Electrical steel
By using superheating temperature electrical steel melt in a double-roll continuous casting machine for thin-band continuous casting, combined with hot rolling, cooling and annealing steps, the problem of magnetic performance control of NGO electrical steel is solved, and efficient production and excellent magnetic performance are achieved electric steel belt.
Patent Information
- Application Number
- CN202380028439.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-18
- Filing Date
- 2023-03-17
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is difficult to effectively control the magnetic properties of NGO electrical steel, especially in the double-roll continuous casting method, and it is difficult to maintain the θ-fiber texture and control the grain size and texture, affecting the magnetic properties.
Double-roll thin-band continuous casting is carried out using electrical steel melt with a superheating temperature of at least 30℃ higher than the melt liquid phase temperature, followed by hot rolling, cooling and curling, and the outlet temperature of the hot rolling mill is controlled at 800-900℃, and the cooling station is cooled. The inlet temperature is between 550-720°C and a coil is formed at the coiler, further by cold rolling and annealing to obtain an electrical steel strip with the desired magnetic properties.
The production of NGO electrical steel strips with excellent magnetic properties is achieved, which meets specific iron loss and magnetic permeability requirements, and improves production efficiency and cost-effectiveness.
Smart Images

Figure CN118922565A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the production of thin steel strip suitable for electrical steel applications in a twin roll continuous caster and in downstream processing steps. Background Art
[0002] In a twin roll continuous caster, molten metal, usually steel, is delivered from a conveyor system to a casting pool supported on the casting surfaces of a pair of counter-rotating horizontal casting rolls, which are internally water-cooled, thereby forming a solidified metal shell on the surfaces of the moving casting rolls. The metal shell is brought together at the nip between the casting rolls to produce a solidified strip product that is conveyed downwardly from the nip between the casting rolls. The term "nip" as used herein refers to the approximate area where the casting rolls are closest together.
[0003] The molten metal may be poured from the ladle into a smaller container or a series of smaller containers from which it flows through one or more metal delivery nozzles located above the nip to form a casting pool of molten metal supported on the casting surfaces of the casting rolls above the nip and extending the length of the nip.
[0004] The casting pool is usually confined between side plates or side closure plates, which are kept in sliding engagement with the ends of the casting rolls to restrict the outflow of the casting pool. The upper surface of the casting pool (commonly called the "meniscus") is usually higher than the lower end of the delivery nozzle, so that the lower end of the delivery nozzle is immersed in the casting pool.
[0005] When steel strip is cast by a twin-roll caster, the thin strip leaves the roll gap, passes through a guide table, through a pinch roll stand, and then through a hot rolling mill, where the thin strip is thinned to the desired thickness. The hot rolled strip is then cooled to form a strip with the microstructure required for the final application. The cooled strip is then coiled, and a shearing machine upstream of the coiler periodically cuts the strip to form the desired length of strip in each coil.
[0006] The twin roll cast, hot rolled and cooled strip can be used for a variety of end applications depending on the steel composition and casting conditions.
[0007] Electrical steel is the focus of this invention.
[0008] Electrical steel is a low carbon iron silicon soft magnetic steel widely used in motors, sensors, generators and transformers. Electrical steel can be divided into non grain oriented (NGO) and grain oriented (GO) electrical steel. Cold rolled non grain oriented steel (CRNGO) is generally cheaper than cold rolled grain oriented steel (CRGO). Therefore, NGO electrical steel is used when cost is important or when the magnetic flux direction of the final application is not constant.
[0009] When used in motors, NGO electrical steel is cut into thin laminations, isolated with an insulating coating and stacked to form the motor core to reduce eddy current losses. Therefore, if thin strip NGO electrical steel can be directly and continuously cast into thin strip, it will help save energy and time. The applicant has recognized that the twin-roll thin strip casting method has good potential because it can directly and continuously cast thin, typically 1-2 mm thick steel strip.
[0010] When NGO electrical steel is cast by conventional thick slab continuous casting process, it is difficult to maintain the θ-fiber texture that is usually formed in the hot rolling step of the process. In the subsequent cold rolling and recrystallization annealing steps of the process, strong α-fiber and γ-fiber textures are usually observed. The formation of shear bands in the deformed matrix directly affects the nucleation and growth of Goss grains during the recrystallization annealing process. In addition, the Goss grains remaining after cold rolling can also promote the formation of Goss grains in the recrystallization annealing step of the process due to the low local dislocation density and sharp lattice curvature.
[0011] Controlling the magnetic properties of NGO electrical steel is important based on the final application. The magnetic properties of NGO electrical steel are greatly affected by the grain size and texture, which in turn are affected by the rolling and recrystallization annealing steps. It is reported that after final annealing, 2.0wt.% Si NGO electrical steel has a strong {110} <001> It has also been reported that for 4.5wt.% Si NGO electrical steel, two-step cold rolling helps to form coarse grains with strong Goss and near-Goss recrystallization textures during annealing.
[0012] As mentioned in the previous paragraph, the magnetic properties of electrical steel are greatly affected by the texture. <001> The axial direction is easy to magnetize, and <111> The axial direction is more difficult to magnetize. It is well known that Goss and cube orientations optimize magnetic properties. It is reported that Brass and Goss orientations are formed in BCC metals through shear deformation textures. It is reported that many Goss grains and Cube grains are formed at the shear bands in the γ fiber deformation zone. It is also reported that after the heavy cold rolling process, some Cube components are retained because the Cube deformation bands also serve as nucleation sites for new Cube grains.
[0013] For NGO electrical steels, it is difficult to control the texture during recrystallization annealing. It has been reported that in some cases, phase transformation can be used to obtain the ideal orientation for magnetic properties. During annealing, due to the anisotropic strain energy, some {100} oriented grains are formed when austenite transforms to ferrite. However, this transformation is not applicable to fully ferritic steel compositions. Methods for obtaining the ideal crystal orientation without phase transformation using chemical composition have also been studied in the literature. The effect of initial annealing on the texture evolution and magnetic properties of 3.4wt.%Si electrical steel with 0.003wt.%C was studied. The recrystallization kinetics of 3wt.%Si electrical steel were also studied.
[0014] It is reported that the rolling process has a significant effect on texture evolution, grain growth and magnetic properties. During the recrystallization annealing process, some ideal textures evolve from the deformation shear bands formed during the rolling process. In addition, the phase transformation during hot deformation will also affect the recrystallization rate and grain size during the subsequent annealing process. It has also been reported that for 6.2wt.%Si electrical steel with C less than 0.01, hot rolling is beneficial to the final magnetic properties. The beneficial effects of annealing before cold rolling on the microstructure and magnetic properties of electrical steel have also been reported.
[0015] While some studies have been conducted to examine the effects of rolling and recrystallization annealing in the manufacture of NGO electrical steel, there are few studies on the effects of rolling and annealing on thin electrical steel strip produced by the twin-roll casting process.
[0016] The above comments are not an admission of common knowledge in China or elsewhere. Summary of the invention
[0017] In a broad sense, the present invention comprises a method and apparatus for producing electrical steel strip and electrical steel strip. The method comprises: liq A strip having a thickness of less than 3 mm is cast from a twin-roll thin strip of electrical steel melt having a temperature of at least 30°C, and the strip is hot rolled, cooled and coiled. The melt comprises, by weight, up to 0.015% carbon, 1.0% to 2.0% manganese, 2.70% to 3.80% silicon, silicon-killed containing less than 0.01% aluminum, and optionally any one or more of Cu, Cr, Ni, Mo, Ti, Nb, V, Sb, Sn, and the remainder being iron, impurities and inclusions.
[0018] The present invention comprises a twin-roll continuous casting method for producing electrical steel strip, comprising:
[0019] - In a twin-roll continuous casting machine, the superheat temperature is higher than the liquidus temperature T of the melt. liqA continuous thin electrical steel strip having a thickness of less than 3 mm cast from an electrical steel melt having a temperature of at least 30°C, the melt comprising, by weight, up to 0.015% carbon, 1.0% to 2.0% manganese, 2.70% to 3.80% silicon, silicon killed with less than 0.01% aluminium, up to 0.4% Cu; up to 0.3% Cr; up to 0.3% Ni; up to 0.2% Mo; up to 0.01% Ti; up to 0.005% Nb; up to 0.005% V, up to 0.3% Sb; up to 0.3% Sn; the remainder being iron, impurities and inclusions,
[0020] - hot rolling of electrical steel strip and reduction of strip thickness in a hot rolling mill;
[0021] - cooling of the electrical steel strip and cooling of the strip in a cooling station; and
[0022] -Electrical steel strip is wound in the coiler and formed into coils of a certain length at the coiler.
