Method for manufacturing laminate
By heating and pressurizing the insulating layer at high temperature, the bonding stability of electronic parts and circuit patterns and poor insulation layer are solved in the high temperature environment, and the electronic parts and circuit patterns are realized at high temperature. Stable bonding and stability of insulating layer.
Patent Information
- Application Number
- CN202380027414.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-22
- Filing Date
- 2023-03-07
- Publication Date
- 2024-11-08
AI Technical Summary
When using electronic parts with high heat generation in high temperature environments, it is difficult for the prior art to maintain stable bonding between the electronic parts and the circuit pattern, and the insulating layer may crack, peel or warp, resulting in poor bonding and abnormal parallelism problems .
By adopting a laminated body manufacturing method, an insulating layer in a semi-hardened state is provided on the base substrate and heated and pressurized at high temperature to transfer it to the surface of the base substrate, and then electronic parts are installed on the insulating layer and heated. and pressurize, so that the circuit pattern temporarily adheres to the insulating layer, and finally formally hardens the insulating layer to ensure stable bonding and insulating properties.
Even if electronic parts with high heat generation are used at high temperatures, the method can suppress adverse conditions in the insulating layer, maintain stable bonding between the electronic parts and the circuit pattern, and ensure insulating and parallelism of the insulating layer.
Smart Images

Figure CN118922922A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a laminated body. Background Art
[0002] A laminated body is known in which a circuit pattern is laminated on the surface side of an insulating layer and electronic components are mounted on the circuit pattern. In order to release the heat generated by the electronic components, a base substrate such as a heat sink or a heat sink is laminated on the back side of the insulating layer. Previously, solder was widely used as a bonding material for mounting electronic components on the circuit pattern.
[0003] In recent years, with the progress of high performance and miniaturization of electronic equipment, the heat generated by electronic parts has become increasingly larger. For example, semiconductor chips using SiC (silicon carbide) (as an example, SiC power elements) can conduct large currents, so sometimes they become high temperatures (for example, above 300°C) during operation. On the other hand, since the melting point of solder is relatively low, if solder is used as a bonding material for electronic parts that operate at such high temperatures, the solder will remelt when the semiconductor chip is operated, which may cause problems such as peeling of the semiconductor chip or short circuits in the circuit pattern.
[0004] As a technique for solving this problem, a method of using a paste containing metal nanoparticles such as Ag nanoparticles or Cu nanoparticles as a bonding material is known (for example, see Patent Document 1). In the method, after a conductive pattern (circuit pattern) is provided on an insulating substrate (insulating layer), a paste containing metal nanoparticles is interposed between the circuit pattern and the electronic component, and the electronic component is pressurized while being heated at a predetermined temperature, thereby sintering the metal nanoparticles and bonding the circuit pattern to the electronic component. According to this technique for sintering metal nanoparticles, higher heat resistance can be obtained compared to the case of using solder.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2008-10703 Summary of the invention
[0008] Problems to be solved by the invention
[0009] Furthermore, when the metal nanoparticles are sintered, the electronic components are pressurized at a high temperature and with a high load. That is, the insulating layer is also pressurized at a high temperature and with a high load, so it is possible that cracks will occur in the insulating layer, or the insulating layer will peel off. In addition, when a ceramic substrate is used as the insulating layer, in addition to the ceramic substrate being broken, the ceramic substrate may also be warped, resulting in poor bonding between the electronic components and the circuit pattern, or the electronic components may be broken. In addition, the warping of the ceramic substrate may cause abnormal parallelism or flatness of the installed electronic components, which may also cause defects in subsequent processes such as wire bonding.
[0010] In view of such conventional problems, an object of the present invention is to provide a method for producing a laminated body, wherein even when using an electronic component that generates a large amount of heat, stable bonding between the electronic component and the circuit pattern can be maintained and defects generated in the insulating layer can be suppressed.
[0011] Technical means of solving problems
[0012] The present invention is a method for manufacturing a laminated body, wherein the laminated body is sequentially laminated with a base substrate, an insulating layer, a circuit pattern, and an electronic component, the manufacturing method comprising: a step of providing the insulating layer on the surface side of the base substrate;
[0013] a step of providing the electronic component on the surface side of the circuit pattern; and a step of laminating the circuit pattern provided with the electronic component on the insulating layer provided on the base substrate.
