Contact lens manufacturing method

By using a multi-stage mold forming process and a positioning support forming mold, the accuracy and stability issues of embedded components in contact lenses have been solved, enabling high-quality contact lens production.

CN118922770APending Publication Date: 2024-11-08MENICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280094019.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-03-25
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing contact lenses have difficulties in achieving high-precision assembly and stable fixation when embedding electronic components. They also suffer from problems such as adhesives affecting optical performance, unsuitability for mass production, and poor forming due to pores.

Method used

By using a positioning support forming mold and a multi-stage mold forming process, the component support mold is removed in the incompletely cured state to reduce the generation of pores. The positioning accuracy and stability of the embedded component are ensured by the flexible part and tightness control, and finally a one-piece molded product is formed.

Benefits of technology

This technology enables high-precision positioning and stable fixation of embedded components in contact lenses, reducing porosity and poor forming, and improving production efficiency and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922770A_ABST
    Figure CN118922770A_ABST
Patent Text Reader

Abstract

Provided are a novel contact lens manufacturing method and a contact lens. It is possible to solve at least one problem among the problems that other members such as electronic components are equipped on the contact lenses. A primary molded article (20) in which an embedding member (36) is embedded is obtained by clamping a member support molding die (14), which supports the embedding member (36), with a first molding die (12) and curing a first molding material (18). After the member support molding die (14) is removed in a state in which the first molding material (18) has not been cured on the side of the member support molding die (14), a second molding die (22) and the first molding die (12) in which the primary molded article (20) remains are clamped, a second molding material (26) is filled, and a curing process is performed. As a result, the contact lens (10) in which the embedding member (36) is embedded is manufactured as an integrally molded article.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a contact lens, and more particularly to a method for manufacturing a contact lens in which a member different from a lens component is embedded, and to a contact lens. Background Art

[0002] Contact lenses are worn on the eyes and are usually provided with certain optical properties for the purpose of vision correction. However, in recent years, research has not only focused on improving optical properties, but also on adding features of appearance design or adding functions different from changes in optical properties and vision correction. As a specific example, the following smart contact lenses are also being studied: contact lenses are given electrical properties or even electronic functions, thereby changing properties, or acquiring biological information, or displaying information such as text in the field of vision, or switching operations by moving the line of sight.

[0003] However, since the contact lenses with new features and functions are different from the existing contact lenses in structure, there are still some obstacles before they can be put into practical use. In particular, in order to realize the addition of new features and functions, it is necessary to equip the contact lenses with other components such as electronic components. Moreover, considering the influence on the biological tissues such as the eyeball and the eyelid, it is desirable to configure other components in the inside of the contact lenses in an embedded state, but when the other components are assembled in the inside of the contact lenses in an integrated manner and with high positional accuracy, there are some problems that must be solved.

[0004] Under such circumstances, patent documents that disclose inventions related to contact lenses equipped with other components include U.S. Patent 10028702B2 (Patent Document 1), Japanese Patent Publication No. 2019-530009 (Patent Document 2), and Japanese Patent No. 6636212 (Patent Document 3).

[0005] Patent Document 1 discloses a method for manufacturing a contact lens by overlapping and fixing a first lens layer in a lens thickness direction onto a second lens layer in which electronic components are embedded.

[0006] However, the inventors' research results show that it is difficult to maintain the first lens layer and the second lens layer in a fixed state with good precision and stability in the contact lens disclosed in Patent Document 1. In particular, when the first lens layer and the second lens layer are fixedly connected by a concave-convex fitting structure, it is not easy to form a concave-convex fitting portion with good dimensional accuracy. In addition, when the first lens layer and the second lens layer are fixedly connected by an adhesive, there is a possibility that the adhesive may have an adverse effect on the optical performance. In addition, for example, in the case where the configuration of electronic components requires precision, even if the first lens layer and the second lens layer are combined, it is not easy to maintain the configuration accuracy. In addition, since the number of precision processes increases overall, there is a problem that it is not suitable for mass production. In addition, when, for example, the first lens layer and the second lens layer are fixedly connected by an adhesive, there is also a problem that it is not easy to maintain its adhesion in the eye, which is a humid environment.

[0007] Patent document 2 discloses the following method for manufacturing contact lenses: when using a lens blank obtained by cutting a rod of lens material in the length direction, when cutting a contact lens from the lens blank, electronic components are embedded at predetermined intervals in the length direction during the manufacturing process of such a rod, thereby arranging electronic components in each lens blank.

[0008] However, the inventors have studied and found that the contact lens disclosed in Patent Document 2 has the following problems: when the electronic components are formed in a rod in an embedded state, the rod polymerization molding is adversely affected depending on the size of the electronic components, or it is difficult to ensure the positioning accuracy of the electronic components in the rod. In addition, before the lens blank is cut to a certain extent, it is difficult to accurately grasp the position and direction of the electronic components in the rod, and there is a limit to correcting the configuration of the electronic components in the lens during the cutting process. In particular, when the contact lens is cut to correspond to the user's individual eyes, the inconsistency of the position of the electronic components in the lens blank becomes a greater problem, and therefore, there is also a problem that it is not suitable for industrial production of contact lenses.

[0009] Patent document 3 discloses a method in which, as a double-layer structure in which a contact lens is stacked, another member is placed in a recess formed on a molded product of the first layer and the second layer is molded in a state in which the other member is positioned, thereby mold-molding the contact lens in which the member is embedded.

[0010] However, the inventors' research results show that in the contact lens disclosed in Patent Document 3, it is considered that voids are easily generated around the other components due to shrinkage during the molding of the second layer, and there is a problem that it is difficult to stably manufacture contact lenses of quality that are not problematic in practical use.

[0011] Patent document 1: U.S. Patent 10028702B2

[0012] Patent Document 2: Japanese Patent Application Publication No. 2019-530009

[0013] Patent Document 3: Japanese Patent No. 6636212

[0014] The problems exemplified above may be interrelated and become problems in practical application depending on the type of component to be equipped, the required characteristics, functions, performance, etc. Here, the problem of the present invention is to solve at least one of the problems that become obstacles when another component is equipped on the contact lens. Summary of the invention

[0015] In order to solve such problems, the embodiments of the present invention are described below. In addition, the components adopted in each embodiment described below can be adopted in any combination as much as possible.

[0016] Aspect 1 of the present invention is as follows.

[0017] A method for manufacturing a contact lens, comprising the following steps: by closing a component-supporting molding mold that positions and supports a component for embedding relative to a first molding mold that provides one of the front surface and the rear surface of the lens, a first molding cavity is defined in which the component for embedding is disposed; when a primary molded product in which the component for embedding is embedded is obtained by curing a first molding material filled in the first molding cavity, the primary molded product is left in the first molding mold while the first molding material is in an uncured state on the side of the component-supporting molding mold, and the component-supporting molding mold is removed from the first molding mold; by closing a second molding mold that provides the other of the front surface and the rear surface of the lens relative to the first molding mold in which the primary molded product remains, a second molding cavity is defined; and the second molding material is filled in the second molding cavity and cured, thereby manufacturing the contact lens in which the component for embedding is embedded as an integral molded product.

[0018] According to this method, the component support forming mold is removed in the state where the solidification of the first forming material is not completed, so that the formation of pores and other forming defects in the primary formed product embedded with the embedded component can be reduced or even avoided. That is, as a result of the research of the inventor, it is known that the generation of pores and the like in the primary formed product is particularly easy to be generated around the embedded component. As a result of further repeated research, it can be known that even if the solidification of the first forming material is carried out to a certain extent, pores and the like have not yet been generated. In addition, it is also known that in the state where the solidification of the first forming material is considered to be almost free of pores, the solidification of the first forming material can be carried out to a state where the embedded component can be maintained in a predetermined position. Therefore, in this method, the component support forming mold is removed before the solidification of the first forming material is completed, and the constraint state and even the closed state of the forming cavity formed by the close contact of the component support forming mold on the surface of the first forming material are released, thereby suppressing the generation of pores in the primary formed product, and the primary formed product in which the component is held in a fixed state can be formed with stable quality.

[0019] Furthermore, in a primary molded product, even if sink marks are assumed to occur and the dimensional accuracy is reduced due to the removal of the component support molding mold when the curing is not complete, the dimensional accuracy of the contact lens as an integrally molded finished product can be fully ensured by the subsequent molding process of the second molding material using the second molding mold.

[0020] Aspect 2 of the present invention is as follows.

[0021] In the contact lens manufacturing method according to the first aspect, the curing of the first molding material is completed before the curing treatment of the second molding material.

[0022] According to this method, the solidification of the first molding material is completed before the second molding material is solidified, preferably before the second molding material is injected into the mold cavity, thereby stabilizing the shape and quality of the single-molded product and further improving the fixing force and positioning accuracy of the embedded component.

[0023] Aspect 3 of the present invention is as follows.

[0024] A method for manufacturing a contact lens, wherein a first molding material is cured in a first molding cavity defined by closing a component-supporting molding mold relative to a first molding mold that provides one of a front lens surface and a rear lens surface, thereby forming a primary molded product in which an embedding component positioned and supported by the component-supporting molding mold is embedded, and after the component-supporting molding mold is removed from the first molding mold while the primary molded product remains in the first molding mold, a second molding material is cured in a second molding cavity defined by closing a second molding mold that provides the other of the front lens surface and the rear lens surface with the first molding mold, thereby manufacturing the contact lens in which the embedding component is embedded as an integral molded product, the component-supporting molding mold has the following structure: a support portion for positioning and supporting the embedding component is provided on a cavity forming surface of the first molding cavity, and a wall portion defining the first molding cavity has a flexible portion that allows deformation due to shrinkage during polymerization molding of the first molding material.

[0025] According to this mode, a supporting portion for positioning and supporting the embedded member is provided in the component support forming die, and a flexible portion is provided in the component support forming die, so that the positioning accuracy of the embedded member using the component support forming die can be ensured, and the generation of poor forming such as pores in the primary molded product embedded with the embedded member can be reduced or even avoided. That is, as a result of the inventor's research, it is known that the generation of pores in the primary molded product is particularly easy to occur around the embedded member. As a result of further repeated research, it is known that pores are easy to be generated along with the shrinkage during the solidification of the first molding material. Therefore, in this mode, in the component support forming die, the support stability of the embedded member supported by the supporting portion of the embedded member is ensured, and the constraint state formed on the surface of the first molding material is reduced or even eliminated by the flexible portion provided on the wall portion that divides the first molding cavity, or the volume change of the molding cavity is allowed, thereby, the generation of pores in the primary molded product can be suppressed, and the primary molded product that holds the member in a fixed state can be formed with stable quality.

[0026] Furthermore, even if the dimensional accuracy of a primary molded product is reduced due to deformation of the flexible portion of the component supporting the molding die, the dimensional accuracy of the contact lens as an integrally molded finished product can be fully ensured by subsequently performing a molding process using a second molding material using a second molding die.

[0027] In addition, in the present method, in the component support forming mold, for example, the substantially entirety of the forming portion of the forming cavity can be made into a flexible portion. In addition, for example, the outer peripheral region of the substantially spherical crown-shaped cavity forming portion can be formed into a flexible portion by annular thinning, thereby making the substantially entirety of the forming portion of the forming cavity move in parallel, and also allowing the cavity forming surface to move toward the inside of the forming cavity due to the contraction during the effect of the first forming material. Alternatively, the present method also includes the following method for manufacturing contact lenses: when the forming portion of the forming cavity is made partially flexible, a flexible portion can also be provided at a position away from the supporting portion of the embedding component. For example, as the above-mentioned component support forming mold, the following structure is adopted, in which a flexible portion that allows deformation due to the contraction during the polymerization molding of the above-mentioned first forming material is provided in the area of ​​the wall portion that demarcates the above-mentioned first forming cavity away from the supporting portion of the above-mentioned embedding component. In all the methods, the constraint state caused by the component supporting the forming mold relative to the surface of the first forming material is reduced or even eliminated by the flexible portion, or the volume change of the forming cavity is allowed, thereby suppressing the generation of pores in the primary molded product, and the primary molded product that holds the component in a fixed state can be formed with stable quality. In addition, the method of reducing or even eliminating the constraint state caused by the component supporting the forming mold relative to the surface of the first forming material by the flexible portion does not refer to the separation between the surface of the first forming material and the cavity forming surface of the component supporting the forming mold. It can be understood as follows: for example, the close contact between the surface of the first forming material and the cavity forming surface of the component supporting the forming mold is maintained and the movement and deformation of the cavity forming surface are allowed by the flexible portion, thereby eliminating or even relaxing the constraint state of the position and shape relative to the surface of the first forming material.

