Optical laminate and image display device
By providing an optical laminate with phase difference layer and printing layer with specified optical characteristics in the image display device, the problem of obvious differences in appearance between the display area and the non-display area is solved, and a seamless effect from the front and inclined directions is achieved. Improves design and concealment.
Patent Information
- Application Number
- CN202410573626.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2024-05-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When the existing image display device is not displayed, the appearance difference between the display area and the non-display area is obvious, making it difficult to improve from a design perspective.
Two polarizers are laminated coaxially on the visible side of the display element of the image display device, and a phase difference layer and a printing layer with specified optical characteristics are provided therebetween to ensure that it is difficult to identify the display area and non-display when viewed from the front and the inclined surfaces. The appearance difference of the area. The specific configuration includes a first polarizer, a phase difference layer, a printing layer and a second polarizer, the phase difference layer includes a birefringent phase difference film, and the first polarizer is substantially parallel to the absorption axis direction of the second polarizer.
It realizes seamless appearance of the display area and the non-display area when viewed from the front and inclined directions, improves the appearance design and conceals components such as wiring and terminals.
Smart Images

Figure CN118938372A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an optical layered body and an image display device. Background Art
[0002] In recent years, automobiles are equipped with displays for various purposes such as various instrument displays, car navigation, reversing monitors, and audio-visual equipment. In such in-vehicle displays, generally, a colored portion is provided along the periphery of the display screen for the purpose of making the display frame, instrument panel, console and other peripheral components coordinate with the appearance, shielding wiring, terminals, etc., etc., thereby forming a display area and a non-display area. In addition, in general-purpose or business-use tablet terminals, a colored portion is often provided along the periphery of the display screen.
[0003] In an image display device having a colored portion along the periphery of a display screen, there is sometimes a noticeable difference in appearance between the display area (black screen) and the non-display area (colored portion) when the display is not in progress (when the power is off), and improvements are required from the perspective of appearance design.
[0004] Regarding the above-mentioned demand, Patent Document 1 proposes a display body that reduces the color difference between a display area and a non-display area during non-display. However, there is a demand for further improvement.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2020-192708 Summary of the invention
[0008] Problems to be solved by the invention
[0009] The present invention is completed to solve the above-mentioned problems, and its main purpose is to provide an image display device provided with a colored portion forming a display area and a non-display area in a display screen, and it is difficult to distinguish the difference in appearance between the display area and the non-display area when not displayed.
[0010] Means used to solve problems
[0011] In order to solve the above problems, the inventors have conducted in-depth research and found that by coaxially stacking two polarizers on the visible side of the display element in the image display device, and arranging a printed layer (coloring portion) therebetween, it is difficult to identify the difference in appearance between the display area and the non-display area when non-displaying. On the other hand, according to such a structure, compared with the situation of observing from the front direction, when observing from the oblique direction, there is a tendency that the above-mentioned appearance is different and obvious. Therefore, the inventors have further repeatedly studied and found that by coaxially stacking two polarizers on the visible side of the display element, a phase difference layer and a printed layer with specified optical properties are sequentially arranged toward the visible side therebetween, so that it is difficult to identify the difference in the above-mentioned appearance in the two directions of the front direction and the oblique direction, thereby completing the present invention. That is, according to an embodiment of the present invention, the following optical laminate and image display device are provided.
[0012] [1] An optical laminate according to an embodiment of the present invention comprises, in order: a first polarizer comprising a first polarizer, a phase difference layer having a phase difference in a thickness direction, a printed layer, and a second polarizer comprising a second polarizer, wherein the phase difference layer comprises a phase difference film having birefringence in a thickness direction, and the absorption axis direction of the first polarizer is substantially parallel to the absorption axis direction of the second polarizer.
[0013] [2] In the optical laminate described in [1] above, the absolute value of the phase difference value Rth(550) in the thickness direction of the above-mentioned phase difference layer (more specifically, the absolute value of the sum of Rth(550) of all phase difference films having birefringence in the thickness direction contained in the above-mentioned phase difference layer) can be greater than 100 nm.
