Method for evaluating lithium ion diffusion rate based on GITT test
By performing constant current intermittent titration test and mathematical post-processing on the battery, the voltage-voltage change rate curve is drawn, which solves the problems of complexity of the GITT test method and difficulty in obtaining parameters, and achieves a fast and simple evaluation of the diffusion rate of lithium ion, which is suitable for Industrialization assessment.
Patent Information
- Application Number
- CN202411005882.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
The existing GITT test methods are complex in calculations and difficult to obtain parameters, which makes the calculation results difficult to compare. They are not suitable for rapid and effective evaluation of lithium ion diffusion rates, especially in industrial evaluation of the lithium ion solid phase diffusion rates of large batches of product-grade batteries.
After the battery to be tested is activated, the constant current intermittent titration test is performed to obtain the time-voltage curve, perform polynomial fit and lead-in processing, draw the voltage-voltage change rate curve, evaluate the lithium ion diffusion rate based on the voltage change rate, and simplify the The evaluation process avoids the need to obtain additional parameter values and complex calculation formulas.
It realizes a fast, simple and intuitive evaluation of the diffusion rate of lithium ion, which is suitable for industrial evaluation of diffusion rate comparison between different batches of batteries, providing a simple and effective method to improve the evaluation efficiency and accuracy.
Smart Images

Figure CN118938035A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of battery technology, and in particular to a method for evaluating lithium ion diffusion rate based on GITT test. Background Art
[0002] According to the basic working principle of lithium-ion batteries, the charging and discharging process of lithium batteries is the process of lithium ions being embedded and removed back and forth between the positive and negative electrodes. This charging and discharging mechanism is heavily dependent on the diffusion kinetics of lithium ions and material phase changes. The diffusion rate of lithium ions in solid phase particles largely determines the reaction rate (which is also related to the fast charging and discharging capabilities of the battery), which seriously restricts the capacity and rate performance release of the battery. Therefore, how to quickly and effectively evaluate the solid phase diffusion rate of lithium ions is an important technical method for analyzing battery kinetic performance.
[0003] The existing methods for calculating the solid-phase diffusion rate of lithium ions include cyclic voltammetry (CV), electrochemical impedance spectroscopy (EIS), potentiostatic relaxation (PRT), constant current intermittent titration (GITT), etc. Among these many calculation methods, the GITT method can obtain the dynamic diffusion rate under different SOC states during the entire charge and discharge process, so it is closer to the actual diffusion rate during the operation of lithium-ion batteries. However, the GITT method also has many disadvantages that make it difficult to be widely used. For example, the calculation process of GITT is complicated, and it is necessary to obtain key parameters such as the relaxation voltage difference under different SOCs and the actual reaction active area of the electrode. Usually, these parameters are difficult to obtain accurate values, and there may be large deviations in the calculation results of samples between different batches. Therefore, the numerical calculation results of GITT often lose their comparative significance, and this method is not conducive to industrial evaluation of the solid-phase diffusion rate of lithium ions in large batches of product-level batteries.
[0004] Based on the above analysis, the existing GITT test method needs to be improved to be suitable for quickly and effectively evaluating the solid-phase diffusion rate of lithium ions. Summary of the invention
[0005] The purpose of this application is to provide a method for evaluating the diffusion rate of lithium ions based on the GITT test, which aims to solve the problems in the existing GITT test technology, such as cumbersome calculation methods, difficult parameter acquisition, difficult comparison of calculation results, and unsuitability for rapid and effective evaluation of the diffusion rate of lithium ions.
[0006] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:
[0007] In a first aspect, the present application provides a method for evaluating lithium ion diffusion rate based on GITT test, comprising the following steps:
[0008] Obtaining a button cell to be tested and performing activation treatment to obtain an activated cell;
[0009] Performing a constant current intermittent titration test on the activated battery to obtain a time-voltage curve;
[0010] Performing polynomial fitting and derivation processing on the time-voltage curve in sequence to obtain a time-voltage change rate curve;
[0011] Draw a voltage-voltage change rate curve based on the voltage change rate value and the corresponding voltage value;
[0012] The speed of lithium ion diffusion in the battery is evaluated based on the voltage-voltage change rate curve.
