Composite powder for corrosion-resistant protective coating of semiconductor and preparation method of composite powder

The preparation of niobium-coated niobium carbide composite powder through ball milling and spray granulation processes solves the problem of poor binding performance of niobium carbide coating in plasma spray preparation, realizes corrosion resistance protection of semiconductor equipment materials, and ensures the uniformity of the coating and performance.

CN118931233APending Publication Date: 2024-11-12GEMCH MATERIAL TECH SUZHOU
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411144755.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art niobium carbide coatings in the field of plasma spraying and preparation of semiconductors have problems such as poor binding performance and low deposition rate, and it is impossible to effectively avoid corrosion of equipment materials in high temperature and corrosive environments.

Method used

The niobium coated niobium carbide composite powder prepared by ball milling and spray granulation technology reduces the particle size of niobium carbide through ball milling, and adds niobium powder and organic adhesive to form appropriate loose density and fluidity to avoid high temperatures. Oxidation and decomposition, used for plasma spraying to prepare corrosion-resistant protective coatings.

Benefits of technology

It realizes effective protection of niobium carbide during plasma spraying, improves the composition uniformity and tissue performance of the coating, and ensures the corrosion resistance of semiconductor equipment materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931233A_ABST
    Figure CN118931233A_ABST
Patent Text Reader

Abstract

The invention discloses composite powder for a corrosion-resistant protective coating of a semiconductor and a preparation method of the composite powder, relates to the field of preparation of semiconductor protective coating materials, and aims to solve the problem of preparation of the corrosion-resistant protective coating in the field of semiconductors through plasma spraying. (2) adding niobium powder and an organic adhesive, and continuing ball milling; (3) preparing the slurry into granulation powder; (4) screening by adopting a vibrating screen to prepare granulation powder; (5) heating and sintering by adopting a heating furnace; and (6) carrying out vibration screening to prepare the composite powder for preparing the corrosion-resistant protective coating in the semiconductor field through plasma spraying, wherein the particle size of the composite powder is 30-80 microns. The preparation method of the composite powder for the corrosion-resistant protective coating of the semiconductor can be used for preparing the composite powder for the corrosion-resistant protective coating of the semiconductor field through plasma spraying.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor protective materials, and more specifically, to a composite powder for semiconductor corrosion-resistant protective coating and a preparation method thereof. Background Art

[0002] The semiconductor industry has developed rapidly in recent years. For example, in the fields of epitaxial growth of semiconductor crystal materials and integrated circuit manufacturing equipment, the operating conditions of manufacturing semiconductor crystal materials and integrated circuit core manufacturing equipment are generally high temperature and plasma corrosive environments. Equipment materials are prone to corrosion failure in such environments. More importantly, it will affect the purity of the manufactured semiconductor materials and the quality of the integrated circuits. Therefore, it is necessary to prepare a protective coating on the surface of the semiconductor manufacturing equipment materials.

[0003] Niobium carbide has excellent high-temperature chemical stability and corrosion resistance, and can effectively prevent equipment materials from corrosion under high-temperature and corrosive conditions. Currently, the widely used method is to use PVD or CVD chemical vapor deposition to prepare a layer of niobium carbide coating on the surface of equipment materials, but the coating preparation efficiency is not high. Although the plasma spraying method has high coating efficiency, niobium carbide is easily oxidized and decomposed at high temperatures, resulting in poor bonding performance and low deposition rate of the coating prepared by plasma spraying, making it impossible to prepare an effective protective coating on the surface of semiconductor equipment materials.

[0004] Therefore, how to prepare a composite powder suitable for plasma spraying to prepare corrosion-resistant protective coatings in the semiconductor field has become a technical problem that urgently needs to be solved. Summary of the invention

[0005] In view of the deficiencies in the prior art, the object of the present invention is to provide a composite powder suitable for preparing corrosion-resistant protective coatings in the semiconductor field by plasma spraying and a preparation method thereof.