[0028] A fourth aspect of the present invention is as follows.

[0029] A method for manufacturing a contact lens, wherein a first molding material is cured in a first molding cavity defined by closing a component-supporting molding mold relative to a first molding mold that provides one of a front lens surface and a rear lens surface, thereby forming a primary molded product in which an embedding component positioned and supported by the component-supporting molding mold is embedded, and after removing the component-supporting molding mold from the first molding mold while leaving the primary molded product in the first molding mold, a second molding material is cured in a second molding cavity defined by closing a second molding mold that provides the other of the front lens surface and the rear lens surface relative to the first molding mold, thereby manufacturing the contact lens in which the embedding component is embedded as an integral molded product, a mold of a material whose adhesion to the first molding material is smaller than the adhesion of the embedding component to the first molding material is used as the component-supporting molding mold.

[0030] According to this method, by using a component support forming die with a lower adhesion to the first forming material than the embedding member, it is possible to ensure the positioning accuracy of the embedding member using the component support forming die and reduce or even avoid the generation of poor forming such as pores in the primary formed product embedded with the embedding member. That is, as a result of the inventor's research, it is known that the generation of pores in the primary formed product is particularly easy to occur around the embedding member. As a result of further repeated research, it is known that pores are easy to be generated along with the shrinkage during the solidification of the first forming material. Therefore, in this method, in the component support forming die, the adhesion between the first forming material and the first forming material is set to be low, so that when the shrinkage accompanying the solidification of the first forming material is formed, the first forming material is easy to leave the component support forming die, and the negative pressure of the first forming material generated around the embedding member during or after forming is reduced. As a result, the generation of pores in the primary formed product can be suppressed, and the primary formed product in which the component is held in a fixed state can be formed with stable quality.

[0031] Furthermore, in a primary molded product, if, during solidification of the first molding material, the first molding material leaves the cavity forming surface of the component supporting molding mold and thereby reduces dimensional accuracy, the dimensional accuracy of the contact lens as an integrally molded finished product can be fully ensured by subsequently performing a molding process of the second molding material using a second molding mold.

[0032] A fifth aspect of the present invention is as follows.

[0033] In the contact lens manufacturing method according to any one of aspects 1 to 4, the first molding die is a molding die for the front surface of the lens, and the second molding die is a molding die for the rear surface of the lens.

[0034] According to this embodiment, the first molding die having a concave molding surface (cavity forming surface) corresponding to the front surface of the lens can accommodate the first molding material using the concave molding surface. Therefore, the molding operation becomes easier and the lens manufacturing equipment can be easily simplified.

[0035] Aspect 6 of the present invention is as follows.

[0036] In the contact lens manufacturing method according to any one of aspects 1 to 5, the primary molded product has a recessed portion opened toward the member support mold at a central portion thereof, and the primary molded product has a smaller thickness dimension at the central portion thereof.

[0037] According to this mode, the thickness dimension of the central part of the primary molded product becomes smaller. Therefore, even if the primary molded product is dimensionally deformed, the size of the deformation of the central part can be suppressed to be small. Therefore, the adverse effects of the deformation of the primary molded product, which have a greater impact on the optical characteristics, can be reduced or even avoided. In addition, in this mode, the concave portion opening toward the component support molding die can be a through hole shape without a bottom in addition to a concave shape with a bottom, and the same effect can be achieved.

[0038] A seventh aspect of the present invention is as follows.

[0039] In the contact lens manufacturing method according to any one of aspects 1 to 6, the member support molding die is provided with a concave and / or convex engaging portion for positioning the embedding member.

[0040] According to this method, in the molding cavity of a primary molded product, the embedded component can be positioned and supported relative to the component supporting molding mold by utilizing mechanical engagement, i.e., concave-convex engagement, or other engagement based on physical effects (in addition to chemical physical effects such as electron sharing (covalent bonds) and intermolecular forces (van der Waals forces)).

[0041] Aspect 8 of the present invention is as follows.

[0042] In the contact lens manufacturing method described in the above-mentioned method 7, when the above-mentioned primary molded product is formed in the above-mentioned first molding cavity, the above-mentioned first molding material is allowed to enter between the above-mentioned component supporting molding mold and the above-mentioned embedding component, and the first molding material is solidified in a state where the embedding component is covered by the first molding material.

[0043] According to this embodiment, the embedding member is not exposed on the surface of the primary molded product and is completely embedded for use in the subsequent molding of the second molding material, etc. Therefore, the adhesion between the primary molded product and the second molding material, etc. is generally uniform and good over the entire surface, and the occurrence of molding defects during the subsequent molding of the second molding material, etc. can be more effectively prevented.

[0044] A ninth aspect of the present invention is as follows.

[0045] In the contact lens manufacturing method according to any one of the above aspects 1 to 8, the embedding member is positioned and supported in a bonded state in the member support molding die.

[0046] According to this method, the embedded component is supported in an attached state relative to the cavity forming surface of the component support forming mold, thereby making it easy to hold the embedded component more stably, and for example, the cavity forming surface of the component support forming mold can also be made into a simple and smooth shape. In addition, when the embedded component is positioned and supported on the component support forming mold, the attached state support mechanism of this method can also be used in conjunction with the support mechanism based on the engaging portion as described in the above method 7.

[0047] In particular, in this embodiment, the cavity molding surface of the component support molding die can be made into a smooth curved surface shape without uneven steps and the embedded component can be positioned and supported in an attached state. As a result, the surface formed by the component support molding die in the primary molded product can be made into a smooth curved surface shape without uneven steps and the like as a whole, including the surface of the embedded component. As a result, the generation of voids and the like during the molding of the first molding material can be more effectively suppressed.

[0048] A tenth aspect of the present invention is as follows.

[0049] In the contact lens manufacturing method according to the ninth aspect, the embedding member is directly formed on the surface of the member support molding die to be positioned and supported in an attached state.

[0050] According to this method, the embedding member is directly formed on the surface of the component support forming mold by, for example, printing, plating, etc., thereby easily obtaining a good adhesion state of the embedding member relative to the surface of the component support forming mold. In addition, it is not necessary to form the entirety of the embedding member on the surface of the component support forming mold. For example, as illustrated in the third embodiment described later, after the embedding member is partially formed on the surface of the component support forming mold and embedded in a primary molded product, the remaining part is formed on the surface of the local embedding member exposed by removing the component support forming mold, or the remaining part formed separately is fixed to the local embedding member, thereby completing the embedding member as a whole. Therefore, by closing the second molding mold 22 to mold the second molding material, a contact lens embedded with the embedding member can also be obtained.

[0051] In addition, according to this embodiment, the cavity forming surface of the component support forming die can be formed to have a smooth surface shape, and the embedded component is supported here, so that the forming surface of the obtained primary molded product formed by the component support forming die can be made into a smooth shape including the exposed surface of the embedded component. Thus, it is also possible to reduce or even avoid forming defects such as those caused by complex concave and convex shapes when forming the first molded product.

[0052] Aspect 11 of the present invention is as follows.

[0053] In the contact lens manufacturing method according to any one of aspects 1 to 10, in the member-supporting mold, the embedding member is positioned and supported without an adhesive.

[0054] According to this aspect, there is no need to worry about the adhesive's adverse effects on biological tissues or lens materials, and the reliability of lens products can be improved.

[0055] A twelfth embodiment of the present invention is as follows.

[0056] In the contact lens manufacturing method according to any one of the above aspects 1 to 11, in the member-supporting mold, a cavity forming surface of the first molding cavity is subjected to a surface treatment for improving mold releasability.

[0057] According to this method, it is possible to reduce or even eliminate the adverse conditions caused by excessive fixing of the embedded component by the component support forming mold. For example, when the first molded product is demolded from the component support forming mold, demolding itself becomes easier. In addition, it is also effective in preventing the adverse condition of the embedded component remaining locally relative to the component support forming mold and the damage to the embedded component associated therewith.

[0058] A thirteenth aspect of the present invention is as follows.

[0059] In the method for manufacturing a contact lens according to any one of aspects 1 to 12, the embedding member is a member that is harder than the lens component.

[0060] According to this aspect, the embedding member is hard and can be used to improve the support stability of the embedding member by the member-supporting forming die. In addition, it is also possible to study the use of the hardness of the embedding member to improve the shape stability of the first molded product.

[0061] A fourteenth aspect of the present invention is as follows.

[0062] In the contact lens manufacturing method according to aspect 13, the embedding member is an electrical component including a metal portion.

[0063] According to this method, the hardness of the embedding member can be ensured by utilizing the metal portion constituting the electrical component. In addition, according to the present invention, the embedding member can be completely embedded in the lens composed of the lens material, so that the electrical component including the metal portion can be avoided from direct contact with the biological body.

[0064] A fifteenth aspect of the present invention is as follows.

[0065] In the contact lens manufacturing method according to any one of aspects 1 to 13, both the first molding material and the second molding material are polymerizable monomers that impart oxygen permeability to a hard lens.

[0066] According to this method, the oxygen permeability of the contact lens as a product can be improved, and the occurrence of defects such as pores associated with the polymerization shrinkage of the first molding material can be reduced or even avoided as described above, and the production efficiency and quality of the molded product can be ensured.

[0067] A sixteenth embodiment of the present invention is as follows.

[0068] In the contact lens manufacturing method according to any one of aspects 1 to 15 above, the first molding material is the same as the second molding material.

[0069] According to this embodiment, by making the first molding material and the second molding material the same to promote integration, mechanical properties and optical properties can be improved and stabilized. In addition, by making the first molding material and the second molding material the same, the equipment and management for each curing process are also easy.

[0070] A seventeenth embodiment of the present invention is as follows.

[0071] In the contact lens manufacturing method described in any one of the above-mentioned methods 1 to 16, when a primary molded product in which the above-mentioned embedding component is embedded is obtained by solidifying the first molding material filled in the above-mentioned first molding cavity, the first molding material is solidified in a manner that pushes it from the side of the first molding mold toward the side of the above-mentioned component supporting molding mold.

[0072] According to this mode, by controlling the progress of solidification of the first molding material, even if shrinkage and deformation accompanying solidification occur, it becomes easy to control them, and it is easy to achieve improved molding quality. In particular, this mode 17 is adopted in combination with the above-mentioned mode 1, so that the side of the component support molding die where pores are likely to occur is left as unfinished solidification, and the solidification process is further advanced on the side of the first molding die, so that the stability of the shape and quality of the first molded product when the component support molding die is removed can be improved.

[0073] Aspect 18 of the present invention is as follows.

[0074] In the contact lens manufacturing method described in any one of the above-mentioned methods 1 to 17, after the above-mentioned first molding material is molded and the above-mentioned component support molding mold is removed from the above-mentioned first molding mold, before the above-mentioned second molding mold is closed relative to the first molding mold, the intermediate molding product is assembled with respect to the above-mentioned primary molding product, and the above-mentioned second molding material is cured in the above-mentioned second molding cavity demarcated by closing the second molding mold with the first molding mold in which the primary molding product including the intermediate molding remains.

[0075] According to this method, the aforementioned technical effects such as positioning of the embedded member based on the member support forming mold and reduction of the generation of pores can be ensured, and the contact lens can be manufactured with a composite structure in which the intermediate molded product is integrated. In addition, the assembly of the intermediate molded product with respect to the primary molded product can be advantageously achieved, for example, by the methods 19 and 20 described later.

[0076] A nineteenth aspect of the present invention is as follows.

