Preparation of alkali metal electrodes and 3D current collectors with {110} or {100} textures

By preparing alkali metal foil and 3D current collector technology with {110} or {100} crystal surface texture, the battery performance problems caused by the growth of lithium metal negative electrode dendrites are solved, and a longer cycle life and higher electricity are achieved Chemical properties.

CN118919665APending Publication Date: 2024-11-08THE CHINESE UNIVERSITY OF HONG KONG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411063823.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-01-14
Filing Date
2023-01-13
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

As an anode material, lithium metal is uneven and surface reaction caused by dendrites during the reciprocating process, resulting in low efficiency and short cycle life. Sharp dendrites may pierce the battery separator and cause safety problems. The existing method is difficult to complete. Inhibit the growth of lithium dendrites.

Method used

By preparing alkali metal foils with {110} or {100} crystal surface texture, the surface of lithium or sodium foil is formed with preferential crystal orientation, combined with 3D current collector technology, lithium is ensured Or uniform nucleation and growth of sodium electrodes extend the cycle life of the battery.

Benefits of technology

It significantly improves the electrochemical performance and cycle life of lithium or sodium electrodes, reduces dendrite growth, extends the service life of the battery, and improves safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919665A_ABST
    Figure CN118919665A_ABST
Patent Text Reader

Abstract

A method of making a lithium foil or a sodium foil for use as an electrode includes applying a crystal texture having a majority of {110} or {100} crystal orientation. For lithium {110} foil, an original foil having a thickness of about 600 [mu] m is heated to about 90 DEG C to randomize crystal orientation, and the foil is rolled to about 300 [mu] m after cooling. The rolled film is then scraped off about 50 [mu] m of the lithium surface, heated to about 75 DEG C, secondarily rolled to about 200 [mu] m, and cooled again to room temperature. The cooled foil may be molded into an electrode. The electrode can be used in a battery, and compared with a lithium battery with a lithium negative electrode lacking a crystal face texture, the service life of the battery is greatly prolonged. The alkali metal may be lithium electrochemically deposited on a 3D scaffold such as a carbon cloth, the deposited alkali metal having a {110} crystal texture.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent application with application date of January 13, 2023, application number 202310066514.6, and invention name “Preparation of alkali metal electrodes and 3D current collectors with {110} or {100} texture”.

[0002] CROSS-REFERENCE TO RELATED APPLICATIONS

[0003] This application claims the benefit of U.S. Application No. 63 / 299,896, filed on January 14, 2022, the entire contents of which are hereby incorporated by reference herein, including any tables, diagrams, or drawings. Technical Field

[0004] The invention belongs to the field of electrochemical technology, and in particular relates to the preparation of lithium and sodium foils with {110} or {100} crystal surface textures and three-dimensional current collectors containing {110} crystal surface textures. Background Art

[0005] Among all candidate negative electrodes, lithium metal has high energy density (3861mAh / g) and the lowest electrode potential (-3.94V vs SHE), and is a promising negative electrode material for lithium-based energy storage devices. However, in practical applications, the fundamental problem that limits lithium metal as a negative electrode is the growth of lithium dendrites during the repeated lithium plating / stripping process. The lithium growth kinetics combined with the inhomogeneity of the electrode surface promote the growth of dendrites. The loose structure of the formed dendrites causes them to break from the substrate, resulting in "dead lithium", while the exposed fresh lithium surface continues to react with the electrolyte, consuming lithium and electrolyte. These two processes result in low coulombic efficiency and shortened cycle life. In addition, sharp dendrites have the potential to pierce the battery separator, which can lead to internal short circuits that can cause thermal runaway in the battery, resulting in safety issues.

[0006] In order to inhibit the growth of lithium dendrites, many solutions have been proposed, including: using a high shear modulus separator or solid electrolyte to mechanically block the growth of lithium dendrites; improving the uniformity of lithium nucleation by designing the three-dimensional structure of the current collector and designing the artificial solid electrolyte interface on the negative electrode surface. Although these methods inhibit the growth of lithium dendrites to a certain extent, the problem of lithium dendrite growth still exists and is still the main obstacle to the cycle performance of lithium metal negative electrodes.

[0007] The effect of the original lithium texture on lithium dendrite growth and electrode cycling performance has not been fully investigated. Texture is the preferred crystal orientation formed in a crystal, rather than a specific surface morphological feature. Since different crystal planes have different surface energies and surface energy diffusion barriers, texture affects the nucleation and growth of lithium during the battery process. It has been found that the texture of zinc foil (0001) is beneficial to improving the cycling performance of zinc-based batteries. Gu et al. have inferred from simulation results that lithium growth on copper (100) preferentially grows along the lithium

[110] crystal plane direction, and lithium plating on copper (100) has successfully extended the battery cycle life. Recently, Zhao et al. have demonstrated that large-capacity lithium electroplating on copper foil can obtain a {110} texture. In an ether electrolyte, this electrode shows a cycle life of 2500 minutes in a symmetric cell. When the research group of Li et al. observed the growth of lithium nanowires using an electron microscope, they found that lithium grew slowly along the

[110] crystal plane direction, and found that by using a specific electrolyte, lithium could grow along the

[110] crystal plane direction, and the growing surface always remained flat. Directly using lithium foil as the negative electrode can avoid the pre-lithiation process in batteries without lithium positive electrodes (such as Li-S, etc.). In this regard, the Archer group obtained lithium {100} crystal plane texture by cold rolling the lithium foil to cause it to deform violently, and improved the electrochemical performance to a certain extent when working as an electrode. However, there is no lithium foil with {110} crystal plane texture to date, and it is not clear whether this texture can improve its cycling performance. Summary of the invention

[0008] Embodiments of the present invention relate to a method for preparing an alkali metal electrode, wherein the electrode has a {110} or {100} crystal plane texture, and in most cases, the surface has a {110} or {100} texture. The thickness of the lithium or sodium metal foil before treatment is about 600 μm, and a first annealing is performed at a first temperature of about 70% to 90% of the melting point of the alkali metal foil, such as about 90°C for lithium or near room temperature for sodium. The annealing is maintained for about 1 to 3 hours and cooled to room temperature as required, wherein the alkali metal foil after annealing has a random surface crystal orientation. The surface of the foil is polished using a chemical polishing solution as required, such as a tetrahydrofuran solution of naphthalene. The chemical polishing solution is then washed from the foil using a solvent (such as diethyl carbonate (DEC) or 1,3-dioxolane (DOL)). For a {110} texture, the foil is first rolled at room temperature until the thickness of the foil is about 300 μm. At a temperature of about 70% of the melting point of the alkali metal foil, such as about 75°C for lithium or room temperature for sodium, the surface is scraped along the same axis as the first rolling to remove a surface layer of about 50 μm thickness from the alkali metal foil. A second annealing is performed at the same temperature for about 0.5 hours, and while maintaining this temperature, the alkali metal foil is rolled a second time to a thickness of about 200 μm. The foil is then cooled as required and cut into electrodes that are primarily composed of a {110} crystal plane texture. The shape of the electrode can be circular. In order to prepare Li or Na foil with a {100} surface crystal orientation, a hydraulic press is used for pressing at room temperature. The pressing pressure for different alkali metals is different, such as about 5 MPa for lithium or about 3 MPa for sodium.

