Optical glass and optical element

By using oxidizing gases to contact specific oxides during the optical glass manufacturing process, the problem of noble metal oxides dissolving into molten glass has been solved, resulting in optical glass with high refractive index and high transmittance, thus improving the homogeneity and transmittance of the glass.

CN118930040APending Publication Date: 2024-11-12OHARA INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410579302.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-05-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the manufacture of high-refractive-index optical glass, the dissolution of precious metal oxides into the molten glass leads to a decrease in transmittance and a deterioration in glass quality. At the same time, the bubbling of oxidizing gases causes the precious metal materials to be oxidized, which is the cause of coloration and affects the homogeneity and transmittance of the glass.

Method used

By bringing oxidizing gases into contact with the surface of molten glass containing specified amounts of Ln2O3, TiO2, Nb2O5, WO3, Bi2O3, etc., the reduction color is reduced, and an oxidizing atmosphere is used in the clarification, homogenization, and forming processes to prevent the dissolution of precious metal oxides.

Benefits of technology

This technology achieves high transmittance and homogeneity in high-refractive-index optical glass, reduces reduced color, slows down the deterioration of the molten bath, and improves the quality of the glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930040A_ABST
    Figure CN118930040A_ABST
Patent Text Reader

Abstract

The invention discloses optical glass and an optical element. The invention provides optical glass which is high in quality, excellent in transmittance and high in refractive index. An optical glass containing: an Ln2O3 component having a total content of 10.0% by mass or more (in the formula, Ln represents at least one selected from the group consisting of La, Gd, Y, and Yb); and at least one component selected from the group consisting of a TiO2 component, an Nb2O5 component, a WO3 component, and a Bi2O3 component. The optical glass is obtained by bringing an oxidizing gas into contact with the surface of a molten glass containing the aforementioned components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to optical glass and an optical element composed of the optical glass. Background Art

[0002] As optical devices and the like become more advanced in performance and functionality, the requirements for optical lenses used in these optical devices are also increasing. Specifically, optical glasses having high homogeneity inside the glass, extremely high transmittance, and satisfying optical properties such as refractive index and Abbe number are required.

[0003] Optical glass with high refractive index usually contains a large amount of TiO 2 , Nb 2 O 5 , WO 3 、Bi 2 O 3 As glass components, there are high refractive index components such as 2-H2O, 2-H2O, 2-H2O, etc. These components are easily reduced during the melting process of glass, and there is a problem that the glass is colored by these reduced components. Therefore, various technologies for reducing the reduced color in optical glass have been proposed.

[0004] For example, Japanese Patent Application Laid-Open No. 2002-12852 proposes to suppress the reduction of high refractive index components by bubbling an oxidizing gas in molten glass, thereby reducing the coloring of glass in the melting process. Summary of the invention

[0005] However, when such a technique is used to manufacture optical glass, the problem of the noble metal material constituting the melting tank dissolving into the molten glass becomes significant. That is, when manufacturing a glass with extremely high transmittance and homogeneity such as optical glass, a melting tank whose container surface is made of noble metal materials such as platinum is used to melt the glass raw materials. As a result, the noble metal sometimes reacts with oxygen to generate PtO. 2 If such noble metal oxides are dissolved in molten glass, the glass quality will be reduced, such as the transmittance will be reduced and bumps will be generated, which will accelerate the degradation of the melting tank. In addition, when melting a large amount of glass containing high refractive index components, the noble metal material will be oxidized by bubbling oxidizing gas, and Pt 4+ Noble metal ions such as MgO are dissolved in molten glass, and these noble metal ions also cause coloration.

[0006] Therefore, an object of the present invention is to provide a high-quality, high-refractive-index optical glass having an excellent transmittance.

[0007] The present inventors have found that by mixing an oxidizing gas with a predetermined amount of Ln 2 O 3 component (wherein Ln represents at least one selected from the group consisting of La, Gd, Y and Yb) and TiO2 Ingredients, Nb 2 O 5 Ingredients,WO 3 Composition and Bi 2 O 3 By bringing the surfaces of molten glasses of at least one glass selected from the group of components into contact with each other, an optical glass having reduced reduction color can be obtained.

[0008] That is, the gist of the present invention is as follows.

[0009] [1] An optical glass comprising: Ln in a total content of 10.0% or more by mass 2 O 3 component (wherein Ln represents at least one selected from the group consisting of La, Gd, Y, and Yb); and TiO 2 Ingredients, Nb 2 O 5 Ingredients,WO 3 Composition and Bi 2 O 3 The optical glass comprises at least one of the group consisting of components, wherein the optical glass is obtained by bringing an oxidizing gas into contact with a surface of a molten glass containing the components.

[0010] [2] An optical element comprising the optical glass described in [1].

[0011] According to the present invention, by mixing an oxidizing gas with a predetermined amount of Ln 2 O 3 component (wherein Ln represents at least one selected from the group consisting of La, Gd, Y, and Yb) and TiO 2 Ingredients, Nb 2 O 5 Ingredients,WO 3 Composition and Bi 2 O 3 The surfaces of molten glasses of at least one component in the group of components are brought into contact with each other, and an optical glass having reduced reduction color can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 This is a schematic cross-sectional view of one embodiment of an apparatus used in the method for producing the optical glass of the present invention.

[0013] Figure 2 This is a schematic cross-sectional view of another embodiment of the apparatus used in the method for producing the optical glass of the present invention.

[0014] Figure 3 This is a schematic cross-sectional view of another embodiment of the apparatus used in the method for producing the optical glass of the present invention. DETAILED DESCRIPTION

[0015] [Glass composition]

[0016] In this specification, unless otherwise specified, the content of each component constituting the optical glass is expressed in mass % relative to the total mass of the oxide conversion composition. Here, the "oxide conversion composition" is the composition of each component contained in the glass, assuming that when the oxides, complex salts, metal fluorides, etc. used as raw materials for glass components are melted, they are all decomposed and changed into oxides, and the total mass number of the generated oxides is set to 100 mass %. The composition range of each component constituting the optical glass of the present invention is described below.