[0077] In the contact lens manufacturing method described in the above-mentioned method 18, after the above-mentioned first molding material is formed and the above-mentioned component supporting molding mold is removed from the above-mentioned first molding mold, before the above-mentioned second molding mold is clamped relative to the first molding mold, the auxiliary molding mold is clamped relative to the first molding mold in which the above-mentioned primary molding product remains to demarcate an intermediate molding cavity, the intermediate molding cavity is filled with a third molding material and cured, so that the above-mentioned intermediate molding product is formed in a state of being assembled to the primary molding product, and then the auxiliary molding mold is removed from the first molding mold and the above-mentioned second molding mold is clamped with the first molding mold in which the primary molding product including the intermediate molding product remains to demarcate the above-mentioned second molding material in the above-mentioned second molding cavity.

[0078] Aspect 20 of the present invention is as follows.

[0079] In the method for manufacturing a contact lens according to claim 18, the intermediate molded product is formed independently of the primary molded product and is assembled to the primary molded product.

[0080] That is, according to methods 19 and 20, even if bumps, gaps, etc. exist in the assembled state of the primary molded product and the intermediate molded product, the accuracy and quality of the contact lens as an integrally molded finished product can be fully and stably ensured by the subsequent molding of the second molding material.

[0081] Aspect 21 of the present invention is as follows.

[0082] In the method for producing a contact lens according to any one of aspects 18 to 20, the intermediate molded product is made of a silicone material.

[0083] According to this method, the high oxygen permeability of silicone materials can be used to improve the oxygen permeability of contact lenses. For example, even if the oxygen permeability of the first molding material and the second molding material is relatively poor, the thickness of the lens layer composed of the first molding material and the second molding material can be suppressed by arranging the intermediate molding product in a buried state (including a state of partial exposure to the lens surface) in the lens, and the thickness of the component can be supplemented by the intermediate molding product composed of silicone materials, thereby ensuring the lens thickness required for the embedding component and achieving good oxygen permeability.

[0084] In addition, as described later, by using hard lens materials such as RGP (oxygen permeable lens material) as the first molding material and the second molding material, it is possible to improve the positioning accuracy of the embedded components when the glasses are worn, and the overall oxygen permeability can be improved by using an intermediate molded product made of silicone material.

[0085] A mode 22 of the present invention is as follows.

[0086] In the contact lens manufacturing method according to any one of aspects 18 to 21, a concave portion is formed in a central portion of the primary molded product, and the intermediate molded product is inserted into and assembled in the concave portion.

[0087] According to this method, the placement area of ​​the intermediate molded product is efficiently set in the central part, and the thickness dimension of the intermediate molded product is easily ensured. For example, when an intermediate molded product formed separately is assembled to a primary molded product, the intermediate molded product can also be positioned by the concave portion. As an intermediate molded product, for example, when a material with high oxygen permeability such as silicone material is used, by providing a concave portion, the thickness dimension of the primary molded product in the central part is reduced and the thickness dimension of the intermediate molded product is increased, and the oxygen permeability as a whole can be further improved. In addition, by assembling the intermediate molded product in the concave portion, the surface unevenness of the primary molded product in the state of assembling the intermediate molded product can be suppressed to be smaller, and when the second molding material is molded thereafter, it is also easy to suppress the molding defects caused by such unevenness.

[0088] Mode 23 of the present invention is as follows.

[0089] In the contact lens manufacturing method described in any one of the above-mentioned modes 18 to 22, the above-mentioned intermediate molded product is arranged in the central part of the lens, and the entire surface of the intermediate molded product on the front surface side of the lens is covered by a surface layer formed by the above-mentioned first molding material or the above-mentioned second molding material.

[0090] According to this method, the front surface of the lens (the convex surface of a roughly spherical crown shape) of the intermediate molded product that directly overlaps the eyelid when the glasses are worn is prevented from being exposed. Therefore, regarding the intermediate molded product, it is possible to avoid research on friction, adsorption, or biological influences associated with contact with the eyelid, avoid reduction in lens performance caused by the intermediate molded product, and achieve expansion of the design freedom and even selection freedom related to the material of the intermediate molded product. Specifically, for example, silicone materials, which are more likely to have problems with adhesion to the biological body, can also be easily adopted as the material of the intermediate molded product.

[0091] Aspect 24 of the present invention is as follows.

[0092] In the contact lens manufacturing method described in any one of the above-mentioned methods 1 to 23, the above-mentioned first molding mold has a concave cavity forming surface that provides a molding surface for the above-mentioned front surface of the lens, and the above-mentioned second molding mold has a convex cavity forming surface that provides a molding surface for the above-mentioned rear surface of the lens, and the molds are closed by overlapping the above-mentioned component-supporting molding mold and the second molding mold with the first molding mold from above in a state in which the first molding mold is opened vertically upward.

[0093] According to this method, the front surface of the lens can be formed into a convex surface of a roughly spherical crown shape by the first molding material, and the rear surface of the lens can be formed into a concave surface of a roughly spherical crown shape by the first molding material. As a result, the supporting surface of the embedded component in the component support molding mold can be made into a convex surface, and compared with a concave surface, it is easier to perform processing for supporting the embedded component from the outside.

[0094] However, in the above-mentioned aspects 1 to 23, the following aspects different from the present aspect can also be adopted, and the following aspects can also be combined with other aspects described later.

[0095] In the method for manufacturing a contact lens described in any one of the above-mentioned methods 1 to 23, the above-mentioned first molding mold has a convex cavity forming surface that provides a molding surface for the rear surface of the lens, and the above-mentioned second molding mold has a concave cavity forming surface that provides a molding surface for the front surface of the lens, and in a state in which the cavity molding surface (the surface of the component for positioning and supporting embedding) of the first molding material that becomes a roughly spherical crown-shaped concave surface in the above-mentioned component support molding mold is opened toward vertically upward, the first molding molds are overlapped and molded from above to demarcate the above-mentioned first molding cavity, and after the above-mentioned primary molded product remains in the first molding mold and the component support molding mold is removed, the first molding mold is overlapped from above with the above-mentioned second molding mold whose concave cavity forming surface is opened toward vertically upward, and the above-mentioned second molding material is molded in the above-mentioned second molding cavity in which the primary molded product is provided.

[0096] Mode 25 of the present invention is as follows.

[0097] In the method for producing a contact lens according to any one of aspects 1 to 24 above, the method is used for producing a scleral lens.

[0098] According to this mode, compared with hard or soft contact lenses, i.e. corneal lenses, which are generally used for vision correction, the movement of the lens on the eyeball when worn can be suppressed by using a scleral lens. Therefore, in the contact lens provided by the present invention as described above, the accuracy and stability of positioning on the eyeball when the embedded member is worn can be advantageously ensured.

[0099] In addition, scleral lenses are interpreted in a broad sense, and various scleral lenses may be included, such as a type with a roughly circular outer peripheral shape that is slightly larger than the cornea, a type that covers roughly half of the sclera, or a type with a non-circular outer peripheral shape that covers roughly the entire sclera.

[0100] However, the present invention is not limited to this mode and is not interpreted. The present invention can also be applied to common corneal contact lenses other than scleral lenses, for example. In addition, for example, by making at least one or both of the first molding material and the second molding material into soft contact lens materials, it can also be applied to soft contact lenses or contact lenses based thereon.

[0101] Aspect 26 of the present invention is as follows.

[0102] A contact lens is a contact lens composed of an oxygen-permeable hard lens component, wherein an embedding component is arranged inside the oxygen-permeable hard lens component in a fixed state, an intermediate component composed of a silicone material is arranged inside the central part of the lens, and a front surface layer composed of the oxygen-permeable hard lens component is provided on the front surface side of the lens of the intermediate component in a manner covering the entire surface, and the surface layer has a smaller thickness dimension than the intermediate component at least on the central axis of the lens.

[0103] According to this embodiment, a contact lens as a composite structure can be provided, which can realize the characteristics required for positioning and supporting the embedding member by using a hard lens component, and the composite structure uses a silicone material that can realize higher oxygen permeability than the oxygen permeable hard lens component. In particular, by making the intermediate member composed of the silicone material thicker than the front surface layer composed of the hard lens component on the central axis of the lens, even if the central part of the lens is assumed to be thick due to the arrangement of the embedding member, the oxygen permeability of the lens as a whole can be advantageously ensured.

[0104] Furthermore, according to this method, the front surface layer formed of the hard lens component can prevent the silicone material from being exposed to the front surface side of the lens, thereby preventing the silicone material from being adsorbed to the eyelid that overlaps with the front surface of the lens when worn, and thus achieving a good wearing feeling. In addition, by, for example, making the scleral lens a lens design that actively ensures a tear layer on the cornea, it is also possible to reduce or avoid the back surface side of the lens from directly contacting the organism (cornea) or even contacting it due to pressure when the lens is worn, allowing more situations in which the intermediate member is exposed on the back surface side of the lens than on the front surface side of the lens.

[0105] However, such a contact lens having a specific structure according to the present embodiment can be advantageously produced by, for example, the production method described in any one of the above-mentioned embodiments 18 to 23.

[0106] Mode 27 of the present invention is as follows.

[0107] In the contact lens described in the above-mentioned method 26, a rear surface layer composed of the above-mentioned oxygen-permeable hard lens component is also provided on the rear surface side of the lens of the above-mentioned intermediate component in a manner covering the entire surface, and the rear surface layer has a thickness dimension smaller than that of the intermediate component at least on the central axis of the lens.

[0108] According to this method, the intermediate member made of silicone material is also prevented from being exposed on the rear surface side of the lens. Therefore, even if the rear surface of the lens overlaps with the cornea when worn, the adsorption of silicone material to the cornea is eliminated, and the wearing feeling can be improved.

[0109] A 28th embodiment of the present invention is as follows.

[0110] In the contact lens described in aspect 26 or 27, the lens peripheral portion is not provided with the intermediate member at least at the outer peripheral end, but is formed of the oxygen-permeable hard lens component.

[0111] According to this method, for example, it is possible to have no intermediate component near the outer periphery of the lens peripheral portion, or to have the thickness of the hard lens component on the front surface side and / or the rear surface side of the lens on the inner peripheral side of the lens peripheral portion be larger than the intermediate component. Thus, the shape retention performance of the entire lens can be advantageously ensured by the hard lens component that is harder than the intermediate component.

[0112] Mode 29 of the present invention is as follows.

[0113] In the contact lens described in any one of methods 26 to 28 above, at the position where the lens thickness becomes maximum, the maximum lens thickness is greater than 0.7 mm, and the total thickness of the above-mentioned surface layer composed of the above-mentioned oxygen-permeable hard lens components arranged on both sides of the above-mentioned intermediate component in the lens thickness direction is less than 0.7 mm.

[0114] According to this method, compared with a case where the lens is composed only of hard lens parts with high oxygen permeability, by utilizing an intermediate member composed of a silicone material, it is possible to more advantageously ensure the overall oxygen permeability of the lens in the thickness direction. For example, even if the maximum lens thickness exceeds 0.7 mm, it is easy to achieve the oxygen permeability required for daily use other than sleeping.

[0115] Aspect 30 of the present invention is as follows.

[0116] In the contact lens according to any one of aspects 26 to 29 above, the contact lens is a scleral lens.

[0117] According to this embodiment, as also described in the above embodiment 25 for a scleral lens, a scleral lens is used, thereby achieving the effects of improving the accuracy and stability of positioning on the eyeball when the embedding member is worn and making it easier to ensure the positioning.

[0118] According to the method of the present invention, it is easy to form a contact lens mold with embedded components in a manner that reduces or even avoids poor forming such as pores. By the way, in optical lenses, for example, it is usually difficult to control the location where pores are generated. If they are generated in the optical part, it may affect the viewing method. Even if they are generated in the peripheral part away from the optical part, the strength of the lens itself will be reduced. In particular, in contact lenses equipped with electronic components, the strength reduction can easily become a fatal defect of the product. In addition, oxygen-permeable materials allow water molecules to pass through, and water droplets are generated in the pores, which may affect the electronic components. Therefore, it is of great technical significance to suppress poor forming such as pores.