[0009] Another embodiment is directed to an alkali metal electrode, the alkali metal consisting essentially of {110} or {100} crystal plane textures. The alkali metal may be lithium or sodium, wherein the {110} or {100} crystal plane textures occupy 95% or more of its surface before the first discharge of a battery in which it is an electrode.

[0010] Another embodiment of the present invention relates to a three-dimensional (3D) alkali metal-based current collector having a {110} crystal plane texture. The alkali metal can be electrochemically deposited on a 3D support such as carbon cloth, and the deposited alkali metal maintains the {110} crystal plane texture.

[0011] Another embodiment of the present invention relates to a battery comprising an alkali metal electrode consisting essentially of a {110} or {100} crystal plane texture. Such a lithium battery or sodium battery can use an alkali metal as an electrode. In this way, the battery has better electrochemical performance and longer cycle life than an alkali metal battery having an alkali metal negative electrode without a {110} or {100} crystal plane texture. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1A flow chart is provided for preparing base metal foils having a {110} or {100} texture.

[0013] Figure 2A SEM image of a typical Li foil after surface treatment.

[0014] Figure 2B Shows from Figure 2A Energy dispersive X-ray (EDX) spectra acquired for the sample shown indicate that the surface is rich in oxygen (O) and carbon (C).

[0015] Figure 2C XRD patterns of three randomly selected pristine Li foils after chemical polishing are shown, which show similar diffraction patterns that can be indexed to bcc Li (JCPDF#15-0401), with different intensity ratios of the diffraction peaks for different samples.

[0016] Figure 3 The pristine Li foil using chemical polishing is shown at a current density of 1 mA / cm 2 and a capacity of 1 mAh / cm 2 Cycling performance diagram of symmetrical batteries assembled under the condition of , where the three batteries (i.e., a, b, and c) show large differences.

[0017] Figure 4A is the SEM image of the treated Li foil with {110} crystal plane texture after surface treatment.

[0018] Figure 4B is the SEM image of the treated Li foil with {100} crystal plane texture after surface treatment.

[0019] Figure 4C Shows Figure 4A EDX spectrum of Li{110} foil.

[0020] Figure 4D Shows Figure 4B EDX spectrum of Li{100} foil.

[0021] Figure 4E Bar chart showing the surface chemical element contents of pristine Li, Li{110}, and Li{100} foils.

[0022] Figure 5A Composite X-ray diffraction (XRD) patterns are shown, wherein: (a) is a Li foil having a {100} crystal plane texture according to one embodiment; and (b) is a Li foil having a {110} crystal plane texture according to one embodiment.

[0023] Figure 5BThe Li{100} (black) and Li{110} (red) symmetric cells are shown at a current density of 1 mA / cm 2 and a capacity of 1 mAh / cm 2 Battery cycling in carbonate electrolyte.

[0024] Figure 5C The Li{100} (black) and Li{110} (red) symmetric cells are shown at a current density of 5 mA / cm 2 and a capacity of 1 mAh / cm 2 Battery cycling in carbonate electrolyte.

[0025] Figure 5D The Li{100} (black) and Li{110} (red) symmetric cells are shown at a current density of 1 mA / cm 2 and a capacity of 5 mAh / cm 2 Battery cycling in carbonate electrolyte.

[0026] Figure 5E The Li{100} (black) and Li{110} (red) symmetric cells are shown at a current density of 1 mA / cm 2 and a capacity of 1 mAh / cm 2 The battery is cycled in an ether electrolyte.

[0027] Fig. 5F The Li{100} (black) and Li{110} (red) symmetric cells are shown at a current density of 5 mA / cm 2 and a capacity of 5 mAh / cm 2 The battery is cycled in an ether electrolyte.

[0028] Fig. 6A Shown at 1mA / cm 2 Current density, 1 mAh / cm 2 Evolution of the XRD pattern of a symmetric cell with Li{100} electrodes at a capacity of 1.1 Å.

[0029] Figure 6B Shown at 1mA / cm 2 Current density, 1 mAh / cm 2 Evolution of the XRD pattern of a symmetric cell with Li{110} electrodes at a capacity of 1.1 Å.

[0030] Figure 6C Shown at 5mA / cm 2 Current density, 1 mAh / cm 2 Evolution of the XRD pattern of a symmetric cell with Li{100} electrodes at a capacity of 1.1 Å.

[0031] Fig.6D Shown at 5mA / cm 2 Current density, 1 mAh / cm 2 Evolution of the XRD pattern of a symmetric cell with Li{110} electrodes at a capacity of 1.1 Å.

[0032] Fig. 6E Shown at 5mA / cm 2 Current density, 1 mAh / cm 2 The XRD pattern of Li foil after 150 cycles at a capacity of 1.5 wt %. In this pattern, (110) still dominates, but (200) and (211) diffractions can also be observed.

[0033] Fig. 7A is 1mA / cm 2 Current density, 1 mAh / cm 2 Scanning electron microscope (SEM) image of the surface morphology of Li{100} after exfoliation at a capacity of .

[0034] Figure 7B is at 5mA / cm 2 Current density, 1 mAh / cm 2 SEM image of the surface morphology of Li{100} after exfoliation at a capacity of .

[0035] Figure 7C is 1mA / cm 2 Current density, 1 mAh / cm 2 SEM image of the surface morphology of Li{110} after exfoliation at a capacity of .

[0036] Fig.7D is at 5mA / cm 2 Current density, 1 mAh / cm 2 SEM image of the surface morphology of Li{110} after exfoliation at a capacity of

[0037] Fig. 7E is 1mA / cm 2 Current density, 1 mAh / cm 2 SEM image of the surface morphology of Li{100} after electroplating at a capacity of .

[0038] Figure 7F is at 5mA / cm 2 Current density, 1 mAh / cm 2 SEM image of the surface morphology of Li{100} after electroplating at a capacity of .

[0039] Figure 7G is 1mA / cm 2 Current density, 1 mAh / cm2 SEM image of the surface morphology of Li{110} after electroplating at a capacity of .

[0040] Figure 7H is at 5mA / cm 2 Current density, 1 mAh / cm 2 SEM image of the surface morphology of Li{110} after electroplating at a capacity of .

[0041] Fig.7I is 1mA / cm 2 Current density, 1 mAh / cm 2 SEM image of the surface morphology of the original Li foil after peeling at a capacity of .

[0042] Fig. 8A is 1mA / cm 2 Current density, 1 mAh / cm 2 SEM image of the Li{100} anode of the symmetric cell after stripping at the first cycle with a capacity of 1.34 W.

[0043] Figure 8B is at 5mA / cm 2 Current density, 1 mAh / cm 2 SEM image of the Li{100} anode of the symmetric cell after stripping at the first cycle with a capacity of 1.34 W.

[0044] Figure 8C is 1mA / cm 2 Current density, 1 mAh / cm 2 SEM image of the Li{110} anode of the symmetric cell after stripping at the first cycle with a capacity of 1.34 W.

[0045] Fig.8D is at 5mA / cm 2 Current density, 1 mAh / cm 2 SEM image of the Li{110} anode of the symmetric cell after stripping at the first cycle with a capacity of 1.34 W.

