Method for producing spherical particle material

The powder compressionability and high-temperature melt quenching process evaluated by powder rheometer solve the problem of particle size distribution and purity control of spherical particle materials in the prior art, and realize spherical particle materials with high melt spherification rate and small specific surface area Manufacturing, resin composition suitable for electronic materials.

CN118922244APending Publication Date: 2024-11-08ADMATECHS CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202380028043.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-15
Filing Date
2023-03-14
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing spherical particle material manufacturing methods, such as VMC method and melting method, are difficult to fully control the particle size distribution and melt spherification rate, resulting in the generated spherical particle material not meeting the target particle size distribution and purity requirements.

Method used

The high correlation between the FF value and the melt spheroidization rate was evaluated by the powder compression of the powder rheometer, and raw material particle materials of inorganic materials were prepared, and then melted and quenched in a high temperature atmosphere, so that the average particle size of the production volume was 1 μm The above spherical particle material less than 10 μm can improve the melt spherification rate.

Benefits of technology

A spherical particle material with high melt spheroidization rate and small specific surface area is achieved, suitable for fillers in resin compositions, and provides better particle size distribution and purity control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005044783900000071
    Figure BDA0005044783900000071
  • Figure BDA0005044783900000081
    Figure BDA0005044783900000081
  • Figure HDA0005044783910000011
    Figure HDA0005044783910000011
Patent Text Reader

Abstract

[Problem] To provide a method for producing a spherical particle material by a melting method, said method having a higher melt-spheroidization rate than conventional methods. The following inventions are completed by finding a high correlation between a powder compressibility evaluation FF value based on a powder rheometer and a melt spheroidization rate with respect to a raw material supplied to a melting method. This method for producing a spherical particle material comprises: a raw material particle material preparation step for preparing a raw material particle material comprising an inorganic material, said raw material particle material being introduced in a high-temperature atmosphere, melted and then quenched; a spheroidizing step for preparing a spherical particle material having a volume average particle diameter of 1 [mu] m or more and less than 10 [mu] m; the raw material particle material has a powder compressibility evaluation FF value of 2.0 or more as determined by a powder rheometer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for manufacturing a spherical particle material. Background Art

[0002] Spherical particle materials formed of inorganic materials are used as fillers for electronic materials such as fillers contained in semiconductor sealing materials and substrate materials. As spherical particle materials, various requirements are imposed on their particle size distribution, circularity, purity, etc.

[0003] Representative existing methods for manufacturing spherical particle materials from inorganic materials include: when the inorganic material is a metal oxide, a method in which a metal particle material formed by a metal constituting the metal oxide is put into a high-temperature oxidizing atmosphere to cause it to explode and then be quenched (VMC method); and a method in which a particle material formed by the inorganic material is put into a high-temperature atmosphere and then be quenched (melting method).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2019-182714 Summary of the invention

[0007] In the VMC method, the particle size distribution of the generated spherical particle material can be controlled by controlling the particle size distribution and the feeding speed of the metal particle material, but the control range is not completely free. In particular, it is difficult to expand the control range when using the VMC method to produce alumina.

[0008] Therefore, when studying the melting method that can control the particle size distribution of the raw material particle material to a certain extent, it is found that in the melting method, although the particle size distribution of the generated spherical particle material can be controlled by the particle size distribution of the raw material particle material, sometimes the melting cannot be completely carried out. For example, when the particle material formed by aluminum oxide is spheroidized by the melting method, a part of the particle material that is not melted is sometimes mixed. The index of the degree to which such a raw material particle material is melted is called the melting spheroidization rate (details are described later).

[0009] In addition, there is also disclosed a method for controlling the particle size distribution by using a large particle size particle material manufactured by granulating a small particle size particle material as a raw material and supplying it to a melting method (Patent Document 1). However, due to undesirable conditions such as the granulated particle material being destroyed, it is sometimes difficult to obtain a spherical particle material with a target particle size distribution.