[0119] Furthermore, in the contact lens according to the present invention, a hard lens component is used to ensure positioning accuracy of the embedded member, and an intermediate member made of a silicone material is also used, so that the oxygen permeability can be easily improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0120] Figure 1 It is an explanatory diagram of the molding process of the first molding material in the first embodiment of the present invention.

[0121] Figure 2 It is an explanatory diagram of the molding process of the second molding material in the first embodiment of the present invention.

[0122] Figure 3 1 is a diagram showing a member support forming die used in the first embodiment. Figure 3 (a) is a stereogram, Figure 3 (b) is a side view, Figure 3 (c) is a longitudinal sectional view.

[0123] Figure 4 It means in Figure 3 A diagram showing a state in which a member for embedding is provided in a member supporting forming die, Figure 4 (a) is a stereogram, Figure 4 (b) is a side view, Figure 4 (c) is a longitudinal sectional view.

[0124] Figure 5 2 is a diagram showing a contact lens manufactured by the first embodiment. Figure 5 (a) is a stereogram, Figure 5 (b) is a top view. Figure 5 (c) is a side view, Figure 5 (d) is a longitudinal sectional view.

[0125] Figure 6 It is an explanatory diagram of the molding process of the second molding material in the second embodiment of the present invention.

[0126] Figure 7 It is an explanatory diagram showing an example of an assembly process of the intermediate member in the second embodiment.

[0127] Figure 8 It is an explanatory diagram showing another example of the assembling process of the intermediate member in the second embodiment.

[0128] Fig. 9 It is an explanatory diagram of the molding process of the first molding material and the second molding material in the third embodiment of the present invention.

[0129] Fig.10 It is a process explanatory diagram of installation and formation of the embedding member in the member support molding die used in the third embodiment.

[0130] Fig.11 It is an explanatory diagram for illustrating another embodiment of the present invention.

[0131] Fig.12 It is an explanatory diagram for illustrating still another embodiment of the present invention.

[0132] Fig.13 It is an explanatory diagram which exemplarily shows the forming process of still another embodiment of the present invention.

[0133] Fig.14 This is a photograph of a primary molded product obtained as an example.

[0134] Fig.15 This is a photograph of a primary molded product obtained as a comparative example.

[0135] Fig.16 The present invention is directed to a component support forming die that can be used. Figure 3Different ways of example diagram, Fig.16 (a) is a top view, Fig.16 (b) is the main view, Fig.16 (c) is Fig.16 The cc cross-sectional view in (a) is Fig.16 (d) is a stereogram. DETAILED DESCRIPTION

[0136] Hereinafter, in order to explain the present invention in more detail, a description will be given based on the embodiments with reference to the drawings.

[0137] first, Figure 1-Figure 3 The following is an overview of one embodiment of a method for producing a contact lens 10 according to the present invention. In this embodiment, the contact lens 10 is produced through two-stage mold forming steps for a lens material.

[0138] More specifically, in the first forming step, Figure 1 (a)- Figure 1 As shown in (c) of FIG. 1 , the first molding material 18 is molded in the first molding cavity 16 defined by combining the first molding die 12 and the member support molding die 14, thereby forming a primary molded product 20. In the subsequent second molding step, as shown in FIG. Figure 2 (a)- Figure 2 As shown in (c), the primary molded product 20 remains, and the second mold 22 is molded with the first mold 12 instead of the component support mold 14 removed from the first mold 12, thereby defining a second molding cavity 24. Then, the second molding material 26 is molded in the second molding cavity 24 in which the primary molded product 20 remains, thereby obtaining the contact lens 10 as a secondary molded product.

[0139] In particular, in the present embodiment, as the first molding die 12, a lens front surface mold having a concave molding surface 28 as a cavity forming surface is used, and the above-mentioned concave molding surface 28 gives the lens front surface composed of a convex surface roughly in the shape of a spherical crown. In addition, as the second molding die 22, a lens rear surface mold having a convex molding surface 30 as a cavity forming surface is used, and the above-mentioned convex molding surface 30 gives the lens rear surface composed of a concave surface roughly in the shape of a spherical crown. The above-mentioned first molding die 12 and second molding die 22 have molding surfaces 28 and 30 of a shape that realizes the required optical characteristics, and can be given a vision correction function as needed relative to the optical area of ​​the light that is located in the central part 32 of the contact lens 10 and passes through the optical system of the eye.

[0140] In addition, the cavity forming surface 34 of the component support molding die 14 is not a structure for imparting a lens surface, and therefore is not limited to a predetermined shape corresponding to the required optical characteristics, but is a convex shape of a spherical crown that roughly corresponds to the concave molding surface 28 of the first molding die 12. Moreover, the first molding cavity 16 and thus the primary molding 20, which are divided by the first molding die 12 and the component support molding die 14, are smaller in thickness throughout the entirety than the contact lens 10 as a secondary molding product. As a result, the rear surface of the primary molding 20 is covered by the second molding material 26 throughout the entirety.

[0141] In addition, the first forming die 12, the second forming die 22, and the component support forming die 14 are not limited in material. It is preferable to use a resin forming die rather than a metal forming die. As a specific example, common thermoplastic resins such as polypropylene, polyethylene, polystyrene, polycarbonate, polyethylene terephthalate, polyamide, polyoxymethylene, and polyvinyl chloride can be used as the die material. The materials of the respective forming dies may be the same, but different materials and surface properties may also be used.

[0142] In addition, the component support forming mold 14 has a support portion 38 for a component 36 for embedding that is separately manufactured and prepared on the cavity forming surface 34. As such a component 36 for embedding, any component for imparting a specific function to the contact lens 10 can be used, and specifically, electronic components such as sensors, cameras, projectors, batteries, antennas, and computing devices for realizing smart contact lenses can be used as the embedding component 36. In addition, the location of the embedding component 36 in the component support forming mold 14 is usually set to a peripheral portion 40 that is away from the central portion 32 of the optical region toward the outer peripheral side, mainly considering avoiding the influence on the field of view, but it can also be arranged in the central portion 32 according to the component, such as a projector that displays information in a visible manner.

[0143] In addition, the specific structure of the support portion 38 is not limited, and for example, it can also be formed by supporting the embedded member 36 in an attached state including bonding, welding, printing, etc., but in this embodiment, as shown in FIG. Figure 3 (a)- Figure 3 As shown in (c) of FIG. 1 , an open concave support portion 38 is formed on the cavity forming surface 34 of the component support forming mold 14. Figure 4 (a)- Figure 4As shown in (c), the embedded member 36 is embedded relative to the concave support portion 38, so that the outer peripheral end of the embedded member 36 is hooked on the engaging portion 42 formed by the peripheral wall of the concave support portion 38, so as to be positioned at a predetermined position and supported. In addition, the specific shape and size of the support portion 38 having the engaging portion 42 can be appropriately set according to the embedded member 36, and a plurality of independent concave and convex support portions 38 corresponding to the shape of the embedded member 36 can be provided in order to clamp the embedded member 36 at multiple locations. In addition, a plurality of support portions 38 can be provided in order to provide a plurality of embedded members 36. In addition, as for the support portion 38, it is also possible to adopt adhesion in combination with the engaging formation in shape so that the embedded member 36 is supported on the cavity forming surface 34.

[0144] In addition, the support strength of the embedding member 36 by the support portion 38 may be such that even if the member support molding die 14 is Figure 4 (b) to Figure 1 The embedding member 36 will not fall off even if the mold is turned over as shown in (a) and further molded with the first molding die 12. The support strength is set in such a way that the embedding member 36 leaves the member support molding die 14 and is embedded in the primary molded product 20 when the member support molding die 14 is removed from the first molding die 12 at least after the first molding material 18 is formed.

[0145] By assembling and supporting the embedding member 36 on the member support molding die 14 in this manner, Figure 1 (a)- Figure 1 As shown in (b), when the first molding material 18 is molded, the embedding member 36 can be set at a predetermined position in the first molding cavity 16. And, by filling the first molding material 18 into the first molding cavity 16 and performing mold molding as described above, the primary molded product 20 can be formed as a molded product in which the embedding member 36 is embedded.

[0146] In addition, in such a primary molded product 20, the embedding member 36 may be embedded in a completely embedded state inside, or may be embedded in a state where it is partially exposed on the molding surface side formed by the member support molding die 14, which becomes the rear surface side of the lens. In addition, the molding surface side formed by the concave molding surface 28 of the first molding die 12 becomes the front surface of the contact lens 10, so it is preferable to avoid exposing the embedding member 36 from the viewpoint of ensuring the wearing feeling, etc.

[0147] In the present embodiment, in the state where the embedding member 36 is supported by the member support forming die 14, a gap-shaped cavity 44 is set partially (preferably near the inner circumference of the peripheral portion 40 where the wall is relatively thick) or substantially over the entirety between the embedding member 36 and the member support forming die 14. Furthermore, by actively applying the first forming material 18 to the surface side of the embedding member 36, at least a part of the surface of the embedding member 36, preferably substantially the entirety, is covered with the first forming material 18 in a thin film-like manner.

[0148] Furthermore, in the present embodiment, a central convex portion 46 is formed in the central portion of the cavity forming surface 34 of the component support forming mold 14. The engaging portion 42 is formed by the outer peripheral surface of the central convex portion 46 in a manner having a larger (higher in the thickness direction of the forming mold) stepped surface that is advantageous for positioning the embedded component 36. Furthermore, when the molds are closed, the protruding end surface of such a central convex portion 46 is close to or even in contact with the central portion of the cavity forming surface 34 of the first forming mold 12, thereby achieving improved shape stability and dimensional accuracy of the first forming cavity 16 in the closed mold state. Furthermore, in the present embodiment, as Figure 1 (c) and Figure 2 As shown in (b), in the first forming cavity 16, a small gap is set between the concave forming surface 28 of the first forming mold 12 and the protruding end surface of the central convex portion 46 of the component supporting forming mold 14 in a manner that expands with a substantially constant thickness, and a thin-walled surface film portion 48 expanded on the surface of the central portion 32 is formed along the concave forming surface 28 of the first forming mold 12.

[0149] However, the present invention is not limited by the material used. The first molding material 18 can be any of various contact lens materials according to the properties required of the contact lens 10 as a product. For example, a known monomer can be used as a polymerizable composition for molding a contact lens.

[0150] As an example for reference, various conventionally known hard contact lens materials can be used as molding materials for hard lenses. For example, a hard contact lens material composed of a polymerizable composition composed of methyl (meth)acrylate (MMA) or the like can be used. However, it is preferred to use a hard contact lens material (RGP) with high oxygen permeability that can be obtained from a polymerizable composition such as a monomer system containing silicone, a monomer system containing fluorine, a styrene-based monomer, or the like.

[0151] In addition, as the molding material for soft lenses, various conventionally known soft contact lens materials can be used, for example, any of a hydrous soft contact lens material obtained from a polymerizable composition such as an alkyl (meth)acrylate, an alkyl (meth)acrylamide, N-methyllactam, etc. containing a hydroxyl group, a non-hydrous soft contact lens material obtained from a polymerizable composition composed of an alkyl (meth)acrylate, etc., a hydrous or non-hydrous soft contact lens material containing silicone obtained from a polymerizable composition composed of a silicone-containing monomer, a silicone-containing macromonomer, etc., and the like.

[0152] However, in this embodiment, it is preferable to use a monomer capable of controlling the curing process by polymerization as at least the first molding material 18. For example, when a polymerizable monomer is used as the first molding material 18 and a curing process by polymerization is performed by a known method, the curing process is preferably performed by thermal polymerization by heating, photopolymerization by irradiation with light such as ultraviolet rays, or a combination thereof.

[0153] The specific method varies depending on the polymerizable monomers used, the molding die materials, etc., but if it is a thermopolymerizable monomer, a thermopolymerization initiator (such as persulfate, peroxide, azo initiator, etc.) is used as needed, and it can be implemented by, for example, gradually raising the temperature from near room temperature and applying heat in the temperature range of 30°C to 120°C for several minutes or even hours. In addition, if it is a photopolymerizable monomer, a photopolymerization initiator (such as benzophenone-based, phosphine oxide-based, benzoin-based, thioxanthone-based, oxime-based photopolymerization initiator, etc.) is used as needed, and it can be implemented by irradiating active energy (electromagnetic waves) such as light and electron beams.

