistic effect of lithium-philic elements and carbon materials to guide lithium to deposit uniformly in the inner chamber of the hollow carbon sphere, thereby improving the huge volume effect of lithium metal in the deposition / dissolution process, reducing interface side reactions, inhibiting the growth of lithium dendrites, and thus improving the coulomb efficiency and cycle life. However, from the perspective of the entire pole piece, since the size of the hollow carbon sphere is very small, such as 15-100 nanometers, even if lithium metal is deposited on the inner wall of the hollow carbon sphere, as lithium metal is continuously deposited, lithium metal is likely to precipitate on the outer surface of the carbon sphere, thereby contacting with the electrolyte, producing side reactions, and reducing the coulomb efficiency and service life of the battery. In addition, the above scheme cannot increase the shuttle speed of lithium ions, which leads to a slow charge and discharge rate (i.e., poor rate performance). Based on this, how to increase the shuttle rate of lithium ions and at the same time, minimize the side reactions between lithium metal and electrolyte, thereby improving the rate performance, coulombic efficiency and service life of lithium metal batteries has become a technical problem that needs to be solved urgently. Summary of the invention
[0005] The present invention provides a lithium metal battery negative electrode plate for solving the above technical problems.
[0006] The present invention provides a lithium metal battery negative electrode plate, comprising: a current collector and a first active material coated on the current collector, a second active material coated on the first active material, and a third active material coated on the second active material, wherein the first active material, the second active material and the third active material comprise carbon materials, wherein the first active material and the second active material further contain a lithium-philic element, wherein the lithium-philic element is independently selected from one or more of Ag, Zn, Sn and Al, and the lithium-philic element exists in the form of a simple substance and / or a metal salt, wherein the atomic content of the lithium-philic element in the first active material is greater than the atomic content of the lithium-philic element in the second active material.
[0007] By adopting the above technical solution, the shuttle rate of lithium ions is increased, and more lithium ions are directed to the first active material close to the current collector side, thereby reducing side reactions and further improving the coulombic efficiency and cycle life of the lithium metal battery.
[0008] Optionally, the negative electrode plate of the lithium metal battery also includes lithium metal element, and the lithium metal element is located on the third active material.
[0009] Optionally, the thickness of the first active material, the second active material and the third active material respectively accounts for 1 / 3 of the total thickness of the three, the atomic content of the lithium-philic element in the first active material is C1, C1 satisfies: 1at%≤C1≤10at%, the content of the lithium-philic element in the second active material is C2, C2 satisfies: 0.2C1≤C2≤0.8C1.
[0010] Optionally, the carbon materials in the first active material, the second active material and the third active material further contain doping elements, and the doping elements are independently selected from one or more of N, P, S and O, and the atomic content of the elements is 0.01 at%-10 at%.
[0011] Optionally, the carbon materials of the first active material, the second active material and the third active material are further coated with a carbon layer, and the material of the carbon layer is amorphous carbon, and the amorphous carbon does not contain the elements N, P, S and O.
[0012] Optionally, the coating thickness of the carbon layer is 5nm-100nm.
[0013] Optionally, the carbon material is amorphous carbon.
[0014] The present invention also provides a lithium metal battery, which contains the above-mentioned lithium metal battery negative electrode plate.
[0015] By adopting the above technical solution, the lithium metal battery has high coulombic efficiency and long service life.
[0016] The present invention also provides a method for activating the above-mentioned lithium metal battery, comprising:
[0017] Injection and rest stage: After the lithium metal battery is injected, it is left to rest for a period of time T1, where T1 satisfies: 6h≤T1≤48h;
[0018] Constant current charging stage: the lithium metal battery is charged at a constant current with a charging voltage of V1 to a cut-off voltage of V2, wherein V1 and V2 satisfy: 0.05+V2≤V1≤0.5+V2, the constant current charging time is T2, and T2 satisfies: 0.5h≤T2≤13h.
[0019] By adopting the above technical solution, a dense and uniform SEI film can be formed, thereby increasing the shuttle rate of lithium ions, and further improving the charge and discharge rate, coulomb efficiency and service life of lithium metal batteries.
[0020] Optionally, the rate of the constant current charging stage is C1, and C1 satisfies: 0.08C≤C1≤0.3C. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A schematic diagram showing a negative electrode sheet of a lithium metal battery of the present invention;
[0022] Figure 2 A schematic diagram showing the negative electrode plate of the lithium metal battery of the present invention.