[0014] The manufacturing method of the stacked body preferably comprises the step of placing the insulating layer in a semi-hardened state during the step of placing the insulating layer on the surface side of the base substrate, and placing the insulating layer in a fully hardened state during the step of stacking the insulating layer placed on the base substrate and the circuit pattern on which the electronic components are placed.
[0015] In addition, in the manufacturing method of the laminate, it is preferred that the step of providing the insulating layer on the surface side of the base substrate includes: a step of heating the resin composition applied to the base sheet to form the insulating layer in a semi-cured state on the base sheet; and a step of heating and pressurizing the insulating layer in a semi-cured state arranged on the base substrate, and then peeling off the base sheet to transfer the insulating layer in a semi-cured state to the surface side of the base substrate. The step of stacking the insulating layer provided on the base substrate and the circuit pattern provided with the electronic components includes: a step of arranging the circuit pattern provided with the electronic components on the semi-cured insulating layer transferred to the surface side of the base substrate and heating and pressurizing the circuit pattern so that the circuit pattern is temporarily attached to the insulating layer; and a step of heating and pressurizing the insulating layer to which the circuit pattern is temporarily attached so that the insulating layer becomes a formally cured state.
[0016] Furthermore, in the method for manufacturing the laminate, it is preferred that, in the step of transferring the semi-cured insulating layer to the front surface of the base substrate, the insulating layer is pressed at a temperature of 30° C. to 180° C. and a pressure of 1 MPa to 25 MPa.
[0017] In addition, the manufacturing method of the laminated body preferably comprises the following steps: in the process of temporarily attaching the circuit pattern to the insulating layer, the insulating layer and the circuit pattern are pressurized at a temperature of 30°C to 180°C with a pressure of 0.1MPa to 25MPa, so that the circuit pattern is temporarily bonded to the insulating layer; and further, the insulating layer and the circuit pattern are pressurized at a temperature of 130°C to 200°C with a pressure of 0.1MPa to 25MPa to temporarily harden the insulating layer; and in the process of bringing the insulating layer into a formally hardened state, the insulating layer is pressurized at a temperature of 150°C to 300°C with a pressure of 0MPa to 25MPa.
[0018] The insulating layer is preferably a cured film of a latent curing resin composition. An example of the latent curing resin composition is an epoxy resin composition containing an epoxy resin, an aromatic amine compound represented by the following general formula (1), a boron-phosphorus complex represented by the following general formula (2), and a phosphorus compound represented by the following general formula (3).
[0019] [Chemistry 1]
[0020]
[0021] In the general formula (1), R1 represents an alkyl group, m represents an integer greater than 2, and n represents an integer greater than 0, and m and n satisfy m+n≦6. When n is an integer greater than 2, a plurality of R1s may be the same or different.
[0022] [Chemistry 2]
[0023]
[0024] In the general formula (2), R2 and R3 each independently represent an alkyl group, r represents an integer of 0 to 5, and s represents an integer of 0 to 5. When r is an integer of 2 or more, a plurality of R2s may be the same or different from each other. When s is an integer of 2 or more, a plurality of R3s may be the same or different from each other.
[0025] [Chemistry 3]
[0026]
[0027] In the general formula (3), R4 represents an alkyl group or an alkoxy group, and t represents an integer of 0 to 5. When t is an integer of 2 or more, a plurality of R4 may be the same as or different from each other.
[0028] Effects of the Invention
[0029] According to the present invention, even when an electronic component that generates a large amount of heat is used, it is possible to suppress a defect from occurring in the insulating layer while maintaining stable bonding between the electronic component and the circuit pattern. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] [ Figure 1 ] is a diagram showing a stacked body manufactured by a stacked body manufacturing method according to one embodiment of the present invention.
[0031] [ Figure 2 ] is a diagram showing the first step to the second step of a method for manufacturing a laminate according to one embodiment of the present invention.
[0032] [ Figure 3 ] is a diagram showing the third step of the method for manufacturing a laminate according to one embodiment of the present invention.
[0033] [ Figure 4 ] is a diagram showing the fourth to sixth steps of a method for manufacturing a laminate according to one embodiment of the present invention. DETAILED DESCRIPTION
[0034] Hereinafter, a method for producing a laminated body according to an embodiment of the present invention will be described with reference to the accompanying drawings. In addition, the figures shown in the accompanying drawings are schematic diagrams, and the thickness or width of each part, the ratio of each part to each other, etc. may be different from the actual implementation.