[0154] In addition, in the first molding cavity 16, the first molding material 18 is cured by polymerization at least on the surface of the side in contact with the cavity forming surface 34 of the component support molding die 14, and the polymerization molding of the primary molded product 20 in the closed mold state is completed, and the component support molding die 14 is separated from the first molding die 12 and the primary molded product 20 to open the mold. At the time of this mold opening, the curing treatment of the first molding material 18 is performed to the extent that the overall shape of the primary molded product 20 is maintained in a close contact state with the first molding die 12. In addition, in the primary molded product 20 after the mold opening, the curing treatment of the first molding material 18 is performed to the extent that the embedding member 36 can be maintained at a predetermined position. That is, in the primary molded product 20 after the mold opening, the embedding member 36 is maintained in a state of being embedded in the first molding material 18 (including a partial embedded state), and in the contact area where the embedding member 36 contacts the first molding material 18, the surface of the embedding member 36 is in a close contact state with the first molding material 18 without a gap.

[0155] The first molding material 18 is in a soft state where the curing is not completed at least on the surface of the side where the embedding member 36 is arranged, thereby avoiding (not producing) or suppressing (not completing) the shrinkage associated with the curing process of the first molding material 18. Therefore, at least in the vicinity of the embedding member 36, a large pressure reduction is avoided in the first molding cavity 16, and by removing the member support molding die 14 and opening the first molding cavity 16, the subsequent curing of the first molding material can be performed without the decompression of the primary molded product 20. As a result, the formation defects in the primary molded product 20, especially the formation of pores and a partially peeled film near the embedding member 36, which are considered to be caused by the decompression of the first molding cavity 16, can be suppressed.

[0156] In addition, the degree of incomplete curing of the first molding material 18 at the time when the component support molding die 14 is removed is sufficient to cure to the extent that the embedding member 36 can be held at the target position in the primary molded product material 18. The reason for this is that the dimensional accuracy of the molding of the first molding material 18 at this time is achieved by the molding of the second molding material 26 described later. The state of incomplete curing of the first molding material 18 can be understood as, for example, a state in which more residual monomers are present than in a state in which curing is completed, a state in which the degree of curing is less, or a state in which the curing process is completed earlier than the estimated curing completion time. As described above, the degree of incomplete curing of the first molding material 18 at the time when the component support molding die 14 is removed can be stopped at a degree in which the shrinkage of the first molding material 18 does not become a problem. For example, on the one hand, if the embedding member can be held at the target position according to the position and shape of the embedding member, the polymerization on the side of the component support molding die 14 may be almost not progressed. On the other hand, if the shrinkage accompanying the curing is greatly generated in the final stage of curing due to the material, the polymerization on the side of the component support molding die 14 may be greatly progressed. As can be judged from this, although it is only an example, the first forming material 18 at the moment when the component support forming mold 14 is removed preferably has a hardness value measured by the depth of indentation of the indenter in a durometer or a barometer (for example, ASTM_D_2240) relative to the hardness at which the curing reaction of the first forming material 18 is completed, and the area where the ratio of such hardness is less than 80% remains on at least a part of the surface on the side of the component support forming mold 14, and it is more preferred that the area where the ratio of such hardness is less than 50% remains on at least a part.

[0157] In this embodiment, it is preferred that the progress of polymerization of the first molding material 18 in the first molding cavity 16 is partially controlled. Specifically, the progress of polymerization of the first molding material 18 filled in the first molding cavity 16 is controlled so as to be slower on the cavity forming surface 34 side of the component support molding die 14 than in other parts. For example, in the case where the polymerization of the first molding material 18 is thermal polymerization, such control of the progress of polymerization can be performed by exposing the outer surface of the convex side of the first molding die 12 to a heat source and heating the first molding material 18 from the first molding die 12 side. In addition, for example, in the case where the polymerization of the first molding material 18 is photopolymerization, it can be performed by irradiating the first molding material 18 with active energy from the first molding die 12 side through the first molding die 12. Incidentally, thermal polymerization and photopolymerization can be achieved by an appropriate polymerization initiator. On the one hand, as a thermal polymerization initiator, persulfate, peroxide, azo-based initiator, etc. can be mentioned, and on the other hand, as a photopolymerization initiator, as mentioned above, for example, benzophenone-based and other photopolymerization initiators can be mentioned. Such a polymerization method and selection of an initiator can be appropriately selected in consideration of the polymerizable composition and mold material, and are not to be construed in a limiting sense.

[0158] Thus, the primary molded product 20 at the time of mold opening can be in a state where polymerization progresses the slowest on the component support mold 14 side and becomes soft, while polymerization progresses sufficiently on the first mold 12 side and curing is completed or substantially completed.

[0159] In addition, when opening the mold, in order to more securely embed and retain the embedding component 36 relative to the uncured primary molded product 20 on the side of the component support molding mold 14 and to better demold the component support molding mold 14 from the primary molded product 20, it is desirable to appropriately set the tightness (close fit) of the first molding material 18 relative to the embedding component 36 and / or the component support molding mold 14.

[0160] That is, in order to make the material of the component support forming mold 14 less closely attached to the first forming material 18 than the closely attached to the embedding member 36 to the first forming material 18, it is preferable to select and set the material of the component support forming mold 14 in consideration of the materials of the first forming material 18 and the embedding member 36. The degree of tightness (closeness) here is a relative comparison of the component support forming mold 14 and the first forming material 18 to the embedding member 36, and therefore, by performing comparative tests for the materials assumed to be used, confirmation can be made in a manner that does not require a lot of labor and time.

[0161] Thus, it is possible to effectively prevent the formation defects caused by partial peeling and roughness of the surface of the primary molded product 20 on the side of the component support mold 14 when the component support mold 14 is removed. In addition, for example, in the primary molded product 20, even if the curing treatment of the first molding material 18 is excessively performed when the component support mold 14 is released, and it is assumed that sink marks or the like are generated, the primary molded product 20 (the first molding material 18, the embedding member 36) can be actively separated from the cavity forming surface 34 of the component support mold 14 to reduce or even avoid the formation defects of the primary molded product 20.

[0162] As mentioned above, through Figure 1 After the primary molded product 20 is formed through the first molding step shown in the figure, the second molding step is then performed with the primary molded product 20 present. In the second molding step, as described above, Figure 2 (a)- Figure 2 As shown in (c), the second molding die 22 having a convex molding surface 30 for imparting a rear surface of the lens is closed against the first molding die 12 in which the primary molded product 20 is not demolded but remains in close contact with the concave molding surface 28, and the second molding material 26 is filled in the demarcated second molding cavity 24. The mold molding is performed by curing the second molding material 26 by, for example, irradiating heat rays, light, etc., thereby obtaining a contact lens 10 as an integral molded product in which an embedding member 36 is embedded by molding the molding material in multiple stages.

[0163] In addition, during the mold injection of the second molding material 26 in the second molding step, the curing of the first molding material 18 may be completed in the primary molded product 20, and the curing may not be completed if the predetermined positioning and holding accuracy can be achieved with respect to the embedding member 36. After the member support molding die 14 is removed from the primary molded product 20 in the first molding step, the curing of the first molding material 18 may be advanced or completed by irradiating the primary molded product 20 with energy such as heat rays or electromagnetic waves from the surface side where the embedding member 36 is provided, as required.

[0164] As with the first molding material 18, the second molding material 26 used in the second molding step can be any of various contact lens materials according to the characteristics required of the contact lens 10 as a product. For example, a known monomer can be used as a polymerizable composition for molding a contact lens. In addition, the first molding material 18 and the second molding material 26 can use the same monomer, thereby being highly or completely integrated, but the first molding material 18 and the second molding material 26 can also be different. For example, on the one hand, the first molding material 18 is emphasized on the close contact with the embedding member 36, and on the other hand, the second molding material 26 is emphasized on the tightness (lubricity, etc.) to the living body such as the cornea, and each molding material can be selected separately according to different required characteristics.

[0165] Furthermore, in this embodiment, the second molding material 26 forms the central portion 32 disposed on the optical path of the eye optical system in cooperation with the first molding material 18, and therefore, a material having transparency with respect to visible light is used. However, when the optical region of the central portion 32 disposed on the optical path of the eye optical system is formed by either the first molding material 18 or the second molding material 26, the other one may not be transparent, and the selection can be made based on biocompatibility in consideration of contact with the eyeball and the eyelid.

[0166] In addition, when the primary molded product 20 exists, the second molding cavity 24 defined by the mating surfaces between the first molding die 12 and the second molding die 22 is as follows: Figure 2 As shown in (b), it is expanded on at least the exposed portion of the embedding member 36 of the primary molded product 20, and is preferably expanded over the entire region covering the embedding member 36. In this embodiment, it is expanded in a manner that covers the entire rear surface (spherical crown concave surface) of the primary molded product 20.

[0167] In particular, in this embodiment, the outer peripheral end of the primary molded product 20 and the outer peripheral end of the second molding cavity 24 are expanded to the outermost edge of the contact lens 10. As a result, the entire contact lens 10 has a laminated composite structure in which the respective molded bodies of the first molding material 18 and the second molding material 26 are overlapped in the lens thickness direction.

[0168] In this way, the second molding material 26 is molded by partitioning the second molding cavity 24 on the rear surface side of the primary molded product 20, thereby covering the embedding member 36 embedded and inserted into at least the front side of the primary molded product 20 on the rear side with the second molding material 26. Therefore, in the molded product obtained by curing the second molding material 26, the embedding member 36 is completely embedded inside and is not exposed on the surface.

[0169] Thereafter, the molded product is demolded by opening the first molding die 12 and the second molding die 22 to obtain the target contact lens 10. After demolding, finishing treatments such as deburring, polishing, degreasing, cleaning, and sterilization may be performed as needed.

[0170] The contact lens 10 obtained as described above is as follows Figure 5 (a)- Figure 5 As shown in (d), the embedding member 36 is embedded in a predetermined position in an embedded state. In such a contact lens 10, the rear surface of the primary molded product 20 is covered and formed by the second molding material 26. Therefore, even if the member support molding die 14 is removed in an uncured state, and even if the rear surface of the primary molded product 20 has a shrinkage mark or a rough surface, which reduces the smoothness and precision, these problems can be eliminated by the molding process of the second molding material 26, and a good quality contact lens 10 can be obtained.

[0171] Furthermore, when the second molding material 26 is molded, it is desirable to fully cure it before demolding it, thereby making it possible to more highly secure the dimensional accuracy of the contact lens 10 as a molded product. In addition, when the curing treatment of the second molding material 26 is performed in the closed second molding cavity 24 of the first molding mold 12 and the second molding mold 22, it is easy to fully and well set the tightness between the first molding material 18 and the second molding material 26 by selecting each molding material. In addition, since the embedding member 36 is also already embedded in the first molding material 18 and the contact area with the second molding material 26 is also suppressed, even if the polymerization shrinkage of the second molding material 26 occurs, the generation of voids in the lens interior (between the primary molded product 20 and the second molding material 26) can be suppressed.

[0172] However, in consideration of the molding accuracy and molding stability of the second molding material 26, for example, the second molding die 22 is preferably made of a material that can suppress the tightness (adhesion) with the second molding material 26 to a low level. Thus, for example, when the second molding material 26 is molded, even if relatively large polymerization shrinkage occurs, molding defects such as voids and roughness of the molding surface can be more effectively suppressed.

[0173] In addition, when adjusting the close contact between the molding surfaces (cavity forming surfaces) 28, 30, 34 of the second molding die 22, the aforementioned first molding die 12, and the member support molding die 14 and the molding materials 18, 26, the close contact between the first molding material 18 and the second molding material 26 can be adjusted by, for example, selecting the material of the molding die. Specifically, for example, in the case of manufacturing a hydrous lens, a hydrophilic monomer is added to the polymerizable composition of the molding material. Therefore, by using a hydrophilic monomer such as polyamide as the material of the molding die, a high close contact between the cavity forming surface and the molding material can be achieved. On the other hand, by using a hydrophobic material such as polypropylene as the material of the molding die, the close contact between the cavity forming surface and the molding material can be set to be low.