[0046] Fig. 8E is 1mA / cm 2 At a current density of 1 mAh / cm 2 Capacity SEM image of the Li{100} cathode of the symmetric cell after electroplating.

[0047] Fig.8F is at 5mA / cm 2 At a current density of 1 mAh / cm 2 Capacity SEM image of the Li{100} cathode of the symmetric cell after electroplating.

[0048] Figure 8G is 1mA / cm 2 At a current density of 1 mAh / cm 2 Capacity SEM image of the Li{110} cathode of the symmetric cell after electroplating.

[0049] Figure 8H is at 5mA / cm 2 At a current density of 1 mAh / cm 2 Capacity SEM image of the Li{110} cathode of the symmetric cell after electroplating.

[0050] Fig. 9A is 1mA / cm 2 The current density and 1 mAh / cm 2 SEM image of Li{100} after 50 cycles at a capacity of 1.38 W.

[0051] Fig. 9B is 1mA / cm 2 The current density and 1 mAh / cm 2 SEM image of Li{100} after 300 cycles at a capacity of .

[0052] Fig. 9C is 1mA / cm 2 The current density and 1 mAh / cm 2 SEM image of Li{110} after 50 cycles at a capacity of 1.38 W.

[0053] Fig.9D is 1mA / cm 2 The current density and 1 mAh / cm 2 SEM image of Li{110} after 300 cycles at a capacity of 1.5 Å.

[0054] Fig. 10A is at 5mA / cm 2 The current density and 1 mAh / cm 2 SEM image of Li{100} after 25 cycles at a capacity of 1.5 Å.

[0055] Fig. 10B is at 5mA / cm 2 The current density and 1 mAh / cm 2 SEM image of Li{110} after 25 cycles at a capacity of 1.5 Å.

[0056] Fig. 10C is at 5mA / cm 2 The current density and 1 mAh / cm 2 SEM image of Li{100} after 50 cycles at a capacity of 1.38 W.

[0057] Fig. 10D is at 5mA / cm 2 The current density and 1 mAh / cm 2 SEM image of Li{110} after 50 cycles at a capacity of 1.38 W.

[0058] Fig.10E is at 5mA / cm 2 The current density and 1 mAh / cm 2 SEM image of Li{100} after 100 cycles at a capacity of .

[0059] Fig.10F is at 5mA / cm 2 The current density and 1 mAh / cm 2 SEM image of Li{110} after 100 cycles at a capacity of .

[0060] Fig.11A This is the electrochemical performance diagram of the Li / / LFP full battery. The performance of the full battery with negative electrodes of Li{100} (blue) and {110} (red) when cycled at 1C rate.

[0061] Fig. 11B This is the electrochemical performance diagram of the Li / / LFP full battery. The performance of the full battery with negative electrodes of Li{100} (blue) and {110} (red) when cycled at a 5C rate.

[0062] Fig. 11C It is the rate capacity diagram of Li / / LFP full battery with negative electrodes of Li{100} (blue) and {110} (red).

[0063] Fig. 12A Shown is the electrochemical performance graph of the Li / / LFP full cell using pristine lithium metal anode at 1C rate.

[0064] Fig. 12B Shown is the electrochemical performance graph of Li / / LFP full cell using pristine lithium metal anode at 5C rate.

[0065] Fig.13 Shown are the charge and discharge curves of Li / / LFP full cells with Li{100} or {110} anode in the first cycle at 1C and 5C rates, respectively.

[0066] Fig.14 Shown are the XRD patterns of lithium foil (a) after chemical polishing and after pressing at (b) 2.5 MPa, (c) 5.0 MPa, and (d) 6.5 MPa.

[0067] Fig.15Shown are XRD patterns of a representative Li{100} sample stored in a glove box at different times with oxygen and water levels below about 0.5 ppm and about 0.5 ppm, respectively.

[0068] Fig.16 Shown at 1mA / cm 2 XRD patterns of Li{100} samples after exfoliation at different capacities at current densities of 2.5 Å.

[0069] Fig.17 XRD patterns of lithium foil after (a) annealing at 90°C, showing random surface crystal orientation; (b) rolling to 300 μm thickness at room temperature; (c) scraping off about 50 μm of the surface layer from a at 75°C; (d) and then further rolling to 200 μm thickness at 75°C.

[0070] Fig.18 XRD patterns are shown for: (a) lithium foil with strong {100} texture; (b) without annealing after {100} surface texture preparation; (c) after annealing showing random surface crystal orientation (no pre-existing texture); and (d) after annealing and after {100} surface texture preparation.

[0071] Fig.19 XRD patterns of (a) annealed and rolled lithium foil; (b) annealed and rolled to 400 μm; (c) annealed and rolled to 300 μm; and (d) annealed and rolled to 200 μm thickness are shown.

[0072] Fig. 20 XRD patterns of lithium foil in the following cases are shown: (a) annealed before rolling; (b) annealed before scraping and rolled to 400 μm; (c) annealed before scraping and rolled to 300 μm.

[0073] Fig.21 XRD patterns of the corresponding lithium foils before the second rolling (a), after the second rolling to 400 μm (b), and after the second rolling to 300 μm (c) are shown.

[0074] Fig. 22 XRD patterns of lithium foil rolled to a thickness of about 200 μm at different temperatures are shown.

[0075] Fig.23 XRD patterns of the Li{110} surface of lithium foil after storage for different durations are shown.

[0076] Fig.24 The {100} textured lithium foil is shown at 1 mA / cm 2Current density and XRD patterns after stripping at different capacities.

[0077] Fig.25 XRD patterns of (a) pristine Na foil; (b) Na foil after pressing at 1 MPa; (c) Na foil after pressing at 3 MPa; and (d) Na foil after pressing at 5 MPa are shown.

[0078] Fig.26 The XRD pattern of the Na foil surface treated to produce a {110} texture is shown, and the sample is named Na{110}.

[0079] Fig.27A and 27B Symmetric cells of Na{100} (black), Na{110} (red), and pristine Na foil (blue) are shown at 5 mA / cm 2 Current density, 1 mAh / cm 2 potential cycle under capacity.

[0080] Fig.28 The XRD patterns of the 3D current collectors obtained after using a Li{110} matrix and after lithium electroplating in a traditional manner are shown. DETAILED DESCRIPTION

[0081] Various embodiments of the present invention relate to the preparation of Li foil or Na foil having Li{110}, Li{100}, Na{110} or Na{100} crystal plane textures, as shown in FIG2 . No specific texture was found in commercially available lithium foil or sodium foil before and after chemical polishing. In contrast, a uniaxial pressure of 5.0 MPa perpendicular to the surface of the Li foil or 3 MPa perpendicular to the surface of the Na foil produced a {100} crystal plane texture on the Li foil and the Na foil. Greater pressure will promote the formation of other crystal plane textures other than {100}, consistent with the formation of crystal plane textures in metals with a body-centered cubic (BCC) structure. The thickness of the Li{100} crystal plane texture layer is estimated to be no less than 48.5 μm, and the Li{100} preferential crystal plane orientation is found to be stable when stored in a glove box at room temperature for 90 days or more.