[0010] The present invention has been made in view of the above-mentioned actual situation, and as a problem to be solved, provides a production method, which is a method for producing spherical particle materials by a melting method, and has a higher melting spheroidization rate than before.

[0011] The present inventors have conducted intensive studies to solve the above problems and have found that the FF value of powder compressibility evaluation using a powder rheometer for a raw material to be used in a melting method is highly correlated with the melt spheroidization rate, thereby completing the following invention.

[0012] The manufacturing method of the spherical particle material of the present invention for solving the above-mentioned problems includes: a raw material particle material preparation step of preparing a raw material particle material formed of an inorganic material, and a spheroidization step of putting the above-mentioned raw material particle material into a high-temperature atmosphere, melting it, and then rapidly cooling it to prepare a spherical particle material with a volume average particle size of greater than 1 μm and less than 10 μm; and the FF value of the above-mentioned raw material particle material based on the powder compressibility evaluation of a powder rheometer is greater than 2.0.

[0013] The powder compressibility evaluation FF value (hereinafter referred to as "FF value" in this specification) refers to the fluidity index, which is a value calculated by maximum principal stress (MPS) / uniaxial yield stress (UYS). Specifically, the FF value is a value measured by a shear stress test using a powder rheometer FT4 of Freeman Technology, a powder fluidity analyzer.

[0014] The method for producing a spherical particle material of the present invention can obtain a spherical particle material having a high melt spheroidization rate or a small specific surface area by having the above-mentioned configuration, and can provide a spherical particle material that is preferable when contained as a filler in a resin composition. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is a diagram showing the particle size distribution of the raw material particle material in Test 1 of the Example.

[0016] Figure 2 This is a SEM photograph of the raw material particle material in Test 1 of the Example.

[0017] Figure 3 This is a diagram showing the particle size distribution of the spherical particle material in Test 1 of the Example.

[0018] Figure 4 This is a SEM photograph of the spherical particle material of Test 1 of the Example. DETAILED DESCRIPTION

[0019] Hereinafter, a method for manufacturing a spherical particle material of the present invention will be described in detail according to an embodiment. The spherical particles manufactured by the method for manufacturing a spherical particle material of the present embodiment are filled as fillers in a resin material to form a resin composition. This resin composition is suitable for electronic materials.

[0020] The method for manufacturing a spherical particle material of the present embodiment has a raw material particle material preparation step, a spheroidization step, and other steps selected as needed. The spherical particle material manufactured by the method for manufacturing a spherical particle material of the present embodiment is composed of an inorganic material, and has a volume average particle diameter of 1 μm or more and less than 10 μm. Examples of the lower limit value of the volume average particle diameter may be 1 μm, 2 μm, 3 μm, and examples of the upper limit value may be 4 μm, 5 μm, 6 μm. These lower limit values and upper limit values can be arbitrarily combined.

[0021] The circularity of the spherical particle material manufactured by the manufacturing method of the present embodiment is 0.9 or more, preferably 0.95 or more, more preferably 0.98 or more, and further preferably 0.99 or more. The circularity in this specification is calculated as the following value: taking a photograph with SEM, and using (circularity) = {4π×(area)÷(perimeter) 2} to calculate based on the observed area and perimeter of the particles. The closer it is to 1, the closer it is to a perfect sphere. Specifically, it is the average value obtained by measuring 100 particles using image analysis software (Asahi Kasei Engineering Corporation: A Image King).

[0022] The inorganic material constituting the spherical particle material of the present embodiment is not particularly limited, but an inorganic material belonging to metal oxides is preferred, and specifically, alumina, silica, titanium dioxide, zirconia, magnesium oxide, and composite oxides of the above substances can be exemplified. As the inorganic material, it is particularly preferred to contain 50% or more, particularly more preferably 50% or more of alumina, based on the total mass, alone or in combination of the above metal oxides.

[0023] The total content of alkali metals and alkaline earth metals as impurities in the inorganic material is preferably 5 ppm or less, more preferably 3 ppm or less, and further preferably 1 ppm or less. In particular, the content of Na is preferably 5 ppm or less, more preferably 3 ppm or less, and further preferably 1 ppm or less.