[0023] The Mn concentration range of between 1.0% and 2.0% allows the melt to have a low Al concentration (ie less than 0.01% aluminium) without affecting the resistivity of the resulting electrical steel strip. The melt is a silicon killed steel, not an aluminium killed steel.
[0024] The term "impurities" refers to elements that are present in the melt as an unavoidable result of steelmaking practices or as a result of the raw materials used to make the steel. These are often non-metallic elements. Examples of impurities are N, P, S and H.
[0025] The term "inclusion" refers to compounds formed during the steelmaking process. Examples of "inclusions" include AlN and MnS.
[0026] The Cu concentration may be less than 0.3%.
[0027] The Cr concentration may be less than 0.2%.
[0028] The Cr concentration may be greater than 0.01%.
[0029] The Ni concentration may be less than 0.2%.
[0030] The Mo concentration may be less than 0.1%.
[0031] The Mo concentration may be less than 0.06%.
[0032] The Mo concentration may be greater than 0.001%.
[0033] The concentration of Sb may satisfy the formula Sn+2*Sb<0.4%.
[0034] The concentration of Sb may be less than 0.2%.
[0035] The concentration of Sb may be less than 0.1%.
[0036] The concentration of Sb may be greater than 0.001%.
[0037] The carbon concentration may be up to 0.0060%.
[0038] The carbon concentration may be up to 0.0080%.
[0039] The carbon concentration may be at most 0.01%.
[0040] The manganese concentration may be at least 1.10%.
[0041] The manganese concentration may be at least 1.20%.
[0042] The manganese concentration may be less than 1.70%.
[0043] The manganese concentration may be less than 1.80%.
[0044] Manganese concentrations may range from 1.10% to 1.55%.
[0045] The silicon concentration may be at least 2.80%.
[0046] The silicon concentration may be at least 3.00%.
[0047] The silicon concentration may not exceed 3.70%.
[0048] The silicon concentration may not exceed 3.60%.
[0049] The silicon concentration may not exceed 3.50%.
[0050] The silicon concentration may be 2.70% to 3.50%.
[0051] The concentrations of C, Mn and Si in the electrical steel melt can be as follows:
[0052] Table 1 - Target chemical composition of C, Mn and Si - wt %
[0053]
[0054]
[0055] In one embodiment, the concentration of residues in the electrical steel melt may be as follows:
[0056] Table 2 - Main impurities and non-metallic elements - weight %
[0057] S P Cr Mo Al Cu Ni Nb Ti V Max 0.002 0.018 0.03 0.0020 0.002 0.03 0.03 0.0020 0.0020 0.0020 typical 0.0020 0.009
[0058] The concentration of residual gas in electrical steel melt can be as follows:
[0059] Table 3 - Gases and Intermetallic Compounds - Weight %
[0060] N O H Max 0.0090 0.0020 typical 0.0050
[0061] * Calculated.
[0062] The electrical steel in the coiled strip may have an at least substantially ferritic microstructure.
[0063] The microstructure of the electrical steel in the coiled strip may be at least substantially equiaxed grains.
[0064] The method may include cold rolling the electrical steel strip to further reduce the thickness of the strip.
[0065] The method may include cold rolling the electrical steel strip to further reduce the strip thickness to no more than 0.50 mm, typically no more than 0.35 mm.
[0066] The method may include pickling the electrical steel strip prior to the cold rolling step.
[0067] The method may include annealing the electrical steel strip to obtain a non-grain oriented electrical steel strip having desired magnetic properties.
[0068] The desired magnetic property may be iron loss or magnetic permeability. These terms are well understood by those skilled in the electrical steel field and are covered by industry standards. Typically, a customer orders electrical steel from a steel mill with a specific thickness and iron loss and / or magnetic permeability.
[0069] The desired magnetic properties may be as described in the Chinese standard GB / T 2521.1-2016, entitled "Cold rolled electrical steel delivered in fully processed state - Part 1: Grain non-oriented steel strip (sheet)".
[0070] For example, the desired magnetic properties may be electrical steel 35W250, 0.35 mm, 2.50 Watts / kg iron loss P1.5 / 50 as described in the standard.
[0071] As a further example, the desired magnetic properties may be described in the standard for electrical steel of 35W300, 0.35 mm, 3.00 W / kg, iron loss P1.5 / 50.
[0072] The annealing step may be performed in a controlled atmosphere, such as a mixture of hydrogen and nitrogen.
[0073] The annealing step may be performed in a controlled atmosphere that reduces the carbon concentration to no more than 0.0030%.
[0074] The electric furnace steel melt may be produced by any suitable steelmaking process.
[0075] For example, electrical steel melt can be manufactured by the following steps and then transferred to a twin-roll strip caster: electric arc furnace (EAF) → ladle furnace → pot or RH degasser → tundish → twin-roll strip caster.
[0076] Alternatively, the electrical steel melt can be manufactured by the following steps and then transferred to the twin-roll strip caster: basic oxygen furnace (BOF) → ladle furnace → RH degasser → tundish → twin-roll strip caster.
[0077] The method may include superheating the electrical steel melt to a superheat temperature prior to transferring the melt to the twin roll caster.
[0078] The method may include preparing a molten electrical steel melt having a superheat temperature.
[0079] The method may include delivering a molten electrical steel melt having a superheated temperature to a twin roll continuous caster.
[0080] The superheat temperature can be T liq + Up to 120°C, i.e. up to 120°C higher than the liquidus temperature.
[0081] The superheat temperature can be T liq + Up to 90°C, i.e. up to 90°C higher than the liquidus temperature.
[0082] The superheat temperature can be T liq + at least 35°C, i.e. at least 35°C higher than the liquidus temperature.
[0083] The superheat temperature can be T liq + at least 40°C, i.e. at least 40°C higher than the liquidus temperature.
[0084] The method may include controlling the hot rolling step so that the hot rolling mill outlet temperature is 800-900°C.
[0085] The method may include taking a 3 Nitrogen is supplied to the hot box surrounding the electrical steel strip between the twin roll continuous caster and the hot rolling mill at a rate of / hr, resulting in a high N concentration in the hot box. Note that 2500m 3 The value of / hr may vary depending on the air leaking into the hot box.
[0086] The method may include controlling the hot rolling step so that the hot rolling mill outlet temperature is 720-820°C.
[0087] The method may include: 3 Nitrogen is supplied to the hot box surrounding the electrical steel strip between the twin roll continuous caster and the hot rolling mill at a rate of 2500 m / hr, so that there is a low nitrogen concentration in the hot box. 3The value of / hr may vary depending on the air leaking into the hot box.
[0088] The method may include varying the nitrogen flow rate to a hot box surrounding the electrical steel strip between a twin roll continuous caster and a hot rolling mill to control the strip temperature, noting that lower nitrogen flow rates may result in more air leaking into the hot box, which air may oxidize the strip and increase its emissivity and thereby increase heat losses and reduce the strip temperature at the hot rolling mill entrance.
[0089] The method may comprise hot rolling the cast strip, the cast strip entering a hot rolling mill at a mill inlet temperature of 140-160°C, typically 150°C higher than the mill outlet temperature.
[0090] The method may comprise coiling the hot rolled and cooled electrical steel strip at a coiler inlet temperature in the range of 550-720°C.
[0091] The present invention also provides an apparatus for producing an electrical steel strip, comprising:
[0092] - for the liquidus temperature T of the melt to be determined by the ratio of the superheat temperature to the liquidus temperature T liq A twin roll thin strip caster for forming a continuous thin metal strip having a thickness of less than 3 mm from a molten electrical steel melt having a temperature of at least 30°C, the melt comprising, by weight, up to 0.015% carbon, 1.0% to 2.0% manganese, 2.70% to 3.80% silicon, silicon killed with less than 0.01% aluminum, up to 0.4% Cu; up to 0.3% Cr; up to 0.3% Ni; up to 0.2% Mo; up to 0.01% Ti; up to 0.005% Nb; up to 0.005% V, up to 0.3% Sb; up to 0.3% Sn; the remainder being iron, impurities and inclusions;
[0093] - Hot rolling mills for reducing the thickness of electrical steel strip;
[0094] - cooling stations for cooling electrical steel strips; and
[0095] - Coilers for forming coils of electrical steel strip of selected length.