[0006] The above technical objectives of the present invention are achieved through the following technical solutions: A method for preparing a composite powder for a semiconductor corrosion resistant protective coating, characterized in that it comprises the following steps:

[0007] (1) adding niobium carbide raw material powder into a planetary ball mill and performing ball milling using niobium carbide abrasive;

[0008] (2) adding niobium powder in an amount of 10 wt.% to 20 wt.% of the mass of the composite powder, and adding an organic adhesive, and continuing ball milling;

[0009] (3) using centrifugal spray granulation equipment to make the slurry into granulated powder;

[0010] (4) screening the granulated powder using a vibrating screen to obtain a granulated powder;

[0011] (5) heating and sintering the granulated powder obtained by screening in a heating furnace;

[0012] (6) The sintered powder is vibrated and sieved to finally obtain a composite powder with a particle size of 30-80 μm for plasma spraying to prepare corrosion-resistant protective coatings in the semiconductor field.

[0013] The present invention is further configured as follows: in step (1), the particle size of the niobium carbide raw material powder is 50-90 μm.

[0014] The present invention is further configured as follows: in step (1), the ball milling is carried out in an argon atmosphere for 10-20 hours, and the particle size of the niobium carbide after ball milling is 20-80 nm.

[0015] The present invention is further configured as follows: in step (2), the particle size of the niobium powder is 40-80 μm.

[0016] The present invention is further configured as follows: in step (2), ball milling is performed for 2-5 hours to obtain a slurry with a solid content of 40wt.%-70wt.%.

[0017] The present invention is further configured as follows: in step (3), the spray granulation process parameters are: inlet temperature 200-400°C, outlet temperature 150-200°C, feed pump speed 600-1000r / min, atomizer speed 5000-6000r / min.

[0018] The present invention is further configured as follows: in step (4), the particle size of the prepared granulated powder is 40-90 μm.

[0019] The present invention is further configured as follows: in step (5), the sintering temperature is 200-250°C.

[0020] The present invention also provides a composite powder for semiconductor corrosion-resistant protective coating, which is obtained through the above-mentioned preparation process.

[0021] In summary, the present invention has the following beneficial effects: the present invention uses micron-sized niobium carbide and micron-sized niobium powder as raw materials, prepares precursor powder of a certain particle size by ball milling and spray granulation, and then prepares niobium-coated niobium carbide composite powder by sintering and screening. The niobium powder has a suitable bulk density and good fluidity. The niobium powder effectively protects the niobium carbide powder to avoid oxidative decomposition of niobium carbide at high temperature. The niobium carbide can be used for plasma spraying to prepare corrosion-resistant protective coatings in the semiconductor field, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a SEM photograph of the appearance of the composite powder obtained by the processing of the present invention. DETAILED DESCRIPTION

[0023] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments.

[0024] The object of the present invention is to provide a composite powder suitable for preparing corrosion-resistant protective coatings in the semiconductor field by plasma spraying and a preparation method thereof.

[0025] The present invention uses micron-sized niobium carbide and micron-sized niobium powder as raw materials, prepares precursor powder of a certain particle size by ball milling and spray granulation, and then prepares niobium-coated niobium carbide composite powder by sintering and screening. The niobium powder has suitable bulk density and good fluidity. The niobium powder effectively protects the niobium carbide powder to avoid oxidative decomposition of niobium carbide at high temperature, and can be used for plasma spraying to prepare corrosion-resistant protective coatings in the semiconductor field, and has good application prospects.

[0026] The composite powder for preparing corrosion-resistant protective coating in the semiconductor field by plasma spraying and the preparation method thereof provided by the present invention include the following steps:

[0027] (1) Add niobium carbide raw material powder (particle size: 50-90 μm) into a planetary ball mill, use niobium carbide abrasive, and ball mill for 10-20 hours in an argon atmosphere. After ball milling, the particle size of niobium carbide is 20-80 nm.

[0028] (2) Add niobium powder (particle size: 40-80 μm) in an amount of 10 wt.%-20 wt.% of the mass of the composite powder, and add an organic adhesive, and continue ball milling for 2-5 hours to obtain a slurry with a solid content of 40 wt.%-70 wt.%.