[0014] [3] In the optical laminate described in [1] or [2] above, the phase difference film having birefringence in the thickness direction may include a phase difference film having a refractive index characteristic of nx>ny>nz, nx>nz>ny or nz>nx=ny when the refractive index in the slow axis direction is set to "nx", the refractive index in the fast axis direction is set to "ny" and the refractive index in the thickness direction is set to "nz".
[0015] [4] In the optical laminate described in any one of [1] to [3] above, the phase difference film having birefringence in the thickness direction has an in-plane phase difference, and its slow axis direction can be substantially parallel to the absorption axis directions of the first polarizer and the second polarizer.
[0016] [5] In the optical layered body according to any one of [1] to [4] above, the printed layer may have a thickness of 3 μm to 30 μm.
[0017] [6] The optical layered body described in any one of [1] to [5] may further include a surface substrate layer on the side of the second polarizer opposite to the side on which the retardation layer is disposed.
[0018] [7] An image display device according to an embodiment of the present invention comprises, in order toward the visible side: a display element and the optical layered body described in any one of [1] to [6] above, wherein the optical layered body is arranged so that the second polarizer is closer to the visible side than the first polarizer.
[0019] [8] In the image display device described in [7] above, the display element may include a liquid crystal unit, an organic electronic element, or an inorganic electronic element.
[0020] [9] The image display device described in [7] or [8] above may further include a touch panel.
[0021]
[10] In the image display device described in any one of [7] to [9] above, the display element is a liquid crystal unit, and the image display device may include, in order toward the visible side: a third polarizer including a third polarizer, the liquid crystal unit, and the optical laminate.
[0022] Effects of the Invention
[0023] The optical laminate according to the embodiment of the present invention comprises: a first polarizing plate including a first polarizer, a phase difference layer having a predetermined optical characteristic, a printed layer, and a second polarizing plate including a second polarizer, wherein the absorption axis direction of the first polarizer is substantially parallel to the absorption axis direction of the second polarizer. By arranging the optical laminate having such a structure on the visible side of the display element, it is difficult to recognize the difference between the appearance of the display area and the non-display area when the image display device is observed from the front direction and the oblique direction when the display is not displayed. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1A (a) is a schematic cross-sectional view of an optical layered body according to one embodiment of the present invention, and (b) is a schematic plan view of the optical layered body shown in (a).
[0025] Figure 1B This is a schematic cross-sectional view of an optical layered body according to one embodiment of the present invention.
[0026] Figure 2A This is a schematic cross-sectional view of an image display device according to one embodiment of the present invention.
[0027] Figure 2B This is a schematic cross-sectional view of an image display device according to one embodiment of the present invention.
[0028] Figure 2C This is a schematic cross-sectional view of an image display device according to one embodiment of the present invention.
[0029] Explanation of symbols
[0030] 10. First polarizer
[0031] 20 First phase difference layer
[0032] 30 Second polarizer
[0033] 40 Printing Layers
[0034] 50 Surface substrate layer
[0035] 60 Second phase difference layer
[0036] 100 Optical laminate
[0037] 110 Backlight unit
[0038] 120 Third polarizer
[0039] 130 Liquid crystal unit
[0040] 140 Organic EL elements
[0041] 150 Touch Panel
[0042] 200 Image display device DETAILED DESCRIPTION
[0043] Hereinafter, preferred embodiments of the present invention will be described, but the present invention is not limited to these embodiments. In addition, in this specification, "to" indicating a numerical range includes the numerical values of the upper limit and the lower limit.
[0044] (Definition of Terms and Symbols)
[0045] The definitions of terms and symbols in this specification are as follows.
[0046] (1) Refractive index (nx, ny, nz)
[0047] “nx” is the refractive index in the direction where the refractive index in the plane is maximum (ie, the slow axis direction), “ny” is the refractive index in the direction orthogonal to the slow axis in the plane (ie, the fast axis direction), and “nz” is the refractive index in the thickness direction.
[0048] (2) In-plane phase difference (Re)
[0049] "Re(λ)" is the in-plane phase difference measured at 23°C using light of wavelength λnm. For example, "Re(550)" is the in-plane phase difference measured at 23°C using light of wavelength 550nm. Re(λ) is obtained by the formula: Re(λ) = (nx-ny) × d, when the thickness of the layer (film) is set to d (nm).