[0017] The optical glass of the present invention contains Ln in a total content of 10.0% or more. 2 O 3 Here, Ln represents one or more selected from the group consisting of La, Gd, Y, and Yb. The optical glass of the present invention contains the above-mentioned components in a total content of 10.0% or more.

[0018] Ln 2 O 3 The component (wherein Ln is selected from one or more of the group consisting of La, Y, Gd, and Yb) can increase the refractive index of the glass, but when contained in excessive amounts, the devitrification of the glass will increase. 2 O 3 The lower limit of the sum of the contents of the components is preferably 35.0% or more, more preferably 40.0% or more, further preferably 45.0% or more, and further preferably 50.0% or more. 2 O 3 The upper limit of the sum of the contents of the components is preferably 70.0% or less, more preferably 65.0% or less, further preferably 60.0% or less, and further preferably 55.0% or less.

[0019] Ln is La 2 O 3 The component is a component that increases the refractive index of the glass and improves the chemical durability of the glass, and is an essential component in the optical glass of the present invention. 2 O 3 The content of the component is 65.0% or less, which can improve the devitrification resistance of the glass and increase the Abbe number. 2 O 3 The upper limit of the content of the component relative to the total mass of the glass in terms of oxide conversion composition is preferably 65.0% or less, more preferably 62.0% or less, and most preferably 59.0% or less. 2 O 3The lower limit of the content of the component relative to the total mass of the glass in terms of oxide conversion composition is preferably 30.0% or more, more preferably 35.0% or more, and most preferably 40.0% or more.

[0020] Ln is Gd 2 O 3 The component is a component that increases the refractive index of the glass and the Abbe number when the content exceeds 0%. In particular, by making Gd 2 O 3 The content of the component is 20.0% or less, and the desired optical data can be obtained while improving the devitrification resistance of the glass. 2 O 3 The upper limit of the content of the component relative to the total mass of the glass in terms of oxide conversion composition is preferably 20.0% or less, more preferably 15.0% or less, more preferably 10.0% or less, more preferably 5.0% or less, and most preferably 3.0% or less.

[0021] Ln is Y 2 O 3 The component is a component that increases the refractive index of the glass and the Abbe number when the content exceeds 0%. 2 O 3 The content of the component is 15.0% or less, and the desired optical values ​​can be obtained while improving the devitrification resistance of the glass. 2 O 3 The upper limit of the content of the component relative to the total mass of the glass in terms of oxide composition is preferably 15.0% or less, more preferably 12.0% or less, and most preferably 11.0% or less. 2 O 3 The lower limit of the content of the component relative to the total mass of the glass in terms of oxide conversion composition is preferably more than 0%, more preferably 3.0% or more, and most preferably 5.0% or more.

[0022] Ln is Yb 2 O 3 The component is a component that increases the refractive index of the glass and the Abbe number when the content exceeds 0%. In particular, by making Yb 2 O 3 The content of the component is 5.0% or less, and the desired optical values ​​can be obtained while improving the devitrification resistance of the glass. 2 O 3 The upper limit of the content of the component with respect to the total mass of the glass in terms of oxide conversion composition is preferably 5.0% or less, more preferably 3.0% or less, and most preferably 1.0% or less.

[0023] The optical glass of the present invention comprises TiO 2 Ingredients, Nb2 O 5 Ingredients,WO 3 Composition and Bi 2 O 3 At least one of the components in the group can improve the refractive index and dispersion. In particular, by making the mass and TiO 2 +Nb 2 O 5 +WO 3 +Bi 2 O 3 5.0% or more and 35.0% or less, it is possible to increase the refractive index (n d ) while reducing the reduction color from the high refractive index component. Therefore, the quality and TiO 2 +Nb 2 O 5 +WO 3 The lower limit of is preferably 5.0% or more, more preferably 7.0% or more, more preferably 12.0% or more, more preferably 15.5% or more, and further preferably 20.0% or more.

[0024] On the other hand, the quality and TiO 2 +Nb 2 O 5 +WO 3 The upper limit of is preferably 35.0% or less, more preferably 30.0% or less, and further preferably 27.0% or less.

[0025] TiO 2 The component is a component that increases the refractive index of the glass and improves the chemical durability of the glass when the content exceeds 0%. In particular, by containing TiO 2 On the other hand, by making TiO 2 The content of the component is 25.0% or less, which can suppress devitrification caused by excessive content and suppress deterioration of transmittance. 2 The lower limit of the content of the component relative to the total mass of the glass in terms of oxide conversion composition is preferably more than 0%, more preferably 3.0% or more, and most preferably 6.0% or more. 2 The upper limit of the content of the component with respect to the total mass of the glass in terms of oxide conversion composition is preferably 25.0% or less, more preferably 20.0% or less, and most preferably 15.0% or less.

[0026] Nb 2 O 5 The component is a component that increases the refractive index and Abbe number of the glass when the content exceeds 0%. On the other hand, by making Nb 2 O 5The content of Nb is 15.0% or less, which can improve the stability of the glass and improve the resistance to devitrification. 2 O 5 The upper limit of the content of the component with respect to the total mass of the glass in terms of oxide conversion composition is preferably 15.0% or less, more preferably 13.0% or less, and most preferably 11.0% or less.

[0027] WO 3 The component is a component that increases the refractive index of the glass when the content exceeds 0%. 3 The content of the component is 15.0% or less, which can improve the devitrification resistance of the glass and suppress the decrease in the transmittance of the glass to short-wavelength visible light. 3 The upper limit of the content of the component with respect to the total mass of the glass in terms of the oxide conversion composition is preferably 15.0% or less, more preferably 10.0% or less, and most preferably 5.0% or less.