[0024] Moreover, the total content of U and Th as impurities in the inorganic material is preferably 5 ppb or less, more preferably 3 ppb or less, and further preferably 1 ppb or less.

[0025] When the inorganic material is alumina, the specific surface area is preferably 1.0 m 2 / g or less, more preferably 0.8 m2 / g or less. Moreover, the melt spheroidization rate is preferably 85% or more. As the lower limit of the melt spheroidization rate, 88%, 90%, 92%, 94%, 95%, 96%, 97%, 98%, and 99% can be cited. The method for determining the melt spheroidization rate will be described in the following examples.

[0026] Raw material particle preparation process

[0027] The raw material particle material preparation step is a step of preparing a raw material particle material formed of an inorganic material. The inorganic material can be the same material as the inorganic material constituting the manufactured spherical particle material. The raw material particle material has a powder compressibility evaluation FF value of 2.0 or more based on a powder rheometer, preferably 2.5 or more, more preferably 3.0 or more, and further preferably 4.0 or more.

[0028] The FF value can be controlled by the particle shape, surface treatment, and particle size distribution of the raw particle material. Taking the overall mass of the raw particle material as a reference, when the content of particles with a particle size less than 1 μm is 2% or more, the FF value can be increased by reducing the circularity of the raw particle material. In this case, it is particularly preferred to make the circularity less than 0.9, more preferably less than 0.88, and further preferably less than 0.85. Taking the overall mass of the raw particle material as a reference, when the content of particles with a particle size less than 1 μm is 2% or less, the higher the circularity of the raw particle material, the better. In this case, it is particularly preferred to make the circularity more than 0.85, more preferably more than 0.88, and further preferably more than 0.90.

[0029] As the surface treatment, it is preferred to use a surface treatment agent capable of introducing trimethylsilyl, isocyanate, amino or phenyl groups as functional groups. For example, the raw particle material can be reacted with an aluminate coupling agent or silane compound having an introduced functional group (surface treatment step).

[0030] Examples of the aluminate coupling agent include acetoalkoxyaluminum diisopropylate, acetoacetate alkylaluminum diisopropylate, acetoacetate ethylaluminum diisopropylate, tris(ethylacetoacetoxy)aluminum, aluminum isopropoxide, diisopropyl sec-butoxyaluminum, sec-butoxyaluminum, aluminum ethoxide, bis(ethyl acetoacetate)mono(acetylacetonate)aluminum, tris(acetylacetonate)aluminum, and monoisopropoxymonooleate ethylacetoacetate aluminum.

[0031] The surface treatment is preferably carried out to a degree where the FF value is 2.0 or more. For example, based on the mass of the raw material particle material, it is preferably made to be a treatment amount of about 0.5 μmol to 10 μmol, and as a lower limit, it can be exemplified as about 0.6 μmol and 0.7 μmol, and as an upper limit, it can be exemplified as about 6.0 μmol and 7.0 μmol. These lower limits and upper limits can be arbitrarily combined.

[0032] As for the particle size distribution, the smaller the dispersion of the particle size distribution, the higher the FF value becomes. For example, preferably D90 / D10 is 1.5 or less, and more preferably 1.2 or less. As a method for reducing dispersion, it is preferred to make the particle size of the raw material particle material uniform or remove particles with a particle size of less than 1 μm. As a method for removing the small particles, a general method can be used, for example, a method using a cyclone separator, a method using a sieve, and a method using the sedimentation velocity difference in the fluid can be cited.

[0033] As the raw material particle material, a particle material having a volume average particle diameter larger than the desired volume average particle diameter is adopted as the coarse raw material particle material, and a raw material particle material having a desired volume average particle diameter can be made by performing a crushing operation. For example, after crushing the coarse raw material particle material, the particle size distribution can be adjusted. In addition, the particle size distribution can also be adjusted before crushing to replace or add the adjustment of the particle size distribution after crushing. As the adjustment of the particle size distribution, it is particularly preferred to remove particles with small particle sizes as described above.