[0050] (3) Retardation in the thickness direction (Rth)
[0051] "Rth(λ)" is the phase difference in the thickness direction measured at 23°C using light of wavelength λnm. For example, "Rth(550)" is the phase difference in the thickness direction measured at 23°C using light of wavelength 550nm. Rth(λ) is obtained by the formula: Rth(λ) = (nx-nz) × d, when the thickness of the layer (film) is set to d (nm).
[0052] (4) Nz coefficient
[0053] The Nz coefficient is obtained using Nz=Rth / Re.
[0054] (5) Angle
[0055] Unless otherwise specified, when an angle is mentioned in this specification, the angle includes both clockwise and counterclockwise relative to the reference direction. Therefore, for example, "45°" means 45° along the clockwise or counterclockwise direction. In addition, in this specification, "substantially parallel" and "approximately parallel" include situations within the range of 0°±10°, preferably within the range of 0°±5°, more preferably within the range of 0°±3°, and further preferably within the range of 0°±1°, and "substantially orthogonal" and "approximately orthogonal" include situations within the range of 90°±10°, preferably within the range of 90°±5°, more preferably within the range of 90°±3°, and further preferably within the range of 90°±1°.
[0056] (6) The terms “layer”, “board”, “sheet” and “film” are not distinguished from each other merely based on the difference in name. For example, the term “layer” is a concept that includes components that can be called “board”, “sheet” and “film”.
[0057] A. Optical laminate
[0058] The optical laminate of the embodiment of the present invention comprises in sequence: a first polarizer including a first polarizer, a phase difference layer having a phase difference in the thickness direction (hereinafter, also referred to as the "first phase difference layer"), a printed layer, and a second polarizer including a second polarizer, wherein the first phase difference layer comprises a phase difference film having birefringence in the thickness direction, and the absorption axis direction of the first polarizer is substantially parallel to the absorption axis direction of the second polarizer. The optical laminate is preferably used in an image display device, in which case the optical laminate is arranged on the visible side of a display element such as an organic electroluminescent (EL) element, an inorganic EL element, a liquid crystal unit, etc. in such a manner that the second polarizer is closer to the visible side than the first polarizer. According to this configuration, it is difficult to recognize the difference in appearance between the display area and the non-display area when the image display device is not displayed when viewed from the front direction and the oblique direction. In addition, in this specification, sometimes the difference in appearance between the display area and the non-display area that is difficult to recognize (making it inconspicuous) is referred to as "seamless display area and non-display area".
[0059] A-1. Overall structure of optical layered body
[0060] Figure 1A 1 is a schematic cross-sectional view (a) and a schematic top view (b) of an optical layered body according to one embodiment of the present invention. Figure 1A In the optical laminate 100A shown, a first polarizing plate 10 including a first polarizer 12, a first phase difference layer 20 having a phase difference in the thickness direction, and a second polarizing plate 30 including a second polarizer 32 are sequentially arranged, and a printed layer 40 is provided on a portion of the main surface of the second polarizing plate 30 on the side where the first phase difference layer 20 is arranged. In the optical laminate 100A, the absorption axis direction of the first polarizer 12 is substantially parallel to the absorption axis direction of the second polarizer 32. The first phase difference layer 20 having a phase difference in the thickness direction includes a phase difference film having birefringence in the thickness direction. Figure 1A In the embodiment, the printed layer 40 is provided with a predetermined width along the outer edge of the main surface of the first phase difference layer 20 side of the second polarizer 30. When the optical laminate 100A is arranged on the visible side of the display element to constitute an image display device, in the display screen, the portion A where the printed layer 40 is not provided becomes the display area, and the portion B where the printed layer 40 is provided becomes the non-display area, thereby making it possible to conceal components such as wiring and terminals provided around the display element.
[0061] In the optical laminate 100A, a surface substrate layer 50 is disposed on the visible side (opposite to the side where the first retardation layer 20 is disposed) of the second polarizing plate 30. The surface substrate layer 50 can function as a front plate of the image display device. The surface substrate layer 50 can be omitted depending on the purpose.
[0062] Figure 1BThis is a schematic cross-sectional view of an optical layered body according to another embodiment of the present invention. Figure 1B The optical laminate 100B shown is different from the optical laminate 100A in that a second phase difference layer 60 is provided on the side opposite to the side where the first phase difference layer 20 is arranged on the first polarizer 10. The second phase difference layer 60 functions as a circular polarizer together with the first polarizer 10, for example. When the optical laminate 100B is applied to an organic EL display device, it is possible to appropriately achieve an anti-reflection function and seamlessness.