[0028] B 2 O 3 The components are components that improve the resistance to devitrification by promoting the formation of stable glass. In particular, by making B 2 O 3 The content of the ingredient is less than 25.0%, which can inhibit the 2 O 3 The refractive index is reduced by the component, so a high refractive index can be easily obtained. 2 O 3 The upper limit of the content of the component relative to the total mass of the glass in terms of oxide conversion composition is preferably 25.0% or less, more preferably 20.0% or less, and still more preferably 15.0% or less. 2 O 3 The lower limit of the content of the component relative to the total mass of the glass in terms of oxide conversion composition is preferably 3.0% or more, more preferably 4.0% or more, and most preferably 5.0% or more.

[0029] SiO 2 The component is an arbitrary component in the optical glass of the present invention. When the content exceeds 0%, the transmittance of short-wavelength visible light is increased by reducing the coloring of the glass, and the devitrification resistance of the glass is improved by promoting stable glass formation. In particular, by making SiO 2 The content of the component is less than 20.0%, which can inhibit the formation of 2 The refractive index is reduced due to the component, so a high refractive index can be easily obtained. 2The upper limit of the content of the component relative to the total mass of the glass in terms of oxide conversion composition is preferably 20.0% or less, more preferably 15.0% or less, more preferably 12.0% or less, and most preferably 9.0% or less. 2 The lower limit of the content of the component relative to the total mass of the glass in terms of oxide conversion composition is preferably more than 0%, more preferably 1.0% or more, and most preferably 2.0% or more.

[0030] Al 2 O 3 The component is an arbitrary component in the optical glass of the present invention. When the content exceeds 0%, the chemical durability of the glass is improved and the viscosity of the glass when it is melted is increased. In particular, by making Al 2 O 3 The content of Al is 10.0% or less, which can improve the melting property of the glass and reduce the tendency of the glass to lose clarity. 2 O 3 The upper limit of the content of the component with respect to the total mass of the glass in terms of oxide conversion composition is preferably 10.0% or less, more preferably 5.0% or less, and most preferably 3.0% or less.

[0031] ZrO 2 The component is an arbitrary component in the optical glass of the present invention. When the content exceeds 0%, the coloring of the glass is reduced to increase the transmittance of short-wavelength visible light, and stable glass formation is promoted to increase the resistance to devitrification of the glass. 2 The content of the component is 15.0% or less, which can reduce the ZrO 2 Excessive amounts of ZrO lead to devitrification. 2 The upper limit of the content of the component relative to the total mass of the glass in terms of oxide composition is preferably 15.0% or less, more preferably 12.0% or less, and most preferably 9.0% or less. 2 The lower limit of the content of the component relative to the total mass of the glass in terms of oxide conversion composition is preferably more than 0%, more preferably 1.0% or more, and most preferably 3.0% or more.

[0032] The ZnO component is an arbitrary component in the optical glass of the present invention. When the content exceeds 0%, the liquidus temperature of the glass is lowered and the devitrification resistance of the glass is improved. In particular, by making the content of the ZnO component less than 15.0%, a high refractive index and low dispersion can be easily obtained. Therefore, the upper limit of the content of the ZnO component relative to the total mass of the glass in terms of oxide conversion composition is preferably less than 15.0%, more preferably less than 12.0%, and most preferably less than 9.0%.

[0033] MgO is an optional component in the optical glass of the present invention. When the content exceeds 0%, the liquidus temperature of the glass is lowered, the devitrification resistance of the glass is improved, and the transmittance to visible light is not easily reduced. In particular, by making the content of the MgO component 10.0% or less, a high refractive index and low dispersion can be easily obtained. Therefore, the upper limit of the content of the MgO component relative to the total mass of the glass in terms of oxide conversion composition is preferably 10.0% or less, more preferably 5.0% or less, and most preferably 3.0% or less.

[0034] The CaO component is an arbitrary component in the optical glass of the present invention. When the content exceeds 0%, it is a component that lowers the liquidus temperature of the glass and improves the resistance to devitrification of the glass. In particular, by making the content of the CaO component 10.0% or less, a high refractive index and low dispersion can be easily obtained, and the resistance to devitrification and chemical durability of the glass can be suppressed. Therefore, the upper limit of the content of the CaO component relative to the total mass of the glass in terms of oxide conversion composition is preferably 10.0% or less, more preferably 5.0% or less, and most preferably 3.0% or less.

[0035] The SrO component is an arbitrary component in the optical glass of the present invention. When the content exceeds 0%, it is a component that lowers the liquidus temperature of the glass and improves the devitrification resistance of the glass. In particular, by making the content of the SrO component 10.0% or less, a high refractive index and low dispersion can be easily obtained, and the devitrification resistance and chemical durability of the glass can be suppressed. Therefore, the upper limit of the content of the SrO component relative to the total mass of the glass in terms of oxide conversion composition is preferably 10.0% or less, more preferably 5.0% or less, and most preferably 3.0% or less.

[0036] BaO is an arbitrary component in the optical glass of the present invention. When the content exceeds 0%, it is a component that increases the refractive index of the glass, increases the resistance to devitrification of the glass, and is not easy to reduce the transmittance to visible light. In particular, by making the content of the BaO component 10.0% or less, it is easy to obtain a high refractive index and low dispersion, and it is possible to suppress the reduction of the resistance to devitrification and chemical durability. Therefore, the upper limit of the content of the BaO component relative to the total mass of the glass in terms of oxide conversion composition is preferably 10.0% or less, more preferably 5.0% or less, and most preferably 3.0% or less.