[0013] In some possible implementations, the polynomial fitting is performed according to a polynomial function.
[0014] In some possible implementations, the derivation processing step includes: derivatizing the voltage data after the polynomial fitting with respect to time data to obtain a curve of the rate of change of voltage over time, that is, the time-voltage rate of change curve.
[0015] In some possible implementations, the step of drawing the voltage-voltage change rate curve includes: drawing the voltage-voltage change rate curve according to the voltage change rate value and the corresponding voltage value at the end of each relaxation.
[0016] In some possible implementations, the counter electrode in the button cell to be tested is lithium metal, and the potential of the counter electrode is 0.
[0017] In some possible implementations, according to the voltage-voltage change rate curve, the smaller the change rate, the faster the diffusion rate.
[0018] In some possible implementations, the activation treatment conditions include: cycling for 1 to 3 times within a rate range of 0.02C to 0.1C.
[0019] In some possible implementations, the activation treatment has a cycle ratio of 0.1C and a cycle number of 3.
[0020] In some possible implementations, the steps of the constant current intermittent titration test include: repeating the constant current and static relaxation procedures under the conditions of a current density of 0.1C, a constant current time of 5min to 20min, and a static relaxation time of 30min to 120min until the battery voltage reaches the upper or lower limit of the test range.
[0021] In some possible implementations, when the electrode material is a positive electrode material, the constant current intermittent titration test first performs a charging test phase, and then performs a discharging test phase.
[0022] In some possible implementations, when the electrode material is a negative electrode material, the constant current intermittent titration test first performs a discharge test phase and then performs a charge test phase.
[0023] In some possible implementations, during the charging test phase, after applying a forward current with a current density of 0.1C and maintaining the constant current for 5 to 20 minutes, the current is interrupted for static relaxation for 30 to 120 minutes, and the constant current charging and static relaxation are repeated until the charging cut-off voltage is reached.
[0024] In some possible implementations, during the discharge test phase, a reverse current with a current density of 0.1C is applied and maintained at a constant current for 5 to 20 minutes, and then the current is interrupted for static relaxation for 30 to 120 minutes, and constant current discharge and static relaxation are repeated until the discharge cut-off voltage is reached.
[0025] In some possible implementations, when the electrode material is a positive electrode material, the steps of the constant current intermittent titration test include: in the charging test phase, a forward current with a current density of 0.1C is applied and maintained at a constant current for 10 minutes, and then the current is interrupted for static relaxation for 60 minutes, and constant current charging and static relaxation are repeated until the charging cut-off voltage is reached; in the discharge test phase, a reverse current with a current density of 0.1C is applied and maintained at a constant current for 10 minutes, and then the current is interrupted for static relaxation for 60 minutes, and constant current discharge and static relaxation are repeated until the discharge cut-off voltage is reached.
[0026] In some possible implementations, when the electrode material is a negative electrode material, the steps of the constant current intermittent titration test include: in the discharge test phase, a reverse current with a current density of 0.1C is applied and maintained at a constant current for 10 minutes, the current is interrupted for static relaxation for 60 minutes, and the constant current reverse charge and static relaxation are repeated until the reverse charge cutoff voltage is reached; in the charging test phase, a forward current with a current density of 0.1C is applied and maintained at a constant current for 10 minutes, the current is interrupted for static relaxation for 60 minutes, and the constant current charging and static relaxation are repeated until the charging cutoff voltage is reached.