[0063] Each component constituting the optical laminate can be laminated via any appropriate adhesive layer (adhesive layer, adhesive layer, etc.), or can be laminated without an adhesive layer. In the example shown in the figure, the first phase difference layer 20 and the second polarizer 30 are laminated via an adhesive layer 70. The optical laminate 100A and 100B can further have an adhesive layer for laminating components adjacent to the display element, etc. on the outside of the first polarizer 10 and the second phase difference layer 60, respectively. In this case, the adhesive layer is typically protected by a release liner until it is used. In addition, the printed layer 40 can be arranged on the side surface of the second polarizer 30 of the first phase difference layer 20, which is different from the example shown in the figure.
[0064] The total light transmittance of the display region of the optical laminate is, for example, more than 35.0%, preferably 39.0% to 42.5%, and more preferably 42.5% to 45%.
[0065] The thickness of the optical layered body is, for example, 100 μm to 4000 μm, or preferably 200 μm to 2000 μm.
[0066] A-2. First polarizer and second polarizer
[0067] The first polarizer 10 and the second polarizer 30 respectively include polarizers, and typically further include a protective layer disposed on one side or both sides of the polarizer. The first polarizer and the second polarizer may have the same structure or different structures. As long as there is no special description about the polarizer and the protective layer that the first polarizer and the second polarizer may include, the following description may be applied in the same manner.
[0068] A-2-1. Polarizer
[0069] The polarizer is typically composed of a polyvinyl alcohol-based resin film containing a dichroic substance (for example, iodine). The polarizer may be composed of a single-layer resin film or may be produced using a laminate of two or more layers.
[0070] Specific examples of polarizers composed of a single-layer resin film include polarizers obtained by dyeing and stretching hydrophilic polymer films such as polyvinyl alcohol (PVA) films, partially formalized PVA films, and partially saponified films of ethylene-vinyl acetate copolymers using dichroic substances such as iodine and dichroic dyes, and polyene-based oriented films such as dehydrated PVA and dehydrochlorinated polyvinyl chloride films. Due to its excellent optical properties, it is preferred to use a polarizer obtained by dyeing a PVA film with iodine and uniaxially stretching it.
[0071] The dyeing using iodine is performed, for example, by immersing the PVA membrane in an iodine aqueous solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching can be performed after the dyeing treatment or while dyeing. In addition, dyeing can be performed after stretching. As needed, the PVA membrane is subjected to swelling treatment, cross-linking treatment, cleaning treatment, drying treatment, etc. For example, by immersing the PVA membrane in water and washing it with water before dyeing, not only can the dirt and anti-blocking agent on the surface of the PVA membrane be washed away, but the PVA membrane can also be swelled to prevent uneven dyeing.
[0072] As a specific example of a polarizer obtained using a laminate, there can be cited a polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate. The polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate can be made, for example, by the following method: a PVA-based resin solution is coated on a resin substrate, and the PVA-based resin layer is formed on the resin substrate by drying, thereby obtaining a laminate of the resin substrate and the PVA-based resin layer; and the PVA-based resin layer is made into a polarizer by stretching and dyeing the above-mentioned laminate. In the present embodiment, stretching typically includes immersing the laminate in a boric acid aqueous solution for stretching. In addition, stretching may further include stretching the laminate in the air at a high temperature (e.g., above 95°C) before stretching in a boric acid aqueous solution as required. The obtained laminate of resin substrate / polarizer can be used directly (that is, the resin substrate can be used as a protective layer of the polarizer), or the resin substrate can be peeled off from the laminate of resin substrate / polarizer, and any appropriate protective layer corresponding to the purpose can be laminated on the peeled surface before use. The details of the manufacturing method of such a polarizer are described in, for example, Japanese Patent Publication No. 2012-73580. The entire contents of the publication are cited in this specification as a reference.
[0073] The thickness of the polarizer is, for example, 30 μm or less, preferably 15 μm or less, more preferably 1 μm to 12 μm, further preferably 2 μm to 10 μm, and further more preferably 2 μm to 8 μm.