[0035] Figure 1The diagram shows a laminate 1 manufactured by the manufacturing method of the present embodiment. The laminate 1 includes a heat sink 2, an insulating layer 3, a circuit pattern 4, an electronic component 5, and a bonding layer 6.
[0036] The heat sink 2 includes a plate-shaped base 2a and comb-shaped fins 2b protruding from the base 2a, and has the function of releasing the heat transferred to the base 2a from the fins 2b to the outside. The heat sink 2 is preferably formed of a raw material with high thermal conductivity, for example, preferably formed of a metal such as copper, aluminum, iron (either a single metal or an alloy).
[0037] The heat sink 2 is equivalent to the "base substrate" in this specification. In addition, the shape of the "base substrate" is not limited to the shape including the fin 2b shown in the figure, and it can also be a plate-shaped body formed only by the base 2a. In addition, the "base substrate" is not limited to being composed of a single component, and it can also be composed of a combination of multiple components. The "base substrate" may include a structure that further improves the effect of releasing heat to the outside, for example, it can also be a structure in which a heat conduction plate (vapor chamber) or a heat pipe (heat pipe) is buried in a metal plate.
[0038] The insulating layer 3 is formed of a material having insulating properties, and is provided so as to cover the surface of the base portion 2a in the heat sink 2. The insulating layer 3 may cover the entire surface of the base portion 2a, or may cover a portion of the surface.
[0039] As a raw material of the insulating layer 3, a resin composition containing a thermosetting resin can be cited as an example. Examples of the thermosetting resin include epoxy resins, phenol resins, melamine resins, urea resins, unsaturated polyester resins, alkyd resins, and cyanate resins. As the thermosetting resin, one type can be used alone, or two or more types can be used in combination.
[0040] As epoxy resins, all monomers, oligomers, and polymers having two or more epoxy groups in one molecule can be used regardless of their molecular weight and molecular structure. Specific examples of such epoxy resins include: bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol E epoxy resin, bisphenol S epoxy resin, hydrogenated bisphenol A epoxy resin, bisphenol M epoxy resin (4,4'-(1,3-phenylenediisopridiene) bisphenol epoxy resin), bisphenol P epoxy resin (4,4'-(1,4-phenylenediisopridiene) bisphenol epoxy resin), bisphenol Z epoxy resin (4,4'-(1,3-phenylenediisopridiene) bisphenol epoxy resin), Bisphenol-type epoxy resins such as hexyldiene bisphenol-type epoxy resins; phenol novolac-type epoxy resins, brominated phenol novolac-type epoxy resins, cresol novolac-type epoxy resins, tetraphenol ethane novolac-type epoxy resins, novolac-type epoxy resins with condensed ring aromatic hydrocarbon structures, etc.; biphenyl-type epoxy resins; aralkyl-type epoxy resins such as xylene-type epoxy resins and biphenyl aralkyl-type epoxy resins; naphthylene ether-type epoxy resins, naphthol-type epoxy resins, naphthalene-type epoxy resins, naphthyl diol-type epoxy resins Epoxy resins with naphthalene skeletons such as epoxy resins, difunctional to tetrafunctional epoxy-type naphthalene resins, binaphthyl-type epoxy resins, and naphthalene aralkyl-type epoxy resins; anthracene-type epoxy resins; phenoxy-type epoxy resins; dicyclopentadiene-type epoxy resins; norbornene-type epoxy resins; adamantane-type epoxy resins; fluorene-type epoxy resins, phosphorus-containing epoxy resins, alicyclic epoxy resins, aliphatic chain epoxy resins, bisphenol A novolac-type epoxy resins, dimethylphenol-type epoxy resins, trisphenol methane-type epoxy resins, trihydroxyphenyl methane-type epoxy resins, tetraphenol-based ethyl Alkane epoxy resin, heterocyclic epoxy resin such as triglycidyl isocyanurate; glycidylamines such as N,N,N',N'-tetraglycidyl meta-xylene diamine, N,N,N',N'-tetraglycidyl bisaminomethylcyclohexane, N,N-diglycidyl aniline, or copolymers of glycidyl (meth)acrylate and compounds having ethylenically unsaturated double bonds, epoxy resins having a butadiene structure, diglycidyl ethers of bisphenols, diglycidyl ethers of naphthalene diols, glycidyl ethers of phenols, etc. The resin composition of this embodiment may contain one or more selected from these as the epoxy resin.