[0027] The method for evaluating the diffusion rate of lithium ions based on the GITT test provided in the first aspect of the present application is to perform a constant current intermittent titration test on the button cell to be tested after activation treatment, and to perform simple mathematical post-processing such as polynomial fitting and derivation on the obtained "pulse-constant current-relaxation" curve, that is, the time-voltage curve, so that the voltage-voltage change rate curve can be drawn according to the voltage change rate value and the corresponding voltage value. According to the voltage-voltage change rate curve, by comparing the magnitude of the voltage change rate, the speed of the lithium ion diffusion rate in the battery can be evaluated. The present application can directly evaluate the speed of the lithium ion diffusion rate in the battery according to the magnitude of the voltage change rate in the voltage-voltage change rate curve. The final result is not the specific value of the diffusion rate, and there is no need to obtain additional parameter values, no complex calculation formulas are required, and the evaluation method is simple and intuitive. In addition, by comparing the magnitude relationship of the voltage change rate, the ion solid phase diffusion rate between large batches and different batches of sample batteries can be intuitively, simply, quickly and efficiently compared, providing a simple and effective method for industrial evaluation of the lithium ion diffusion rate in batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0029] Figure 1 1 is a flow chart of a method for evaluating lithium ion diffusion rate based on GITT test provided in an embodiment of the present application;
[0030] Figure 2 is a time-voltage GITT curve of the battery provided in Example 1 of the present application;
[0031] Figure 3 is a time-voltage change rate curve of the battery charging stage provided in Example 1 of the present application;
[0032] Figure 4 is a time-voltage change rate curve of the battery discharge stage provided in Example 1 of the present application;
[0033] Figure 5 The voltage-voltage change rate curve of the battery provided in Example 1 of the present application is Figure 1 ;
[0034] Figure 6 The voltage-voltage change rate curve of the battery provided in Example 1 of the present application is Figure 2 ;
[0035] Figure 7The voltage-voltage change rate curve of the battery provided in Example 2 of the present application is Figure 1 ;
[0036] Figure 8 The voltage-voltage change rate curve of the battery provided in Example 2 of the present application is Figure 2 ;
[0037] Fig. 9 This is the time-voltage GITT curve of the battery at 25% SOC provided in Comparative Example 1 of the present application;
[0038] Fig.10 This is the battery SOC-ion diffusion rate diagram provided in Comparative Example 1 of the present application. DETAILED DESCRIPTION
[0039] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0040] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0041] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0042] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0043] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0044] The weight of the relevant components mentioned in the embodiments of the present specification can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components in the embodiments of the present specification is proportionally enlarged or reduced, it is within the scope disclosed in the embodiments of the present specification. Specifically, the mass described in the embodiments of the present specification can be μg, mg, g, kg and other mass units known in the chemical industry.
[0045] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.
[0046] The term "GITT" is the abbreviation of "Galvanostatic Intermittent Titration Technique", which means constant current intermittent titration technique, and is a transient measurement method. The GITT test is a cyclic process of pulse-constant current-relaxation. The pulse refers to a short current flow process, and relaxation refers to a process without current flow. The basic principle is: within a unit time t, a constant current I is applied for charging or discharging, and then the current is disconnected, and the voltage changes of the constant current process and the relaxation process are recorded at the same time. The specific steps can be referred to in the following example: Charge the NCM / Li half-cell at a constant current of 0.2C for 10 minutes, then leave it for 1 hour to reach equilibrium, and continue to cycle the process to the upper limit voltage. The discharge process can refer to the charging process.
[0047] The first aspect of the present application embodiment provides a method for evaluating the lithium ion diffusion rate based on the GITT test, as shown in the attached Figure 1 As shown, the following steps are included:
[0048] S10. Obtain the button cell to be tested and perform activation treatment to obtain an activated battery;
[0049] S20. Perform a constant current intermittent titration test on the activated battery to obtain a time-voltage curve;
[0050] S30. Perform polynomial fitting and derivation processing on the time-voltage curve in sequence to obtain a time-voltage change rate curve;
[0051] S40. Draw a voltage-voltage change rate curve according to the voltage change rate value and the corresponding voltage value;
[0052] S50. Evaluate the diffusion rate of lithium ions in the battery based on the voltage-voltage change rate curve.
[0053] The method for evaluating the diffusion rate of lithium ions based on the GITT test provided in the first aspect of the embodiment of the present application is to perform a constant current intermittent titration test on the button cell to be tested after activation treatment, and to perform simple mathematical post-processing such as polynomial fitting and derivation on the obtained "pulse-constant current-relaxation" curve, that is, the time-voltage curve, so that the voltage-voltage change rate curve can be drawn according to the voltage change rate value and the corresponding voltage value. According to the voltage-voltage change rate curve, by comparing the magnitude of the voltage change rate, the speed of the lithium ion diffusion rate in the battery can be evaluated. The embodiment of the present application can directly evaluate the speed of the lithium ion diffusion rate in the battery according to the magnitude of the voltage change rate in the voltage-voltage change rate curve. The final result is not the specific value of the diffusion rate, and there is no need to obtain additional parameter values, no complex calculation formulas are required, and the evaluation method is simple and intuitive. In addition, by comparing the magnitude relationship of the voltage change rate, the ion solid phase diffusion rate between large batches and different batches of sample batteries can be intuitively, simply, quickly and efficiently compared, providing a simple and effective method for industrial evaluation of the lithium ion diffusion rate in batteries.