[0082] In one embodiment, a method for preparing a Li foil having a {110} crystal plane texture comprises: annealing a commercial lithium foil having a diameter of, but not limited to, about 16 mm and a thickness of, for example, about 600 μm at 90° C. for 2 hours before cooling to room temperature. This step removes any pre-existing crystal plane texture in the lithium foil and randomizes the surface crystal orientation. The surface of the commercial lithium foil is cleaned by polishing. The polished sample is first rolled at room temperature, for example, to a thickness of about 300 μm. A surface layer having a thickness of, for example, about 50 μm is scraped off by a scraper, wherein the scraping direction is the rolling direction. The scraped lithium foil is annealed, for example, at 75° C. for 30 minutes, and rolled a second time at this high temperature to a thickness of 200 μm. To complete the Li electrode, the lithium foil is cooled to room temperature and cut into a circular shape, which, as an exemplary embodiment, has a diameter of about 12 mm. The Na foil with {110} crystal plane texture does not require annealing temperature or second rolling above room temperature, although the other steps are similar to the method of Li foil with {110} crystal plane texture. As used in this article, the term annealing is used to refer to the holding process at a temperature at which the desired crystal plane texture is observed after the process, and annealing does not necessarily require high temperatures as required by typical common annealing processes, which require heat to promote relaxation or other structural changes. Therefore, if the desired crystal plane texture has been achieved, the holding at room temperature can be referred to as annealing in this article.

[0083] After polishing the Li foil, its surface becomes flat, as Figure 2A As shown, the surface chemical composition of the samples is consistent, as Figure 2B The X-ray diffraction (XRD) of chemically polished pristine Li foil shows almost no preferential texturing or crystal plane orientation, and the intensity ratios of the diffraction peaks of different samples are different, as shown in Figure 2. Figure 2C All diffraction peaks can be indexed to body-centered cubic (bcc) Li (JCPDF#15-0401).

[0084] When a symmetrical cell is used with polished lithium foil electrodes without further treatment and carbonate as the electrolyte, the overpotential of the cell will change with the cycling of the cell. Figure 3 It shows that at a current density of 1 mA / cm 2 And the capacity is 1mAh / cm 2 When , there is a large fluctuation in the overpotential at the beginning of the cycle, which is attributed to the formation of SEI, and then it stabilizes at 0.1 mV. Figure 3In one exemplary cell of the three cells plotted in Figure 1, a sudden increase in overpotential occurred at the 99th cycle, as well as frequent overpotential fluctuations. This is a common indicator of device failure, where lithium dendrite growth and the formation of dead lithium are known to be the main factors. The cycling performance of different polished lithium foils varies significantly, with the sharp increase in overpotential varying significantly in different cells, with some cells appearing after 50 cycles and others after 200 cycles.

[0085] When Li{110} and Li{100} foils are treated as Figure 2A When polished in the same manner as the original foil shown, the Li{110} and Li{100} foils exhibit similar flatness and chemical composition, as shown in Figure 2. Figures 4A-4E As shown. XRD taken from chemically polished Li{100} shows that bcc Li has a strong (200) diffraction, such as Figure 5A As shown in (a), there are almost no diffraction signals (211) and (110), which indicates the preferential {100} crystal plane texture of Li{100} foil. In contrast, the XRD of Li{110}, such as Figure 5A (b) shows the (110) diffraction of bcc Li, with almost no other diffraction peaks, indicating that the foil sample has a {110} preferential texture. Symmetric cells using Li{110} and Li{100} as electrodes at 1 mAh / cm 2 Capacity and 1 and 5 mA / cm 2 The constant current charge and discharge performance in carbonate electrolyte at different current densities is shown in Figure 2. Figure 5B As shown, an example cell. At 1 mA / cm 2 At a current density of 5 mA / cm2, the overpotentials of the Li{110} and Li{100} example batteries were stable before 250 cycles, with the overpotential of Li{100} increasing rapidly from 180 mV in the 250th cycle to 323 mV in the 350th cycle, at which time the overpotential curve fluctuated. In contrast, the overpotential of Li{110} increased slowly from 141 mV to 203 mV from the 1st cycle to the 400th cycle, without much fluctuation. When the current density increased to 5 mA / cm2, the overpotential of Li{100} increased rapidly from 180 mV in the 250th cycle to 323 mV in the 350th cycle, at which time the overpotential curve fluctuated. 2 When Li{100} has overpotential fluctuation after about 100 cycles, short circuit occurs after about 120 cycles, as shown in Figure 5C In contrast, Li{110} was stable for 150 cycles. 2 At low current densities of 5 mA / cm 2At higher current densities, the overpotentials of Li{100} and Li{110} are similar in the first 65 cycles, and the appearance of increased ion flow inhomogeneity and the intensification of side effects also begin to offset the benefits of the Li{110} crystal plane, but Li{110} can still achieve a longer cycle life. Figure 5D When the capacity is 1mA / cm 2 The current density increased to 5 mAh / cm 2 When Li{110} (60 cycles) was used, it consistently showed significantly better performance than Li{100} (35 cycles) and pristine lithium foil (25 cycles). Symmetric cells with Li{110} achieved better performance when using ether electrolytes. Figure 5E In 1mA / cm 2 At a current density of 2.5 Å, the overpotentials of Li{110} and Li{100} remain stable before 500 cycles ( Figure 3 ). After that, the overpotential of Li{100} increases rapidly from 80 mV to about 200 mV before short circuit occurs. In contrast, from the 1st cycle to the 1000th cycle, the overpotential of Li{110} increases slowly from about 50 mV to about 120 mV without much fluctuation. When the capacity is increased to 5 mAh / cm 2 When the overpotential of Li{100} increases to about 150 mV, the battery life decreases to 80 cycles, while Li{110} Fig. 5F Without artificial SEI, the Li{110} symmetric cells demonstrate comparable performance to technologies that use artificial SEI, such as LiDFOB and graphite fluoride.

[0086] Fig. 6A and 6B The results show that for 1 mA / cm 2 The current density and 1 mAh / cm 2 Ex situ XRD of the lithium {110} and {100} electrodes at different cycle numbers for an exemplary symmetric cell with a capacity of 1 mAh / cm2. 2 After the capacity of the battery was increased, the positive electrode of the symmetric battery using Li{100} underwent a stripping process. Fig. 6A As shown in , there is almost no (110) diffraction signal in the initial positive electrode (no cycles). At the same time, the (110) diffraction signal is found in the negative electrode that has undergone electroplating. At the end of the 50th cycle, the (200) diffraction is still the strongest, but the intensity of the (110) diffraction continues to grow with each cycle until the end of the 100th cycle, when the (110) diffraction becomes dominant. At the end of the 300th cycle, the diffraction intensity of (211) also exceeds that of (200). On the contrary, as Figure 6BAs shown, for the Li{110} electrode, the main diffraction intensity of (110) is maintained from the first cycle to the last cycle, while the diffraction intensity of (211) or (200) is almost absent and can only be observed in the 300th cycle.