[0037] Li 2 The O component is an optional component in the optical glass of the present invention, and when the content exceeds 0%, it is a component that lowers the melting temperature of the glass. 2 When the content of O is 10.0% or less, a high refractive index can be easily obtained, and the stability of the glass can be improved, and the occurrence of devitrification can be reduced. 2The upper limit of the content of the O component with respect to the glass total mass of the oxide conversion composition is preferably 10.0% or less, more preferably 5.0% or less, most preferably 3.0% or less.

[0038] Na 2 O component is an optional component in the optical glass of the present invention, and when the content exceeds 0%, the melting temperature of the glass is lowered. 2 When the content of O is 10.0% or less, a high refractive index can be easily obtained, and the stability of the glass can be improved, and the occurrence of devitrification can be reduced. 2 The upper limit of the content of the O component with respect to the glass total mass of the oxide conversion composition is preferably 10.0% or less, more preferably 5.0% or less, most preferably 3.0% or less.

[0039] K 2 O component is an optional component in the optical glass of the present invention, and when the content exceeds 0%, the glass melting temperature is lowered. 2 When the content of O component is 10.0% or less, a high refractive index can be easily obtained, and the stability of the glass can be improved, and the occurrence of devitrification can be reduced. 2 The upper limit of the content of the O component with respect to the glass total mass of the oxide conversion composition is preferably 10.0% or less, more preferably 5.0% or less, further preferably 3.0% or less.

[0040] Ta 2 O 5 The component is a component that can increase the refractive index of glass and improve the devitrification resistance when the content exceeds 0%. 2 O 5 The upper limit of the content of the component is preferably 5.0% or less, more preferably 3.0% or less, more preferably 1.0% or less, and further preferably 0.5% or less.

[0041] P 2 O 5 The component is a component that lowers the liquidus temperature of glass and improves the devitrification resistance when the content exceeds 0%. 2 O 5 The upper limit of the content of the component is preferably 5.0% or less, more preferably 3.0% or less, more preferably 1.0% or less, and further preferably 0.5% or less.

[0042] GeO 2 The component is a component that can increase the refractive index of glass and improve the devitrification resistance when the content exceeds 0%. GeO 2 The upper limit of the content of the component is preferably 5.0% or less, more preferably 3.0% or less, more preferably 1.0% or less, and further preferably 0.5% or less.

[0043] Ga 2 O 3 The component is a component that can improve the chemical durability of glass and the devitrification resistance of molten glass when the content thereof exceeds 0%. 2 O 3 The upper limit of the content of the component is preferably 5.0% or less, more preferably 3.0% or less, more preferably 1.0% or less, and further preferably 0.5% or less.

[0044] Bi 2 O 3 The component is a component that can increase the refractive index and lower the glass transition temperature when the content thereof exceeds 0%. 2 O 3 The upper limit of the content of the component is preferably 5.0% or less, more preferably 3.0% or less, more preferably 1.0% or less, and further preferably 0.5% or less.

[0045] TeO 2 The component is a component that can increase the refractive index and lower the glass transition temperature when the content exceeds 0%. TeO 2 The upper limit of the content of the component is preferably 5.0% or less, more preferably 3.0% or less, more preferably 1.0% or less, and further preferably 0.5% or less.

[0046] SnO 2 When the content of SnO exceeds 0%, it reduces oxidation of molten glass to clarify it and can also increase the visible light transmittance of the glass. 2 The upper limit of the content of the component is preferably 5.0% or less, more preferably 3.0% or less, more preferably 1.0% or less, and further preferably 0.5% or less.

[0047] The F component is a component that can improve the meltability of the glass when the content exceeds 0%, but when the content is too high, devitrification may occur due to the volatilization of the F component. The upper limit of the content of the F component is preferably 5.0% or less, more preferably 3.0% or less, more preferably 1.0% or less, and further preferably 0.5% or less.

[0048] Sb 2 O 3 The component is an arbitrary component that promotes clarification and degassing when molten glass. 2 O 3 The content of the component is 0.1% or less, which can suppress the coloring of high refractive index glass. In addition, by setting it to 0.1% or less, it is not easy to produce excessive foaming when the glass is melted, so Sb 2 O 3The components are not easy to alloy with melting equipment (especially precious metals such as Pt). 2 O 3 The upper limit of the content of the component is preferably 0.1% or less, more preferably 0.08% or less, further preferably 0.05% or less, but may be 0%.

[0049] It should be noted that the component for clarifying and defoaming the glass is not limited to the above-mentioned Sb. 2 O 3 As the component, a clarifier, a defoaming agent or a combination thereof known in the field of glass manufacturing can be used.

[0050] The C component is a component that can maintain a reducing atmosphere in the platinum crucible, suppress the mixing of platinum into the glass due to oxidation, and improve the transmittance. However, when the content is too high, the cationic components in the glass are reduced and the glass is colored. Therefore, the upper limit of the content of the C component is preferably 8.0% or less, more preferably 5.0% or less, more preferably 3.0% or less, and most preferably 1.0% or less. On the other hand, the lower limit of the content of the C component is preferably greater than 0%, more preferably 0.3% or more, further preferably 0.5% or more, and most preferably 0.8% or more, but it may also be 0%.

[0051] The S component is a component that can maintain a reducing atmosphere in the platinum crucible, suppress the mixing of platinum into the glass due to oxidation, and improve the transmittance. However, when the content is high, the cationic components in the glass are reduced and the glass is colored. Therefore, the upper limit of the content of the S component is preferably 8.0% or less, more preferably 5.0% or less, more preferably 3.0% or less, and most preferably 1.0% or less. On the other hand, the lower limit of the content of the S component is preferably greater than 0%, more preferably 0.3% or more, further preferably 0.5% or more, and most preferably 0.8% or more, but it may also be 0%.