[0054] In the above step S10:
[0055] In some possible implementations, a button cell to be tested is obtained for activation treatment, in which the counter electrode in the button cell to be tested is lithium metal, and the potential of the counter electrode is 0. In the embodiment of the present application, the object to be tested adopts a button cell, preferably a button half-cell with a counter electrode potential of 0, to exclude interference from non-test electrode materials. It can evaluate the lithium ion diffusion rate of all positive electrode materials, and the lithium ion diffusion rate of all negative electrode materials, and is flexible and convenient to apply, and has wide practicality. In some specific embodiments, lithium metal is used for the counter electrode, and the counter electrode potential is kept at 0. Exemplarily, when the negative electrode material matches lithium metal, the counter electrode lithium metal has a potential of 0, and the negative electrode material is at a high potential relative to the lithium metal, that is, in the actual assembled button test, the negative electrode material is the positive electrode, and the lithium metal is the negative electrode, which also excludes the interference of the positive electrode material.
[0056] In some possible implementations, the conditions for the activation treatment include: cycling 1 to 3 times within the range of 0.02C to 0.1C. In the embodiment of the present application, the button cell to be tested is activated to form a stable SEI film, i.e., a solid electrolyte interface film (Solid Electrolyte Interphase), on the surface of the electrode material, so as to facilitate the subsequent more stable and accurate evaluation of the lithium ion diffusion kinetics. In the embodiment of the present application, a low rate charge and discharge activation of 0.02C to 0.1C is used, and a stable SEI film can be formed by 1 to 3 activation cycles. Exemplarily, the cycle rate of the activation treatment can be any typical non-restrictive point value or an interval value between any two point values such as 0.02C, 0.05C, 0.08C, 0.1C, and the number of cycles can be any typical non-restrictive point value or an interval value between any two point values such as 1, 2, 3, and the like.
[0057] In some possible implementations, the activation treatment cycle ratio is 0.1C, and the number of cycles is 3. In this case, 0.1C is a more appropriate activation ratio. It is generally believed that 3 cycles of activation can better form a stable SEI film. A lower activation ratio such as 0.05C will take too long to affect production efficiency, and a higher ratio is not conducive to forming a stable SEI film.
[0058] In the above step S20:
[0059] In some possible implementations, the steps of the constant current intermittent titration test include: under the conditions of a current density of 0.1C, a constant current time of 5min to 20min, and a static relaxation time of 30min to 120min, repeat the constant current and static relaxation procedures until the battery voltage reaches the upper or lower limit of the test interval. The embodiment of the present application uses a small current and a small rate to perform a constant current intermittent titration test, because GITT tests the diffusion coefficient of the solid phase of active particles. Excessive current will produce other polarizations, for example: the concentration polarization of the electrolyte will cause voltage fluctuations, etc., which will interfere with the solid phase diffusion assessment. In addition, because the GITT test needs to meet the assumption that the diffusion process only occurs on the surface, the constant current pulse time t is relatively short, so the constant current duration is selected. The choice of relaxation time is to take into account the degree to which the solid phase diffusion concentration is as uniform as possible. Exemplarily, the current density of the constant current intermittent titration test can be 0.1C, the constant current time can be 5min, 10min, 15min, 20min, etc., typical non-restrictive arbitrary point values or an interval value between any two point values, and the static relaxation time can be 30min, 40min, 50min, 80min, 100min, 120min, etc., typical non-restrictive arbitrary point values or an interval value between any two point values.