[0174] In addition, for example, the cavity forming surfaces 28, 30, 34 of the forming mold may be subjected to a treatment for changing the characteristics related to the adhesion, and the adhesion with the forming materials 18, 26 may be increased or decreased by performing surface property adjustment treatments such as plasma treatment, UV irradiation, corona discharge, laser irradiation, and application of a surfactant. In addition, the adhesion with the forming materials 18, 26 may be adjusted by heating or cooling the first forming mold 12, the second forming mold 22, and the component support forming mold 14 to manage the temperature.

[0175] In addition, the contact lens 10 composed of an integrally formed product in which the embedding member 36 is embedded can provide a well-known soft contact lens, a hard contact lens, etc. that is worn overlapping on the cornea, but can also provide a scleral lens that is worn with the edge of the lens located on the sclera outside the cornea. For a scleral lens, the size of the area covering the sclera can be set arbitrarily. For example, in the case of covering the sclera in a large area, the peripheral shape of the lens edge can also be non-circular. For example, it is preferably a scleral lens that suppresses the movement on the eyeball in the wearing state to be small when it is desired to position the embedding member 36 on the eyeball with high precision in the wearing state.

[0176] However, for the contact lens 10 composed of an integrally molded product with an embedded member 36, the lens thickness is often large. In this case, it goes without saying that the contact lens is worn continuously for many days. Even if it is assumed that the contact lens is worn for a day from waking up to going to bed, it is expected that the contact lens has sufficient oxygen permeability.

[0177] Specifically, for example, in Figure 1-Figure 5In the above-described embodiment, when manufacturing the contact lens 10 as a scleral lens, the positioning accuracy of the embedding member 36 is ensured by using RGP (hard contact lens material with high oxygen permeability) as the first molding material 18, and a lens material with higher oxygen permeability such as a monomer such as (meth)acrylate containing silicone or a macromonomer containing silicone is preferably used as the second molding material 26. At this time, in particular, for the central portion 32 located on the cornea, the thickness of the lens formed by the second molding material 26 is made thicker than that of the first molding material 18, so that higher oxygen permeability can be given to the contact lens 10.

[0178] Considering the balance between high oxygen permeability and good wearing feeling, it is preferred Figure 6 In the following embodiments, descriptions of components, locations, and steps having the same structure as those of the first embodiment will be omitted.

[0179] In such a second embodiment, by using the same method as the first embodiment, Figure 1 (a)- Figure 1 The same process as (c) yields Figure 6 After the primary molded product 20 shown in (a), before the second molding material 26 is molded, as shown in Figure 6 As shown in (b) of FIG. 1 , an intermediate member 50 formed of a material different from the first and second molding materials 18 and 26 is provided with respect to the primary molded product 20 in close contact with the first molding die 12 .

[0180] In the present embodiment, on the one hand, hard lens materials are used as the first and second molding materials 18, 26, so as to achieve the position stability of the contact lens 10 in the wearing state and thus improve the positioning accuracy of the embedding member 36. It is preferable to use a hydrophilic high oxygen permeable material (RGP) as the first and second molding materials 18, 26. On the other hand, the intermediate member 50 is a lens component with higher oxygen permeability than the first and second molding materials 18, 26, and is formed of a silicone material containing monomers such as (meth) alkyl acrylate containing silicone, a macromonomer containing silicone, etc.

[0181] In addition, in this embodiment, the central convex portion 46 (see Figure 1 In (a) to (b), a central recess 52 is formed in the region where the optical portion is formed in the primary molded product 20. The intermediate member 50 is assembled while being inserted into the central recess 52.

[0182] Such an intermediate member 50 is assembled to the primary molded product 20, for example, Figure 7 (a)- Figure 7As shown in (b) of FIG. 1 , by die molding in the presence of the primary molded product 20, it is also possible to integrally mold the primary molded product 20. Specifically, Figure 7 As shown in (a) of FIG. 1 , after the primary molded product 20 is formed, the primary molded product 20 is not demolded but remains in a state of being closely attached to the first mold 12, and the above-mentioned highly oxygen-permeable intermediate molding material 49 containing silicone is injected into the first mold 12. Figure 7 As shown in (b), by closing the intermediate forming mold 54 to the first forming mold 12, the intermediate forming material is filled in the intermediate forming cavity demarcated on the rear surface side of the primary molded product 20 and a curing treatment is performed, thereby obtaining a primary molded product 20 in which the intermediate component 50 is integrally assembled in a tightly fitted state.

[0183] In addition, the cavity forming surface of the intermediate forming mold 54 (the forming surface of the intermediate member 50) protrudes as a whole toward the first forming mold 12 side than the cavity forming surface of the second forming mold 22 (the forming surface of the second forming material 26) used in the forming of the second forming material implemented in the subsequent process. As a result, the rear surface of the intermediate member 50 formed by the intermediate forming mold 54 is not given the rear surface of the contact lens 10, but the rear surface of the intermediate member 50 is substantially covered with the second forming material layer throughout the entirety by the forming of the second forming material implemented in the subsequent process. In addition, the material of the intermediate forming mold 54 is the same as that of other forming molds, and is not particularly limited, as long as it can be removed from the first forming mold 12 and opened while keeping the primary molded product 20 assembled with the intermediate member 50 remaining in the first forming mold 12 after the intermediate member 50 is formed.

[0184] Incidentally, as the intermediate member 50, Figure 8 As shown in the figure, it is also possible to adopt an intermediate member 50 that is separately formed using a predetermined forming die or by cutting from a block, etc. Such a separately formed intermediate member 50 is assembled to the central portion of the primary molded product 20 by being inserted into the central recess 52 of the primary molded product 20 to which the first forming die 12 remains in a close contact state.

[0185] After the intermediate member 50 is assembled as described above, Figure 6 (b)- Figure 6 As shown in (e) of the embodiment, the second molding material 26 is molded using the intermediate molding die 54. Such molding can be performed in the same manner as in the first embodiment. Figure 2 (a)- Figure 2In such molding, the primary molded product 20 including the embedding member 36 and the rear surface of the intermediate member 50 are entirely covered with the second molding material 26. Therefore, in the obtained contact lens 10, the embedding member 36 and the intermediate member 50 are both prevented from being exposed to the lens surface.

[0186] In addition, in the primary molded product 20 assembled with the intermediate member 50, if there are unevenness on the rear surface side, or there is a rough surface on the surface of the intermediate member 50, or there is a gap between the intermediate member 50 and the primary molded product 20, it can be corrected by filling the second molding material 26 on the rear surface side of the primary molded product 20 including the intermediate member 50 and performing mold molding, thereby avoiding adverse effects on the contact lens 10 as a product.

[0187] In the contact lens 10 thus obtained, the oxygen permeability at the central portion 32 can be improved, in particular, by the intermediate member 50 made of a silicone material sandwiched between the RGP materials in an embedded structure in the lens thickness direction. In particular, by making the thickness dimension of the intermediate member 50 larger than the thickness dimension of the RGP material on the front and rear surfaces of the lens, the oxygen permeability can be more effectively ensured.

[0188] Specifically, if the oxygen permeability of the common RGP material is taken into consideration, when the recommended level is met for the oxygen permeability (Dk value) for daily use, when the maximum lens thickness of the central portion 32 exceeds 0.7 mm, it becomes difficult to achieve a single-layer structure of the RGP material. Therefore, for the contact lens 10 with a maximum lens thickness of more than 0.7 mm in the central portion 32, it is more meaningful to adopt a laminated structure such as the present embodiment. In addition, it is more effective to suppress the total thickness of the RGP material in the central portion 32 to less than 0.7 mm, and it is expected that the lens thickness required for embedding the embedding member 36 can be actively ensured by the intermediate member 50.

[0189] In addition, in the peripheral portion 40 of the contact lens 10, especially the peripheral portion where the lens thickness decreases, there is almost no problem of oxygen permeability. Therefore, it can also be a single structure of RGP material composed of the first molding material 18 and / or the second molding material 26 in which the central portion 32 is not a sandwich structure.

[0190] In addition, in the contact lens 10 of the present embodiment, the front and rear surfaces of the intermediate member 50 made of a silicone material are covered with the surface film parts 48 and 55 made of an RGP material, so that the intermediate member 50 is prevented from directly contacting the biological surface (cornea, eyelid) when worn. Therefore, excellent oxygen permeability is achieved by the intermediate member 50, and the reduction of the wearing feeling caused by the waterproofness of the intermediate member 50, the adsorption property to the biological surface, etc. can also be avoided, and a good lens wearing feeling can be achieved based on the hydrophilicity of the RGP material and the lubricity between the lens and the biological body.

[0191] However, in the contact lens 10 such as a scleral lens, the following structure can also be adopted: in the wearing state, the peripheral portion 40 overlaps with the eyeball surface and the central portion 32 is supported, so that the rear surface of the central portion 32 is away from the eyeball and a tear layer is always formed, thereby stably avoiding the rear surface of the central portion 32 from directly contacting the eyeball. In this case, even if the rear surface of the lens of the central portion 32 is formed of a silicone material, etc., it will not directly cause a problem in the wearing feeling, so it is not a problem even if the rear surface of the intermediate member 50 is not partially or entirely covered by the second molding material 26 and is directly exposed on the rear surface of the lens.

[0192] Next, Fig. 9 , an example of another method of using an embedding member supported by a component support forming die and embedded in a primary molded product as a third embodiment of the present invention is shown. That is, in the above-mentioned first embodiment, the embedding member 36 is supported by mechanical engagement with the component support forming die 14, and the entire embedding member 36 is supported by the component support forming die 14 and embedded in the primary molded product to be integrally formed. In contrast, in this embodiment, the embedding member 58 is supported in a state of being attached to a smooth surface relative to the component support forming die 56, and a part of the embedding member 58 is supported by the component support forming die 14 and embedded in the primary molded product to be integrally formed, and then the entire embedding member 58 is completed after the primary molded product is formed.

[0193] In more detail, the component support forming die 56 of the present embodiment does not have a concavo-convex support portion for engaging the embedded component at the cavity forming surface 34, but has a smooth spherical shell convex cavity forming surface 34 as a whole without concavo-convex. In addition, such a cavity forming surface 34, when the mold is closed to the first forming die 12, protrudes toward the first forming die 12 side than the cavity forming surface of the second forming die 22 that divides the forming cavity of the second forming material 26 in the subsequent process, and is arranged close to the first forming die 12.

[0194] Moreover, at the cavity forming surface 34 of such a component support forming die 56, the embedding component 58 is directly formed on the cavity forming surface 34, thereby being supported in a tightly attached state to be fixed in position. In particular, in this embodiment, such an embedding component 58 includes a foil-like metal member 58a such as an antenna and a power supply wiring, and the foil-like metal member 58a is directly formed on the cavity forming surface 34 by a plating layer of a metal member.

[0195] Specifically, for example Fig.10 (a)- Fig.10 As shown in (b), when a foil-like metal part 58a is formed at the cavity forming surface 34 of the component support forming mold 56, the component support forming mold 56 is formed of a synthetic resin material such as polyamide and polypropylene. Therefore, first, a first plating layer 58a' is formed by a chemical plating method or a direct electroplating method. Then, the foil-like metal part 58a can be formed in a manner having a target thickness, size, and shape only by the first plating layer 58a'. However, if this is not the case, the target foil-like metal part 58a can be obtained by further forming a second plating layer 58a" in a stacked state relative to the first plating layer 58a'. In addition, the second plating layer 58a" is formed when the first plating layer 58a' exists on the cavity forming surface 34 of the component support forming mold 56, and therefore, it can be formed by a metal plating method.