[0023] (Explanation of symbols)
[0024] 1-lithium metal battery negative electrode plate, 1.1-first active material, 1.2-second active material, 1.3-third active material,
[0025] 1.4-Current collector DETAILED DESCRIPTION
[0026] The following specific embodiments illustrate the implementation of the present invention, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Although the description of the present invention will be introduced in conjunction with the preferred embodiment, this does not mean that the features of this invention are limited to this implementation. On the contrary, the purpose of introducing the invention in conjunction with the implementation is to cover other options or modifications that may extend based on the claims of the present invention. In order to provide a deep understanding of the present invention, the following description will include many specific details. The present invention can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present invention, some specific details will be omitted in the description. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
[0027] It should be noted that in this specification, similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, it does not need to be further defined and explained in the subsequent drawings.
[0028] In order to make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be further described in detail below with reference to the accompanying drawings.
[0029] Since strong side reactions will occur when lithium metal contacts the electrolyte, a suitable high-capacity carbon material is needed to carry lithium metal to reduce the side reactions. However, the existing carrying structure cannot effectively avoid the side reactions. To this end, the present invention provides the following technical solutions to solve the above technical problems.
[0030] The present invention provides a lithium metal battery negative electrode plate, comprising: a current collector and a first active material coated on the current collector, a second active material coated on the first active material, and a third active material coated on the second active material, wherein the first active material, the second active material and the third active material comprise carbon materials, wherein the first active material and the second active material further contain a lithium-philic element, wherein the lithium-philic element is independently selected from one or more of Ag, Zn, Sn and Al, and the lithium-philic element exists in the form of a simple substance and / or a metal salt, wherein the atomic content of the lithium-philic element in the first active material is greater than the atomic content of the lithium-philic element in the second active material.
[0031] By adopting the above technical solution, the shuttle rate of lithium ions is increased, and more lithium ions are directed to the first active material close to the current collector side, thereby reducing side reactions and further improving the coulombic efficiency and cycle life of the lithium metal battery.
[0032] like Figure 1 As shown, the negative electrode plate 1 of the lithium metal battery provided by the present invention includes a current collector 1.4 and a current collector 1.4 extending outward ( Figure 1 In the embodiment of the present invention, a first active material 1.1, a second active material 1.2 and a third active material 1.3 are sequentially provided along the X direction in the image. The second active material 1.2 is coated on the first active material 1.1, and the third active material 1.3 is coated on the second active material 1.2. The first active material 1.1, the second active material 1.2 and the third active material 1.3 include carbon materials, which may be graphite, graphene, carbon nanotubes, amorphous carbon, etc.
[0033] Furthermore, the carbon material of the present invention is doped with lithium-philic elements, wherein doping refers to the introduction of specific elements or ions into the electrode material. The lithium-philic elements refer to those elements or compounds that can form a stable interface layer with the surface of lithium metal. These elements or compounds form a passivation layer on the surface of lithium metal, which helps to reduce the direct contact between lithium metal and the electrolyte, thereby reducing the occurrence of side reactions and improving the cycle stability and safety of the battery. Ag, Zn, Sn and Al are lithium-philic, which can reduce the overpotential of lithium deposition during lithium deposition and make lithium deposition more uniform. Based on this, the first active material and the second active material of the present invention also contain lithium-philic elements, wherein the lithium-philic elements are independently selected from one or more of Ag, Zn, Sn and Al, and the lithium-philic elements exist in the form of simple substances and / or metal salts. For example, the lithium-philic element of the first active material can contain only silver simple substance or only zinc simple substance, only tin simple substance or only aluminum simple substance, or can contain only one metal salt, which contains the above-mentioned lithium-philic element, such as silver nitrate. The metal salt is specifically a salt of the type of nitrate, sulfate, phosphate, etc. Further, the lithium-philic element of the first active material may contain two or more of the above-mentioned simple substances at the same time, such as silver simple substance and zinc simple substance, etc. It can also contain the above-mentioned two or more metal salts, and the metal salt contains the above-mentioned lithium-philic element, such as silver nitrate and zinc phosphate, etc. Further, the lithium-philic element of the first active material may contain one or more of the above-mentioned simple substances, and also contain one or more of the above-mentioned metal salts. For example, silver simple substance and silver nitrate, zinc nitrate, etc.
[0034] The lithium-loving element of the second active material may contain only silver or only zinc, only tin or only aluminum, or may contain only one metal salt, which contains the above-mentioned lithium-loving element, such as silver nitrate. The metal salt is specifically a salt of the type of nitrate, sulfate, phosphate, etc. Further, the lithium-loving element of the second active material may contain two or more of the above-mentioned elements at the same time, such as silver and zinc, etc. It can also contain two or more of the above-mentioned metal salts, which contain the above-mentioned lithium-loving elements, such as silver nitrate and zinc phosphate, etc. Further, the lithium-loving element of the second active material may contain one or more of the above-mentioned elements, and also contain one or more of the above-mentioned metal salts. For example, silver and silver nitrate, zinc nitrate, etc. It is explained here that the selection of the lithium-loving element in the first active material and the lithium-loving element in the second active material is independent of each other, that is, what metal element, what metal element, what metal salt, and what metal salt are selected for the first active material are irrelevant to what metal element, what metal element, what metal salt, and what metal salt are selected for the second active material. In addition, the lithium-philic elements selected for the first active material and the second active material may be the same or different.