[0060] In some possible implementations, when the electrode material is a positive electrode material, the constant current intermittent titration test first performs a charging test phase, and then a discharging test phase. In some possible implementations, when the electrode material is a negative electrode material, the constant current intermittent titration test first performs a discharging test phase, and then a charging test phase. In the above case, the positive electrode material releases ions and electrons during charging, so it is necessary to charge first to accumulate enough lithium ions and electrons for subsequent discharge. The negative electrode receives ions and electrons during the charging process and releases them during the discharging process. Therefore, in order to study the performance of the negative electrode during the discharge process, it is necessary to discharge it first. The positive electrode is charged first and then discharged, and the negative electrode is discharged first and then charged, in order to study the lithium ion diffusion behavior of the positive and negative electrode materials during the charging and discharging process respectively.
[0061] In some possible implementations, during the charging test phase, a forward current with a current density of 0.1C is applied and maintained at a constant current for 5 to 20 minutes, and then the current is interrupted for static relaxation for 30 to 120 minutes, and constant current charging and static relaxation are repeated until the charging cut-off voltage is reached.
[0062] In some possible implementations, during the discharge test phase, a reverse current with a current density of 0.1C is applied and maintained at a constant current for 5 to 20 minutes, and then the current is interrupted for static relaxation for 30 to 120 minutes, and constant current discharge and static relaxation are repeated until the discharge cut-off voltage is reached.
[0063] In some possible implementations, when the electrode material is a positive electrode material, the steps of the constant current intermittent titration test include: in the charging test phase, a forward current with a current density of 0.1C is applied and maintained at a constant current for 10 minutes, and then the current is interrupted for static relaxation for 60 minutes, and constant current charging and static relaxation are repeated until the charging cut-off voltage is reached; in the discharge test phase, a reverse current with a current density of 0.1C is applied and maintained at a constant current for 10 minutes, and then the current is interrupted for static relaxation for 60 minutes, and constant current discharge and static relaxation are repeated until the discharge cut-off voltage is reached.
[0064] In some embodiments, the cut-off voltage is generally determined by the selected active material. For example, the cut-off voltage of lithium iron phosphate is generally 2.5V to 4.2V, and the cut-off voltage of some high-voltage materials such as lithium nickel manganese oxide may be 2.5V to 4.6V.
[0065] In some possible implementations, when the electrode material is a negative electrode material, the steps of the constant current intermittent titration test include: in the discharge test phase, a reverse current with a current density of 0.1C is applied and maintained at a constant current for 10 minutes, the current is interrupted for static relaxation for 60 minutes, and the constant current reverse charge and static relaxation are repeated until the reverse charge cutoff voltage is reached; in the charging test phase, a forward current with a current density of 0.1C is applied and maintained at a constant current for 10 minutes, the current is interrupted for static relaxation for 60 minutes, and the constant current charging and static relaxation are repeated until the charging cutoff voltage is reached.
[0066] In the above step S30:
[0067] In some possible implementations, polynomial fitting is performed according to the polynomial function. The purpose of performing polynomial fitting in the embodiment of the present application is to reduce data points, simplify the amount of data processing, and keep the curve without significant changes.
[0068] In some embodiments, the principle of polynomial fitting is based on the properties of polynomial functions, which can be expressed as follows: y=w0+w1x+w2x 2 +w3x 3 +…+w n x n , where y is the dependent variable (output), x is the independent variable (input), w0, w1, ..., W n are polynomial coefficients. By determining the coefficient values, a polynomial function can be obtained for fitting data. Polynomial fitting is to find the best coefficient value so that the error between the fitting function and the target function is minimized. The most commonly used method is the least squares method, that is, to determine the coefficients by minimizing the residual sum of squares. The residual is the difference between the actual observed value and the predicted value of the fitting function. In data processing software such as origin, sigmaplot, and matlab, basically all have built-in polynomial fitting functions. By selecting different orders (n values in the above formula) and the number of selected data points, fitting curves with different fitting effects can be obtained. The residuals of the fitting curve and the actual curve are compared to determine whether the fitting result is usable. The number of data points for polynomial fitting can be freely selected in the software. Usually, within the reasonable residual range (that is, achieving the ideal fitting effect), the fewer data points, the better.