[0196] In addition, when forming the first plating layer 58a', usually, first, the cavity forming surface 34 of the component support forming mold 56 is subjected to a preliminary treatment such as etching treatment using acid, alkali, etc. to roughen the surface, and then a catalyst treatment is performed on the plating target area of ​​the cavity forming surface 34. In such a catalyst treatment, a known chemical plating catalyst such as a palladium (Pd)-based catalyst or a Cu-based catalyst replacing Pd is attached to the cavity forming surface 34 of the component support forming mold 56. In addition, the attachment of the chemical plating catalyst can be performed by applying the catalyst to the cavity forming surface 34 by screen printing, pad printing, inkjet printing, etc. Then, after the catalyst treatment, the chemical plating treatment is performed, so that the first plating layer 58a' can be formed on the surface printed with the chemical plating catalyst.

[0197] In addition, the material of the first plating layer 58a' and the second plating layer 58a" can be appropriately selected from plating metals with a small ionization tendency. For example, in addition to nickel (Ni), copper (Cu), gold (Au), silver (Ag), etc., the second plating layer 58a" can also be made of iron (Fe) or the like, and a plurality of different metal layers can also be formed in a stacked state.

[0198] In particular, in this embodiment, Fig.10 (a)- Fig.10As shown in (b) of FIG. 5 , a catalyst for chemical plating is attached to the cavity forming surface 34 of the component support forming mold 56 by printing or the like, a first plating layer 58a′ is formed by chemical plating, and a second plating layer 58a″ is further formed by electroplating, thereby forming a foil-like metal member 58a. Then, as shown in FIG. Fig. 9 (a)- Fig. 9 As shown in (c) of the embodiment, such a component support forming mold 56 is molded together with the first forming mold 12 to mold the first forming material 18, thereby obtaining a primary formed product 20 in which the foil-like metal member 58a is embedded. In addition, when the first forming material 18 is formed, it is desirable to remove the component support forming mold 56 before the solidification of the first forming material 18 is completed to release the constraint on the surface of the first forming material 18, as in the first embodiment.

[0199] In the primary molded product 20 obtained in this way, the foil-like metal part 58a is embedded in a buried state, and in particular, the cavity forming surface 34 of the component support forming mold 56 becomes a smooth surface shape. Therefore, the rear surface of the primary molded product 20 after the component support forming mold 56 is removed can become that the surface of the foil-like metal part 58a is flush with the surface of the primary molded product 20 (a smooth and continuous surface connected without steps).

[0200] If the target embedding member is formed only by the foil-like metal member 58a, the primary molded product 20 may be formed immediately. Fig. 9 The second molding material 26 is formed as shown in (e), but in this embodiment, as shown in Fig. 9 As shown in (d), after the primary molded product 20 is formed, an embedded component 58b such as an electronic component is assembled. Such an embedded component 58b is installed, for example, in a manner of being mounted on a foil-like metal member 58a, and the embedded component 58b becomes conductive to the foil-like metal member 58a, and the embedded component 58b constitutes the embedded member 58 of this embodiment.

[0201] Such embedded component 58b can be fixed to foil-like metal member 58a in an electrically conductive state by welding such as brazing. In addition, the presence or absence of the residual electroless plating catalyst on the surface of primary molded product 20 does not hinder the installation of embedded component 58b to foil-like metal member 58a.

[0202] However, the embedded component 58b such as the electronic component described above can also be fixedly supported on the cavity forming surface 34 of the component support forming mold 56 as an embedded component, so that it can be included in the primary molded product 20 in an embedded state by mold forming of the first molding material 18. In this case, the embedded component 58b can also be fixedly connected to the foil-like metal member 58a by brazing or the like, or can be directly attached and supported on the cavity forming surface 34 of the component support forming mold 56.

[0203] Next, the embedding member 58 is formed by the plating treatment and the installation of the embedding component, and the primary molded product 20 is fixedly connected to the embedding member 58 in a partially embedded state. Fig. 9 (e)- Fig. 9 As shown in (f), similar to the first embodiment, the second molding material 26 is molded in the molding cavity defined by overlapping the second molding die 22 with the first molding die 12. After such molding, the mold is opened and demolded, so that Fig. 9 As shown in (g) of FIG. 1 , the contact lens 10 can be obtained as an integrally molded product in which the embedding member 58 is embedded.

[0204] In particular, in the present embodiment, the foil-like metal member 58a is exaggeratedly shown thicker than the actual thickness in the drawings for easy understanding, but the thickness of the foil-like metal member 58a formed by the plating layer is not large. In particular, when the embedding member 58 is formed only by the foil-like metal member 58a, the rear surface of the primary molded product 20 becomes flush, thereby suppressing the unevenness of the rear surface of the primary molded product 20. Therefore, it is also possible to effectively suppress the formation defects such as pores caused by the embedding member 36 when the second molding material 26 is molded.

[0205] Although several embodiments of the present invention have been described above, the present invention is not to be construed as being limited to these embodiments.

[0206] For example, in the above-mentioned embodiment, the following method is illustrated: when forming the primary molded product 20, in order to avoid poor forming conditions such as pores around the embedded component 36, the generation of a locally peeled film, etc., the component support molding mold 14 is removed before the first molding material 18 is completely solidified. However, in order to achieve such a purpose, a method different from the above-mentioned embodiment can be adopted, for example, which can reduce or even avoid cavity decompression caused by polymerization shrinkage of the first molding cavity 16 during the molding of the first molding material 18.

[0207] If a specific example is given, for example Fig.11As shown in the figure, as the member support forming die 14, a structure in which a flexible wall portion 62 as a flexible portion that is easily deformed is formed at a position of the support portion 38 of the embedding member 36 on the cavity forming surface 34. When the primary molded product 20 is formed using such a member support forming die 14, when the pressure of the first molding cavity 16 decreases due to polymerization shrinkage of the first molding material 18, the flexible wall portion 62 is deformed in a manner that bulges toward the inside of the cavity, thereby reducing or even eliminating the pressure decrease in the first molding cavity 16, and the primary molded product 20 in which the embedding member 36 is embedded is molded.

[0208] In addition, for example Fig.12 As shown in the figure, the following method may be adopted: in the component support forming mold 14 and / or the first forming mold 12, a cavity-outside receiving portion 66 for receiving an excess of the first forming material 18 is formed by communicating with the first forming cavity 16 through a communication path 64 when the mold is closed. If such a cavity-outside receiving portion 66 is adopted, when the polymerization of the first forming material 18 in the first forming cavity 16 is started, the first forming material 18 that becomes an excess after filling the first forming cavity 16 and is received in the cavity-outside receiving portion 66 is used as a riser, thereby reducing or even eliminating the pressure drop in the first forming cavity 16 caused by shrinkage etc. generated during the polymerization process. In addition, after molding (preferably after molding of the primary molded product or after molding of the contact lens), the excess portion of the solidified riser can be cut off and processed in the same manner as burrs etc.

[0209] Alternatively, the component support molding die 14 may have a structure in which the close contact of the cavity forming surface 34 with the first molding material 18 is sufficiently reduced by selecting a material, performing a surface treatment, etc. Specifically, for example, when a hydrophilic monomer is added to the first molding material 18, the component support molding die 14 made of a hydrophobic material is used, and in addition to smoothing the cavity forming surface 34, a surface treatment such as plasma treatment, UV irradiation, corona discharge, laser irradiation, and application of a surfactant is performed, thereby reducing the close contact with the first molding material 18 and the molded product.

[0210] In addition, when controlling the properties of the cavity forming surface 34 as described above, a substance with less polymerization shrinkage can be selected for the composition of the first molding material 18. For example, it is also preferable to add a non-reactive substance that does not participate in the polymerization to the polymerizable plastic used as the first molding material 18, thereby suppressing the pressure reduction generated by the first molding cavity 16 when the first molding material 18 is molded.

[0211] In addition, any combination of these methods (flexible wall portion 62, cavity outer receiving portion 66, control of the close contact of cavity forming surface 34 with respect to first molding material 18, etc.) and the method shown in the first embodiment (removal of component support molding die 14 before first molding material 18 is completely solidified) can also be adopted. Moreover, it is possible to select a method by considering the degree of pressure reduction generated in first molding cavity 16 when molding first molding material 18.

[0212] Furthermore, in the above embodiment, the first molding die 12 has a spherical crown concave molding surface for molding the front surface of the lens, and the member support molding die 14 supports the embedding member 36 on the substantially corresponding spherical crown convex cavity forming surface 34, but this is not limited thereto.

[0213] Specifically, if Fig.13 (a)- Fig.13 As in another embodiment shown in (f), as the first molding die 70, a structure having a spherical crown convex molding surface 72 for molding the rear surface of the lens is adopted, and as the component support molding die 74, a structure having a spherical crown concave molding surface 76 substantially corresponding to the molding surface 72 is adopted, and the embedding member 78 can be positioned and supported on the molding surface 76 to mold the first molding material 18. In such an embodiment, the basic process is the same as that of the first embodiment, and the component support molding die 74 is removed before the solidification of the first molding material 18 is completed. In addition, as the second molding die 80, a structure having a spherical crown concave molding surface 82 for molding the front surface of the lens is adopted, and the mold molding of the second molding material 26 is performed in the presence of an integral molded product 84 of the first molding material 18 in which the embedding member 78 is embedded between the mating surfaces of the first molding die 70 and the second molding die 80, so that the contact lens 10 can be obtained as a molded product in which the embedding member 78 is embedded in an embedded state, as in the above-mentioned embodiment.

[0214] Hereinafter, a specific example of die-forming the primary molded product 20 as an intermediate molded product when manufacturing the contact lens 10 according to the first embodiment described above will be given as a reference example.

[0215] In this embodiment, a forming mold made of synthetic resin is used as the first forming mold 12 and the component supporting forming mold 14, and the component supporting forming mold 14 for positioning and supporting the embedded component 36 is clamped relative to the first forming mold 12 injected with the first forming material 18 and the first forming material 18 is cured, thereby forming a primary molded product 20 embedded with the embedded component 36.

[0216] After a photopolymerizable composition monomer is used as the first molding material 18 and the first molding die 12 and the member-supporting molding die 14 are closed, the first molding material 18 is polymerized by irradiating light for polymerization.

[0217] In such a polymerization process by light irradiation, light irradiation is performed from the first mold 12 side, so that the first molding material 18 is polymerized first on the first mold 12 side and the polymerization of the first molding material 18 is advanced toward the component support mold 14 side.

[0218] Furthermore, at the time when the curing process of the first molding material 18 is fully progressed on the surface of the first molding die 12 side but the curing process is not completed on the surface of the component support molding die 14 side, the component support molding die 14 is removed. At this stage, the front surface side of the primary molding 20 is supported by being in close contact with the concave molding surface 28 of the first molding die 12. On the other hand, the rear surface side of the primary molding 20 is almost completely buried in the primary molding 20 and is held at a predetermined position, and the component support molding die 14 can be opened by separating from the embedding member 36, but the surface curing of the rear surface side of the primary molding 20 released from the component support molding die 14 is not completed and becomes almost gel-like.

[0219] Thereafter, the primary molded product 20 is completely cured while being kept in close contact with the first molding die 12 , thereby obtaining the primary molded product 20 after mold forming as an example.

[0220] The obtained primary molded product 20 is as follows Fig.14 Whether viewed from the front surface side (convex surface side) or the back surface side (concave surface side) of the lens, the lens is judged to be in a good molding state without defects such as pores.

[0221] On the other hand, when the first molding material 18 same as that in the above-mentioned embodiment is molded under the same conditions using the component support molding mold 14 and the first molding mold 12 which are positioned and supported with the embedded component 36 same as those in the above-mentioned embodiment, a polymerization treatment based on light irradiation is performed until the first molding material 18 is completely cured, and after the first molding material 18 is completely cured as a whole, the component support molding mold 14 is opened and demolded, thereby obtaining a primary molded product as a comparison example.

[0222] The obtained primary molded product is as follows Fig.15 In particular, when observed from the rear surface side (concave surface side) of the lens, many pore-like molding defects can be confirmed around the embedded embedding member 36, and film-like defective parts that are partially peeled off due to large pores are also confirmed.