[0074] The polarizer preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The single transmittance of the polarizer is, for example, 41.0% or more, preferably 43.0% to 46.0%, and more preferably 44.5% to 46.0%. The polarization degree of the polarizer is preferably 97.0% or more, more preferably 99.0% or more, and further preferably 99.9% or more.
[0075] A-2-2. Protective layer
[0076] The protective layer is made of any suitable film that can be used as the protective layer of the polarizer. As the specific example of the material that becomes the main component of the film, cellulose resins such as triacetyl cellulose (TAC), polyester resins, polyvinyl alcohol resins, polycarbonate resins, polyamide resins, polyimide resins, polyether sulfone resins, polysulfone resins, polystyrene resins, polynorbornene resins, polyolefin resins, (methyl) acrylic resins, transparent resins such as acetate resins, etc. can be enumerated. In addition, thermosetting resins or ultraviolet curing resins such as (methyl) acrylic acid, carbamate, (methyl) acrylic acid carbamate, epoxy, silicone can also be enumerated. In addition, glassy polymers such as siloxane polymers can also be enumerated. In addition, the polymer film recorded in Japanese Patent Publication No. 2001-343529 (WO01 / 37007) can also be used. As the material of the film, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain and a thermoplastic resin having a substituted or unsubstituted phenyl and nitrile group in the side chain can be used, for example, a resin composition containing an alternating copolymer formed by isobutylene and N-methylmaleimide and an acrylonitrile-styrene copolymer can be mentioned. The polymer film can be, for example, an extrusion molding of the above resin composition.
[0077] The thickness of the protective layer is typically 300 μm or less, preferably 100 μm or less, more preferably 5 μm to 80 μm, and further preferably 10 μm to 60 μm. When surface treatment is performed, the thickness of the protective layer includes the thickness of the surface treatment layer.
[0078] A-3. First phase difference layer
[0079] The first phase difference layer 20 has a phase difference in the thickness direction. In addition, the first phase difference layer 20 includes a phase difference film having birefringence in the thickness direction. The first phase difference layer may include only one phase difference film having birefringence in the thickness direction, or may include two or more. By configuring such a phase difference layer between the first polarizer and the printed layer and the second polarizer, when the optical laminate is configured on the visible side of the display element, it is possible to suppress light leakage in the oblique direction, resulting in improved seamlessness in the oblique direction. In addition, in this specification, "a phase difference film having birefringence in the thickness direction" refers to a phase difference film having ny / nz less than 1 or greater than 1, preferably having an Nz coefficient of less than 0.9 or greater than 1.1. Representatively, the "phase difference film having birefringence in the thickness direction" does not include a phase difference film (positive A plate) and an isotropic film having a refractive index characteristic of nx>ny=nz. Here, "ny=nz" includes not only the case where ny and nz are completely equal, but also the case where they are substantially equal. Therefore, the positive A plate may have an Nz coefficient of, for example, more than 0.9 and less than 1.1. The isotropic film refers to a film satisfying the relationship of Re(550)<10 nm and -10 nm<Rth(550)<10 nm.
[0080] The absolute value of the phase difference value Rth(550) in the thickness direction of the first phase difference layer is preferably greater than 100 nm, for example, it can be greater than 250 nm, greater than 400 nm, or greater than 550 nm. In addition, the upper limit of the absolute value of Rth(550) of the first phase difference layer is not particularly limited, for example, it can be less than 1000 nm. When the Rth(550) of the first phase difference layer is in such a range, the effect of the present invention can be suitably obtained. When the first phase difference layer includes more than two phase difference films, the Rth(550) of the first phase difference layer is calculated as the sum of the Rth(550) of all phase difference films having birefringence in the thickness direction contained in the first phase difference layer.
[0081] As a phase difference film having birefringence in the thickness direction, any appropriate phase difference film can be used as long as the effect of the present invention can be obtained. For example, a phase difference film having a refractive index characteristic of nz>nx=ny, nx=ny>nz, nx>ny>nz, nx>nz>ny or nz>nx>ny can be preferably exemplified, among which a phase difference film having a refractive index characteristic of nz>nx=ny, nx>ny>nz or nx>nz>ny is preferred. In addition, when the phase difference film having birefringence in the thickness direction has an in-plane phase difference (for example, when having Re(550) of 10 nm or more, 20 nm or more, or for example, 200 nm or less), the phase difference film is preferably configured in such a manner that the slow axis direction is substantially parallel to the absorption axis direction of the first polarizer and the second polarizer.