[0052] Organic components such as sucrose are components that can maintain a reducing atmosphere in a platinum crucible, inhibit platinum from mixing into the glass due to oxidation, and improve transmittance, but when the content is high, the cationic components in the glass are reduced and the glass is colored. Therefore, the upper limit of the content of organic components such as sucrose is preferably 10.0% or less, more preferably 8.0% or less, more preferably 6.0% or less, and most preferably 5.0% or less. On the other hand, the lower limit of the content of organic components such as sucrose is preferably more than 0%, more preferably 0.5% or more, further preferably 1.0% or more, and most preferably 2.0% or more, but it may also be 0%.

[0053] In addition, the components of the reduced glass are not limited to the above-mentioned C component, S component, and organic components such as sucrose, and any reducing agent known in the field of glass production or a combination thereof can be used.

[0054] <About ingredients that should not be contained>

[0055] Next, components that should not be contained in the optical glass of the present invention and components that are not preferably contained are described.

[0056] Other components not mentioned above may be added as needed within the range that does not impair the characteristics of the glass of the present invention. However, each transition metal component such as Ce, V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo has the following properties: even if they are contained in a small amount alone or in combination, the glass will be colored and absorption will occur at a specific wavelength in the visible region, thereby weakening the effect of improving the visible light transmittance of the present invention. Therefore, it is preferably not substantially contained in the glass that transmits wavelengths in the visible region.

[0057] In addition, lead compounds such as PbO and As 2 O 3 Arsenic compounds such as these are components that have a high environmental load, and therefore, it is preferred that they are not substantially contained, that is, not contained at all except for unavoidable contamination.

[0058] Furthermore, in recent years, the use of Th, Cd, Tl, Os, Be and Se has tended to be regulated as harmful chemical substances, and when used, environmental measures are required not only in the glass manufacturing process but also in the processing process and the disposal after productization. Therefore, when the environmental impact is important, it is preferred that these are substantially not contained.

[0059] [Method for producing optical glass]

[0060] The optical glass of the present invention can reduce the reduction color of the glass by bringing an oxidizing gas into contact with the surface of the molten glass. The molten glass is characterized in that: the glass includes a melting process, a clarification process, a homogenization process and a molding process, and in at least one process among the clarification process, the homogenization process and the molding process, the oxidizing gas is brought into contact with the surface of the molten glass under an oxidizing gas atmosphere. As in the past, if oxygen is bubbled in the molten glass, the noble metal elements (such as platinum) constituting the surface of the melting tank also react with oxygen, and the noble metal oxides are dissolved in the molten glass, resulting in a decrease in transmittance and a decrease in glass quality such as the generation of bumps. In the present invention, in at least one process among the clarification process, the homogenization process and the molding process, the reduction color can be reduced by bringing an oxidizing gas into contact with the surface of the molten glass under an oxidizing gas atmosphere. Below, each process of the method for manufacturing the optical glass of the present invention is described in detail.

[0061] [Glass Raw Material Melting Process]

[0062] As glass raw materials, in order to obtain an optical glass having desired properties, the above-mentioned glass components can be appropriately selected, raw materials corresponding to the glass components are weighed, and the raw materials are sufficiently mixed to obtain a prepared raw material (batch raw material) or prepared cullet.

[0063] When cullet is used as glass raw material, a culletizing step (rough melting step) of roughly melting the batch raw material to culletize is performed before the melting step (remelting step). In addition, the refractive index of the cullet is preferably measured in advance, and the cullets are mixed so as to have a desired refractive index value to prepare the cullet.

[0064] As a melting tank for heating glass raw materials for melting, a container or an appliance made of refractory materials such as quartz can be used, and a melting tank whose inner wall (surface contacted by the molten glass) is composed of a noble metal element can also be used. The shape of the melting tank is not particularly limited, for example, a container with an upper opening can be preferably used, and the inner wall of the tank is composed of a noble metal such as a platinum-rhodium, platinum-gold alloy, rhodium, gold, iridium, palladium, etc.

[0065] The melting tank is equipped with a heating unit such as a heating element or a high-frequency induction, and the glass raw material is melted by the heating. The heating unit is preferably heated in a manner that the temperature of the molten glass is kept substantially constant. Thus, melting and vitrification are easily performed by being divided into multiple times, and the generation rate of bubbles from the glass raw material and the molten glass is reduced, so that the thermal uniformity of the glass raw material and the molten glass is improved, and an optical glass with a more uniform composition and characteristics can be obtained.

[0066] The temperature at which the glass raw material is melted in the melting process is appropriately selected from temperatures at which the glass raw material can be melted and vitrified after cooling. More specifically, the lower limit of the melting temperature is preferably above 1100°C, more preferably above 1150°C, and most preferably above 1200°C. In addition, the upper limit of the melting temperature is preferably less than 1500°C, more preferably less than 1450°C, and most preferably less than 1400°C. By setting the melting temperature range to this, the dissolution of the glass raw material can be prevented. In addition, the "melting temperature" in the present specification refers to the average value of the temperature of the glass raw material at the top of the melting tank and the temperature of the glass raw material at the bottom of the melting tank.

[0067] The melting time is not particularly limited as long as it is a time period sufficient for the molten residue of the glass to disappear, and can be appropriately adjusted according to the amount of glass raw materials and the melting temperature.

[0068] In addition, continuous melting may be performed by continuously feeding glass raw materials into a melting tank, or batch melting may be performed by melting glass raw materials once. When continuous melting is performed, it is preferably performed in a continuous melting tank. The continuous melting tank will be described later.

[0069] [Clarification process]

[0070] Next, the molten glass is clarified. The clarification step is a step of degassing and defoaming to further vitrify the glass, wherein the degassing and defoaming removes dissolved gasified components and bubbles contained in the glass that has undergone the melting step. By implementing the clarification step, the devitrification of the glass can be reduced.