[0069] In some possible implementations, the derivation processing step includes: derivatizing the voltage data after polynomial fitting with respect to the time data to obtain a voltage change rate curve over time, that is, a time-voltage change rate curve. In the embodiment of the present application, the voltage data after polynomial fitting is derivatized with respect to the time data, that is, the voltage change rate. By derivation, the speed of voltage change over time can be intuitively obtained. Exemplarily, after the time-voltage curve is polynomially fitted, the y-axis is voltage, the x-axis is time, and the y-axis is derivatized with respect to the x-axis, that is, dV / dt satisfies the definition of derivative, and the rate of change of voltage V over time t.
[0070] In the above step S40:
[0071] In some possible implementations, the step of drawing a voltage-voltage rate of change curve includes: drawing a voltage-voltage rate of change curve according to the voltage rate of change value at the end of each relaxation and the corresponding voltage value. The voltage rate of change at the end of relaxation extracted in the embodiment of the present application is obtained based on the GITT test principle. The relaxation process reflects the diffusion of lithium ions in the natural state inside the solid phase particles after the current is removed. The faster the diffusion, the more gradual the voltage change at the end of relaxation. Therefore, the voltage rate of change at the end of relaxation is used to represent the speed of diffusion. The obtained dV / dt derivative voltage rate of change data is used as the y-coordinate, and the voltage is re-plotted as the x-coordinate to obtain a voltage-voltage rate of change curve data graph.
[0072] In other embodiments, the x-coordinate can be not only a voltage value but also an SOC (State of Charge, which is the percentage of the remaining battery power to the rated capacity of the battery). According to the voltage change rate value and the corresponding SOC value at the end of each relaxation, an SOC-voltage change rate curve is drawn, which serves as a basis for determining the charge and discharge state.
[0073] In the above step S50: according to the voltage-voltage change rate curve, the speed of lithium ion diffusion in the battery is evaluated. In some possible implementations, according to the voltage-voltage change rate curve, the smaller the change rate, the faster the diffusion rate. At the end of relaxation of the battery of the embodiment of the present application, the bulk ion concentration tends to be uniform, and the smaller the voltage change rate, the more uniform the bulk ion concentration is within the same diffusion time, that is, the bulk ions diffuse faster within the same time.
[0074] In order to enable the above implementation details and operations of the present application to be clearly understood by those skilled in the art, as well as to demonstrate the significant improvement in the performance of the method for evaluating lithium ion diffusion rate based on the GITT test in the embodiment of the present application, the above technical solution is illustrated by means of multiple embodiments below.
[0075] Example 1
[0076] A method for evaluating lithium ion diffusion rate based on GITT test, comprising the following steps:
[0077] 1. NCA (LiNi 0.8 Co 0.15 Al 0.05 The ternary positive electrode material O2) is made into a button battery for standby use, and the button battery is activated by cycling 3 times at a rate of 0.1C.
[0078] 2. Perform GITT test on button cell. In the charging test phase, apply 0.1C forward current and keep it for 10min, then interrupt the current and relax it for 30min, repeat the above steps until the charging cut-off voltage reaches 4.3V; in the discharge test phase, apply 0.1C reverse current and keep it for 10min, then interrupt the current and relax it for 30min, repeat the above steps until the discharge cut-off voltage reaches 2.5V, and obtain the time-voltage GITT curve, as shown in the attached figure. Figure 2 shown.
[0079] 3. After polynomial fitting of the obtained GITT curve data, the voltage is derived to obtain the time-voltage change rate curve, as shown in the attached figure. Figure 3 (Charging stage) and Figure 4 (Discharge phase) as shown.
[0080] 4. Take the voltage change rate value and the corresponding voltage value at the end of each relaxation, and draw the final voltage (x-axis)-voltage change rate (y-axis) curve, as shown in the attached figure. Figure 5 and attached Figure 6 As shown, Figure 6 Yes Figure 5 A local enlarged view is provided to facilitate more obvious observation of voltage changes.
[0081] 5. Through intuitive analysis Figure 5 and attached Figure 6 The voltage change rate in the figure can be used to simply and quickly evaluate the speed of lithium ion diffusion rate at different stages of charge and discharge without further calculation. It can be seen from the figure that the lithium ion diffusion in the discharge stage is faster than that in the charge stage, and there is an obvious voltage change rate fluctuation at the end of charge and the beginning of discharge, indicating that the lithium diffusion rate in these two stages is slow.