[0035] Furthermore, the atomic content of the lithium-philic element doped in the first active material 1.1 is C1, and the atomic content of the lithium-philic element doped in the second active material 1.2 is C2. In addition to using the above-mentioned lithium-philic elements, the atomic content C1 of the lithium-philic element in the first active material 1.1 and the atomic content C2 of the lithium-philic element in the second active material 1.2 provided by the present invention are increased outward along the current collector 1.4 ( Figure 1 In the X direction of the graph, the third active material 1.3 decreases successively, that is, C1>C2, wherein the third active material 1.3 is not doped with a lithium-philic element. By setting a gradient, the shuttle rate of lithium ions can be effectively increased, thereby increasing the charge and discharge rate of the battery. Since the higher the atomic content of the lithium-philic element, the better its lithium-philic effect, therefore, by setting a gradient, more lithium ions can be directed to the first active material 1.1 close to the side of the current collector 1.4, and fewer lithium ions can be directed to the second active material 1.2 with the second highest atomic content of the lithium-philic element. Since the third active material 1.3 does not contain a lithium-philic element, the third active material 1.3 contains almost no lithium ions, which also causes more lithium ions to be directed to the first active material 1.1 and the second active material 1.2, thereby being reduced to lithium metal on the first active material 1.1 and the second active material 1.2, thereby reducing the possibility of contact between lithium metal and electrolyte. Since the above-mentioned carbon material has a good capacity, the volume effect of lithium deposition is also reduced, thereby improving the coulombic efficiency and service life of the battery. Atomic content refers to the atomic percentage of a lithium-philic element in a compound. The specific testing method is: take the prepared powder sample (i.e., the first active material or the second active material containing the lithium-philic element) and stick it to the conductive glue, and use an energy dispersive spectrometer (EDS) to analyze the element type and content of the material.
[0036] Furthermore, the negative electrode plate of the lithium metal battery in the above embodiment may contain lithium metal or may not contain lithium metal. When the negative electrode plate of the lithium metal battery does not contain lithium metal, the lithium metal negative electrode plate will be deposited with lithium metal during the charge and discharge process, and the carbon material in the above active material can form a stable interface with the surface of the lithium metal, thereby reducing the side reaction between the lithium metal and the electrolyte and improving the cycle stability and safety of the battery. When the negative electrode plate of the lithium metal battery contains lithium metal, the lithium metal is located on the third active material. Since the lithium metal is coated on the third active material, the lithium metal is more likely to be consumed in large quantities to form SEI or participate in side reactions during the first charge and discharge process, and the remaining active lithium from the positive electrode is deposited more in the negative electrode in the form of a single substance, thereby compensating for the loss of active lithium, and thus having a longer service life.
[0037] Furthermore, if Figure 2As shown, in the above embodiments, the total thickness of the first active material 1.1, the second active material 1.2 and the third active material 1.3 is L, and the first active material 1.1, the second active material 1.2 and the third active material 1.3 respectively account for 1 / 3 of the total thickness L, that is, the thickness of the first active material 1.1, the second active material 1.2 and the third active material 1.3 are all 1 / 3L, wherein the atomic content C1 of the lithium-philic element in the first active material 1.1 satisfies: 1at%≤C1≤10at%, and the content C2 of the lithium-philic element in the second active material 1.2 satisfies: 0.2C1≤C2≤0.8C1. The higher the concentration of the lithium-philic element doped in the first active material 1.1 close to the current collector 1.4, the easier it is for lithium to be deposited there, and the lower the concentration of the lithium-philic element doped in the third active material 1.3 away from the current collector 1.4, the harder it is for lithium to be deposited. Since the third active material 1.3 is outward ( Figure 2 In the X direction) are electrolyte and separator. In order to avoid contact between lithium metal and electrolyte, the third active material 1.3 of the present invention is not doped with lithium-philic elements, thereby effectively preventing lithium from depositing on the surface of the negative electrode to form lithium dendrites and piercing the separator to cause a short circuit. Furthermore, if the concentration of C1 is set too low, it will not be able to reduce the deposition overpotential. If it is set too high, it will cause excessive deposition of lithium metal at the bottom (i.e., deposition in the first active material 1.1). Therefore, in this embodiment, 1at%≤C1≤10at%, the concentration of C2 is lower than that of C1, and its concentration varies with C1. In this embodiment, 0.2C1≤C2≤0.8C1. By setting C1 and C2 in the above-mentioned gradient range, on the one hand, the shuttling rate of lithium ions is improved, and on the other hand, lithium can be effectively induced to move outward from the side of the current collector 1.4 ( Figure 2 The X direction in the middle is deposited in an orderly manner, thereby improving the cycle performance and safety performance.