[0041] In addition to the thermosetting resin, the resin composition may include a hardener, for example. The hardener is selected according to the type of the thermosetting resin, and is not particularly limited as long as it is a hardener that reacts with the thermosetting resin. For example, when an epoxy resin is used, an amine hardener, an imidazole hardener, a phenol hardener, etc. may be used as the hardener.
[0042] An example of the curing agent includes an aromatic amine compound represented by the following general formula (1).
[0043] [Chemistry 4]
[0044]
[0045] In the general formula (1), R1 represents an alkyl group, m represents an integer greater than 2, and n represents an integer greater than 0, and m and n satisfy m+n≦6. When n is an integer greater than 2, a plurality of R1s may be the same or different.
[0046] m, which indicates the number of substitutions of the amino group on the benzene ring, is 2 to 6, or 2 to 5, or 2 or 3, or 2. When m is 2, the arrangement of the two amino groups with respect to the benzene ring is preferably at the meta position or ortho position with respect to one of the amino groups.
[0047] R1 is an arbitrary substituent for the benzene ring. The number of carbon atoms of the alkyl group represented by R1 may be 1 to 4, or 1 or 2. Specific examples of the alkyl group include methyl, ethyl, propyl, and butyl. n, which represents the number of substitutions of R1 for the benzene ring, is 0 to 4, 0 to 3, or 1 to 3.
[0048] The aromatic amine compound represented by the general formula (1) has a small steric hindrance and is therefore excellent in the effect of improving curability, and can exhibit sufficient performance even in a short curing time.
[0049] The resin composition may contain a filler (inorganic filler). The filler is preferably a filler having excellent insulation and high thermal conductivity, and examples thereof include alumina, silica, aluminum nitride, boron nitride, silicon nitride, and magnesium oxide.
[0050] The resin composition may contain a hardening accelerator, a stabilizer, an ion scavenger, a solvent, etc. The resin composition may also contain a flexibility-imparting material.
[0051] An example of the hardening accelerator is a boron-phosphorus complex represented by the following general formula (2).
[0052] [Chemistry 5]
[0053]
[0054] In the general formula (2), R2 and R3 each independently represent an alkyl group, r represents an integer of 0 to 5, and s represents an integer of 0 to 5. When r is an integer of 2 or more, a plurality of R2s may be the same or different from each other. When s is an integer of 2 or more, a plurality of R3s may be the same or different from each other.
[0055] R2 and R3 are any substituents for the benzene ring. Specific examples of the alkyl group represented by R2 and R3 include a methyl group, an ethyl group, and the like.
[0056] r, which represents the number of substitutions of the benzene ring substituted by R2 for the P atom, is 0 to 5, 0 to 3, 0 to 2, or 0 or 1. When r is 1, the alkyl group represented by R2 may be arranged at any of the ortho, meta, or para positions relative to the P atom.
[0057] s, which represents the number of substitutions of the benzene ring substituted by R3 on the B atom, may be 0 to 5, may be 0 to 3, may be 0 to 2, or may be 0.
[0058] When the hardening accelerator contains the boron-phosphorus complex represented by the general formula (2), it is preferable to contain a phosphorus compound represented by the following general formula (3) as a stabilizer.
[0059] [Chemistry 6]
[0060]
[0061] In the general formula (3), R4 represents an alkyl group or an alkoxy group, and t represents an integer of 0 to 5. When t is an integer of 2 or more, a plurality of R4 may be the same as or different from each other.
[0062] R4 is an arbitrary substituent for the benzene ring. Specific examples of the alkyl group represented by R4 include methyl, ethyl, propyl, etc. Specific examples of the alkoxy group represented by R4 include methoxy, butoxy, etc.
[0063] As described later, the insulating layer 3 is preferably a cured film formed of a latent curing resin composition, which has a latent curing property that is difficult to cure near room temperature, but can be transferred to an object or temporarily attached when heated to a specified temperature. For example, in the case where the insulating layer 3 is a cured film of an epoxy resin composition containing an epoxy resin, an aromatic amine compound represented by the general formula (1), a boron-phosphorus complex represented by the general formula (2), and a phosphorus compound represented by the general formula (3), the latent curing property can be manifested. In addition, the latent curing resin composition is preferably a system that can be stored for a long time in a state where the epoxy resin and the hardener are mixed, and a curing reaction begins when a stimulus such as heat, light, pressure, and moisture is applied. In addition, the rise in the exothermic peak accompanying the curing reaction (curing start temperature) is preferably 40° C. or above as measured by differential scanning calorimetry. In addition, as a hardener for epoxy resins, or an additive between epoxy resins and hardeners, dicyandiamide, dihydrazide compounds, various amine adduct-based latent hardeners, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, onium salts (sulfonium salts, phosphonium salts), boron halide-amine complexes, vinyl ether block carboxylic acids, active esters of polycarboxylic acids, ketimine compounds, silanol group-containing polymers, and the like can be used.