[0082] Example 2
[0083] A method for evaluating lithium ion diffusion rate based on GITT test, comprising the following steps:
[0084] 1. Assemble NCA and NCM622 materials into button batteries for standby use, and activate the two button batteries by cycling them at a rate of 0.1C for 3 cycles.
[0085] 2. Perform GITT test on the two button cells, only test the charging stage curve, apply 0.1C forward current and keep it for 10min, then interrupt the current relaxation and keep it for 60min, repeat the above steps until the charging cut-off voltage of 4.3V is reached, and the time-voltage GITT charging curves of the two materials are obtained.
[0086] 3. After polynomial fitting of the obtained GITT curve, the voltage is derived to obtain the voltage-voltage change rate curve, as shown in the attached figure. Figure 7 and attached Figure 8 As shown, Figure 8 Yes Figure 7 The local enlarged view makes it easier to observe the voltage change rate.
[0087] 4. Through intuitive analysis Figure 7 and attached Figure 8 The voltage change rate in the figure can be used to simply and quickly evaluate the lithium ion diffusion rate of the two different materials during the charging stage without further calculation. As can be seen from the figure, the voltage change rate of NCM622 is smaller than that of NCA overall, and the fluctuation is also smaller, indicating that the lithium ion diffusion rate of NCM622 is faster than that of NCA material.
[0088] Example 3
[0089] Comparative Example 1
[0090] A method for evaluating lithium ion diffusion rate based on GITT test, comprising the following steps:
[0091] 1. NCA (LiNi 0.8 Co 0.15 Al 0.05 The ternary positive electrode material O2) is made into a button battery for standby use, and the button battery is activated by cycling 3 times at a rate of 0.1C.
[0092] 2. The GITT test method is the same as that in Example 1, and a time-voltage GITT curve is obtained, as shown in the attached figure. Figure 2 shown.
[0093] 3. The lithium ion diffusion rate under different SOC states is calculated by the GITT calculation formula. The calculation formula is as follows:
[0094]
[0095] When the external current is very small, The linear relationship can be further simplified as follows:
[0096]
[0097] In the above formula, τ is the relaxation time, nm is the number of moles, V m is the molar volume of the electrode material, S is the contact area between the electrode and the electrolyte, △E s is the voltage change caused by the pulse, △E t is the voltage change of constant current charge and discharge. The above parameters can be obtained from material data and GITT curve. For example, a section of GITT curve can be intercepted for analysis, as shown in the attached figure. Fig. 9 By repeatedly intercepting the GITT curves under different SOC states to obtain parameters and calculate, the lithium ion diffusion rate under all different SOCs can be obtained, as shown in the attached figure. Fig.10 shown.
[0098] It can be clearly seen from the analysis of the above embodiments and comparative examples that the data processing method in the embodiments of the present application is simple and efficient, and the lithium ion diffusion rates of different states and different materials can be compared without additional calculation formulas and complex parameter calculations. This method has strong applicability and a wide range of applications. It is very suitable for scenarios where there is no need to calculate specific lithium ion diffusion rate values, and only the kinetic performance of products needs to be compared.
[0099] In contrast, although the conventional GITT method in comparative example 1 can calculate the specific lithium ion diffusion rate value, the parameter acquisition fluctuates greatly, which also leads to poor comparability of the final calculation results, and is more suitable for academic mechanism research rather than industrial production evaluation. Therefore, the method of the embodiment of the present application has opened up a fast and effective technical route for industrial evaluation of the kinetic performance of lithium ion battery materials.
[0100] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for evaluating lithium ion diffusion rate based on GITT test, characterized in that: The following steps are involved: Obtaining a button cell to be tested and performing activation treatment to obtain an activated cell; Performing a constant current intermittent titration test on the activated battery to obtain a time-voltage curve; Performing polynomial fitting and derivation processing on the time-voltage curve in sequence to obtain a time-voltage change rate curve; Draw a voltage-voltage change rate curve based on the voltage change rate value and the corresponding voltage value; The speed of lithium ion diffusion in the battery is evaluated based on the voltage-voltage change rate curve.