[0034] The coarse raw material particle material is preferably manufactured by the VMC method (deflagration process). The particle material manufactured by the VMC method can also be directly used as the raw material particle material. The deflagration process is a process for preparing the raw material particle material or the coarse raw material particle material by deflagration of the metal particle material formed by the metal (metal aluminum, etc.) constituting the metal oxide in a high temperature oxidizing atmosphere.

[0035] For example, when alumina is produced by the VMC method, a mixture of a particle material having a large particle size and a particle material having a small particle size is obtained. Therefore, the part having a large particle size can be classified and used as a coarse raw particle material.

[0036] The pulverization method is not particularly limited, and general pulverization methods such as jet mill, ball mill, and vibration ball mill can be used. In particular, the jet mill is preferred because there is less mixing of impurities caused by the medium used for pulverization, and the micron-level pulverization efficiency is also high. The granular material produced by the VMC method has a high circularity, and sometimes in the particle size distribution, the particles with a particle size of less than 1 μm only contain a certain amount. Therefore, by reducing the circularity through pulverization, the FF value tends to become larger.

[0037] It is preferred to use the metal oxide particle material produced by the VMC method directly as a crude raw material particle material or to use it as a crude raw material particle material after classification. The metal constituting the metal particle material that becomes the raw material of the VMC method is easier to purify than its metal oxide, so it is easy to improve the purity of the raw material particle material obtained by the VMC method.

[0038] The amount of impurities (alkali metal, alkaline earth metal, Na, U, Th, etc.) in the metal particle material is preferably equal to or less than the impurity content of the inorganic material constituting the spherical particle material of the present embodiment.

[0039] Spheroidization process

[0040] The spheroidization step is a method similar to the method for producing a spherical particle material, which is called a melting step. The spherical particle material is produced by introducing a raw particle material into a high-temperature atmosphere, melting it, and then rapidly cooling it.

[0041] The temperature of the high temperature atmosphere is a temperature not less than the melting point of the inorganic material constituting the raw particle material. When the inorganic material constituting the raw particle material is alumina, the temperature of the high temperature atmosphere is preferably 2000°C or more, more preferably 3000°C or more.

[0042] As a method of forming a high temperature atmosphere, it is preferable to use a flame formed by burning a combustible gas and an oxidizing gas together. Examples of the combustible gas include hydrocarbon gases such as propane and natural gas, and hydrogen gas and ammonia gas. Examples of the oxidizing gas include oxygen and air.

[0043] A flame is formed inside the furnace body, and the raw material particles are dispersed in a suitable medium (gas, liquid) and then put into the furnace body. By reducing the concentration of the particles dispersed in the medium, the raw material particles are not melted and bonded, so that a spherical particle material having a particle size distribution equal to that of the raw material particles put in can be obtained, or by increasing the concentration of the particles dispersed in the carrier to the extent that the raw material particles are melted and bonded, a spherical particle material can be obtained that moves to a particle size side larger than the particle size distribution of the raw material particles put in.

[0044] The molten raw material particle material moves to the outside of the high temperature atmosphere, where it is rapidly cooled and solidified to become a spherical particle material. The produced spherical particle material is recovered by a cyclone separator, a bag filter, or the like.

[0045] The produced spherical particle material may be surface treated, for example, by using the aforementioned silane compound.

[0046] Example

[0047] The method for producing the spherical particle material of the present invention will be described in detail based on examples.

[0048] (Test 1)

[0049] After removing fine powder from alumina (made by Admatechs, AO-909, volume average particle size 10 μm: made in the deflagration process) produced by the VMC method, the material after the fine powder removal is used as a coarse raw material particle material. The coarse raw material particle material is crushed by a jet mill to adjust the particle size distribution (crushing process), and three types of raw material particle materials with volume average particle sizes of 2.1 μm (Test Example 1-1), 3.0 μm (Test Example 1-2), and 4.1 μm (Test Example 1-3) are obtained (the above is summarized as the raw material particle material preparation process). The obtained raw material particle material is put into a high temperature atmosphere (about 2000°C) and quenched to produce a spherical particle material (spheroidization process).