[0029] (3) Use centrifugal spray granulation equipment to make the slurry into granulated powder of a certain particle size.

[0030] Spray granulation process parameters: inlet temperature 200-400℃, outlet temperature 150-200℃, feed pump speed 600-1000r / min, atomizer speed 5000-6000r / min.

[0031] (4) The granulated powder is sieved using a vibrating screen to obtain a granulated powder with a particle size of 40-90 μm.

[0032] (5) The granulated powder obtained by screening is heated and sintered in a heating furnace at a sintering temperature of 200-250°C.

[0033] (6) The sintered powder is vibrated and sieved to finally obtain a composite powder with a particle size of 30-80 μm for plasma spraying to prepare corrosion-resistant protective coatings in the semiconductor field.

[0034] As attached Figure 1 The figure shows a SEM photograph (200x) of the appearance of the composite powder obtained in the present invention.

[0035] The following is a detailed description:

[0036] Example 1

[0037] (1) adding niobium carbide raw material powder (particle size: 50 μm) into a planetary ball mill, using niobium carbide abrasive, and ball milling for 14 hours in an argon atmosphere. After ball milling, the particle size of niobium carbide is 30 nm;

[0038] (2) adding niobium powder (particle size: 60 μm) in an amount of 20 wt.% of the mass of the composite powder, and adding an organic binder, and continuing ball milling for 4 hours to obtain a slurry with a solid content of 60 wt.%;

[0039] (3) using centrifugal spray granulation equipment to make the slurry into granulated powder of a certain particle size;

[0040] Spray granulation process parameters: inlet temperature 200℃, outlet temperature 200℃, feed pump speed 600r / min, atomizer speed 5000r / min;

[0041] (4) using a vibrating screen to sieve the granulated powder to obtain a granulated powder with a particle size of 90 μm;

[0042] (5) Using a heating furnace to heat and sinter the granulated powder obtained by screening, the sintering temperature is 200°C;

[0043] (6) The sintered powder is vibrated and sieved to finally obtain a composite powder for plasma spraying to prepare corrosion-resistant protective coatings in the semiconductor field.

[0044] Example 2

[0045] (1) adding niobium carbide raw material powder (particle size: 90 μm) into a planetary ball mill, using niobium carbide abrasive, and ball milling for 20 hours in an argon atmosphere. After ball milling, the particle size of niobium carbide was 20 nm;

[0046] (2) adding niobium powder (particle size: 80 μm) in an amount of 10 wt.% of the composite powder mass, and adding an organic binder, and continuing ball milling for 5 hours to obtain a slurry with a solid content of 40 wt.%;

[0047] (3) using centrifugal spray granulation equipment to make the slurry into granulated powder of a certain particle size;

[0048] Spray granulation process parameters: inlet temperature 200℃, outlet temperature 150℃, feed pump speed 800r / min, atomizer speed 6000r / min;

[0049] (4) using a vibrating screen to sieve the granulated powder to obtain a granulated powder with a particle size of 40 μm;

[0050] (5) Using a heating furnace to heat and sinter the granulated powder obtained by screening, the sintering temperature is 250°C;

[0051] (6) The sintered powder is vibrated and screened to finally obtain a composite powder for preparing a corrosion-resistant protective coating in the semiconductor field by plasma spraying;

[0052] Example 3

[0053] (1) Niobium carbide raw material powder (particle size: 70 μm) was added to a planetary ball mill, using niobium carbide as abrasive, and ball milled for 1720 hours in an argon atmosphere. After ball milling, the particle size of niobium carbide was 40 nm.

[0054] (2) Add niobium powder (particle size: 60 μm) in an amount of 17 wt.% of the mass of the composite powder, and add an organic binder, and continue ball milling for 3 hours to obtain a slurry with a solid content of 50 wt.%.

[0055] (3) Use centrifugal spray granulation equipment to make the slurry into granulated powder of a certain particle size.

[0056] Spray granulation process parameters: inlet temperature 320℃, outlet temperature 160℃, feed pump speed 700r / min, atomizer speed 5500r / min.