[0071] The clarification temperature is appropriately selected from the temperatures at which vitrification can be performed, and is preferably a temperature higher than the melting temperature. More specifically, the lower limit of the clarification temperature is preferably 1300°C or higher, more preferably 1350°C or higher, and most preferably 1400°C or higher. In addition, the upper limit is preferably less than 1450°C, more preferably less than 1500°C, and most preferably less than 1550°C. By setting the clarification temperature range to this, the melt viscosity of the molten glass is reduced, and dissolved gasified components and bubbles are easily removed.

[0072] When a continuous melting tank is used to carry out the clarification process, a clarification tank different from the melting tank is used, but the shape of the clarification tank is not particularly limited. For example, a container with an opening on the top can be preferably used, and the inner wall of the tank is composed of platinum-containing alloys such as platinum-rhodium, platinum-gold, rhodium, gold, iridium, palladium and other precious metals.

[0073] It is preferred that the clarification time be shortened within a range in which the effect of removing dissolved gasified components and bubbles can be obtained, thereby suppressing the coloring of the glass.

[0074] [Homogenization process]

[0075] Next, the clarified molten glass is stirred and homogenized. The homogenization step is also a step of reducing ribs and the like of the glass to be molded by homogenizing the molten glass and adjusting the viscosity of the molten glass to a viscosity suitable for molding.

[0076] Stirring can also be implemented by a stirrer having a stirring wing at the front end of a rotating shaft. In this case, it is preferred to configure a stirring device in a manner that the stirring wing rotates along the bottom surface of a melting tank (a homogenizing tank in the case of using a continuous melting tank). Thus, when discharging molten glass from the stirring tank, it is also possible to stir the molten glass until the stirring tank is about to become empty, thereby being able to reduce the formation of bubbles from the beginning of the outflow process to the end. The material of the part in contact with the molten glass, such as a stirring wing or a rotating shaft, can be appropriately selected from a material that is low in reactivity with the molten glass and can withstand the temperature of the stirring process. More specifically, the above-mentioned noble metal can be preferably used.

[0077] The temperature (stirring temperature) for implementing the homogenization process is preferably a temperature below the clarification temperature. More specifically, the upper limit of the stirring temperature is preferably less than 1350°C, more preferably less than 1300°C, and most preferably less than 1250°C. In addition, the lower limit of the stirring temperature is preferably 1100°C or more, more preferably 1150°C or more, and most preferably 1200°C or more. Within such a temperature range, bubbles can be removed or the molten glass can be made uniform.

[0078] The time for carrying out the homogenization step is not particularly limited as long as the clarified molten glass can be homogenized and the viscosity can be adjusted to an appropriate range.

[0079] [Molding process]

[0080] Next, the molten glass that has undergone the homogenization step is made to flow out from the melting tank and to be formed. For example, an outflow pipe extending from the lower part of the melting tank is provided in advance, and the molten glass is made to flow out through the outflow pipe.

[0081] The outflow temperature is preferably a temperature lower than the clarification temperature and the stirring temperature. More specifically, the outflow temperature in the outflow process is preferably less than 1300°C, more preferably less than 1250°C, and most preferably less than 1200°C. In addition, the lower limit of the outflow temperature is preferably above 1000°C, more preferably above 1050°C, and most preferably above 1100°C. By setting the outflow temperature to the range, the fluidity of the molten glass can be kept constant. In addition, the outflow temperature here does not refer to the temperature of the melting tank, but refers to the temperature of the molten glass flowing in the outflow pipe.

[0082] The molten glass flowing out from the melting tank is formed into a specified shape. As long as the molding process can shape the molten glass into a specified shape, then known molding methods can be appropriately utilized. For example, the molten glass can be made to flow into a mold and become a block, or the molten glass flow flowing down from the outflow pipe can be cut off at regular intervals of a certain length (a certain amount) to become a glass block. In addition, in subsequent processes, when performing a more accurate shape processing, the shape of each glass obtained through the molding process can also be uneven.

[0083] [Contact step with oxidizing gas]

[0084] In the present invention, in at least one of the clarification step, the homogenization step, and the molding step, an oxidizing gas is brought into contact with the surface of the molten glass in an oxidizing gas atmosphere. By bringing the oxidizing gas into contact with the surface of the molten glass without bubbling the oxidizing gas, the reduced color of the glass can be reduced, and degradation of the melting tank can be suppressed.

[0085] The oxidizing gas is not particularly limited, and for example, oxygen, halogenated oxygen, or the like can be used.

[0086] In order to make the melting tank into an oxidizing gas atmosphere, in the clarification process and the homogenization process, by blowing oxidizing gas from the upper opening of the melting tank, the oxidizing gas can be contacted with the surface of the molten glass. In addition, in the molding process, when the molten glass is made to flow out via the outflow pipe and molded, it is preferably carried out by blowing oxidizing gas to the surface of the molded object. Even in the surrounding atmosphere (air), it is also in contact with the molten glass. Although it helps to reduce the reduction color to a certain extent, it cannot be said to be sufficient. In the present invention, by blowing oxidizing gas, etc., the surface of the molten glass is made into an oxidizing gas atmosphere and contacted with oxidizing gas, thereby reducing the reduction color of the glass. The flow rate of the oxidizing gas at this time can be appropriately changed according to the volume of the melting tank. In addition, by making the melting tank be in a roughly closed state, the reduction effect of the reduction color can be improved. In addition, when blowing oxidizing gas to the molten glass from the upper opening of the melting tank, the closer the blowing position is to the surface of the molten glass, the higher the reduction effect of the glass reduction color.

[0087] The contact with the oxidizing gas may be performed continuously or intermittently while the molten glass is stored in the melting tank.