[0050] For the raw material particle material of each test example, the specific surface area measured by the BET method using nitrogen, the moisture content measured by the Karl Fischer method (KF moisture content), the uranium content (U) and the thorium content (Th) measured by the inductively coupled plasma emission spectrometer, and the FF value (maximum principal stress (MPS) and uniaxial yield stress (UYS) are also recorded) are measured and shown in Table 1. The results of the particle size distribution measured for the raw material particle material of each test example are shown in Table 1. Figure 1 , SEM photos are shown in Figure 2 .

[0051] The raw material particles of each test example were supplied to a spheroidizing step. In the spheroidizing step, the raw material particles were dispersed into a 7.5 Nm 3 / h of oxygen and supplied to the flame. The flame is composed of 7.5Nm 3 / h LPG and 9.0Nm as combustion-supporting gas 3 / h oxygen. 21.0Nm 3 / h oxygen is flowed in as sheath gas and combustion-supporting gas. The raw particle material is put into the flame, melted and then quenched to obtain a spherical particle material. The obtained spherical particle material is recovered by a bag filter. For the spherical particle material of each test sample, the particle size (D50), mode diameter, specific surface area, KF moisture content, and the amount of U and Th are measured using the aforementioned method, as shown in Table 1. The results of the particle size distribution of the spherical particle material of each test example are shown in Table 1. Figure 3 As shown in the SEM photos Figure 4 shown.

[0052] The melting spheroidization rate was also measured and is shown in Table 1. The melting spheroidization rate is a value calculated by the following formula, assuming that a completely melted sample (melting spheroidization rate of 100%) is a perfect sphere and that the closer to a perfect sphere, the more advanced the melting.

[0053] Formula (1): (melting spheroidization rate) = [1-{(specific surface area of ​​spherical particle material)-(specific surface area when the melting spheroidization rate of spherical particle material is assumed to be 100%)} / {(specific surface area of ​​raw material particle material)-(specific surface area when the melting spheroidization rate of raw material particle material is assumed to be 100%)}]×100(%)

[0054] (Specific surface area when the melting spheroidization rate of the spherical particle material is assumed to be 100%) = 6 / {(True specific gravity of the inorganic material constituting the spherical particle material)×(D50 of the spherical particle material)}

[0055] (Specific surface area when the melting spheroidization rate of the raw material particle material is assumed to be 100%) = 6 / {(True specific gravity of the inorganic material constituting the spherical particle material)×(D50 of the raw material particle material)}

[0056] Here, the unit of specific surface area in formula (1) is (m 2 / g), the unit of D50 is (μm), the unit of true specific gravity is (g / cm 3 ).

[0057] Table 1

[0058]

[0059] It is clear from the table that the melting spheroidization rate of the spherical particle material made from the raw particle material of Test Example 1-3 with an FF value of more than 3.0 is close to 100%, and the specific surface area is also small. In addition, the melting spheroidization rate of the spherical particle material made from the raw particle material of Test Example 1-2 with an FF value of more than 2.0 is slightly smaller than the spherical particle material made from the raw particle material of Test Example 1-1 with an FF value of less than 2.0, but the specific surface area is greatly reduced. Basically, each spherical particle material of each test example is a material with high roundness, so a large specific surface area means that the content ratio of particles with a smaller particle size than D50 is high, which means that the dispersion is large.

[0060] according to Figure 1 It is clear that the raw material particle material of Test Example 1-1 has a large peak of about 1 μm and a shoulder peak of about 4 μm, and the content of particles with relatively small particle size is high and the particle size distribution is wide. Therefore, the particle size of the spherical particle material of Test Example 1-1 is also relatively small. The content of particles with relatively small particle size distribution is wide. This situation can also be based on Figure 4 This is clearly shown in the SEM photograph. Figure 1 and2 It is found that the particle size distribution of the raw material particle materials of Test Examples 1-2 and 1-3 is narrower than that of the raw material particle material of Test Example 1-1.