[0096] The apparatus may include a cold rolling mill to reduce the thickness of the electrical steel strip.
[0097] The apparatus may comprise an annealing unit for annealing the electrical steel strip to obtain a non-grain oriented electrical steel strip having desired magnetic properties.
[0098] As mentioned above, electrical steel strip may be produced from a molten electrical steel melt.
[0099] The twin-roll thin strip caster can be configured to cast a molten electrical steel melt having an overheat temperature T liq Maximum 120°C higher than liquidus temperature.
[0100] The twin-roll thin strip caster can be configured to cast a molten electrical steel melt having an overheat temperature T liq Up to 90°C higher than the liquidus temperature.
[0101] The twin-roll thin strip caster can be configured to cast a molten electrical steel melt having an overheat temperature T liq At least 35°C above the liquidus temperature.
[0102] The twin-roll thin strip caster can be configured to cast a molten electrical steel melt having an overheat temperature T liq At least 40°C above the liquidus temperature.
[0103] The present invention also provides a twin-roll thin strip cast and hot rolled electrical steel strip having a thickness of less than 3 mm, having the following composition by weight: maximum 0.015% carbon, 1.0% to 2.0% manganese, 2.70% to 3.80% silicon, silicon killed containing less than 0.01% aluminum, maximum 0.4% Cu; maximum 0.3% Cr; maximum 0.3% Ni; maximum 0.2% Mo; maximum 0.01% Ti; maximum 0.005% Nb; maximum 0.005% V, maximum 0.3% Sb; maximum 0.3% Sn; the remainder being iron, impurities and inclusions.
[0104] The concentrations of the residues are shown in Table 2.
[0105] The electrical steel strip may have a microstructure which is at least substantially a ferritic microstructure.
[0106] The microstructure of the electrical steel strip may be at least substantially equiaxed grains.
[0107] The Cu concentration may be less than 0.3%.
[0108] The Cr concentration may be less than 0.2%.
[0109] The Cr concentration may be greater than 0.01%.
[0110] The Ni concentration may be less than 0.2%.
[0111] The Mo concentration may be less than 0.1%.
[0112] The Mo concentration may be less than 0.06%.
[0113] The Mo concentration may be greater than 0.001%.
[0114] The concentration of Sb may satisfy the formula Sn+2*Sb<0.4%.
[0115] The concentration of Sb may be less than 0.2%.
[0116] The concentration of Sb may be less than 0.1%.
[0117] The concentration of Sb may be greater than 0.001%.
[0118] The carbon concentration may be up to 0.0060%.
[0119] The carbon concentration may be up to 0.0080%.
[0120] The carbon concentration may be at most 0.01%.
[0121] The manganese concentration may be at least 1.10%.
[0122] The manganese concentration may be at least 1.20%.
[0123] The manganese concentration may be less than 1.70%.
[0124] The manganese concentration may be less than 1.80%.
[0125] Manganese concentrations may range from 1.10% to 1.55%.
[0126] The silicon concentration may be at least 2.80%.
[0127] The silicon concentration may be at least 3.00%.
[0128] The silicon concentration may not exceed 3.70%.
[0129] The silicon concentration may not exceed 3.60%.
[0130] The silicon concentration may not exceed 3.50%.
[0131] The silicon concentration may be 2.70% to 3.50%.
[0132] The present invention also provides a twin-roll thin strip cast, hot rolled, cold rolled and annealed electrical steel strip with a thickness of less than 3 mm, having the following composition by weight: maximum 0.015% carbon, 1.0% to 2.0% manganese, 2.70% to 3.80% silicon, maximum 0.4% Cu; maximum 0.3% Cr; maximum 0.3% Ni; maximum 0.2% Mo; maximum 0.01% Ti; maximum 0.005% Nb; maximum 0.005% V, maximum 0.3% Sb; maximum 0.3% Sn; the rest is iron, impurities and inclusions.
[0133] The electrical steel strip may have a microstructure which is at least substantially a ferritic microstructure.
[0134] The microstructure of the electrical steel strip may be at least substantially equiaxed grains.
[0135] The concentrations of carbon, manganese, silicon and residues may be as described above, noting that when the electrical steel strip is annealed, the carbon concentration may be lower than the melt concentration due to decarburization.
[0136] The electrical steel strip may have desirable magnetic properties.
[0137] The desired magnetic properties may be as described in the Chinese standard GB / T 2521.1-2016, entitled "Cold rolled electrical steel delivered in fully processed state - Part 1: Grain non-oriented steel strip (sheet)".
[0138] For example, the desired magnetic performance may be 35W250 0.35mm iron loss P1.5 / 50-2.50Wkg -1 or 35W3000.35mm iron loss P1.5 / 50–3.00Wkg -1 .
[0139] Note that while 100% ferrite may be present in the microstructure of (a) twin roll strip cast and hot rolled electrical steel strip and (b) twin roll strip cast and hot / cold rolled and annealed electrical steel strip, the present invention may be extended to situations where this is not the case, e.g. where some austenite is present in the microstructure.
[0140] It should also be noted that the microstructure will be a function of a number of factors including composition, superheat and the choice of casting, hot rolling, cold rolling and annealing conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0141] In order to describe the present invention in more detail, some illustrative examples will be given with reference to the accompanying drawings, in which:
[0142] Figure 1 is a schematic side view of an embodiment of a twin-roll continuous casting machine of the present invention;
[0143] Figure 2 yes Figure 1 An enlarged partial cross-sectional view of a portion of a twin-roll continuous casting machine;
[0144] Figure 3 yes Figure 1 A partial schematic side view of an outlet end of a twin-roll continuous casting machine;
[0145] Figure 4 (a) shows a schematic diagram of a sampler used in the experimental work for the vacuum assisted (VA) rapid cooling method to produce samples;
[0146] Figure 4 (b) shows the as-cast sample after solidification in a VA sampler;
[0147] Figure 5 is a schematic diagram of the thermomechanical processing route used in the experimental work;
[0148] Figure 6 It is the dendrite structure of VA cast sample;
[0149] Figure 7 (a) is an image showing the structure of a processed sample without hot rolling (HR);
[0150] Figure 7 (b) is an image showing the structure of 25% HR and 47% HR samples;
[0151] Figure 8 (a) is a graph of average grain size versus annealing time for high C and S samples with 0%, 25% and 47% HR after batch annealing at 1050°C for 1, 6, 18 and 24 hours;
[0152] Figure 8 (b) is a graph of average grain size versus annealing time for low C and S samples with 0%, 25% and 47% HR after batch annealing at 1050°C for 1, 6, 18 and 24 hours;
[0153] Fig. 9 is a graph showing the precipitate size distribution of VA samples before and after final annealing;
[0154] Fig.10 shows the typical texture of the orientation distribution function ("ODF") section of a fully processed electrical steel sample reported in the literature;
[0155] Fig.11 The final annealing of high C and S strip samples is shown in ODF diagram of the cross section, where (a) 0% HR, (b) 25% HR, (c) 47% HR, and ODF diagram of the cross section, where (d) 0% HR, (e) 25% HR, (f) 47% HR;
[0156] Fig.12 The final annealed low C and S strip samples are shown in ODF diagram of the cross section, where (a) 0% HR, (b) 25% HR, (c) 47% HR, and ODF diagram of the cross section, where (d) 0% HR, (e) 25% HR, (f) 47% HR;
[0157] Figures 13 to 18 Is the VA sample in and a series of further ODF plots showing 45° cross sections for samples batch annealed at 1050 °C for 1, 6, and 24 h;
[0158] Fig.19is a series of graphs of volume fraction of the major textures versus annealing time for high C and S VA samples having (a) 0% HR, (b) 25% HR, (c) 47% HR, and low C and S VA samples having (d) 0% HR, (e) 25% HR, (f) 47% HR; and
[0159] Fig. 20 is the iron loss P 1.5 / 50 Comparison chart between predicted values and measured results. DETAILED DESCRIPTION
[0160] The following description of an embodiment of electrical steel strip produced by a twin roll thin strip casting process is not the only embodiment of the present invention.