[0038] Furthermore, the carbon material in each of the above embodiments is amorphous carbon. Amorphous carbon has a very high capacity and is an ideal carrier for storing lithium. Its storage mechanism is mainly composed of two parts. First: the slope zone capacity. During the discharge process of the lithium metal battery, the battery voltage gradually decreases as the discharge proceeds. Before the voltage drops to a certain level, the capacity of the battery will drop rapidly as the voltage drops. This stage is called the slope zone. The slope zone capacity refers to the capacity provided by the battery at this stage. The slope zone capacity that appears in the initial stage comes from the lithium embedded in the lattice gap of the carbon material and the surface adsorption of the carbon material; second: the platform zone capacity. When the battery voltage drops to a certain threshold, the capacity of the battery will remain relatively stable. This stage is called the platform zone. The platform zone capacity refers to the capacity provided by the battery at this stage. The capacity of the platform zone that appears after the slope zone is mainly related to the contribution of lithium deposition in the pores inside the carbon material. It is explained here that the lithium metal negative electrode plate 1 provided by the present invention may contain lithium metal alone or not. After lithium is deposited, it enters the interior of the carbon material. Compared with using lithium metal as the negative electrode, its volume effect is significantly smaller.
[0039] Further, the carbon materials in the first active material, the second active material and the third active material also contain doping elements, and the doping elements are independently selected from one or more of N, P, S and O, and the atomic content of the elements is 0.01at%-10at%. For example, the doping elements of the first active material can contain only N, only P, only S or only O. It can also contain N and S, N and P or other two of the above elements at the same time. It can also contain N, P, S or other three of the above elements, and it can also contain four elements of N, P, S and O at the same time. It is explained here that the selection of doping elements in the first active material, the doping elements in the second active material and the doping elements in the third material is independent of each other, that is, what doping elements are selected for the first active material, and how many doping elements are selected are not related to the type and quantity of the doping elements selected for the second active material and the third active material. In addition, the types and numbers of doping elements in the first active material, the doping elements in the second active material and the doping elements in the third material can be the same or different.
[0040] Furthermore, the above elements are doped into the carbon material by doping, and structural defects are generated by the above heteroatoms N, P, S, and O doping, thereby increasing more structural holes and holes, thereby increasing the capacity of the platform area. At the same time, the heteroatoms themselves have an adsorption effect on lithium ions, so the capacity of the slope area can also be increased. In addition, after the heteroatoms are doped, the interlayer spacing of the carbon material will also increase, which can increase the capacity of the intercalation effect in the slope area, thereby improving the ability to accommodate lithium. Therefore, element doping of carbon materials can effectively increase the gram capacity of carbon materials, which is beneficial to improving the energy density of lithium metal batteries. The doping amount of the above elements of the present invention is about 0.01at% to 10at%. If the amount of element doping is too little, the capacity cannot be effectively increased. If the element doping is too high, the contribution to the capacity is limited, that is: continuously increasing the amount of element doping cannot infinitely increase the capacity. When the capacity reaches a certain value, continuing to increase the amount of element doping will not only not increase the capacity, but will also bring more active sites, thereby increasing the amount of side reactions. In particular. The doping amount is 1at% to 5at%.
[0041] Furthermore, the outer peripheral wall of the carbon material of the first active material 1.1, the second active material 1.2 and the third active material 1.3 is also coated with a carbon layer, and the material of the carbon layer is amorphous carbon, and the amorphous carbon does not contain the elements N, P, S and O. Since the carbon materials in the above embodiments are doped with one or more of the elements N, P, S and O, and the doping elements N, P, S and O will cause the carbon material to produce more pores, wherein the pores include open pores and closed pores, and the closed pores are cavities caused by structural defects, which can be used to accommodate lithium metal, thereby increasing the capacity. Open pores not only do not provide capacity, but also increase the specific surface area of the material reacting with the electrolyte. In order to reduce the reaction activity of the carbon material and the electrolyte in the above embodiments and reduce the loss of active lithium, the present invention coats a thin carbon layer on the surface of the carbon material. Since the carbon layer does not contain the elements N, P, S and O, the carbon layer will not contain many open pores, but rather plays a protective role. Therefore, some open pores (open pores) can be closed into closed pores (closed pores), and the platform capacity of the carbon material can be increased by increasing the closed pores.