[0061] according to Figure 3 It is clear that the spherical particle material of Test Example 1-1 has a wider particle size distribution than the spherical particle materials of Test Examples 1-2 and 1-3, and also has a larger specific surface area than the spherical particle materials of Test Examples 1-2 and 1-3.

[0062] (Test 2)

[0063] After removing fine powder from alumina manufactured by the VMC method (manufactured by Admatechs, AO-909, volume average particle size 10 μm: manufactured by a deflagration process), the material after the fine powder removal is used as a coarse raw material particle material. The coarse raw material particle material is crushed by a jet mill to adjust the particle size distribution, so that two types of raw material particle materials with a volume average particle size of 2.0 μm (Test Example 2-1) and 4.1 μm (Test Example 2-2) can be obtained. The obtained raw material particle material is reacted with an aluminum coupling agent (Ajinomoto Fine-Techno Co., Inc.: PLENACTAL-M, 2-propanol aluminum complex) or hexamethyldisilazane (HMDS) as a surface treatment agent for surface treatment. The amount of the surface treatment agent is shown in Table 2.

[0064] For the raw material particle material of each test example, Cohesion, UYS, and MPS were measured using a powder rheometer, as shown in Table 2. FF value was calculated based on UYS and MPS, as shown in Table 2.

[0065] Table 2

[0066]

[0067] As is clear from the table, for the sample with a particle size of 1.5 μm, the FF values ​​of the surface-treated test examples 2-2 to 2-5 were improved compared to the test example 2-1 which was not surface-treated. The FF value of the test example 2-5 treated with HMDS was improved compared to the treatment with the aluminum-based coupling agent. Regarding the aluminum-based coupling agent, even if the treatment amount was changed, almost no change in the FF value was observed.

[0068] Regarding the sample with a particle size of 3.0 μm, no improvement in FF value was observed even in Test Example 2-7 which was surface treated with HMDS, a highly effective surface treatment agent, compared with Test Example 2-6 which was not surface treated. In other words, it was found that the effect of surface treatment becomes smaller as the particle size increases.

Claims

1. A method for producing a spherical particle material, comprising: a raw material particle material preparation step, preparing a raw material particle material formed of an inorganic material, and A spheroidizing step of putting the raw particle material into a high temperature atmosphere to melt it and then rapidly cooling it to prepare a spherical particle material having a volume average particle size of 1 μm or more and less than 10 μm; Furthermore, the raw material particle material has a powder compressibility evaluation FF value of 2.0 or more using a powder rheometer.

2. The method for producing a spherical particle material according to claim 1, wherein: The raw material particle material preparation step includes a pulverizing step of pulverizing a spherical coarse raw material particle material to prepare the raw material particle material, wherein the spherical coarse raw material particle material is composed of the inorganic material and has a larger volume average particle diameter than the raw material particle material.

3. The method for producing a spherical particle material according to claim 1 or 2, wherein: The inorganic material is aluminum oxide.

4. The method for producing a spherical particle material according to claim 3 as cited in claim 2, wherein: The raw material particle material preparation step includes a deflagration step of preparing the coarse raw material particle material by deflagration of a metal particle material composed of metal aluminum in a high-temperature oxidative atmosphere.

5. The method for producing a spherical particle material according to claim 4, wherein: The Na content of the metal particle material is 5 ppm or less, The Na content of the spherical particle material is 5 ppm or less.

6. The method for producing a spherical particle material according to claim 4 or 5, wherein: The total content of U and Th in the metal particle material is 5 ppb or less, The total content of U and Th in the spherical particle material is 5 ppb or less.

Citation Information

Patent Citations

  • Method for producing spherical high-temperature powder material

    CN101549268A

  • Method for producing spherical aluminum powder

    CN102249276A

  • Particle production apparatus, particle production method and method for producing semiconductor encapsulating resin composition

    CN106268501A

  • Electronic heat conduction spherical aluminum oxide and preparation method

    CN107555455A

  • Large-particle-size alumina raw material preparation method and spherical alumina product

    CN113060746A