[0064] t indicating the number of substitutions of R4 on the benzene ring may be 0 to 5, may be 0 to 4, may be 0 to 2, or may be 0.
[0065] The circuit pattern 4 is obtained by forming a predetermined pattern using a conductive raw material. Examples of such raw materials include copper or aluminum metal foil. The thickness of the metal foil is, for example, about 0.01 mm to 2.0 mm. Examples of methods for forming the predetermined pattern include a method of forming a mask pattern on the metal foil and removing the exposed portion of the metal foil by etching, or a method of stamping the metal foil using a mold.
[0066] The electronic component 5 is, for example, a semiconductor chip. The electronic component 5 used in the present embodiment is not limited, but the method for manufacturing a laminated body according to the present embodiment is particularly suitable for using a semiconductor chip (for example, a SiC power element) that reaches a high temperature during operation.
[0067] The bonding layer 6 has the function of electrically connecting the circuit pattern 4 and the electronic component 5 and fixing the electronic component 5 to the circuit pattern 4. The bonding layer 6 is appropriately selected in consideration of the raw material forming the circuit pattern 4 or the heat generated from the electronic component 5, the load on the environment, etc. As an example of the bonding layer 6, a solder layer (for example, a Sn-based solder layer or a Zn-Al-based solder layer) obtained by melting solder, or a sintered metal layer obtained by sintering metal nanoparticles (Ag nanoparticles, Cu nanoparticles, etc.) can be cited.
[0068] Next, refer to Figure 2 to Figure 4 A method for producing the laminate 1 will be described. Figure 2 1 is a diagram showing a first step and a second step in a method for producing a laminate 1. Figure 3 is a diagram showing the third process, Figure 4 : is a diagram showing the fourth step, the fifth step, and the sixth step. The first step is equivalent to the "step of heating the resin composition applied to the base sheet to form a semi-cured insulating layer on the base sheet" in this specification, and the second step is equivalent to the "step of heating and pressurizing the semi-cured insulating layer arranged on the base substrate, and then peeling off the base sheet to transfer the semi-cured insulating layer to the surface side of the base substrate" in this specification. In addition, the third step is equivalent to the "step of providing electronic components on the surface side of the circuit pattern" in this specification. Moreover, the fourth step and the fifth step are equivalent to the "step of arranging a circuit pattern with electronic components on the semi-cured insulating layer transferred to the surface side of the base substrate and heating and pressurizing the circuit pattern so that the circuit pattern is temporarily attached to the insulating layer" in this specification, and the sixth step is equivalent to the "step of heating and pressurizing the insulating layer to which the circuit pattern is temporarily attached so that the insulating layer is officially cured". In addition, in the following description, the first step, the second step, etc. are described in order, but the present invention is not limited to the case where it is implemented in the above order, and the order can be changed within the scope of each step, and each step can also be implemented simultaneously. The temperature, pressure, and time conditions described below are exemplified for the case where an epoxy resin (for example, bisphenol A epoxy resin) is used for the resin composition.
[0069] First, in the first step, a base sheet made of, for example, polyethyleneterephthalate (PET) is prepared, the resin composition is applied to the base sheet, and the base sheet and the resin composition are heated together to form a semi-hardened insulating layer 3 on the base sheet. In the first step, the base sheet and the resin composition are heated together at a temperature of 50°C to 200°C, and the heating time is set to 10 minutes to 200 minutes. In addition, the heating conditions in the first step are more preferably set to a temperature of 50°C to 180°C and a heating time of 10 minutes to 180 minutes, and more preferably set to a temperature of 50°C to 160°C and a heating time of 10 minutes to 160 minutes.