[0042] Furthermore, the coating thickness of the carbon layer is 5nm-100nm. If the coating carbon layer is too thin, it is not conducive to stabilizing the interface, and the effect of closing the open pores will also be poor. If the coating carbon layer is too thick, it will extend the lithium ion transmission path and affect the dynamic performance of the battery. Preferably, the coating thickness of the carbon layer is 15nm to 50nm.
[0043] The present invention also provides a lithium metal battery, which comprises the lithium metal battery negative electrode sheet in the above embodiments.
[0044] By adopting the above technical solution, the lithium metal battery has high coulombic efficiency and long service life.
[0045] Furthermore, the battery needs to be activated and charged before cycling to form SEI, and a dense and uniform SEI is of great significance to the battery. For example: 1) It can prevent the negative electrode material from directly reacting with the electrolyte, thereby protecting the electrode material from being corroded by the electrolyte and extending the service life of the battery; 2) It helps to maintain the stable state of the electrode material, reduce the side reactions during the charging and discharging process, and improve the cycle stability and coulomb efficiency of the battery; 3) It can provide a good ion transmission channel, reduce the diffusion resistance of ions on the electrode surface, thereby improving the rate performance of the battery; 4) It can reduce the uneven deposition of lithium ions on the electrode surface, thereby inhibiting the formation of lithium dendrites, improving the safety of the battery, etc. Therefore, in order to form a uniform and dense SEI, the present invention designs a separate activation method according to the characteristics of the lithium metal battery in the above embodiments. Specifically, the positive electrode, the isolation membrane, and the negative electrode sheet of the lithium metal battery in the above embodiments are stacked in order, then superimposed, and the pole ears are welded and placed in the outer packaging aluminum-plastic film, and the lithium metal battery is obtained by vacuum packaging and standing.
[0046] The present invention also provides a method for activating the above-mentioned lithium metal battery, comprising:
[0047] Injection and rest stage: After the lithium metal battery is injected, it is left to rest for a period of time T1, where T1 satisfies: 6h≤T1≤48h;
[0048] Constant current charging stage: the lithium metal battery is charged at a constant current with a charging voltage of V1 to a cut-off voltage of V2, wherein V1 and V2 satisfy: 0.05+V2≤V1≤0.5+V2, the constant current charging time is T2, and T2 satisfies: 0.5h≤T2≤13h.
[0049] Among them, when the negative electrode plate of the lithium metal battery contains lithium metal, the lithium metal can be used to form SEI or participate in side reactions after the above activation method, and the remaining active lithium is deposited on the negative electrode in the form of lithium metal, thereby compensating for the loss of active lithium. When the negative electrode plate of the lithium metal battery does not contain lithium metal, after activation, part of the active lithium will be consumed to form SEI or participate in side reactions, and the remaining active lithium will be deposited on the negative electrode in the form of a single substance, and the deposited metal lithium can participate in the subsequent charging and discharging process.
[0050] Furthermore, in this embodiment, a lithium metal battery obtained by directly using amorphous carbon as the negative electrode is taken as an example, and the lithium metal battery is activated as follows. It should be noted that the following activation method is specially designed for the above lithium metal battery.
[0051] The activation method is as follows:
[0052] The lithium metal battery is injected with electrolyte, and after the injection is completed, it is sealed and then allowed to stand, wherein the standing time is T1 hours, and T1 satisfies: 6h≤T1≤48h. Since lithium-philic metal elements are doped in this amorphous carbon material, and copper is usually used as the negative electrode current collector in lithium metal batteries, it can be seen from the active metal sequence table that copper has different activities from these lithium-philic metals. Therefore, after the electrolyte is injected, the lithium-philic elements and copper will form a primary battery, and the more active metals will oxidize and dissolve. Therefore, the standing time after the injection needs to be strictly controlled. If the standing time is too short, the diaphragm cannot be well infiltrated. If the standing time is too long, there will be too many primary battery reactions, resulting in the dissolution of active metals. Based on this, in the present invention, the standing time is T1 and satisfies: 6h≤T1≤48h.
[0053] The design capacity of the known lithium metal battery is C, wherein the design capacity of the battery is measured by using the coating weight and gram capacity of the known pole piece, the product of which is the unit surface capacity, and then multiplying by the total pole piece area to obtain the design capacity, the cyclic charging cut-off voltage of the lithium metal battery is V2 volts, the charging voltage cut-off upper limit is set to V1 volt, and after the standing is completed, the lithium metal battery after standing is charged at a constant current of T2 hours with the charging voltage cut-off upper limit being V1 volt, wherein 0.5h≤T2≤13h, 0.05+V2≤V1≤0.5+V2. The activation process of the high-capacity amorphous carbon negative electrode provided by the present invention, the charging voltage upper limit is set to be 0.05~0.5V higher than the cycle voltage, because lithium will have a maximum deposition overpotential during the initial deposition, and the negative pole point will reach the lowest point, which is manifested in the full battery as a maximum point of the battery voltage. If the activation cut-off voltage is not set enough, it cannot be fully activated. If the activation voltage is set too high, there may be a risk of overcharging the battery, and serious safety risks may also result. Specifically, due to the design of the above-mentioned concentration gradient, the lithium metal battery of the present invention will have a higher overpotential during the initial deposition, while the existing lithium metal battery will not have an excessively high overpotential during the initial deposition.