[0087] Similar exemplary symmetric cells are respectively 2 At the same current density (1 mAh / cm 2 ) cycles, the evolution of the XRD patterns of the Li electrodes composed of Li{110} or Li{100} foils, respectively, as shown in Figure 6C and 6D As shown, charging to 1mAh / cm 2 After the capacity is reached, the Li{100} electrode quickly loses the preferred texture of {100}, and the (110) diffraction becomes dominant only after 50 cycles. The (211) diffraction intensity increases sharply from the 50th cycle to the 100th cycle and becomes dominant after the 100th cycle. In contrast, the diffraction intensity of (110) maintains its dominance in the Li{110} electrode through the 100th cycle. The exemplary Li{100} electrode shorts after the 100th cycle, while the Li{110} operates longer, although also up to about 150 cycles, the (211) and (200) diffractions become apparent, as shown in Figure 2. Fig. 6E shown.

[0088] The crystal morphology of these exemplary Li{100} and {110} electrodes shows the changes in surface features during cycling by SEM, such as Figures 7A to 7H The peeled surface of Li{100} foil after the first cycle is shown in Fig. 7A and 7B As shown, at a current density of 1 mA / cm 2 and 5mA / cm 2 The pitting surface was observed on Li{100} at 1 mA / cm 2 The battery cycle was 5 mA / cm 2 More pits appeared in the cycled samples. Fig. 7A and 7B The enlarged image of the pit area in shows the porous surface inside the pit. Similar pitting occurs for Li foil without preferential texturing, as shown in Fig.7I In contrast, the exfoliation surface of Li{110} foil is very different: at low current density (1 mA / cm 2 ), the Li surface remains flat with almost no pitting, e.g. Figure 7C As shown, at 5mA / cm 2 At higher current densities, such as Fig.7DAs shown in Figure 2, some pits appeared, but their size was significantly smaller than that on the Li{100} surface. When lithium was plated on the Li negative electrode surface, granular deposits formed on the Li{100} and Li{110} surfaces. The Li{100} negative electrode showed a 2 The particles formed at a current density of Fig. 7E , its density is greater than 5mA / cm 2 The particles formed under Figure 7F This trend is observed in Li{110} anodes, such as Figure 7G and 7H , the density of Li plated on Li{110} is higher than that on Li{100} at both current densities tested. During discharge after the first cycle, the newly plated Li anode was stripped, and significant pitting was observed for the Li{100} surface, but not for Li{110}, which is similar to the pitting of the Li cathode surface at the end of the first charge, as shown in Figure 2. Figures 8A to 8D The discharge process leads to the plating of the lithium cathode that was stripped during the initial charge. Most of the pit surfaces of Li{100} are covered by new deposits, and it is observed that the surface of the Li{110} cathode is denser than that of the Li{100} cathode, as shown in Figure 2. Figures 8E to 8H shown.

[0089] At 1mA / cm 2 The current density and 1 mAh / cm 2 The morphology of lithium foil after cycling at a capacity of Figures 9A to 9D shown. Fig. 9B The morphology of the Li{100} surface after 300 cycles is Fig. 9A The initial surface shown is much rougher. In contrast, the Li{110} (e.g. Fig.9D ) on the starting surface ( Fig. 9C ) was not significantly degraded. When the current density was increased to 5 mA / cm 2 When the Li foil surface morphology evolves faster, exceeding 1 mA / cm 2 The Li{100} sample showed obvious surface roughening at 50 cycles at a low current density, and deteriorated with further cycling, such as Fig. 10A , as shown in 10C and 10E. In contrast, the surface smoothness of Li{110} is maintained at the same number of cycles, as shown in Fig. 10B , 10D and 10F.

[0090] The full cell uses Li / / LiFePO4 (Li / / LFP), demonstrating the advantages of Li{110} crystal texture. After pre-activation at 0.1C rate, the full cell with Li{100} positive electrode reaches a discharge capacity of 143.7mAh / g after 400 cycles at 1C rate, and the capacity retention rate is 23.3% (33.5mAh / g), as shown in Figure 2. Fig.11A The initial discharge capacity of other equivalent full cells with Li{110} cathodes is slightly lower at 136.4 mAh / g, but after 400 cycles at 1C rate, the capacity retention rate is significantly improved to 81.9% (111.7 mAh / g), as shown in Figure 2. Fig.11A As shown. Li / / LFP full cells with Li{100} or Li{110} anodes show higher capacity retention than cells built using pristine lithium foil lacking preferential crystal plane texture. The electrochemical performance of full cells with pristine lithium foil anodes varies. For example, although their initial discharge capacities are similar, about 140 mAh / g, the "short-life" cells show about 20% capacity retention after 250 cycles, and the "long-life" cells show about 20% capacity retention after 350 cycles, as shown in Figure 2. Fig. 12A When the magnification is increased to 5C, as shown in Fig. 11B As shown, the initial discharge capacity of the exemplary cell with Li{100} anode is 111.5 mAh / g, the capacity retention after 400 cycles is 63.3% (70.6 mAh / g), and after 750 cycles is 21.9% (19.9 mAh / g), and the capacity retention of the cell containing Li{110} is 96.6% (106.9 mAh / g) after 400 cycles and 75.9% (82.4 mAh / g) after 750 cycles. Again, the performance of the cells made with Li{100} and {110} is much better than that of the full cell made with the original lithium foil anode, which shows about 20% capacity retention (19.4 mAh / g) after only 500 cycles, as shown in Figure 2. Fig. 12B The rate performance of the full battery is shown in Fig. 11C As shown, the battery with Li{100} negative electrode provides discharge capacities of 145.2 mAh / g, 130.1 mAh / g and 115.7 mAh / g at 1C, 2C and 5C rates, respectively, which are slightly higher than the discharge capacities of 138.5 mAh / g, 125.1 mAh / g and 113.5 mAh / g of the battery with Li{110} negative electrode at 1C, 2C and 5C rates. Fig.13As shown in Figure 2, at the lower 1C rate, the small overpotentials of cells with Li{100} and {110} are similar, with the overpotential of Li{110} being slightly lower than that of Li{100}. The difference becomes larger for cells cycled at 5C (0.623 V for Li{110} and 0.744 V for Li{100}).

[0091] Thus, in the embodiments, the Li metal electrode with {110} texture significantly improves the cycling stability of devices with symmetric cell and full cell configurations relative to the equivalent Li metal electrode or pristine Li foil with {100} texture or without any specific texture. These cells lack any artificial SEI, but the Li{110} electrode shows comparable performance to artificial SEI cells disclosed in the literature. Compared with the lithium {100} electrode or the pristine lithium foil electrode, the lithium metal electrode with {110} texture has a significantly improved cycling stability even at 5 mA / cm 2 The preferred {110} crystal plane orientation and surface flatness are maintained during repeated cycles at high current densities. Due to its low surface energy and surface diffusion barrier, Li is uniformly stripped and densely plated on the Li{110} surface, demonstrating that the use of Li{110} can significantly enhance the cycling performance.

[0092] Na{110} and Na{100} symmetric batteries with 1 mAh / cm 2 Capacity and 1mA / cm 2 and 5mA / cm 2 The constant current charge-discharge performance of different current densities in diethylene glycol dimethyl ether is Fig.27A and 27B Shown as an example cell. At 1 mA / cm 2 At a current density of 5 mA / cm, the Na{110} electrode can stably cycle for more than 1200 times, while the Na{100} and pristine sodium foil electrodes show fluctuations at about 80 and 200 cycles, respectively. 2 At a current density of , the overpotentials of the Na{110} and Na{100} example batteries were stable before 150 cycles, with the overpotential of Na{100} increasing rapidly after 170 cycles. In contrast, from the 1st cycle to the 300th cycle, the overpotential of Na{110} remained stable at around 100 mV without much fluctuation.