[0057] (4) The granulated powder is sieved using a vibrating screen to obtain a granulated powder with a particle size of 50 μm.

[0058] (5) The granulated powder obtained by screening is heated and sintered in a heating furnace at a sintering temperature of 220°C.

[0059] (6) The sintered powder is vibrated and sieved to finally obtain a composite powder for plasma spraying to prepare corrosion-resistant protective coatings in the semiconductor field.

[0060] The bulk density, fluidity and particle size of the composite powders obtained in Example 1, Example 2 and Example 3 were tested to obtain the results shown in Table 1:

[0061] Table 1: Test results

[0062]

[0063] In summary, the present invention can achieve the following beneficial effects:

[0064] (1) The composite powder material for preparing the corrosion-resistant protective coating in the semiconductor field by plasma spraying prepared by the present invention has a spherical appearance and a structure of niobium coated with niobium carbide. Figure 1 As shown, it has suitable bulk density and good fluidity, can avoid high-temperature oxidation and decomposition of niobium carbide during plasma spraying, and can ensure the continuity and stability of powder feeding.

[0065] (2) The components of the composite powder for preparing the corrosion-resistant protective coating in the semiconductor field by plasma spraying prepared by the present invention are evenly distributed, which can ensure the uniformity of the composition, structure and performance of the coating prepared by plasma spraying.

[0066] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing a composite powder for a semiconductor corrosion resistant protective coating, characterized in that: The following steps are involved: (1) adding niobium carbide raw material powder into a planetary ball mill and performing ball milling using niobium carbide abrasive; (2) adding niobium powder in an amount of 10 wt.% to 20 wt.% of the mass of the composite powder, and adding an organic adhesive, and continuing ball milling; (3) using centrifugal spray granulation equipment to make the slurry into granulated powder; (4) screening the granulated powder using a vibrating screen to obtain a granulated powder; (5) heating and sintering the granulated powder obtained by screening in a heating furnace; (6) The sintered powder is vibrated and sieved to finally obtain a composite powder with a particle size of 30-80 μm for plasma spraying to prepare corrosion-resistant protective coatings in the semiconductor field.

2. The method for preparing a composite powder for a semiconductor corrosion resistant protective coating according to claim 1, characterized in that: In step (1), the particle size of the niobium carbide raw material powder is 50-90 μm.

3. The method for preparing a composite powder for a semiconductor corrosion resistant protective coating according to claim 1 or 2, characterized in that: In step (1), the ball milling is carried out in an argon atmosphere for 10-20 hours, and the particle size of the niobium carbide after ball milling is 20-80 nm.

4. The method for preparing a composite powder for a semiconductor corrosion resistant protective coating according to claim 1, characterized in that: In step (2), the particle size of the niobium powder is 40-80 μm.

5. The method for preparing a composite powder for a semiconductor corrosion resistant protective coating according to claim 1 or 4, characterized in that: In step (2), ball milling is performed for 2-5 hours to obtain a slurry with a solid content of 40wt.%-70wt.%.

6. The method for preparing a composite powder for a semiconductor corrosion resistant protective coating according to claim 1, characterized in that: In step (3), the spray granulation process parameters are: inlet temperature 200-400°C, outlet temperature 150-200°C, feed pump speed 600-1000r / min, atomizer speed 5000-6000r / min.

7. The method for preparing a composite powder for a semiconductor corrosion resistant protective coating according to claim 1, characterized in that: In step (4), the particle size of the granulated powder obtained is 40-90 μm.

8. The method for preparing a composite powder for a semiconductor corrosion resistant protective coating according to claim 1, characterized in that: In step (5), the sintering temperature is 200-250°C.

9. A composite powder for semiconductor corrosion resistant protective coating, characterized in that: The method comprises preparing the product by the preparation method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Composite powder for anti-corrosion coating of cavity of semiconductor integrated circuit and preparation method of composite powder

    CN117820889A

  • Production of carbon containing refractory

    JP1998053454A