[0054] Furthermore, the rate of the constant current charging stage is C1, and C1 satisfies: 0.08C≤C1≤0.3C. Among them, C is the design capacity of the lithium metal battery. The activation current and time directly affect the quality of the film formation. Within the above range, a dense and uniform SEI can be obtained under the optimized current. Thereby, the shuttle rate of lithium ions can be increased, thereby improving the charge and discharge rate, coulomb efficiency and service life of the lithium metal battery.
[0055] The present invention will be further described in detail below through specific embodiments and comparative examples in conjunction with the accompanying drawings.
[0056] Example 1
[0057] Weigh concentrated phosphoric acid and liquid phenolic resin and add them to 80mL of ethanol, and stir magnetically for 20min. Weigh petroleum coke (i.e., amorphous carbon) and add it to the above mixed solution, and continue magnetic stirring for 30min to fully disperse the petroleum coke. Put the above solution into a blast dryer and dry it at 85°C for 24h to completely evaporate the solution to obtain a dried material. Transfer the dried material to a tubular furnace, heat it to 900°C at a heating rate of 3°C / min, keep it warm for 3h, and finally cool it to room temperature to obtain phosphorus-doped and surface-carbon-coated petroleum coke amorphous carbon. Divide the obtained phosphorus-doped and surface-carbon-coated petroleum coke amorphous carbon into three parts, each of which is mixed with different amounts of silver nanoparticles, and then add a conductive agent (Super P conductive carbon) and a binder polyvinylidene fluoride to obtain a slurry, wherein the weight ratio of the added amorphous carbon, conductive agent and binder polyvinylidene fluoride is about 80:10:10. Then, three portions of slurry with different silver contents were coated on the negative electrode current collector copper foil in batches, and then dried. After cold pressing, cutting and slitting, they were dried under vacuum conditions at about 85°C for about 4 hours to obtain the negative electrode sheet of the lithium metal battery.
[0058] Example 2
[0059] The same experimental method as in Example 1 was used to obtain a negative electrode sheet for a lithium metal battery.
[0060] Example 3
[0061] The negative electrode sheet of a lithium metal battery was obtained by the same experimental method as in Example 1, the only difference being the different atomic content of the doping element P.
[0062] Example 4
[0063] The same experimental method as in Example 1 was used to obtain a negative electrode sheet for a lithium metal battery, the only difference being the coating thickness of the carbon layer.
[0064] Example 5
[0065] The negative electrode sheet of a lithium metal battery was obtained by the same experimental method as in Example 1, the only difference being the different atomic content of the silver nanoparticle in the first active material.
[0066] Example 6
[0067] The negative electrode sheet of a lithium metal battery was obtained by the same experimental method as in Example 1, the only difference being the different atomic content of the silver nanoparticle in the second active material.
[0068] Example 7
[0069] The negative electrode sheet of a lithium metal battery was obtained by the same experimental method as in Example 1. The only difference was the different atomic content of the doping element P.
[0070] Example 8
[0071] The same experimental method as in Example 1 was used to obtain a negative electrode sheet for a lithium metal battery, the only difference being the coating thickness of the carbon layer.
[0072] Example 9
[0073] The same experimental method as in Example 1 was used to obtain a negative electrode sheet for a lithium metal battery.
[0074] Example 10
[0075] The negative electrode sheet of a lithium metal battery was obtained by the same experimental method as in Example 1, the only difference being that the atomic content of Ag doped in the first active material and the second active material was different.
[0076] Comparative Example 1
[0077] The negative electrode sheet of a lithium metal battery was obtained by the same experimental method as in Example 1. The only difference was the atomic content of the silver nanoparticle in the first active material.
[0078] Comparative Example 2
[0079] A negative electrode sheet of a lithium metal battery was obtained by the same experimental method as in Example 1. The difference is that the second active material does not contain silver element.
[0080] Comparative Example 3
[0081] The negative electrode sheet of a lithium metal battery was obtained by the same experimental method as in Example 1. The difference is that the first active material and the second active material are not doped with silver.