2. The method for evaluating lithium ion diffusion rate based on GITT test according to claim 1, characterized in that: The polynomial fitting is processed by a polynomial function or a polynomial fitting function of a data processing software; And / or, the derivation processing step includes: derivatizing the voltage data after the polynomial fitting with respect to the time data to obtain a curve of the rate of change of voltage over time, that is, the time-voltage rate of change curve.
3. The method for evaluating lithium ion diffusion rate based on GITT test according to claim 2, characterized in that: The step of drawing the voltage-voltage change rate curve includes: drawing the voltage-voltage change rate curve according to the voltage change rate value and the corresponding voltage value at the end of each relaxation.
4. The method for evaluating lithium ion diffusion rate based on GITT test according to any one of claims 1 to 3, characterized in that: The counter electrode in the button cell to be tested is lithium metal, and the potential of the counter electrode is 0; And / or, the smaller the change rate of the voltage-voltage change rate curve is, the faster the lithium ion diffusion rate is.
5. The method for evaluating lithium ion diffusion rate based on GITT test according to claim 4, characterized in that: The activation treatment conditions include: cycling for 1 to 3 times within a rate range of 0.02C to 0.1C.
6. The method for evaluating lithium ion diffusion rate based on GITT test according to claim 5, characterized in that: The activation treatment has a cycle ratio of 0.1C and a cycle number of 3.
7. The method for evaluating lithium ion diffusion rate based on GITT test according to any one of claims 1 to 3, 5 to 6, characterized in that: The steps of the constant current intermittent titration test include: under the conditions of a current density of 0.1C, a constant current time of 5min to 20min, and a static relaxation time of 30min to 120min, repeating the constant current and static relaxation procedures until the battery voltage reaches the upper or lower limit of the test interval.
8. The method for evaluating lithium ion diffusion rate based on GITT test according to claim 7, characterized in that: When the electrode material is a positive electrode material, the constant current intermittent titration test is first performed in a charging test phase, and then in a discharging test phase; Alternatively, when the electrode material is a negative electrode material, the constant current intermittent titration test first performs a discharge test phase and then performs a charge test phase.
9. The method for evaluating lithium ion diffusion rate based on GITT test according to claim 8, characterized in that: In the charging test phase, a forward current with a current density of 0.1C is applied and the constant current is maintained for 5 to 20 minutes, and then the current is interrupted for static relaxation for 30 to 120 minutes, and constant current charging and static relaxation are repeated until the charging cut-off voltage is reached; And / or, in the discharge test phase, after applying a reverse current with a current density of 0.1C and maintaining the constant current for 5 minutes to 20 minutes, the current is interrupted for static relaxation for 30 minutes to 120 minutes, and the constant current discharge and static relaxation are repeated until the discharge cut-off voltage is reached.
10. The method for evaluating lithium ion diffusion rate based on GITT test according to claim 9, characterized in that: When the electrode material is a positive electrode material, the steps of the constant current intermittent titration test include: in a charging test phase, applying a forward current with a current density of 0.1C and maintaining the constant current for 10 minutes, interrupting the current for static relaxation for 60 minutes, repeating constant current charging and static relaxation until the charging cut-off voltage is reached; in a discharge test phase, applying a reverse current with a current density of 0.1C and maintaining the constant current for 10 minutes, interrupting the current for static relaxation for 60 minutes, repeating constant current discharge and static relaxation until the discharge cut-off voltage is reached; Alternatively, when the electrode material is a negative electrode material, the steps of the constant current intermittent titration test include: in a discharge test phase, applying a reverse current with a current density of 0.1C and maintaining the constant current for 10 minutes, interrupting the current for static relaxation for 60 minutes, repeating the constant current reverse charge and static relaxation until the reverse charge cutoff voltage is reached; in a charging test phase, applying a forward current with a current density of 0.1C and maintaining the constant current for 10 minutes, interrupting the current for static relaxation for 60 minutes, repeating the constant current charging and static relaxation until the charging cutoff voltage is reached.
Citation Information
Cited By
Method for measuring reaction rate constant of active particles of lithium ion battery
CN119688535A
A method for measuring reaction rate constants of active particles in lithium-ion batteries
CN119688535B
Method for testing cycle performance of battery negative electrode material
CN121476955A