[0088] As an embodiment of making the oxidizing gas contact with the surface of the molten glass, it is preferred to blow the oxidizing gas to the surface of the molten glass. At this time, in order to make the glass surface into an oxidizing gas atmosphere, the blowing position of the oxidizing gas is preferably close to the molten glass surface, for example, it is preferred to blow the oxidizing gas from a position below 200 mm, below 150 mm, below 100 mm, below 90 mm, below 80 mm, below 70 mm, below 60 mm, below 50 mm, or below 40 mm above the upper part of the molten glass surface.

[0089] On the other hand, the blowing position of the oxidizing gas is preferably away from the surface of the molten glass to such an extent that no bubbles are generated inside the molten glass. For example, the oxidizing gas is preferably blown from a position more than 0 mm, 5 mm, or 10 mm above the upper part of the molten glass surface.

[0090] As an embodiment of the present invention, in the clarification step and the homogenization step, it is preferred that the interior of each melting tank be an oxidizing gas atmosphere so that oxygen is brought into contact with the surface of the molten glass.

[0091] In addition, in the present invention, an oxidizing gas may be brought into contact with the molten glass surface during the melting process. In particular, when the melting tank used in the melting process is made of quartz, the reduction color of the glass can be further reduced by bringing the oxidizing gas into contact with the molten glass surface under an oxidizing gas atmosphere. Furthermore, since a platinum crucible is not used, the reduction color of PtO can be suppressed. 2 Dissolution of precious metal oxides.

[0092] [Continuous melting tank]

[0093] The above-mentioned melting step, clarification step and homogenization step can be carried out using one melting tank, but the melting step, clarification step and homogenization step can also be carried out in consecutive and different melting tanks. Figure 1 The cross-sectional structure of an optical glass manufacturing device 1 having a continuous melting tank used in the optical glass manufacturing method of the present embodiment is shown. The optical glass manufacturing device 1 includes a melting tank 10, a clarification tank 20, and a homogenization tank 30. The melting tank 10 and the clarification tank 20 are connected at the bottom through a connecting pipe 11, and the clarification tank 20 and the homogenization tank 30 are connected at the bottom through a connecting pipe 21.

[0094] In the melting tank 10, a melting step of melting glass raw material 12 is performed. Next, the molten glass in the melting tank 10 is discharged to the clarification tank 20 through the connecting pipe 11, and a clarification step is performed in the clarification tank 20. Next, the clarified molten glass is discharged from the clarification tank 20 to the homogenization tank 30 through the connecting pipe 21, and a stirring step is performed in the homogenization tank 30. Thus, the molten glass flows in the order of the melting tank 10, the clarification tank 20, and the homogenization tank 30.

[0095] Next, the molten glass that has undergone the homogenization step is discharged to the forming mold 40 through the outflow pipe 31 extending from the bottom of the homogenization tank 30, and is solidified therein to become glass.

[0096] When the manufacturing method of the present invention is implemented using the manufacturing apparatus 1 for optical glass having the above-mentioned continuous melting tank, the contacting step with the oxidizing gas is as follows: Figure 1 As shown, an oxidizing gas is supplied to the melting tank 10, the clarification tank 20 and the homogenization tank 30 via a gas sharing pipe 51 extending from an oxidizing gas supply device 50, and is supplied to the upper opening of each tank (between the opening of the tank and the surface of the molten glass), thereby forming an oxidizing gas atmosphere. In addition, by providing a gas supply valve 52 in the middle of the gas sharing pipe 51, the flow rate of the oxidizing gas can be adjusted or the supply can be stopped. By closing a part of the gas supply valves, it is also possible to supply oxidizing gas to each desired tank. Furthermore, by appropriately adjusting the distance from the gas outlet of the gas sharing pipe 51 to the surface of the molten glass, it is also possible to more effectively form an oxidizing gas atmosphere. In addition, as Figure 2 As shown, the same effect can be obtained by making each groove substantially sealed and providing an oxidizing gas atmosphere in the groove.

[0097] In addition, during the molding process, Figure 1As shown, when the molten glass flows into the forming mold 40, by blowing an oxidizing gas from the upper opening of the forming mold 40 through the gas sharing pipe 51 to the molten glass, the surrounding of the forming mold can be made into an oxidizing gas atmosphere, so that oxygen contacts the surface of the molten glass. Figure 3 As shown, oxygen may be brought into contact with the surface of the molten glass by blowing an oxidizing gas from the back side of the forming mold 40 onto the molten glass flowing into the forming mold 40 .

[0098] [physical properties]

[0099] The refractive index (n d ) is preferably 1.80000 or more. The refractive index (n d The lower limit of the refractive index (n) is preferably 1.80000 or more, more preferably 1.85000 or more, further preferably 1.90000 or more, and further preferably 1.95000 or more. d The upper limit of ) is preferably 2.15000 or less, more preferably 2.10000 or less, and further preferably 2.05000 or less. In addition, the Abbe number (ν d The lower limit of ) is preferably 22.00 or more, more preferably 25.00 or more, and further preferably 27.00 or more. d ) is preferably 45.00 or less, more preferably 40.00 or less, and further preferably 37.00 or less.

[0100] The optical glass of the present invention preferably has a high visible light transmittance, particularly a high transmittance of light on the short wavelength side of visible light, because it has little coloration.

[0101] The shortest wavelength (λ) at which the optical glass of the present invention shows a spectral transmittance of 70% in a sample having a thickness of 10 mm 70 ) is preferably below 470 nm, more preferably below 450 nm, further preferably below 430 nm, and further preferably below 420 nm.

[0102] In the optical glass of the present invention, (λ 70 ) and refractive index (n d ) preferably satisfies λ 70 ≤(n d -2)×200+420, preferably satisfying λ 70 ≤(n d -2)×200+415, and preferably satisfies λ 70 ≤(n d -2)×200+410, and preferably satisfies λ 70 ≤(nd -2)×200+405.

[0103] Glass having a high refractive index tends to have poor transmittance. Therefore, it is considered that an optical glass having a high refractive index and good transmittance can be obtained by satisfying the above relationship.