[0093] The prepared Li{110} foil can also be used as a substrate to further prepare Li-based 3D electrodes with {110} texture. To prepare such 3D electrodes, Li metal is electroplated onto a 3D template (e.g., carbon cloth) located on a Li{110} substrate. 2 The current density is 10 mAh / cm 2Li was plated on the 3D template. XRD obtained from the electroplated sample showed Fig.28 The main (110) diffraction of bcc Li in the 3D current collector indicates that the preferential {110} texture of Li metal forms a 3D composite structure with the original 3D current collector (carbon cloth). In comparison, without the guiding effect of Li{110} foil, the lithium plating in the current collector has no texture (e.g. Fig.28 ).

[0094] The following are examples of the process of implementing the present invention. These examples should not be construed as limiting. Unless otherwise indicated, all percentages are by weight and all solvent mixture ratios are by volume.

[0095] Materials and methods

[0096] Li foil (Zhongneng Lithium Co., Ltd.) was polished using a naphthalene tetrahydrofuran solution (0.192 g naphthalene crystals (>99.5%, SigmaAldrich) dissolved in 15 mL anhydrous tetrahydrofuran (>99.8%, Sigma Aldrich)) for 2 min. Subsequently, the Li foil was rinsed three times with DEC to remove the polishing solution. All processes were performed in a glove box with oxygen and water content below 0.5 ppm.

[0097] Preparation of lithium foil with {110} crystal texture

[0098] To prepare Li foil with {110} surface crystal orientation, the original Li foil with a thickness of about 600 μm and a diameter of 16 mm was first rolled to a thickness of about 300 μm using a stainless steel roller at room temperature (about 20°C). The surface of the lithium foil was then unidirectionally scraped at 75°C. After that, the thickness of the lithium foil was further reduced to about 200 μm by a second rolling at 75°C using the same stainless steel shaft. A circle with a thickness of about 200 μm and a diameter of 12 mm was cut from the center of the oval lithium foil and used as a Li{110} electrode.

[0099] Preparation of lithium foil with {100} crystal texture

[0100] To prepare Li foil with {100} surface crystal orientation, the original Li foil was pressed at 5 MPa for 5 seconds at room temperature using a hydraulic press. The thickness of the lithium foil after pressing was reduced to about 250 μm and the diameter increased to about 20 mm. A circle with a diameter of 12 mm was cut from the center of the treated lithium foil and used as a Li{100} electrode.

[0101] CR-2032 type button cells were assembled to study the electrochemical performance of Li or Na foils with specific textures. Symmetric cells were prepared using lithium or sodium foils with the same surface crystal orientation as both electrodes (i.e., {100} and {100}, {110} and {110}).

[0102] For the lithium electrode, symmetric cells were constructed using 1 M lithium hexafluorophosphate (LiPF6) in 1:1 ethylene carbonate (EC) / diethyl carbonate (DEC) and 1 M lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) in 1:1 1,3-dioxolane (DOL) / 1,2-dimethoxyethane (DME) and 1% LiNO3 as the electrolyte. 2 and 5mA / cm 2 At a current density of 1 mAh / cm 2 A series of symmetric cells were assembled and cycled with a capacity of 1.5 Å. At different cycle numbers, the cells were stopped and disassembled. The disassembled electrodes were rinsed with DEC to remove the electrolyte. The electrodes from the cells were sealed with Kapton film in a glove box and then subjected to ex-suit XRD experiments to complete the texture evolution test. The transfer from the glove box to the scanning electron microscope (SEM) was performed by a vacuum transfer device to complete the surface morphology imaging of the Li foil.

[0103] For the sodium electrode, a symmetric cell was constructed using 1 M sodium hexafluorophosphate (NaPF6) in diethylene glycol dimethyl ether (DEGDME) as the electrolyte. The symmetric cell was operated at 5 mA / cm 2 At a current density of 1 mAh / cm 2 capacity cycle.

[0104] Standard CR2032 button cells were assembled to produce Li / / liFePO4 full cells. The electrolyte for the full cell was 1.0 m LiPF6 dissolved in EC / DEC (v / v = 1:1), and 60 μl of liquid electrolyte was added to each cell. The positive electrode was prepared by mixing LiFePO4 active material, carbon black (TIMCAL) and polyvinylidene fluoride (PVDF) in anhydrous N-methyl-2-pyrrolidone (NMP) in a weight ratio of 8:1:1, and casting the resulting slurry on lithium foil, so that the mass loading of LiFePO4 in the positive electrode was about 8.0 mg. The full cell was pre-cycled three times at a 0.1C rate to activate the positive electrode, and then cycled at 1C and 5C rates, respectively, and the relative Li+ / Li voltage range was about 2.2-4.0 V.

[0105] A 3D current collector (carbon-based) with a {110} texture was prepared by electrochemical plating. The 3D current collector was placed on a Li{110} foil. 2 The current density is 10 mAh / cm 2 Li was plated in a half-cell with Li foil as the counter electrode. After stripping the lithium foil, the 3D current collector was washed three times with DOL to remove the electrolyte and then tested by XRD.

[0106] Characteristics of lithium foil at different preparation stages

[0107] Li{100}

[0108] Just as multiple diffraction peaks with similar intensities in X-ray diffraction (such as Fig.14 As shown by XRD (a), no preferential crystal texture was observed in most polished Li foil samples. When the pressure increases, it is found that the relative intensity of the (200) diffraction increases first (e.g. Fig.14 XRD (b) and (c)), and then reached its highest level at a pressure of 5 MPa ( Fig.14 XRD (c)). Under higher pressure, the relative intensity of (200) diffraction begins to decrease ( Fig.14 XRD (d)). Therefore, 5.0 MPa was selected as the loading pressure for preparing Li foil with {100} crystal plane texture (referred to as Li{100}). When stored in a glove box at room temperature for up to 90 days, it was observed that the crystal plane texture of the Li{100} sample changed little, such as Fig.15 The time-dependent X-ray diffraction pattern is shown.

[0109] Thickness estimation of Li{100} crystal texture

[0110] 1 mAh stripping capacity is equivalent to about 4.85 μm of {100} lithium layer in the experimental setup. A specific crystal orientation (hkl) becomes dominant when the total intensity of all other diffraction planes is less than 1 / 5 of that of the specific crystal orientation (hkl). Taking it as a standard, when the stripping capacity reaches 10 mAh, the total intensity of all other crystal planes reaches 19.5% of the (200) diffraction, as shown in Fig.16 Therefore, it is found that the {100} plane texture is maintained at a stripping capacity of 10 mAh, corresponding to a texture layer thickness of about 48.5 μm.

[0111] Li{110}

[0112] After annealing, the lithium foil (600 μm) has no obvious texture ( Fig.17 XRD (a)). After the first rolling to a thickness of about 300 μm at room temperature, the relative intensity of the (200) diffraction increases significantly ( Fig.17 XRD (b)). A 300 μm thick lithium foil was scraped off once with a blade, and the thickness was reduced by 50 μm). The corresponding X-ray diffraction showed that {110} diffraction dominated ( Fig.17 XRD (c)). After the second rolling at 75°C to a thickness of about 200 μm, the {110} diffraction dominated ( Fig.17 XRD (d) shows that the Li foil forms a {110} crystal plane texture.