[0223] In addition, Figure 4 In the embodiment shown, as a mechanism for positioning and supporting the embedded member 36 in the member support forming die 14, a concave support portion 38 provided in a manner for embedding the embedded member 36 and having stepped engaging portions 42 facing each other in the radial direction are exemplified, but the positioning and supporting mechanism for the embedded member 36 is not limited thereto. For example, Fig.16 As shown in the example, a radially extending support protrusion 90 is formed in the member support forming die 14, and the facing surfaces of the circumferentially facing support protrusions 90, 90 are used as engaging portions 42, 42, and the embedding member 36 is assembled in a manner of inserting the concave support portion 38 formed between the above-mentioned engaging portions 42, 42, and such an embedding member 36 is sandwiched in the circumferential direction between the opposing engaging portions 42, 42 for positioning and supporting. In addition, Fig.16 In, with Figure 4 The component support forming die 14 of the embodiment is also provided with a stepped engaging portion 42 extending in the circumferential direction, which can accurately position the supporting embedded component 36 in the radial direction, but it is not necessarily necessary to provide such a stepped engaging portion extending in the circumferential direction. Fig.16 In the figure, the support protrusions 90 extending in the radial direction are separated from each other in the circumferential direction and a total of four are provided, and a total of four support portions 38 are formed between the support protrusions 90 and 90 adjacent to each other in the circumferential direction, so that the embedded component 36 can be positioned and supported at any support portion 38.

[0224] In this way, there is no limitation on the specific shape, method, structure, etc. of the mechanism for positioning and supporting the embedded member 36 by engaging in the component support forming mold 14. For example, the outer periphery of the embedded member 36 may be positioned and supported by the steps all around or partially by providing steps around the supporting portion 38 so that the configuration portion of the embedded member 36 becomes concave. Alternatively, a convex portion such as a pin may be provided around the configuration portion of the embedded member 36 so that the outer peripheral surface of the embedded member 36 engages with the convex portion for positioning and supporting. In addition, in the case where the embedded member 36 has a hole or a protrusion, the embedded member 36 may be positioned and supported in the component support forming mold 14 by engaging the engaging protrusion protruding from the component support forming mold 14 with the hole, or engaging the protrusion with respect to the engaging hole provided in the component support forming mold 14.

[0225] Furthermore, although not listed one by one, the present invention can be implemented in a manner in which various changes, corrections, improvements, etc. are added based on the knowledge of those skilled in the art. Moreover, such implementation modes are of course included in the scope of the present invention as long as they do not depart from the gist of the present invention.

[0226] Industrial Applicability

[0227] The present invention relates to a contact lens having other components buried inside, such as a smart contact lens, and proposes a new manufacturing method and structure of a contact lens. The invention is applicable to industrial fields such as the manufacturing of contact lenses.

[0228] Description of Reference Numerals

[0229] 10...contact lens; 12...first forming die; 14...member support forming die; 16...first forming cavity; 18...first forming material; 20...primary forming product; 22...second forming die; 24...second forming cavity; 26...second forming material; 28...concave forming surface; 30...convex forming surface; 32...central portion; 34...cavity forming surface (member support forming die); 36...embedded member; 38...supporting portion; 40...peripheral portion; 42...engaging portion; 44...gap-shaped cavity; 46...central convex portion; 48...surface film portion; 50...intermediate member; 52...middle Central recess; 54...intermediate forming die; 55...surface film portion; 56...component supporting forming die; 58...embedded component; 58a...foil-like metal part; 58a′...first plating layer; 58a″...second plating layer; 58b...embedded component; 62...flexible wall portion; 64...connecting path; 66...outer cavity receiving portion; 70...first forming die; 72...forming surface; 74...component supporting forming die; 76...forming surface (component supporting forming die); 78...embedded component 80...second forming die; 82...forming surface (second forming die); 84...integrally formed product; 90...supporting protrusion.

Claims

1. A method for manufacturing a contact lens, It is characterized in that Including the following processes: The first molding cavity in which the embedding member is disposed is defined by closing the member-supporting molding die in which the embedding member is positioned and supported with respect to the first molding die for providing one of the front surface and the rear surface of the lens; When the primary molded product in which the embedding member is embedded is obtained by curing the first molding material filled in the first molding cavity, the primary molded product is left in the first molding die while the first molding material is in an uncured state on the side of the member supporting molding die, and the member supporting molding die is removed from the first molding die; A second molding cavity is defined by closing a second molding die for imparting the other of the front surface of the lens and the rear surface of the lens with respect to the first molding die in which the primary molding remains; as well as The second molding cavity is filled with a second molding material and solidified. Thus, the contact lens in which the embedding member is embedded is manufactured as an integrally molded product.

2. The method for producing a contact lens according to claim 1, It is characterized in that Before the curing process of the second molding material, the curing of the first molding material is completed.

3. A method for manufacturing a contact lens, It is characterized in that A first molding material is cured in a first molding cavity defined by closing a component-supporting molding mold relative to a first molding mold that provides one of the front surface and the rear surface of the lens, thereby forming a primary molded product in which an embedding component positioned and supported by the component-supporting molding mold is embedded, and after the component-supporting molding mold is removed from the first molding mold while leaving the primary molded product in the first molding mold, a second molding material is cured in a second molding cavity defined by closing a second molding mold that provides the other of the front surface and the rear surface of the lens with the first molding mold, thereby manufacturing a contact lens in which the embedding component is embedded as an integral molded product, As the component support forming die, the following structure is adopted: A support portion for positioning and supporting the embedding member is provided on the cavity forming surface of the first forming cavity, and A wall portion defining the first molding cavity includes a flexible portion that allows the first molding material to deform in response to shrinkage during polymerization molding.

4. A method for manufacturing a contact lens, It is characterized in that A first molding material is cured in a first molding cavity defined by closing a component-supporting molding mold relative to a first molding mold that provides one of the front surface and the rear surface of the lens, thereby forming a primary molded product in which an embedding component positioned and supported by the component-supporting molding mold is embedded, and after the component-supporting molding mold is removed from the first molding mold while leaving the primary molded product in the first molding mold, a second molding material is cured in a second molding cavity defined by closing a second molding mold that provides the other of the front surface and the rear surface of the lens with the first molding mold, thereby manufacturing a contact lens in which the embedding component is embedded as an integral molded product, As the member support molding die, a die made of a material having a lower adhesion to the first molding material than the adhesion of the embedding member to the first molding material is used.

5. The method for producing a contact lens according to any one of claims 1 to 4, It is characterized in that The first forming mold is a forming mold for the front surface of the lens, The second forming mold is a forming mold for the rear surface of the lens.

6. The method for producing a contact lens according to any one of claims 1 to 5, It is characterized in that The primary molded product is provided with a recessed portion opened toward the member support molding die at a central portion thereof, and the central portion of the primary molded product has a smaller thickness dimension.

7. The method for producing a contact lens according to any one of claims 1 to 6, It is characterized in that In the component support forming die, A concave and / or convex engaging portion is provided for positioning the embedding member.

8. The method for producing a contact lens according to claim 7, It is characterized in that When the primary molded product is molded in the first molding cavity, the first molding material is introduced between the component support molding die and the embedding component, and the first molding material is cured while the embedding component is covered by the first molding material.

9. The method for producing a contact lens according to any one of claims 1 to 8, It is characterized in that In the component support forming die, The embedding member is positioned and supported in an attached state.

10. The method for producing a contact lens according to claim 9, It is characterized in that The embedding member is directly formed on the surface of the member support molding die, and is thereby positioned and supported in an attached state.

11. The method for producing a contact lens according to any one of claims 1 to 10, It is characterized in that In the component support forming die, The embedding member is positioned and supported without the aid of an adhesive.

12. The method for producing a contact lens according to any one of claims 1 to 11, It is characterized in that In the component support forming die, The cavity forming surface of the first molding cavity is subjected to a surface treatment for improving mold release properties.

13. The method for producing a contact lens according to any one of claims 1 to 12, It is characterized in that The embedding member is a member that is harder than the lens component.

14. The method for producing a contact lens according to claim 13, It is characterized in that The embedded member is an electrical component including a metal portion.

15. The method for producing a contact lens according to any one of claims 1 to 13, It is characterized in that The first molding material and the second molding material are both polymerizable monomers that impart oxygen permeability to a hard lens.

16. The method for producing a contact lens according to any one of claims 1 to 15, It is characterized in that The first forming material is the same as the second forming material.

17. The method for producing a contact lens according to any one of claims 1 to 16, It is characterized in that When the primary molded product in which the embedding member is embedded is obtained by curing the first molding material filled in the first molding cavity, the first molding material is cured so as to be pushed from the first molding die side toward the member supporting molding die side.

18. The method for producing a contact lens according to any one of claims 1 to 17, It is characterized in that After the first molding material is molded and the component supporting molding die is removed from the first molding die, before the second molding die is closed relative to the first molding die, the intermediate molding product is assembled relative to the primary molding product, and the second molding material is solidified in the second molding cavity demarcated by closing the second molding die with the first molding die in which the primary molding product including the intermediate molding remains.

19. The method for producing a contact lens according to claim 18, It is characterized in that After the first molding material is molded and the component support molding die is removed from the first molding die, before the second molding die is closed relative to the first molding die, the auxiliary molding die is closed relative to the first molding die in which the primary molding product remains to define an intermediate molding cavity, the intermediate molding cavity is filled with a third molding material and cured, thereby molding the intermediate molding product in a state of being assembled to the primary molding product, The second molding material is cured in the second molding cavity defined by removing the auxiliary molding die from the first molding die and closing the second molding die with the first molding die in which the primary molding including the intermediate molding remains.

20. The method for producing a contact lens according to claim 18, It is characterized in that The intermediate molded product is formed independently of the primary molded product and is assembled to the primary molded product.

21. The method for producing a contact lens according to any one of claims 18 to 20, It is characterized in that The intermediate molded product is made of silicone material.

22. The method for producing a contact lens according to any one of claims 18 to 21, It is characterized in that A concave portion is formed in a central portion of the primary molded product, and the intermediate molded product is inserted into and assembled in the concave portion.

23. The method for producing a contact lens according to any one of claims 18 to 22, It is characterized in that The intermediate molded product is provided at the center portion of the lens, and the entire surface of the intermediate molded product on the front surface side of the lens is covered with a surface layer portion formed of the first molding material or the second molding material.

24. The method for producing a contact lens according to any one of claims 1 to 23, It is characterized in that The first molding die has a concave cavity forming surface that provides a molding surface for the front surface of the lens, and The second molding die has a convex cavity forming surface that provides a molding surface for the rear surface of the lens. The molds are clamped by overlapping the component supporting mold and the second mold with the first mold from above in a state where the first mold chair is opened vertically upward.

25. The method for producing a contact lens according to any one of claims 1 to 24, It is characterized in that Used to make scleral lenses.

26. A contact lens comprising an oxygen-permeable hard lens component, The embedding member is arranged inside the oxygen-permeable hard lens component in a fixed state. An intermediate member made of silicone material is disposed inside the central portion of the lens, and a front surface layer made of the oxygen-permeable hard lens component is provided on the front surface side of the lens of the intermediate member in a manner covering the entire surface, and At least on the central axis of the lens, the surface layer has a smaller thickness dimension than that of the intermediate member.

27. The contact lens according to claim 26, It is characterized in that A rear surface layer composed of the oxygen-permeable hard lens component is also provided on the rear surface side of the lens of the intermediate member so as to cover the entire surface, and The rear surface layer has a smaller thickness dimension than the intermediate member at least on the central axis of the lens.

28. The contact lens according to claim 26 or 27, It is characterized in that The lens peripheral portion is not provided with the intermediate member at least at the outer peripheral end, but is formed of the oxygen-permeable hard lens component.

29. The contact lens according to any one of claims 26 to 28, It is characterized in that At the position where the lens thickness is maximum, the maximum lens thickness is greater than 0.7 mm, and the total thickness of the surface layers composed of the oxygen-permeable hard lens components provided on both sides of the intermediate member in the lens thickness direction is 0.7 mm or less.

30. The contact lens according to any one of claims 26 to 29, It is characterized in that For scleral lenses.