[0161] Furthermore, the following description of an embodiment of a twin roll continuous caster is not the only embodiment of a twin roll continuous caster suitable for producing electrical steel strip according to the present invention.
[0162] All other embodiments obtained by ordinary technicians in this field based on the embodiments described in the present invention, without any creative effort, belong to the protection scope of the present invention.
[0163] Unless otherwise defined, technical or scientific terms used in the present disclosure should have the meanings that are commonly understood by one of ordinary skill in the art in the field of the present invention.
[0164] Reference now Figure 1 and Figure 2 , a twin roll continuous casting machine is shown, which includes a main frame 10 erected from the factory floor and supporting a pair of counter-rotatable casting rolls 12 mounted in modules of a roll box 11. The casting rolls 12 are mounted in the roll box 11 for easy operation and movement as described below. The roll box 11 facilitates the rapid movement of the casting rolls 12 ready for casting from a setup position to an operational casting position as a unit in the continuous casting machine, and the easy removal of the casting rolls 12 from the casting position when the casting rolls 12 are to be replaced. No particular configuration of the roll box 11 is desired, as long as it performs the function of facilitating the movement and positioning of the casting rolls 12 as described herein.
[0165] The twin roll continuous caster includes a pair of counter-rotatable casting rolls 12 having casting surfaces 12A positioned laterally to form a nip 18 therebetween. Molten metal, more specifically molten electrical steel as further described below, is supplied from a ladle 13 by a metal delivery system to a metal delivery nozzle 17 (core nozzle) located between the casting rolls 12 above the nip 18. The molten metal so delivered forms a casting pool 19 of molten metal above the nip 18, which is supported on the casting surfaces 12A of the casting rolls 12. The casting pool 19 is confined within a casting region at the ends of the casting rolls 12 by a pair of side closure plates or side closure plates 20. The upper surface of the casting pool 19 (commonly referred to as a "meniscus") can rise above the lower end of the delivery nozzle 17 so that the lower end of the delivery nozzle 17 is submerged within the casting pool 19. The casting region includes the addition of a protective atmosphere above the casting pool 19 to inhibit oxidation of the molten metal in the casting region.
[0166] The ladle 13 is generally of conventional construction supported on a rotating turret 40. For metal delivery, the ladle 13 is positioned above a movable tundish 14 at a casting location to fill the tundish 14 with molten metal. The movable tundish 14 may be positioned on a tundish car 66 that is capable of transferring the tundish 14 from a heating station (not shown) to a casting location where the tundish 14 is heated to approximately casting temperature.
[0167] The movable tundish 14 may be equipped with a slide gate 25 that may be actuated by a servo mechanism to allow molten metal to flow from the tundish 14 through the slide gate 25 and then through the refractory exit shroud 15 to a transition piece or distributor 16 in the casting position. From the distributor 16, the molten metal flows to a delivery nozzle 17 located between the casting rolls 12 above the roll gap 18.
[0168] The side closure plates 20 may be made of a refractory material, such as zirconia graphite, graphite alumina, boron nitride, boron nitride zirconia, or other suitable composite materials. The side closure plates 20 have surfaces capable of physically contacting the casting rolls 12 and the molten metal in the casting pool 19. The side closure plates 20 are mounted in side closure plate holders (not shown), which can be moved by side closure plate actuators (not shown), such as hydraulic or pneumatic cylinders, servo mechanisms, or other actuators, to engage the side closure plates 20 with the ends of the casting rolls 12. In addition, the side closure plate actuators can position the side closure plates 20 during the casting process. During the casting operation, the side closure plates 20 form end caps for the molten metal pool on the casting rolls 12.
[0169] Figure 1A twin roll continuous caster for producing a cast strip 21 is shown, wherein the cast strip initially moves downward, then bends upward through a hot box to a guide table 30, the hot box containing a controlled protective atmosphere, such as nitrogen, to minimize strip oxidation, and the strip 21 moves through the guide table 30 to a pinch roll stand 31 including pinch rolls 31A. Upon leaving the pinch roll stand 31, the cast strip 21 may pass through a hot rolling mill 32, which includes a pair of work rolls 32A and backup rolls 32B, forming a gap capable of hot rolling the cast strip 21 delivered from the casting rolls 12, where the cast strip 21 is hot rolled to reduce the strip to a desired thickness, improve the strip surface, and increase the strip flatness. The work rolls 32A have working surfaces associated with the desired strip profile on the work rolls 32A. The hot rolled cast strip 21 is then transferred to the output table 33 in the cooling station 97, where it can be cooled by contact with a coolant (e.g., water) supplied via an atomizing nozzle 90 or other suitable means, as well as by convection and radiation. In any case, the cooled hot rolled cast strip 21 passes through a second pinch roll stand 91 having a pair of rollers 91A that provide tension to the cast strip 21. Finally, the cooled hot rolled cast strip 21 is then coiled, and a shear at a shearing station 98 upstream of the coiler periodically cuts the strip to form a strip of the desired length per coil.
[0170] As described below, the casting rolls 12 are internally water cooled so that as the casting rolls 12 rotate in opposite directions, the shell solidifies on the casting surface 12A as the casting surface 12A moves into contact with and through the casting pool 19 with each rotation of the casting rolls 12. The shell is brought together at the nip 18 between the casting rolls 12 to produce a cast strip product 21 that is conveyed downwardly from the nip 18. The cast strip product 21 is formed from the shell at the nip 18 between the casting rolls 12 and is conveyed downwardly and moves downstream as described above.
[0171] In operation, the strip leaves the roll gap at a temperature of 1400°C or higher. To prevent oxidation and scaling of the strip, the metal strip is cast downwardly into a housing 27 that supports a protective atmosphere just below the casting rolls at the casting location. The housing 27 may extend along the path of the cast strip up to the first pinch roll stand 31 and may extend along the path of the cast strip up to the hot rolling mill 32 to reduce oxidation and scaling.
[0172] After the hot rolling mill 32, the rolled thin strip then enters a cooling station 97 where the strip is cooled by water delivered by atomizing nozzles 90 of a plurality of rows of water spray assemblies extending through the output table 33 as the strip moves on the output table 33 in the cooling station 97. Although the atomizing nozzles atomize the coolant to produce a spray, any other coolant discharge port may be used in place of the atomizing nozzle in any embodiment. In addition to producing a spray, other types of coolant discharge ports may discharge a non-atomized coolant stream.
[0173] exist Figure 3 In the exemplary embodiment shown, the cooling station 97 extends along the belt path 99 between the hot rolling mill 32 and the second pinch roll stand 91, and a plurality of atomizing nozzles 90 in a plurality of rows of water spray assemblies are arranged therebetween. Figure 3 It is not discernible in the view shown, but the rows of atomizing nozzles 90 extend substantially across the width of the belt or cooling station in the width direction and are spaced apart along the length of the cooling station.
[0174] Finally, the cooled hot rolled strip is coiled.
[0175] about Figure 1-3 Further details of the described twin-roll continuous casting machine can be found in the specification of Chinese patent application No. 201780029304.2 filed in the name of the present applicant, the disclosure of which is incorporated herein by cross-reference.
[0176] The above-described embodiments of the twin roll continuous casting machine and method are suitable for producing electrical steel strip having a thickness of less than 3 mm from a molten electrical steel melt having a liquidus temperature T liq The superheat temperature is at least 30℃ higher and the superheat temperature is at most T liq + 120°C at most, the melt comprising: by weight, at most 0.015% carbon, typically at most 0.0060% carbon, 1.0 to 2.0% manganese, typically 1.1 to 1.55% manganese, 2.70 to 3.80% silicon, killed silicon containing less than 0.01% aluminum, at most 0.4% Cu; at most 0.3% Cr; at most 0.3% Ni; at most 0.2% Mo; at most 0.01% Ti; at most 0.005% Nb; at most 0.005% V, at most 0.3% Sb; at most 0.3% Sn; the remainder being iron, impurities and inclusions.