[0104] The optical glass obtained by the manufacturing method of the present invention is precision pressed and molded, and can be typically used for lens, prism, and reflector applications. In particular, it can be used as a preformed material for press molding, or molten glass can be directly pressed. When used as a preformed material, its manufacturing method and precision press molding method are not particularly limited, and known manufacturing methods and molding methods can be used.

[0105] Optical glass is useful for various optical elements and optical designs, and it is particularly preferred to press-form the optical glass obtained by the manufacturing method of the present invention to produce optical elements such as lenses, prisms, and reflectors. Thus, when the obtained optical element is used in optical devices that transmit visible light, such as cameras and projectors, high-definition and high-precision imaging characteristics can be achieved, and the optical system in these optical devices can be miniaturized.

[0106] [Example]

[0107] Next, the present invention will be described in further detail with reference to Examples, but the present invention is not limited to these Examples.

[0108] [Preparation of glass raw materials]

[0109] As raw materials of the following components, high-purity raw materials used in general optical glass, such as oxides, carbonates, nitrates, fluorides, and metaphosphate compounds, are used.

[0110] SiO 2 4.8%

[0111] B 2 O 3 9.2%

[0112] La 2 O 3 53.1%

[0113] Y 2 O 3 4.8%

[0114] ZrO 2 5.8%

[0115] TiO 2 13.4%

[0116] Nb 2O 5 8.0%

[0117] WO 3 0.8%

[0118] Li 2 O 0.1%

[0119] S 0.4%

[0120] [Example 1]

[0121] The prepared glass raw materials were put into a melting tank whose inner wall was made of platinum alloy, and the glass raw materials were melted at a temperature of 1250° C. for 7.0 hours. The molten glass was clarified (clarification process) for 0.5 to 1.5 hours to remove bubbles, etc., and then the temperature was lowered to a temperature below 1250° C. and finally stirred (homogenization process) to remove ribs. In the homogenization process, oxygen gas was supplied from the opening of the homogenization tank at a flow rate of 0.5 L / min, and oxygen gas was blown from a position 60 mm away from the surface of the molten glass to make the oxidizing gas contact the surface of the molten glass.

[0122] Next, the molten glass is poured from the melting tank into a casting mold and slowly cooled (molding step), thereby obtaining glass.

[0123] [Example 2]

[0124] Glass was produced in the same manner as in Example 1 except that the flow rate of the supplied oxygen gas was changed to 1.0 L / min in the homogenization step.

[0125] [Example 3]

[0126] Glass was produced in the same manner as in Example 1 except that the flow rate of the supplied oxygen gas was changed to 2.7 L / min in the homogenization step.

[0127] [Example 4]

[0128] Glass was produced in the same manner as in Example 1 except that the flow rate of the supplied oxygen gas was changed to 1.0 L / min in the homogenization step and was supplied to the mold at a flow rate of 5.0 L / min in the molding step.

[0129] [Comparative Example 1]

[0130] Glass was produced in the same manner as in Example 1 except that oxygen gas was not supplied.

[0131] [Measurement of refractive index and Abbe number]

[0132] The refractive index (n d ), Abbe number (ν d) is measured according to the V-block method specified in JIS B 7071-2:2018. Here, the refractive index (n d ) is expressed as the measured value relative to the d line (587.56 nm) of a helium lamp. d ) using the refractive index of the helium lamp relative to the d-line (n d ), the refractive index of hydrogen lamp relative to F line (486.13nm) (n F ), the refractive index (n) relative to the C line (656.27nm) C ) value, according to the Abbe number (ν d ))=[(n d -1) / (n F -n C )] can be calculated. These refractive indices (n d ), Abbe number (ν d ) is obtained by measuring a glass obtained by slowly cooling at a temperature drop rate of -25°C / hr.

[0133] The measurement results are shown in Table 1 below.

[0134] [Evaluation of coloration]

[0135] The degree of coloration of the glass is evaluated by the transmittance. The transmittance was measured for each glass.

[0136] The transmittance of glass is measured according to the standard of the Japan Optical Glass Industry Association (JOGIS02-2019 Method for Determination of Coloring of Optical Glass). Specifically, a plate-shaped glass sample with two parallel surfaces and a thickness of 10 mm ± 0.1 mm polished to a flat surface is prepared, and light is incident on the polished surface from a vertical direction. The spectral transmittance including surface reflection loss is measured within the wavelength range of 200 nm to 700 nm. The wavelength at which the spectral transmittance is 70% is set to λ 70 .

[0137] The evaluation results are shown in Table 1 below.

[0138] [Table 1]

[0139]

Table 1

[0140]

[0141] It can be seen from the evaluation results in Table 1 that, by bringing an oxidizing gas into contact with the glass melted in an oxidizing gas atmosphere in any process after the melting process (clarification process, homogenization process, molding process), a high-refractive-index optical glass having excellent transmittance among optical glasses can be obtained (Examples 1 to 4).

[0142] On the other hand, it was found that the reduction color of the glass could not be sufficiently reduced in the conventional production method in which the oxidizing gas was not brought into contact with the molten glass (Comparative Example 1).

Claims

1. An optical glass comprising: A total content of 10.0% by mass of Ln2O3 components, wherein Ln represents at least one selected from the group consisting of La, Gd, Y and Yb; and At least one selected from the group consisting of TiO2, Nb2O5, WO3 and Bi2O3, The optical glass is obtained by bringing an oxidizing gas into contact with the surface of molten glass containing the components. 2 . The optical glass according to claim 1 , comprising the Ln 2 O 3 component in a total content of 10.0% to 70.0%.

3. An optical element, comprising the optical glass according to claim 1 or 2.

Citation Information

Patent Citations

  • Sealing material

    JP2002012852A