[0082] The atomic content of the doping element P in the first active material, the second active material and the third active material, the coating thickness of the carbon layer, the atomic content C1 of the silver nanoparticle in the first active material, the atomic content C2 of the silver nanoparticle in the second active material and the atomic content C3 of the silver nanoparticle in the third active material in the above embodiments and comparative examples are recorded in Table 1. The method for measuring the coating thickness of the carbon layer is to take the above-mentioned cooled powder sample and detect it under a transmission electron microscope, and the detected thickness results are recorded in Table 1.
[0083] Table 1
[0084]
[0085] Next, prepare the positive electrode sheet, separator and electrolyte. The specific preparation process is as follows:
[0086] Preparation of positive electrode sheet:
[0087] The positive electrode active material lithium iron phosphate (LFP), the conductive agent (Super P conductive carbon), and the binder polyvinylidene fluoride are mixed in a weight ratio of about 97:1.4:1.6, N-methylpyrrolidone (NMP) is added, and the system is stirred under the action of a vacuum mixer until the system is uniform to obtain a positive electrode slurry, wherein the solid content of the positive electrode slurry is about 72wt%; the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil; dried, and then cold pressed, cut and slit, and dried under vacuum conditions of about 85°C for about 4h to obtain a positive electrode sheet.
[0088] Preparation of diaphragm:
[0089] Polyethylene (PE) having a thickness of about 15 μm was used as the separator.
[0090] Preparation of electrolyte
[0091] In a dry argon atmosphere, ethylene carbonate and ethyl methyl carbonate are mixed uniformly at a mass fraction of 3:7, and then lithium salt lithium hexafluorophosphate is added to the obtained mixed solution and dissolved uniformly to obtain an electrolyte.
[0092] The positive electrode, the separator, the negative electrode obtained in the above embodiment and the comparative example are stacked in order, and then superimposed; the electrode ears are welded and placed in the outer packaging aluminum plastic film, and the lithium metal battery application example and the application comparative example are obtained after vacuum packaging and standing, and then activated, wherein the cycle cutoff voltage of the lithium metal battery in the application example and the application comparative example is 3.75V. The specific activation process parameters are shown in Table 2, wherein the unit of the standing time T1 and the constant current charging time T2 is h (hours), and the unit of the charging voltage V1 and the cutoff voltage V2 is V (volts).
[0093] Table 2
[0094]
[0095] Take the activated lithium metal battery application example and application comparison example to test its cycle performance and first-cycle coulomb efficiency. Among them, the test method of cycle performance is: place the lithium metal battery in a 25°C constant temperature box and let it stand for 30 minutes to make the lithium metal battery reach a constant temperature. The lithium metal battery that reaches a constant temperature is charged in different charging methods, and then discharged at a constant current of 0.5C to a voltage of 2.5V, which is a charge and discharge cycle. With the capacity of the first discharge as 100%, the charge and discharge cycle is repeated until the discharge capacity decays to 80%, the test is stopped, and the number of cycles is recorded. Among them, the number of cycles can be used as an indicator for evaluating the cycle performance of lithium metal batteries. The more cycles, the better the cycle performance of the battery. The method for the first cycle coulomb efficiency of lithium metal batteries is: record the first charging capacity of the lithium metal battery, and its value is recorded as C1. Record the first discharge capacity of the lithium metal battery, and its value is recorded as C2. The calculation formula for the first cycle coulomb efficiency of lithium metal batteries is as follows: C2 / C1*100%, and the higher the first cycle coulomb efficiency, the better the performance of the lithium metal battery. The test results of the above application examples 1-10 and application comparative examples 1-3 are recorded in Table 3.
[0096] Table 3
[0097]
[0098] According to Table 1-3, compared with comparative application example 1-3, application example 1-10 has better cycle performance and first-cycle coulomb efficiency. This shows that setting the atomic content of the lithium-philic element in the first active material and the second active material of the negative electrode plate to a gradient, the third active material does not contain the lithium-philic element, and adopting the activation method provided by the present invention is conducive to improving the room temperature cycle performance and first-cycle coulomb efficiency of the lithium metal battery. This is ultimately reflected in the cycle performance and first-cycle coulomb efficiency of the application example due to the comparative application example.
[0099] Furthermore, Examples 1-9 satisfy 1at%≤C1≤10at%, 0.2C1≤C2≤0.8C1, and adopt the activation method provided by the present invention, while Example 10 does not meet the above ranges, which ultimately manifests itself in that the cycle performance and coulombic efficiency of Application Examples 1-9 are better than those of Application Example 10.
[0100] Furthermore, the P element doping amount of Examples 1-6 and Example 8 meets 0.01at%-10at%, so its capacity is higher than that of other examples, and the side reactions can be reduced within the above range. At the same time, the activation method provided by the present invention is adopted, which ultimately shows that the cycle performance and first-cycle coulomb efficiency of Application Examples 1-6 and Application Example 8 are better than those of Application Example 7.