[0177] In this case, although not described above, there are a range of options for preparing a molten electrical steel melt having an overheated temperature, and for conveying the molten electrical steel melt having an overheated temperature to a twin roll continuous caster, which options are known to steel manufacturers and need not be described further here.
[0178] Typically, the hot rolling conditions are selected so that with a high N concentration in the hot box, the cast strip leaves the hot rolling mill at a mill outlet temperature of 800-900° C., and with a low N concentration in the hot box, the cast strip leaves the hot rolling mill at a mill outlet temperature of 720-820° C. Usually, the mill inlet temperature is selected to be 140-160° C. higher than the mill outlet temperature.
[0179] Typically, the cooled hot cast strip is coiled at a coiler inlet temperature in the range of 550-720°C.
[0180] According to embodiments of the present invention, the electrical steel strip may optionally be cold rolled to further reduce the thickness of the steel strip.
[0181] According to embodiments of the present invention, the cold rolled electrical steel strip may be annealed to develop desired magnetic properties of the resulting non-grain oriented electrical steel strip.
[0182] Typically, the annealing step is performed in a controlled atmosphere, such as a mixture of hydrogen and nitrogen.
[0183] Typically, the desired magnetic properties are as described in the Chinese standard GB / T 2521.1-2016, entitled "Cold rolled electrical steel delivered in fully processed state - Part 1: Grain non-oriented steel strip (sheet)". For example, the desired magnetic properties may be 35W250 0.35mm iron loss P1.5 / 50-2.50Wkg -1 or 35W300 0.35mm iron loss P1.5 / 50-3.00Wkg -1 .
[0184] It should be noted that typically, the steel has a target C concentration in the end-use product. For example, for a motor, the target C concentration is 0.003%. The target concentration level in the end-use product is a result of (1) the C concentration in the steel melt and (2) the annealing step - decarburizing the steel.
[0185] The applicant conducted experimental work summarized below through external research institutions to investigate the hot rolling and annealing conditions of the present invention.
[0186] Experimental work
[0187] In the experimental work, the vacuum-assisted rapid cooling sampling method was used to simulate the solidification conditions of the thin strip twin-roll casting process to produce Fe-3.4wt.%Si non-oriented electrical steel. The effects of rolling deformation on magnetic properties, grain growth and texture were analyzed.
[0188] Materials and methods
[0189] Material
[0190] Two types of non-oriented electrical steels with different carbon and sulfur contents were melted in a coreless medium frequency induction furnace under argon protective atmosphere.
[0191] Table 4 shows the chemical compositions of these steels.
[0192] Table 4 Chemical composition of the studied 3.4wt.%Si steel (wt. %)
[0193]
[0194] Steel 1 was produced using high carbon and sulfur (C and S) compositions, while Steel 2 was produced using low C and S chemical compositions to avoid the negative effects of precipitation and phase transformation on the magnetic properties of NGO Si steel. In order to control the effects of MnS precipitation and α-γ phase transformation during annealing, low C and S chemical compositions are usually used in the industry to produce industrial-grade NGO electrical steel.
[0195] The charges of Steels 1 and 2 were melted in a 90 kg coreless medium frequency induction furnace with an argon protective atmosphere.
[0196] Samples were taken directly from the induction furnace at a superheat temperature of 100 °C using a vacuum sampler as described below.
[0197] Sampling method
[0198] The vacuum-assisted rapid cooling (VA) sampling method was used to sample, simulating the solidification conditions of the industrial twin-roll casting process. Specifically, the liquid steel was pulled into a thin inner cavity in a copper mold using a vacuum-assisted process to produce a strip sample with a high solidification cooling rate. The thickness of the cast sample was 2 mm. Figure 4 (a) shows a schematic diagram of a VA sampler, Figure 4 (b) shows the as-cast sample after solidification in the VA sampler. As reported in previous studies, this method can obtain a uniform 2 mm thick strip sample with an appropriate dendrite structure and a calculated solidification cooling rate (~1700 K / s), which appropriately simulates the solidification conditions of the twin-roll thin strip casting process.
[0199] Processing plan
[0200] Thermomechanical treatments were performed on 2 mm thick as-cast samples to simulate the implementation scheme of the industrial thin strip twin-roll casting process. Three thermomechanical processing routes were designed. One processing route included hot rolling with different hot rolling (HR) deformations (25% and 47%) at hot rolling temperatures in the range of 950-1000°C. After hot rolling to deformations of 25% and 47%, the samples were cooled to ambient temperature by an initial water spray, followed by furnace cooling and cold rolling to a final thickness of 0.35 mm. The other processing route included only cold rolling without a hot rolling step. Higher HR deformation resulted in lower CR deformation, and the total thickness of HR+CR was reduced from 2 mm to 0.35 mm. After the rolling process, the samples were batch annealed at 1050°C for different times (1, 6, 18, 24 h). Schematic diagrams of the above thermomechanical processing routes are shown in Figure 5 shown.
[0201] Experimental Procedure
[0202] The grain size, precipitate size distribution, magnetic properties and texture distribution of samples with different annealing times were analyzed. The average grain size was measured using the linear intercept method from ASTM E112-13, the magnetic properties were measured using a single-piece tester, the precipitates were analyzed using automatic feature analysis (AFA) on an ASPEX PICA1020SEM, and the texture distribution was analyzed using electron backscatter diffraction (EBSD) on a Helios SEM device. The magnetic properties test samples were cut into a size of 100×30mm along the rolling direction. EBSD analysis was scanned along the RD-ND cross section (rolling direction-normal plane). The harmonic series expansion method was used in the orientation distribution function (ODF) calculation.
[0203] Microstructure characterization and magnetic properties testing
[0204] The samples were prepared metallographically and etched with water-based picric acid to reveal the dendrite structure and with nitric acid etchant to reveal the grain structure. As described above, the linear intercept method according to ASTM E112-13 was used to make secondary dendrite arm spacing (SDAS) and grain size measurements.
[0205] The solidification cooling rates of the VA as-cast samples were calculated from the measured SDAS. Based on the expected cooling rates and chemical composition, the Suzuki equation was used for this calculation in each case.
[0206] S2 = 688 (60×r) -0 .36 (1),
[0207] where S2 is the SDAS in μm and r is the solidification cooling rate in K / s.
[0208] For different test conditions, the optimum grain size is used to minimize the core loss. This is because it is reported that a particularly coarse grain size leads to higher permeability, lower coercivity and large domain size, which in turn increases the core loss. It is reported that the optimum grain size (GsOp) can be described as follows:
[0209] G sOp = (cρ / (B 0.4 t 2 f (1 / 2) ) 2 / 3 (2)
[0210] where c is an experimentally determined constant, ρ is the resistivity, B is the magnetic induction intensity, t is the sample thickness, and f is the operating frequency.
[0211] The magnetic properties were measured using a single-piece tester based on ASTM A1036. The test samples were prepared by cutting the processed material into strips of 100 mm length and 30 mm width in the rolling direction. The iron loss (P) was measured at 50 and 60 Hz, 1.5 and 1.0 T. 1.5 / 50 ,P 1.5 / 60 ,P 1.0 / 50 ,P 1.0 / 60 ). The magnetic induction intensity (B) was measured at 2500 and 5000 A / m. 25 ,B 50 The final recrystallized crystal orientation was analyzed using electron backscatter diffraction (EBSD) in a Helios SEM (30 kV, 11 nA). Scanning was performed on the RD-ND (rolling direction-normal plane) cross section. The harmonic series expansion method was used in the calculation of the orientation distribution function (ODF).
[0212] Results and discussion
[0213] Solidification cooling rate
[0214] The dendrite structure of VA cast sample is as follows Figure 6 As shown. Using the linear intercept method, the SDAS was measured to be about 10 m. Using equation (1), the solidification cooling rate was calculated to be about 1700 K / s, which is within the range of the direct twin roll casting process for 2 mm thick strip reported in the industry.
[0215] The structure of the sample treated with 0% HR (100% CR) is as follows Figure 7 (a). As can be observed, many undesirable edge cracks propagate after the cold rolling process. This is caused by the residual stress and microstructure of the steel, which is formed on the basis of the high solidification cooling rate. On the other hand, Figure 7 As shown in (b), almost no edge cracking was observed during processing of the 25% HR and 47% HR samples.