[0070] Then, in the second step, the semi-hardened insulating layer 3 formed on the base sheet is arranged on the Figure 2 The surface side of the heat sink 2 shown is heated and pressurized, and then the base sheet is peeled off, and the semi-cured insulating layer 3 is transferred to the surface side of the heat sink 2. The heating and pressurizing conditions in the second step are set to pressurize at a temperature of 30°C to 180°C with a pressure of 1MPa to 25MPa, and the pressurizing time is set to 10 seconds to 300 seconds. In addition, the heating and pressurizing conditions in the second step are more preferably set to heat at a temperature of 30°C to 160°C and pressurize at 3MPa to 25MPa, and the pressurizing time is set to 10 seconds to 240 seconds, and more preferably set to heat at a temperature of 30°C to 140°C and pressurize at 5MPa to 25MPa, and the pressurizing time is set to 10 seconds to 180 seconds.
[0071] In addition, as another method replacing the first step and the second step, the following method may be used: the resin composition is applied to the surface of the base 2a of the heat sink 2 by roller coating, rod coating or screen printing, and then heated and pressurized, thereby setting the semi-hardened insulating layer 3 on the surface of the base 2a.
[0072] When the insulating layer 3 is brought into a semi-hardened state, for example, when the resin composition is applied to the surface of the base 2a by a roller coating method, the resin composition is applied to the surface of the base 2a and heated. In the method, when an epoxy resin (for example, bisphenol A epoxy resin) is used as a thermosetting resin, for example, after the resin composition is applied, it is heated at a temperature of 80°C for 60 minutes, and then heated at a temperature of 90°C and pressurized at a pressure of 23 MPa.
[0073] exist Figure 3In the third step shown, the electronic component 5 is mounted on the surface side of the circuit pattern 4. When mounting the electronic component 5 on the circuit pattern 4, for example, solder paste is applied to a predetermined position in the circuit pattern 4, the electronic component 5 is arranged thereon, and the solder is heated at a predetermined temperature to melt the solder, thereby joining the two. Instead of the solder paste, a paste containing metal nanoparticles may be used. In the above case, a paste containing metal nanoparticles is applied to the circuit pattern 4, the electronic component 5 is arranged thereon, and the electronic component 5 is heated at a predetermined temperature while being pressurized, thereby sintering the metal nanoparticles and joining the circuit pattern 4 and the electronic component 5. When applying the solder paste or the paste containing metal nanoparticles, various methods represented by, for example, a roll coating method, a rod coating method, or a screen printing method can be used.
[0074] After the first to third steps are completed, Figure 4 The fourth to sixth steps are shown. In the fourth step, the insulating layer 3 in a semi-hardened state provided on the heat sink 2 is temporarily bonded to the circuit pattern 4 on which the electronic component 5 is mounted. In the fifth step, the insulating layer 3 temporarily bonded to the circuit pattern 4 is temporarily hardened, thereby temporarily attaching the circuit pattern 4 to the insulating layer 3. In the sixth step performed thereafter, the temporarily hardened insulating layer 3 is formally hardened. In addition, as an apparatus used when performing the fourth to sixth steps, any apparatus that can heat and pressurize at the same time may be used, and may be a hot press or an autoclave.
[0075] In the fourth step, the electronic component 5 and / or the circuit pattern 4 are heated at a temperature of 30°C to 180°C and pressurized at a pressure of 0.1MPa to 25MPa. The pressurization time is set to 10 seconds to 300 seconds. In addition, the temperature and pressure conditions in the fourth step are more preferably heated at a temperature of 30°C to 160°C and pressurized at a pressure of 0.1MPa to 20MPa, and the pressurization time is 10 seconds to 240 seconds, and more preferably heated at a temperature of 30°C to 140°C and pressurized at a pressure of 0.1MPa to 15MPa, and the pressurization time is 10 seconds to 180 seconds.
[0076] In the fifth step, the electronic component 5 and / or the circuit pattern 4 are heated at a temperature of 130°C to 200°C and pressurized at a pressure of 0.1MPa to 25MPa. The pressing time is set to 1 minute to 30 minutes. In addition, the temperature and pressure conditions in the fifth step are more preferably heated at a temperature of 130°C to 200°C and pressurized at a pressure of 0.1MPa to 20MPa, and the pressing time is 1 minute to 30 minutes, and more preferably heated at a temperature of 130°C to 200°C and pressurized at a pressure of 0.1MPa to 15MPa, and the pressing time is 1 minute to 30 minutes.