[0101] Furthermore, in Application Example 9, since the rate C1>0.3C is used in the activation stage, the current is too large, which is not conducive to forming a stable and dense SEI on the negative electrode surface. Ultimately, the cycle performance and first-cycle coulomb efficiency of Application Example 9 are worse than those of Application Examples 1-6 and Application Example 8.
[0102] Since the gradient of the lithium-philic element is not set in Comparative Example 1, even if the activation method provided by the present invention is used, its performance is poor. This shows that if the lithium-philic element doped in the amorphous carbon material is not set into a concentration gradient to guide the orderly deposition of lithium ions, the cycle performance and the coulomb efficiency of the first cycle of the battery will be affected. Ultimately, the cycle performance and the coulomb efficiency of the first cycle of Comparative Example 1 are worse than those of Application Examples 1-10.
[0103] In Comparative Example 2, since the gradient of the lithium-philic element is not set, the standing time T1 is not within the range of 6h-48h disclosed in the present invention, which ultimately manifests as poor battery cycle performance and first-cycle coulombic efficiency.
[0104] Since there is no lithium-philic element doping in Comparative Example 3, the standing time T1 is not within the range of 6h-48h disclosed in the present invention, which ultimately results in poor battery cycle performance and first-cycle coulomb efficiency.
[0105] Although the present invention has been illustrated and described with reference to certain preferred embodiments of the present invention, it should be understood by those skilled in the art that the above is a further detailed description of the present invention in conjunction with specific embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. Those skilled in the art may make various changes in form and details, including making several simple deductions or substitutions, without departing from the spirit and scope of the present invention.
Claims
1. A negative electrode plate for a lithium metal battery, characterized in that: include: A current collector and a first active material coated on the current collector, a second active material coated on the first active material, and a third active material coated on the second active material, wherein the first active material, the second active material and the third active material include carbon materials, wherein the first active material and the second active material also contain a lithium-philic element, and the lithium-philic element is independently selected from one or more of Ag, Zn, Sn and Al, and the lithium-philic element exists in the form of a simple substance and / or a metal salt, wherein the atomic content of the lithium-philic element in the first active material is greater than the atomic content of the lithium-philic element in the second active material.
2. The negative electrode plate of a lithium metal battery according to claim 1, characterized in that: The negative electrode plate of the lithium metal battery also includes a lithium metal element, and the lithium metal element is located on the third active material.
3. The negative electrode plate of a lithium metal battery according to claim 1, characterized in that: The thickness of the first active material, the second active material and the third active material respectively account for 1 / 3 of the total thickness of the three, the atomic content of the lithium-philic element in the first active material is C1, and C1 satisfies: 1at%≤C1≤10at%, and the content of the lithium-philic element in the second active material is C2, and C2 satisfies: 0.2C1≤C2≤0.8C1.
4. The negative electrode plate of a lithium metal battery according to claim 1, characterized in that: The carbon material in the first active material, the second active material and the third active material further contains a doping element, and the doping element is independently selected from one or more of N, P, S and O, and the atomic content of the element is 0.01 at%-10 at%.
5. The negative electrode plate of a lithium metal battery according to claim 4, characterized in that: The carbon materials of the first active material, the second active material and the third active material are further coated with a carbon layer. The material of the carbon layer is amorphous carbon. The amorphous carbon does not contain the elements N, P, S and O.
6. The negative electrode plate of a lithium metal battery according to claim 5, characterized in that: The coating thickness of the carbon layer is 5nm-100nm.
7. The negative electrode plate of a lithium metal battery according to claim 1, characterized in that: The carbon material is amorphous carbon.
8. A lithium metal battery, characterized in that: The lithium metal battery comprises the lithium metal battery negative electrode sheet according to any one of claims 1 to 7.
9. A method for activating the lithium metal battery according to claim 8, characterized in that: include: Injection and rest stage: After the lithium metal battery is injected, it is left to rest, and the rest time is T1, and T1 satisfies: 6h≤T1≤48h; Constant current charging stage: the lithium metal battery is charged at a constant current with a charging voltage of V1 to a cut-off voltage of V2, wherein V1 and V2 satisfy: 0.05+V2≤V1≤0.5+V2, the constant current charging time is T2, and T2 satisfies: 0.5h≤T2≤13h.
10. The method according to claim 9, characterized in that The rate of the constant current charging stage is C1, and C1 satisfies: 0.08C≤C1≤0.3C.
Citation Information
Patent Citations
Noble metal elementary substance @ nitrogen-doped carbon hollow sphere material, lithium metal negative electrode active material, lithium metal negative electrode and preparation and application of lithium metal negative electrode
CN112447949A
Cited By
All-solid-state lithium metal battery interface protection layer and preparation method and application thereof
CN119419389A