[0113] Effect of pre-existing crystal plane texture of Li foil on the formation of {110} crystal plane texture

[0114] To determine whether pre-existing texture would affect the formation of the desired texture, samples with strong {100} texture were used in the method for preparing Li foil ( Fig.18 XRD (a)), where the crystal texture ( Fig.18 XRD(c)) will be reduced to a value similar to that of the non-textured sample ( Fig.18 XRD (b)), which allows the method according to the example to transform the pre-existing {100} crystal plane texture to {110} crystal plane texture ( Fig.18 XRD(d)).

[0115] The effect of the first rolling thickness on the formation of {110} plane texture is shown in Fig.19 As shown. Since there is no specific crystal plane texture in the annealed lithium foil, the first rolling produces a stronger (200) diffraction. In addition, the mechanical strength of Li foil decreases with decreasing thickness. Therefore, on thicker original lithium foil, the first rolling thickness is not selected to be 200 μm to avoid cracking.

[0116] After scraping, Fig. 20 As shown in Figure 3, lithium foils with thicknesses of 400 μm and 300 μm exhibit obvious {110} crystal plane textures, and the relative intensity of (110) diffraction appears stronger in the 300 μm sample. In both samples, diffraction from other crystal planes is still visible.

[0117] like Fig.21 As shown, {110} plane texture was observed from 400 μm or 300 μm thick lithium foil after the second rolling to 200 μm thickness at 75° C. The best {110} plane texture was obtained in 300 μm thick lithium foil.

[0118] Effect of annealing temperature on the formation of {110} plane texture during secondary rolling

[0119] like Fig. 22 As shown in Figure 2, at low temperatures (<50°C), the relative intensity of the (200) diffraction increases with decreasing temperature. Increasing the temperature causes the (110) diffraction to rise, becoming dominant at 75°C. Further increases in temperature above 75°C cause the (211) diffraction to exceed the (110) diffraction. Therefore, 75°C appears to be the optimal temperature for annealing during the second rolling. The {110} plane texture of the prepared Li foil remained stable when stored in a glove box at room temperature for 90 days, as shown in Figure 2. Fig.23 shown.

[0120] Thickness estimation of Li{110} crystal texture

[0121] The 1 mAh stripping capacity corresponds to a lithium layer of about 4.85 μm. It is found that the {110} crystal plane texture is still dominant when the stripping capacity reaches 20 mAh, such as Fig.24 As shown, it corresponds to a crystal texture layer with a thickness of about 97 μm. When the lithium foil is treated on both sides, the texture thickness can reach about 200 μm, which is the thickness of the entire lithium sheet.

[0122] Preparation of Sodium Foil with {100} Crystalline Texture

[0123] The formation of Na foil with {100} texture was carried out in a glove box with oxygen and water contents less than about 0.5 ppm and about 0.5 ppm, respectively, in a manner similar to the preparation of lithium foil with {100} texture. Since the Brinell hardness of sodium (0.69 MPa) is lower than that of lithium (5 MPa), the uniaxial pressure applied on sodium is lower than that of lithium. Therefore, a commercial sodium block (Sigma-Aldrich, 15 mm×15 mm×15 mm) was sliced ​​to form a sodium foil with a thickness of 1.5 mm. The sodium foil was placed under a hydraulic press, and a uniaxial pressure (P=3 MPa) was applied perpendicular to the sample surface. As Fig.25 As shown, this pressure is determined to be optimal. The pressure is then maintained for about 5 seconds. A flat circular electrode with a diameter of about 12 mm is cut from the center portion of the pressed sodium foil.

[0124] Preparation of Sodium Foil with {110} Crystalline Texture

[0125] The formation of the {110} textured sodium foil was performed in a glove box with oxygen and water contents less than about 0.5 ppm and about 0.5 ppm, respectively, in a manner similar to the preparation of lithium foil with a {110} texture. Since the temperature for generating lithium {110} is 50 to 100°C (70%-80% of the melting point of lithium). In this way, 70%-80% of the melting point of sodium is -13.5°C to 23.6°C. As a result, the Na foil {110} texture is obtained at room temperature, as shown in FIG. Fig.26 As shown. After producing 1.5 mm Na foil, the sodium foil was first rolled to a thickness of about 300 μm at room temperature as described above. A surface layer of about 50 μm thick was scraped off using a blade with the scraping direction being the same as the rolling direction. The sodium foil was second rolled to a thickness of 200 μm at room temperature. A flat circular electrode of about 12 mm in diameter was cut from the center portion of the rolled sodium foil.

[0126] All patents, patent applications, provisional applications, and publications mentioned or cited herein are hereby incorporated by reference in their entirety, including all figures and tables, to the extent they are not inconsistent with the explicit teachings of this specification.

[0127] It should be understood that the examples and embodiments described herein are for illustrative purposes only, and that various modifications or changes that may be suggested by a person skilled in the art should be included within the spirit and scope of the present invention and the scope of the appended claims. In addition, any element or limitation of any invention or embodiment thereof disclosed herein may be combined with any and / or all other elements or limitations disclosed herein (alone or in any combination) or any other invention or embodiment thereof, and all such combinations are considered without limitation to the scope of the present invention.

[0128] Preparation of Li-based 3D current collectors with {110} surface texture

[0129] Taking the prepared Li{110} foil as the substrate, a 3D Li metal electrode with {110} texture can be prepared by electroplating Li onto carbon cloth (serving as a 3D substrate template) placed on top of the Li{110} foil.

[0130] References

[0131] 1.Li,L.et al.,Self-heating–induced healing of lithiumdendrites.Science,2018.359(6383):p.1513-1516.

[0132] 2.Tang,W.et al.,Chemically polished lithium metal anode for highenergy lithium metal batteries.Energy Storage Materials,2018.14:p.289-296.

[0133] 3.Coblas,DGet al.,Manufacturing textured surfaces:State of art and recent developments.Proceedings of The Institution of Mechanical Engineers,Part J:Journal Of Engineering Tribology,2015.229(1):p.3-29.

[0134] 4.Zheng,J.et al.,Textured Electrodes:Manipulating built-inCrystallographic Heterogeneity of Metal Electrodes via Severe PlasticDeformation.Advanced Materials,2021.2106867.

[0135] 5.Gu,Y.et al.,Lithiophilic Faceted Cu(100)Surfaces:High Utilizationof Host Surface and Cavities for Lithium Metal Anodes.Angewandte ChemieInternational Edition,2019.58(10):p.3092-3096.

[0136] 6.Li,Y.et al.,Atomic structure of sensitive battery materials andinterfacesrevealed by cryo–electron microscopy.Science,2017.358(6362):p.506-510.

[0137] 7.Zhao,Q.et al.,On the crystallography and reversibility oflithiumelectrodeposits at ultrahigh capacity.Nature Communications,2021,12(1),1-10.

[0138] 8.Shi,F.et al.,Strong texturing of lithium metal inbatteries.Proceedings of theNational Academy of Sciences,2017.114(46):p.12138-12143.