[0216] Grain size effect
[0217] To minimize the iron loss of a 0.35 mm thick 3.4 wt.% Si NGO electrical steel sample (4.70×10-7 Ω·m) at 1.5 T and 50 Hz, equation (2) was used to calculate the optimum grain size, which was determined to be about 250 μm under experimental conditions. Therefore, a steel with a grain size close to 250 μm is expected to show reduced iron loss at 1.5 T and 50 Hz.
[0218] The average grain size after batch annealing at 1050°C for 1, 6, 18, and 24 hours is shown in Figure 8As shown. For the high C and S samples annealed for 24 hours, the average grain size increased to 89, 148 and 190 μm with increasing HR deformation. For the low C and S samples annealed for 24 hours, the average grain size increased to 136, 199, 249 μm with increasing HR deformation. The measured average grain sizes are all smaller than the calculated optimal grain size. Among samples with the same HR deformation, samples with lower C and S levels show coarser average grain sizes at each measured annealing time. Among samples with similar C and S levels, samples with higher HR deformation show coarser average grain sizes at each measured annealing time (sample 47% HR greater than sample 25% HR greater than sample 0% HR). The growth rate is higher in the first 6 hours of batch annealing and slows down in the time range of 6-24 hours. This phenomenon is observed in every sample under each condition.
[0219] For samples with high C and S concentrations, the final grain size is affected by the α-γ phase transformation during annealing, which may retard grain boundary migration.
[0220] As reported in previous studies, MnS and different types of oxides are the main precipitates found in these NGO electrical steel strip samples. Recrystallization and grain growth during annealing can be inhibited by the pinning effect of these precipitates on grain boundaries.
[0221] The pinning force for small precipitates is reported as follows:
[0222]
[0223] where γ GB is the grain boundary energy, F v is the sediment volume fraction, and r is the average radius of the sediment.
[0224] Initially, the pinning force is higher than the driving force for recrystallization and grain growth, then, as Fig. 9 As shown, the precipitates coarsen during the annealing process, which results in fewer small precipitates (less than 0.85 μm) and more large precipitates (greater than 0.85 μm) after the final annealing.
[0225] According to equation (1), larger precipitates have lower pinning force, which reduces the grain boundary pinning effect.
[0226] Magnetic properties
[0227] The magnetic properties of samples deformed with different HR and batch annealed at 1050 °C for 24 h are shown in Table 5.
[0228] Table 5 Magnetic properties after final annealing
[0229]
[0230] For all chemical compositions, the 25% HR and 47% HR samples meet the magnetic property requirements of 35W250NGO electrical steel in GB / T 2521.1. 1.5 / 50 It is 2.50W / kg.
[0231] In general, samples processed at higher HR deformation (with the same chemical composition) and samples with lower C and S levels (with the same HR deformation) show better magnetic properties. The results are directly related to the average grain size discussed previously. Comparing the magnetic property results in Table 5 and Fig. 9 As a result of the average grain size, the magnetic properties improve with the increase of the average grain size. The only exception is the sample with 25% HR. Although the samples with low C and S have a coarser average grain size than those with high C and S, they show similar iron losses under 1.5T test conditions.
[0232] According to inclusion analysis reported in previous studies, the VA samples all have similar inclusion size distributions. Therefore, in addition to the grain size differences discussed previously, the magnetic properties are also affected by texture, which will be discussed in the following subsections.
[0233] Texture Effect
[0234] Fig.10 shows the typical texture expected in the orientation distribution function ("ODF") section of fully processed electrical steel samples reported in the literature, while Fig.11 and 12 The evolving texture intensity and pattern of several samples as a function of the rolling process are shown. Cube{100} <001> , Brass{110} <112> , Goss{110} <001> are the main directions obtained in these ODF image results.
[0235] For high C and S samples, increasing HR deformation shows a decrease in the intensity of the Goss orientation. There is a high intensity of the Cube orientation on the sample with 47% HR, while there is a lower intensity of the Cube orientation on the samples with 25% HR and 0% HR. The γ fibers in each sample disappear after annealing, which is beneficial to the improvement of magnetic properties. Compared with the γ fiber texture, the magnetic properties of Cube and Goss textures are more ideal.
[0236] For the low C and S samples, a rotated Goss orientation was observed in each sample. On the sample with 0% HR, there was a low intensity of Cube orientation and some rotated Goss orientation. This 0% HR sample was greatly affected by the γ-fibers formed during the cold rolling process, while γ-fibers were absent in the samples with 25% HR and 47% HR.
[0237] The recrystallization texture after final annealing is greatly affected by the deformation structure and texture during rolling. Strain-induced grain boundary migration (SIBM) and subgrain growth at grain boundaries are considered to be the main mechanisms of grain nucleation. Subgrain growth usually occurs at <111> / / ND (γ fibers) are observed in deformed grains, while nucleation via SIBM usually occurs <100> / / ND (θ fiber) deformed grains. HR-preferred CR treatment reduces the proportion of γ fiber shear bands while improving the retention of {100} deformation microstructure. The widely distributed shear bands in the γ fiber deformation zone provide a large number of new Goss grains.
[0238] Among the samples deformed at 25% HR, the samples with high C and S show a higher intensity of Goss orientation, while the Cube texture is lower in intensity for the samples with low C and S. This seems to explain why at 25% HR, despite the coarser grain size, the low C and S samples have similar iron loss results compared to the high C and S samples at 1.5T.
[0239] Texture evolutionTexture composition
[0240] exist Figures 11 to 18 In and 45° cross sections show the ODF images of samples batch annealed at 1050 °C for 1, 6, and 24 h.
[0241] Fig.13 , 15 and 17 show the ODF images of high C and S steels, while Fig.14 , 16 and 18 show the ODF images of low C and S steel. In addition, Fig.14 and 15 The ODF image of the 0% HR sample is shown. Fig.15 and 16 The ODF image of the 25% HR sample is shown. Fig.17 and 18 The ODF image of the 47% HR sample is shown. The main texture volume fraction changes with annealing time as shown in Fig.19 shown.
[0242] For high C and S 0% HR samples ( Fig.13 ), after annealing for 1 hour, uneven α-fibers can be observed ( <110> / / rolling direction [RD]) and α*-fibers ({hhl}<h / l+1h / l+2h / l> ) texture. After 6 hours of annealing, the inhomogeneous α*-fiber texture can still be observed, while the α-fiber texture has disappeared. After 24 hours of annealing, the α*-fiber texture has also disappeared.
[0243] As a comparison, the low C and S 0% HR samples ( Fig.14 )γ fibers formed before annealing process ( <111> / / ND) texture. After 1 hour of annealing, a strong γ-fiber texture and a weak non-uniform α*-fiber texture were observed. After 6 hours of annealing, a strong γ-fiber texture was still observed, but it became non-uniform. After 24 hours, the strong γ-fiber texture became more non-uniform. Non-uniform α*-fiber textures could be observed after 6 and 24 hours.
[0244] This phenomenon can be explained by the fiber texture evolution. The 0% HR sample is greatly affected by the α*-fiber and γ-fiber textures formed before annealing. The formation of α*-fiber and γ-fiber textures is related to the high CR deformation and strain of the 0% HR sample. During the CR process, as the deformation and strain increase, the rotated Goss orientation will gradually rotate to {111} <110> Finally, with the further increase of deformation and strain, α-fiber and α*-fiber textures appear.
[0245] The main texture volume fraction of 0% HR sample ( Fig.19 (a) and 19(d)) mostly decrease between 1 and 6 hours of annealing time. Between 6 and 24 hours, the volume fraction of the Goss orientation increases significantly, while the fractions of the other major orientations remain essentially unchanged. The main difference is that the volume fraction of the Brass orientation also increases between 6 and 24 hours for the high C and S samples compared to the low C and S samples.
[0246] Theory in the literature on the thermodynamic driving force of grain growth and the critical radius helps explain the evolution of texture. The critical radius can be described as follows:
[0247]
[0248] where γ is the boundary energy, ΔG v It’s the driving force.
[0249] The velocity at the grain boundary can be described as follows:
[0250]
[0251] where γ is the boundary energy, R is the radius, and M is the grain boundary mobility (which depends on the orientation of adjacent grains).