[0082] In order to make the phase difference value (for example, Rth (550)) of the first phase difference layer in the thickness direction into the desired range, the phase difference film having birefringence in the thickness direction can be used alone, or a plurality of the same or different phase difference films (for example, phase difference values, refractive index characteristics, phase difference films with different formation materials, etc.) can be used in combination. The number of combined phase difference films is not limited as long as the effect of the present invention can be obtained. In the case of using a plurality of phase difference films in combination, each phase difference film can be integrated via an adhesive layer.
[0083] The phase difference value in the thickness direction of the phase difference film (positive C plate) having the refractive index characteristic of nz>nx=ny can be appropriately set according to the desired phase difference value of the first phase difference layer, the presence or absence of the phase difference film used in combination or its phase difference value, manufacturability, etc., for example, it can be less than -50nm, less than -200nm, or less than -400nm. In one embodiment, the positive C plate has an Rth(550) of -50nm to -300nm, preferably -70nm to -250nm, and more preferably -90nm to -200nm. The Re(550) of the positive C plate can be less than 10nm.
[0084] The positive C plate can be formed of any appropriate material. The positive C plate is preferably formed of a film containing a liquid crystal material fixed in a vertical orientation. The liquid crystal material (liquid crystal compound) capable of vertical orientation can be a liquid crystal monomer or a liquid crystal polymer. As a specific example of the method for forming the liquid crystal compound and the positive C plate, there can be cited the method for forming the liquid crystal compound and the phase difference film described in
[0020] to
[0028] of Japanese Patent Gazette No. 2002-333642. In this case, the thickness of the positive C plate is preferably 0.5μm to 10μm, more preferably 0.5μm to 8μm, and further preferably 0.5μm to 5μm.
[0085] The phase difference value in the thickness direction of the phase difference film (negative B plate) having the refractive index characteristic of nx>ny>nz can be appropriately set according to the desired phase difference value of the first phase difference layer, the presence or absence of the phase difference film used in combination or its phase difference value, manufacturability, etc. In one embodiment, the negative B plate has an Rth (550) of, for example, 50nm to 400nm, preferably 70nm to 350nm, and more preferably 90nm to 300nm. The Nz coefficient of the negative B plate is, for example, greater than 1.1, preferably greater than 3, and more preferably greater than 5.
[0086] The negative B plate is formed of, for example, a resin film, and the resin film is formed of any appropriate resin capable of achieving the above-mentioned characteristics. As the resin forming the resin film, for example, polycarbonate resins, cyclic olefin resins, cellulose resins, polyester resins, polyvinyl alcohol resins, polyamide resins, polyimide resins, polyether resins, polystyrene resins, acrylic resins, polyester carbonate resins can be cited. Among these, cyclic olefin resins or polycarbonate resins can be appropriately used.
[0087] Cyclic olefin resin is a general term for resins that are polymerized using cyclic olefins as polymerization units, and examples thereof include resins described in Japanese Patent Publication No. 1-240517, Japanese Patent Publication No. 3-14882, and Japanese Patent Publication No. 3-122137. As specific examples, there are: ring-opening (copolymer) polymers of cyclic olefins, addition polymers of cyclic olefins, copolymers of cyclic olefins with α-olefins such as ethylene and propylene (representatively random copolymers), and grafted modified products modified with unsaturated carboxylic acids and their derivatives, as well as their hydrogenated products. As specific examples of cyclic olefins, there are norbornene monomers. As norbornene monomers, there are monomers described in Japanese Patent Publication No. 2015-210459, etc. The above-mentioned cyclic olefin resins are available in various products on the market. Specific examples include: products named “ZEONEX” and “ZEONOR” manufactured by ZEON Corporation of Japan, “Arton” manufactured by JSR Corporation, “TOPAS” manufactured by TICONA Corporation, and “APEL” manufactured by Mitsui Chemicals, Inc.