[0077] In the sixth step, the electronic component 5 and / or the circuit pattern 4 are heated at a temperature of 150°C to 300°C and pressurized at a pressure of 0MPa to 25MPa. The pressurization time is set to 30 minutes to 180 minutes. In addition, the temperature and pressure conditions in the sixth step are more preferably heated at a temperature of 150°C to 300°C and pressurized at a pressure of 0MPa to 20MPa, and the pressurization time is 30 minutes to 180 minutes, and more preferably heated at a temperature of 150°C to 300°C and pressurized at a pressure of 0MPa to 15MPa, and the pressurization time is 30 minutes to 180 minutes.
[0078] In addition, in the above pressure range, the pressure during pressurization is 0 MPa, which means a non-pressurized state. In addition, when the circuit pattern 4 is temporarily attached to the insulating layer 3, it can be implemented in one process instead of two processes, namely the fourth process and the fifth process, or it can be implemented in three or more processes. In addition, when the insulating layer 3 is formally hardened, it is not limited to the above one process, but it can be implemented in two or more processes.
[0079] In the method for manufacturing the laminated body 1, even when a paste containing metal nanoparticles is used when joining the circuit pattern 4 and the electronic component 5, the insulating layer 3 is not laminated with the circuit pattern 4 and the electronic component 5 in the process of sintering the metal nanoparticles. That is, the influence of the pressurization under a high load in a high temperature environment required for sintering the metal nanoparticles does not affect the insulating layer 3, so that the undesirable conditions such as the cracking of the insulating layer 3 that may have occurred before can be suppressed. In addition, when the circuit pattern 4 on which the electronic component 5 is mounted is laminated on the insulating layer 3 in a semi-hardened state, when the electronic component 5 is pressurized, the semi-hardened insulating layer 3 is not excessively crushed and can maintain a predetermined thickness, so the insulation of the insulating layer 3 can be stably ensured.
[0080] The following describes examples of the present invention, but the present invention is not limited to the examples.
[0081] <Example>
[0082] A resin composition was prepared as a raw material for the insulating layer 3. The resin composition used was prepared by mixing 100 parts by mass of a bisphenol A epoxy resin (trade name EXA-850CRP; manufactured by DIC Corporation) with 28 parts by mass of a hardener ("DETDA-80"; manufactured by Lonza Corporation), 0.9 parts by mass of a hardening accelerator ("TTP-S"; manufactured by Hokko Chemical Industry Co., Ltd.), 0.3 parts by mass of a stabilizer ("TPP"; manufactured by Hokko Chemical Industry Co., Ltd.), 24 parts by mass of a flexibility-imparting material, 3 parts by mass of an ion scavenger, and as A resin composition comprising 210 parts by mass of alumina (trade name AS40; manufactured by Showa Denko K.K.) as a filler, 339 parts by mass of boron nitride (BN) agglomerates (trade name HP40MF100; manufactured by Mizushima Iron & Steel Co., Ltd.), 60 parts by mass of boron nitride (BN) fine powder (trade name NX1; manufactured by Momentive Corporation), and 248 parts by mass of ethyl 3-ethoxypropionate (EEP) as a solvent.
[0083] Then, the resin composition is applied to a base sheet and heated, thereby forming a semi-hardened insulating layer 3 on the base sheet.
[0084] Then, the base sheet and the insulating layer 3 are placed on the heat sink 2 in such a direction that the surface of the heat sink 2 contacts the semi-cured insulating layer 3, and the heat sink 2 is pressed in a vacuum press at a temperature of 90° C. and a pressure of 23 MPa for 30 seconds. Thereafter, the base sheet is peeled off, thereby transferring the semi-cured insulating layer 3 to the heat sink 2.
[0085] Furthermore, the electronic component 5 is disposed on the circuit pattern 4 to which the paste containing metal nanoparticles is applied, and then the electronic component 5 is mounted on the circuit pattern 4 by heating it at a predetermined temperature while being pressurized.
[0086] Thereafter, the circuit pattern 4 with the electronic component 5 mounted thereon is arranged at a predetermined position of the semi-cured insulating layer 3. Then, the circuit pattern 4 is temporarily bonded to the insulating layer 3 by applying pressure at 75°C and 4 MPa for 40 seconds in a vacuum press.
[0087] Next, the vacuum press was placed in a vacuum exhaust state (open to the atmosphere), and pressurization was performed at a temperature of 180° C. and a pressure of 4 MPa for 780 seconds to temporarily cure the insulating layer 3 .