[0252] Fig.13 and 14 The texture evolution in the lattice can be divided into two steps.
[0253] The decrease in the volume fraction of Goss grains in the first step can be explained by the boundary energy difference between grains. High-energy boundaries are more likely to appear around Goss grains. Therefore, in order to reduce the total energy of the system, it is energetically favorable to consume Goss grains in the early stage of the grain growth process. This phenomenon can also be explained by the critical radius difference. In the initial stage, a large number of grains smaller than the critical radius are consumed. According to equation (4), the higher boundary energy also gives the Goss grains a larger critical radius. According to literature reports, the critical radius of Goss grains is about 9% higher than that of grains of other textures. Therefore, more Goss grains are consumed in the initial step. In addition, this phenomenon can also be explained by considering the pinning effect of precipitates. In the first step, according to equations (3) and (5), the pinning force from the precipitates is still high, and only grains with high-energy boundaries can move.
[0254] Then, in the second step, as the precipitate coarsens at longer annealing times, the pinning force decreases according to equation (3). In this case, pinning provides a mobility advantage for the remaining Goss grains larger than the critical size. As shown in equation (5), this mobility advantage leads to faster Goss grain growth by consuming other grains smaller than the critical size.
[0255] In addition, the evolution of this main texture is also related to the evolution of α*-fiber and γ-fiber textures. With the extension of annealing time, the fiber texture nucleates and grows toward other texture orientations. It is reported that the Goss orientation on BCC metals is more likely to be formed by shear deformation orientation and deformed fiber texture.
[0256] For the 25% HR sample ( Fig.15 and 16 ), no high-intensity α*-fiber and γ-fiber textures were observed. For the main texture volume fractions in high C and S25% HR samples ( Fig.19 (b)), the fraction of Goss and Brass textured grains increases significantly, while the fraction of Cube textured grains decreases significantly between 1 and 6 hours. Then, between 6 and 24 hours, the fraction of Goss textured grains decreases gradually as the fraction of Cube textured grains increases. For the sample with low C and S25% HR ( Fig.19 (e)), the fraction of Goss textured grains gradually increases between 1 and 24 h, while the fraction of Cube textured grains gradually decreases between 6 and 24 h.
[0257] It can be considered that the volume fraction of Cube grains at 1 hour is affected by the presence of Cube grains formed before the annealing process. In some cases, the Cube texture component is retained after heavy cold rolling because the deformed Cube grains serve as nucleation sites for new Cube grains. For the high C and S samples ( Fig.11 (b)) and low C and S samples from 1 to 24 hours ( Fig.11 (e)), the increase in the Goss grain fraction can be explained by the second step, which is caused by the reduction of the pinning force giving the large Goss grains a boundary mobility advantage. Finally, with further reduction of the pinning force and increase of the Goss grains, the mobility advantages of all grains become similar. At this point, the selective growth of Goss grains stops and normal grain growth is established.
[0258] For the 47% HR sample ( Fig.17 and 18 ), and no high-strength α*-fiber and γ-fiber textures were observed. For the sample with 47% HR ( Fig. 20 (b) and (d)), between 1 and 6 hours, the fraction of Goss grains increases, while the fraction of Cube grains decreases significantly. Between 6 and 24 hours, the fraction of Goss grains decreases as the fraction of Cube grains increases sharply.
[0259] In this case, the fractional inversion of Goss and Cube grains is associated with a high volume fraction change in the final step (6 to 24 hours), which is believed to be caused by the formation of Cube grains from rotated Goss grains. It is reported that the Cube-oriented crystal volume or crystallites are formed by the shear bands of the rotated Goss orientation. It is reported that with increasing strain, the Cube orientation is the most stable orientation formed by the shear bands of the rotated Goss grains.
[0260] Iron loss model
[0261] Core loss is affected by both grain size and texture distribution. It is difficult to distinguish their respective contributions to core loss. A qualitative model and equation for predicting core loss will help to distinguish the contributions of grain size and texture distribution to core loss.
[0262] Regarding the effect of grain size on core loss, it is reported that the effect of grain size can be expressed as follows
[21] :
[0263] P G =A+Bd -1 +Cd -2 (6)
[0264] where d is the average grain size and A to C are positive constants that depend on chemical composition, precipitate size distribution and test conditions.
[0265] According to the model, A represents the energy loss in each individual grain caused by eddy currents and domain magnetic direction rotation. It is affected by the chemical composition. (-1) It is the energy loss of the domain wall when migrating inside the grain. This energy loss is affected by the grain size and the size distribution of the precipitate. (-2) Represents the energy loss when the eddy current passes through the grain boundary. In fact, this energy loss is very small because it is difficult for the domain wall to pass through the grain boundary.
[0266] Due to the influence of texture distribution, Goss and Cube textures play a major role in magnetic properties. We assume that this effect is linear. The equation for the effect of texture distribution is:
[0267] P T =DF C +EF G (7)
[0268] where D to E are positive constants, and F_C and F_G are the percentages of grains with Cube and Goss textures.
[0269] Combining equations (6) and (7) with the measured results, all constants were determined using MATLAB calculations. For Fe-3.4wt.%Si non-oriented electrical steel, at 1.5T 50HZ, the synthetic equation relating iron loss to grain size and texture distribution is as follows:
[0270] P 1.5 / 50 =P G +P T =3.011+7.604d -1 +244.255d -2 -0.016F C -0.031F G (8)
[0271] Calculated iron loss value and measured iron loss (P 1.5 / 50 ) is compared with Fig. 20 As shown, the calculated values agree well with the measured core loss values for a range of processing conditions. This equation separates the effects of grain size and texture fraction on core loss.
[0272] To test the model, two additional groups of samples with similar average grain sizes (Table 6) were selected for evaluation. In Group 1, the "Low C and 25% HR (6 hours)" samples were used, which had larger grain sizes and lower percentages of Goss and Cube grains. As calculated using equation (6), the "Low C and S25% HR (6 hours)" samples had higher iron losses, as predicted by equation (6). In Group 2, the average grain sizes of the samples were similar to each other. The "High C and 25% HR (24 hours)" samples had a higher percentage of Goss and Cube grains and, as predicted, had lower calculated iron losses. The measured results for these samples are fairly consistent with the calculated iron loss values.
[0273] Table 6 Comparison of grain size, texture grain fraction and magnetic properties
[0274]
[0275] Although equation (8) separates the effects of grain size and texture, it is a simple semi-empirical model. For example, anomalous losses are not considered in the calculation, and the effect of texture fraction is assumed to be linear, which still requires more theoretical research. Further research is needed to make this calculation more accurate and applicable to different silicon steel compositions and service conditions.
[0276] in conclusion
[0277] In the above experimental work, Fe-3.4wt.%Si non-oriented electrical steel strip samples were produced in the laboratory to simulate the solidification conditions of the thin strip twin roll casting process. Thermomechanical processing routes with 0% HR, 25% HR and 47% HR were studied for samples with high and low C and S.
[0278] The measured magnetic properties of the fully processed 25% HR and 47% HR samples all meet the requirements of GB / T 2521.1 for 35W250 NGO electrical steel. 1.5 / 50 It is 2.50W / kg.
[0279] For samples with the same HR deformation, it is observed that the low C and S samples have a coarser average grain size after final annealing. The high C and S samples may be affected by the α-γ phase transformation that occurs during the recrystallization annealing and the presence of austenite during hot deformation. With increasing HR deformation, the average grain size after final annealing also increases. This coarser grain size also leads to lower iron loss (P 1.5 / 50 ,P 1.5 / 60 ,P 1.0 / 50 ,P 1.0 / 60 ) and higher magnetic induction intensity (B 25 ,B 50 ).
[0280] In some cases, Goss orientation appears to have a more positive effect on reducing iron loss than grain size. For example, the 25% HR, low C and S and high C and S samples show similar iron loss (1.5T condition) results despite the fact that the former has a coarser grain size than the latter. For the final annealed samples with high C and S, the Goss orientation intensity decreases with increasing HR deformation. This observation is believed to be influenced by the reduction in the proportion of shear bands.