[0088] As a polycarbonate resin, any appropriate polycarbonate resin can be used as long as the effect of the present invention can be obtained. Preferably, the polycarbonate resin comprises a structural unit derived from an isosorbide-based dihydroxy compound and a structural unit derived from at least one dihydroxy compound selected from alicyclic diols, alicyclic dimethanol, diethylene glycol, triethylene glycol or polyethylene glycol and an alkylene glycol or spiro glycol. More preferably, the polycarbonate resin comprises a structural unit derived from an isosorbide-based dihydroxy compound, a structural unit derived from alicyclic dimethanol and / or a structural unit derived from diethylene glycol, triethylene glycol or polyethylene glycol. The polycarbonate resin may include a structural unit derived from other dihydroxy compounds as required. In addition, the details of the polycarbonate resin and the method for manufacturing the phase difference film that can be appropriately used in the present invention are, for example, recorded in International Publication Gazette No. 2011 / 062239, which is cited in this specification as a reference.
[0089] The negative B plate is produced by stretching the resin film. The stretching temperature and stretching ratio can be appropriately set according to the desired thickness direction retardation value and thickness of the negative B plate, the type of resin used, Tg, and the like.
[0090] The thickness of the negative B plate is, for example, 10 μm to 150 μm, preferably 10 μm to 100 μm, and more preferably 10 μm to 30 μm.
[0091] The phase difference value in the thickness direction of the phase difference film (Z plate) having the refractive index characteristic of nx>nz>ny can be appropriately set according to the desired phase difference value of the first phase difference layer, the presence or absence of the phase difference film used in combination or its phase difference value, manufacturability, etc. In one embodiment, the Z plate has an Rth (550) of, for example, 50nm to 300nm, preferably 70nm to 250nm, and more preferably 90nm to 200nm. The Nz coefficient of the Z plate is, for example, 0.1 to 0.5, preferably 0.15 to 0.45, and more preferably 0.2 to 0.4.
[0092] The Z plate is typically formed of a resin film, and the resin film is formed of any appropriate resin that can achieve the above-mentioned characteristics. As the resin forming the resin film, for example, polycarbonate resins, cyclic olefin resins, cellulose resins, polyester resins, polyvinyl alcohol resins, polyamide resins, polyimide resins, polyether resins, polystyrene resins, acrylic resins, polyester carbonate resins can be cited. Among these, cyclic olefin resins or polycarbonate resins can be preferably used, and cyclic olefin resins or polycarbonate resins that can form Z plates can be preferably exemplified.
[0093] The Z plate can be formed, for example, by applying a coating liquid obtained by dissolving or dispersing the above-mentioned resin in any appropriate solvent on a shrinkable film to form a coating film, and shrinking the coating film. Representatively, with respect to the shrinkage of the coating film, the shrinkable film and the laminate of the coating film are heated to shrink the shrinkable film, and the coating film is shrunk by the shrinkage of such a shrinkable film. The shrinkage rate of the coating film is preferably 0.50 to 0.99, more preferably 0.60 to 0.98, and further preferably 0.70 to 0.95. The heating temperature is preferably 130°C to 170°C, and more preferably 150°C to 160°C. In one embodiment, when shrinking the coating film, the laminate can be stretched in a direction orthogonal to the shrinkage direction. In this case, the stretching ratio of the laminate is preferably 1.01 to 3.0 times, more preferably 1.05 to 2.0 times, and further preferably 1.10 to 1.50 times. Specific examples of materials constituting the shrinkable film include polyolefin resins, polyester resins, acrylic resins, polyamide resins, polycarbonate resins, norbornene resins, polystyrene resins, polyvinyl chloride resins, polyvinylidene chloride resins, cellulose resins, polyethersulfone resins, polysulfone resins, polyimide resins, acetate resins, polyarylate resins, polyvinyl alcohol resins, and liquid crystal polymers. These can be used alone or in combination. The shrinkable film is preferably a stretched film formed from these materials.
[0094] The thickness of the Z plate is, for example, 10 μm to 150 μm, preferably 10 μm to 100 μm, and more preferably 10 μm to 30 μm.
[0095] The thickness (total thickness) of the first retardation layer is, for example, 1 μm to 500 μm, or preferably 1 μm to 300 μm.