[0139] 9.Hagopian,A.et al.,Thermodynamic origin of dendrite growth in metalanodebatteries.Energy Environ.Sci.2020,13:p.5186-5197.

[0140] 10.Zaghib,K.et al.,Relationship between local structure andelectrochemicalperformance of LiFePO4 in Li-ion batteries[J].Ionics,2008,14(4):p.271-278.

[0141] 11.Luning,W.et al.,Identifying the components of the solid–electrolyteinterphase in Li-ion batteries.Nature Chemistry 2019,11,789–796.

[0142] 12.Guo,W.et al.,Mixed Ion and Electron-Conducting Scaffolds for High-Rate.Adv.Energy Mater.2019,9,1900193.

[0143] 13.Qin,L.et al.The role of mechanical pressure on dendritic surfacetowardstable lithium metal anode.Nano Energy 2020,77,105098.

[0144] 14.Jens,B.et al.,Lithium-Metal Foil Surface Modification:AnEffectiveMethod to Improve the Cycling Performance of Lithium-MetalBatteries.Adv.Mater.Interfaces 2017,4,1700166.

[0145] 15.Gu,Y.et al.,Designable ultra-smooth ultra-thin solid-electrolyteinterphasesof three alkali metal anodes.Nature Communication 2018,9,1339.

[0146] 16.Zheng,G.et al.,Additives synergy for s table interface formationonrechargeable lithium metal anodes.Energy Storage Materials,2020,29:p.377-385.

[0147] 17.Zhang,P.et al.,Influence of current density on graphite anodefailure inlithium-ion batteries[J].Journal of The Electrochemical Society,2019,166(3):A5489.

[0148] 18.Jiao,S.et al.,Behavior of lithium metal anodes under variouscapacityutilization and high current density in lithium metal batteries[J].Joule,2018,2(1):110-124.

[0149] 19.Shen,X.et al.,Lithium anode stable in air for low-cost fabricationof adendrite-free lithium battery[J].Nature Communications,2019,10(1):1-9.

[0150] 20.Yu,L.et al.,A localized high-concentration electrolyte withoptimizedsolvents and lithium difluoro(oxalate)borate additive for stablelithium metalbatteries[J].ACS Energy Letters,2018,3(9):2059-2067.

[0151] 21.Gireaud,L.et al.,Lithium metal stripping / plating mechanismsstudies:Ametallurgical approach.Electrochemistry Communications,2006,8(10),p.1639-1649.

[0152] 22.Gehrmann,G.et al.,Texture effects on plastic deformation ofmagnesium.Materials Science and Engineering A 395(2005)338–349.

[0153] 23.Liu,D.et al.,Improving single pass reduction during cold rollingbycontrolling initial texture of AZ31 magnesium alloy sheet.TransactionsofNonferrous Metals Society ofChina 28.2(2018):244-250.

[0154] 24.Hayakawa,Y.et al.,A new model of Goss texture developmentduringsecondary recrystallization of electrical steel.Acta Materialia 45.11(1997):4713-4720.

Claims

1. A method for preparing an alkali metal electrode having a {110} crystal plane texture, characterized in that: include: providing a base metal foil; Performing a first annealing on the alkali metal foil at a first annealing temperature of about 70% to 90% of the melting point of the alkali metal foil, and maintaining the temperature at the first annealing temperature for 1 to 3 hours; Optionally, cooling the alkali metal foil to room temperature for the first time, at which time the alkali metal foil has a random surface crystal orientation; Optionally, washing the annealed base metal foil with a chemical polishing solution to remove surface contaminants; The alkali metal foil was first rolled to about 300 μm at room temperature; Scraping off a surface layer having a thickness of about 50 μm from the alkali metal foil at a temperature of about 70% to 90% of the melting point of the alkali metal foil, wherein the scraping is performed along the same axis as the first rolling; performing a second annealing treatment on the alkali metal foil at a second annealing temperature of about 70% of the melting point of the alkali metal foil for about 0.5 hour; rolling the alkali metal foil for a second time at the second annealing temperature to a thickness of about 200 μm; Optionally, cooling the alkali metal foil to room temperature a second time; and The alkali metal foil is cut into an electrode shape, wherein the alkali metal electrode includes a {110} crystal plane texture.

2. The method according to claim 1, characterized in that The alkali metal is lithium, the first annealing temperature is about 90°C, the scraping temperature is about 75°C, and the second annealing temperature is about 75°C.

3. The method according to claim 1, characterized in that The alkali metal is sodium, the first annealing temperature is about room temperature, and the second annealing temperature is about room temperature.

4. The method according to claim 1, characterized in that The polishing solution was 0.192 g of naphthalene crystals (>99.5%, Sigma Aldrich) dissolved in 15 mL of anhydrous tetrahydrofuran (>99.8%, Sigma Aldrich).

5. The method according to claim 1, characterized in that The electrode is circular in shape.

6. The method according to claim 1, characterized in that The sizes of the provided alkali metal foils are all larger than the sizes of the alkali metal electrodes.

7. A method for preparing an alkali metal electrode comprising a {100} crystal plane texture, characterized in that: include: providing a base metal foil; Pressing the alkali metal foil to a thickness of about 250 μm; The alkali metal foil is cut into an electrode shape, where the alkali metal electrode is substantially composed of a {100} crystal plane texture.

8. The method according to claim 7, characterized in that The alkali metal is lithium, and the pressing pressure is 5 MPa.

9. The method according to claim 7, characterized in that: The alkali metal is sodium, and the pressing pressure is 3 MPa.

10. The method according to claim 7, characterized in that The electrode is circular in shape.

11. An alkali metal electrode, characterized in that Included are alkali metals consisting essentially of {110} or {100} crystal plane textures.

12. The alkali metal electrode according to claim 11, characterized in that The alkali metal is lithium.

13. The alkali metal electrode according to claim 11, characterized in that The alkali metal is sodium.

14. The alkali metal electrode according to claim 11, characterized in that The {110} crystal plane texture is at least 80% of the surface of the alkali metal electrode before the first discharge of the battery.

15. The alkali metal electrode according to claim 11, characterized in that The alkali metal electrode is a lithium metal negative electrode.

16. The alkali metal electrode according to claim 11, characterized in that The alkali metal electrode is a sodium metal positive electrode.

17. A battery, characterized in that: An alkali metal electrode consisting essentially of a {110} or {100} crystal plane texture is included.

18. The battery according to claim 17, characterized in that The alkali metal electrode is a lithium electrode.

19. The battery according to claim 17, characterized in that The alkali metal electrode is a positive sodium electrode.

20. The battery according to claim 17, characterized in that The alkali metal electrode is an alkali metal negative electrode.

21. The battery according to claim 17, characterized in that The alkali metal electrode is an alkali metal positive electrode.

22. The battery according to claim 17, characterized in that The {110} crystal plane texture occupies at least 80% of the surface of the alkali metal electrode before the first discharge of the battery.

23. A method for preparing a 3D current collector comprising a {110} crystal plane texture, characterized in that: include: Providing lithium {110} foil and 3D current collector; The 3D current collector is placed on top of the lithium {110} foil to form a sandwich structure; Lithium is plated onto the sandwich structure by electrochemical deposition, where the 3D current collector includes a {110} crystal plane texture.