[0088] Then, the insulating layer 3 was fully cured by leaving it at a temperature of 185° C. and a pressure of 0 MPa (non-pressurized state) for 60 minutes.
[0089] The laminate 1 manufactured by the above method was checked and found that even when the electronic component 5 was operated at a high temperature, no cracks or peeling were found in the insulating layer 3. In addition, the parallelism and flatness of the electronic component 5 were normal.
[0090] Above, an embodiment of the present invention has been described, but the present invention is not limited to the specific embodiment, and various modifications and changes can be made within the scope of the gist of the present invention as described in the claims unless otherwise specified in the description. In addition, the effects in the embodiment are merely illustrative of the effects produced by the present invention, and are not intended to limit the effects brought about by the present invention to the effects described.
[0091] For example, the layer structure in the laminate 1 is not limited to the above-described embodiment, and other layers may be interposed between the layers. As an example of a change in the layer structure, an adhesive sheet may be interposed between the heat sink 2 and the insulating layer 3. In addition, a liquid adhesive may be applied to the surface of the insulating layer 3. In the case where pores are formed on the surface of the insulating layer 3, the pores are filled with the liquid adhesive by applying the liquid adhesive. That is, in the bonding between the insulating layer 3 and the object, the bonding function of the portion where the pores are formed can be compensated by the liquid adhesive. Moreover, the insulating layer 3 only needs to have insulating properties and is not limited to being formed by a resin composition. As an insulating layer 3 other than a resin composition, for example, a ceramic substrate may be cited.
[0092] Explanation of symbols
[0093] 1: Laminated body
[0094] 2: Heat sink (base substrate) 3: Insulation layer
[0095] 4: Circuit pattern 5: Electronic parts
Claims
1. A method for manufacturing a laminate, wherein a base substrate, an insulating layer, a circuit pattern, and an electronic component are sequentially stacked, the method comprising: A step of providing the insulating layer on the surface side of the base substrate; a step of providing the electronic component on the surface side of the circuit pattern; as well as A step of laminating the insulating layer provided on the base substrate and the circuit pattern provided with the electronic component.
2. The method for manufacturing a laminate according to claim 1, wherein in the step of providing the insulating layer on the surface side of the base substrate, the insulating layer is brought into a semi-hardened state, In the step of laminating the insulating layer provided on the base substrate and the circuit pattern provided with the electronic component, the insulating layer is brought into a fully cured state.
3. The method for manufacturing a laminate according to claim 2, wherein the step of providing the insulating layer on the surface side of the base substrate comprises: The step of heating the resin composition applied to the base sheet to form the insulating layer in a semi-hardened state on the base sheet; as well as The insulating layer in a semi-cured state disposed on the base substrate is heated and pressurized, and then the base sheet is peeled off to transfer the insulating layer in a semi-cured state to the front surface side of the base substrate. The step of laminating the insulating layer provided on the base substrate and the circuit pattern provided with the electronic component includes: A step of arranging the circuit pattern having the electronic component on the semi-cured insulating layer transferred to the surface side of the base substrate and applying heat and pressure to temporarily adhere the circuit pattern to the insulating layer; and The step of heating and pressurizing the insulating layer to which the circuit pattern is temporarily attached to put the insulating layer into a fully cured state. 4 . The method for manufacturing a laminate according to claim 3 , wherein in the step of transferring the semi-cured insulating layer to the front surface of the base substrate, the insulating layer is pressurized at a temperature of 30° C. to 180° C. and a pressure of 1 MPa to 25 MPa.
5. The method for manufacturing a laminate according to claim 3 or 4, wherein in the step of temporarily attaching the circuit pattern to the insulating layer, the insulating layer and the circuit pattern are pressurized at a temperature of 30° C. to 180° C. with a pressure of 0.1 MPa to 25 MPa, so that the circuit pattern is temporarily attached to the insulating layer, and further the insulating layer and the circuit pattern are pressurized at a temperature of 130° C. to 200° C. with a pressure of 0.1 MPa to 25 MPa to temporarily harden the insulating layer, In the step of bringing the insulating layer into a fully cured state, the insulating layer is pressurized at a temperature of 150° C. to 300° C. and a pressure of 0 MPa to 25 MPa. 6 . The method for producing a laminated body according to claim 1 , wherein the insulating layer is a cured film of a latent curing resin composition.