[0281] With increasing annealing time from 1 to 24 hours at 1050°C, the average grain size increases and the iron loss of the fully processed samples decreases. In addition, increasing annealing time also has a great influence on the evolution of grain texture. The texture evolution in the 0% HR sample is affected by the presence of high-strength α*-fiber and γ-fiber textures, which are formed by the high percentage of cold reduction used in this processing path before the annealing treatment.
[0282] The texture evolution can be divided into several different stages. In the early stage of annealing, the fraction of grains smaller than the critical radius decreases, but the consumption of Goss grains accelerates. Then, in the second stage of annealing, the fraction of Goss grains increases by consuming other grains.
[0283] It is believed that as the precipitate coarsens, the reduction in pinning provides a mobility advantage for the surviving Goss grains that are larger than the critical size for growth. Finally, as the pinning force is further reduced and the grain size increases, normal grain growth is established. In this step, Cube grains can be formed from rotated Goss grains.
[0284] A simple core loss model was established to explain the effects of grain size and texture distribution on core loss. By comparing the two sets of results, the equation successfully separated the effects of grain size and texture distribution on core loss.
[0285] Additional experimental work
[0286] The applicant has carried out additional experimental work on the following electrical steel melt: 0.0034% carbon, 1.23% manganese, 2.82% silicon, 0.0029% sulphur, 0.067% phosphorus and 0.03% chromium.
[0287] Samples were produced by the vacuum assisted rapid cooling method described above, hot rolled at 25% and 47% reduction, cold rolled to 0.35 mm, and annealed at 950°C, 1000°C, and 1050°C for 60 seconds.
[0288] The magnetic properties of the samples are consistent with the results reported above.
[0289] While the principles and modes of operation of this invention have been explained and illustrated with respect to particular embodiments, it must be understood that the invention may be practiced otherwise than as specifically explained and illustrated without departing from the spirit or scope of the invention.
Claims
1. A method for producing an electrical steel strip, comprising: - In a twin-roll continuous casting machine, the superheat temperature is higher than the liquidus temperature T of the melt. liq A continuous thin electrical steel strip having a thickness of less than 3 mm is cast from an electrical steel melt having a temperature of at least 30°C, the melt comprising: By weight, 0.015% maximum carbon, 1.0% to 2.0% manganese, 2.70% to 3.80% silicon, silicon killed with less than 0.01% aluminum, 0.4% maximum Cu; 0.3% maximum Cr; 0.3% maximum Ni; 0.2% maximum Mo; 0.01% maximum Ti; 0.005% maximum Nb; 0.005% maximum V; 0.3% maximum Sb; 0.3% maximum Sn; the remainder being iron, impurities and inclusions; - hot rolling of electrical steel strip in a hot rolling mill and reduction of the strip thickness; - cooling the electrical steel strip in a cooling station and cooling the strip; and - The electrical steel strip is wound in a coiler and formed into coils of a certain length at the coiler.
2. The method according to claim 1, wherein: The Cu concentration is less than 0.3%.
3. The method according to claim 1 or 2, wherein: The Cr concentration is less than 0.2%.
4. A method according to any one of the preceding claims, wherein: The Ni concentration is less than 0.2%.
5. A method according to any one of the preceding claims, wherein: The Mo concentration is less than 0.06%.
6. A method according to any one of the preceding claims, wherein: The concentration of Sb satisfies the formula Sn+2*Sb<0.4%.
7. A method according to any one of the preceding claims, wherein: The concentrations of C, Mn and Si in electrical steel melt are as follows: Table 1 - Target chemical composition of C, Mn and Si - wt % 。 8. A method according to any one of the preceding claims, wherein: The concentration of residues in electrical steel melt is as follows: Table 2 - Main impurities and non-metallic elements - weight % 。 9. A method according to any one of the preceding claims, wherein: The gas concentration in the electrical steel melt is as follows: Table 3 - Gases and Intermetallic Compounds - Weight % 。 10. A method according to any one of the preceding claims, wherein: The electrical steel strip has at least a substantially ferritic microstructure.
11. A method according to any one of the preceding claims, comprising cold rolling the electrical steel strip to further reduce the strip thickness.
12. A method according to any one of the preceding claims, comprising annealing the electrical steel strip to obtain a non-grain oriented electrical steel strip having the desired magnetic properties, such as those described in the Chinese standard GB / T 2521.1-2016 entitled "Cold rolled electrical steel delivered in fully processed condition - Part 1: Grain non-oriented steel strip (sheet)".
13. The method according to claim 11, wherein: The annealing step is performed in a controlled atmosphere, such as a mixture of hydrogen and nitrogen.
14. A method according to any one of the preceding claims, wherein: The overheat temperature is T liq + Up to 120°C, i.e. up to 120°C higher than the liquidus temperature.
15. A method according to any one of the preceding claims, comprising controlling the hot rolling step such that the hot rolling mill exit temperature is 800-900°C.
16. A method according to any one of the preceding claims, comprising: 3 Nitrogen is supplied to a hot box surrounding the electrical steel strip between the twin roll continuous caster and the hot rolling mill at a rate of / hr so that there is a high concentration of N in the hot box.
17. The method according to any one of claims 1 to 14, comprising controlling the hot rolling step so that the hot rolling mill outlet temperature is 720-820°C.
18. The method according to claim 17, comprising: 3 Nitrogen is supplied to a hot box surrounding the electrical steel strip between the twin roll continuous caster and the hot rolling mill at a rate of / hr so that there is a low concentration of N in the hot box.
19. A method according to any one of the preceding claims, comprising controlling the hot rolling step such that the hot rolling mill inlet temperature is 140-160°C higher than the hot rolling mill outlet temperature.
20. A method according to any preceding claim comprising coiling the electrical steel strip at a coiler inlet temperature in the range 550 to 720°C.
21. An apparatus for producing electrical steel strip, comprising: - for the liquidus temperature T of the melt to be determined by the ratio of the superheat temperature to the liquidus temperature T liq A twin roll thin strip caster for forming a continuous thin metal strip having a thickness of less than 3 mm from a molten electrical steel melt having a temperature of at least 30°C, the melt comprising, by weight, up to 0.015% carbon, 1.0% to 2.0% manganese, 2.70% to 3.80% silicon, silicon killed with less than 0.01% aluminum, up to 0.4% Cu; up to 0.3% Cr; up to 0.3% Ni; up to 0.2% Mo; up to 0.01% Ti; up to 0.005% Nb; up to 0.005% V, up to 0.3% Sb; up to 0.3% Sn; the remainder being iron, impurities and inclusions; - Hot rolling mills for reducing the thickness of electrical steel strip; - cooling stations for cooling electrical steel strips; and - Coilers for forming coils of electrical steel strip of selected length.
22. Apparatus according to claim 21, comprising a cold rolling mill to reduce the thickness of the strip in the coil.
23. The apparatus according to claim 22, comprising an annealing unit for annealing the electrical steel in the coil to obtain a non-grain oriented electrical steel strip having desired magnetic properties.
24. A twin-roll thin strip cast and hot rolled electrical steel strip having a thickness of less than 3 mm, having the following composition by weight: maximum 0.015% carbon, 1.0% to 2.0% manganese, 2.70% to 3.80% silicon, maximum 0.4% Cu; maximum 0.3% Cr; maximum 0.3% Ni; maximum 0.2% Mo; maximum 0.01% Ti; maximum 0.005% Nb; maximum 0.005% V, maximum 0.3% Sb; maximum 0.3% Sn; the remainder being iron, impurities and inclusions.
25. Electrical steel strip according to claim 24, the microstructure of which is at least substantially a ferritic microstructure.
26. Electrical steel strip according to claim 24 or 25, having a microstructure which is at least substantially equiaxed grains.
27. A twin-roll thin strip cast, hot rolled, cold rolled and annealed electrical steel strip having a thickness of less than 3 mm, having the following composition by weight: maximum 0.015% carbon, 1.0% to 2.0% manganese, 2.70% to 3.80% silicon, maximum 0.4% Cu; maximum 0.3% Cr; maximum 0.3% Ni; maximum 0.2% Mo; maximum 0.01% Ti; maximum 0.005% Nb; maximum 0.005% V, maximum 0.3% Sb; maximum 0.3% Sn; the remainder being iron, impurities and inclusions.
28. An electrical steel strip according to claim 27, the microstructure of which is at least substantially a ferritic microstructure.