[0096] A-4. Printing layer
[0097] The printed layer 40 is a colored layer obtained by coloring by printing according to the purpose and the desired design. The printed layer can be a design layer that implements a specified design, or it can be a solid colored layer. The printed layer is preferably a solid colored layer, and more preferably a colored layer of dark colors such as black, blue, dark blue, purple, and tea (for example, L* of the L*a*b* color space of the SCI method is 50 or less, a* value is +10 to -10, and b* value is in the range of +10 to -10), and further preferably a colored layer of black (for example, L* of the L*a*b* color space of the SCI method is 20 or less, a* value is +5 to -5, and b* value is in the range of +5 to -5). By forming the printed layer into a black colored layer, wiring, terminals, backlights, and other components can be appropriately concealed in non-display areas.
[0098] The printed layer can be formed by any appropriate pattern corresponding to the purpose. Typically, the printed layer is formed in a frame shape along the outer periphery on the main surface of the polarizer, for example, it can be formed at a position corresponding to the frame. If it is such a structure, the non-display area can be concealed without using a frame.
[0099] The printed layer can be formed by any appropriate printing method using the printed layer-forming composition, and specific examples of the printing method include gravure printing, offset printing, screen printing, and transfer printing from a transfer sheet.
[0100] The composition for forming the printing layer typically includes a colorant, a solvent and / or a binder, and any appropriate additive that can be used as needed. As a binder, chlorinated polyolefins (such as chlorinated polyethylene, chlorinated polypropylene), polyester resins, urethane resins, acrylic resins, vinyl acetate resins, vinyl chloride-vinyl acetate copolymers, and cellulose resins can be cited. The binder resin can be used alone or in combination of two or more. In one embodiment, the binder resin is a thermal polymerizable resin. Compared with photopolymerizable resins, thermal polymerizable resins can be used in small amounts, so the amount of colorant used (the colorant content in the coloring layer) can be increased. As a result, in particular, in the case of forming a black coloring layer, a coloring layer with very small total light transmittance and excellent concealment can be formed. In one embodiment, the binder resin is a (meth) acrylic resin, preferably a (meth) acrylic resin containing a multifunctional monomer (such as pentaerythritol tri (meth) acrylate) as a copolymer component. By using a (meth) acrylic resin containing a multifunctional monomer as a copolymer component, a printing layer with an appropriate elastic modulus can be formed. In addition, a height difference caused by the thickness of the printed layer is also formed, and this height difference can effectively play a function of preventing sticking.
[0101] As a colorant, any appropriate colorant can be used according to the purpose and the desired color. The colorant can be a pigment or a dye, preferably a pigment. As specific examples of colorants, inorganic pigments such as titanium white, zinc white, carbon black, iron black, red iron oxide, chrome vermilion, ultramarine, cobalt blue, chrome yellow, titanium yellow, etc. can be cited; organic pigments or dyes such as phthalocyanine blue, indanthrene blue, isoindolinone yellow, benzidine yellow, quinacridone red, polyazo red, perylene red, and aniline black; metallic pigments formed by flaky foils such as aluminum and brass; pearlescent pigments (pearlescent pigments) formed by flaky foils such as titanium dioxide coated mica and basic lead carbonate. In the case of forming a black coloring layer, carbon black, iron black, and aniline black can be used appropriately. In this case, the colorant is preferably used in combination. This is because it can absorb visible light in a wide range and evenly to form a coloring layer without color (i.e., pure black). For example, in addition to the above-mentioned colorants, azo compounds and / or quinone compounds can also be used. In one embodiment, the colorant contains carbon black and other colorants (e.g., azo compounds and / or quinone compounds) as main components. According to such a composition, a coloring layer without coloring and excellent stability over time can be formed. In the case of forming a black coloring layer, the colorant can be used in a ratio of preferably 50 to 200 parts by weight relative to 100 parts by weight of the binder resin. In this case, the content of carbon black in the colorant is preferably 80% to 100%. By using the colorant (especially carbon black) in such a ratio, a coloring layer with very low total light transmittance and excellent stability over time can be formed.
[0102] The total light transmittance of the printed layer is preferably 0.01% or less, and more preferably 0.008% or less. When the total light transmittance is within such a range, the non-display area of the image display device can be well concealed.
[0103] The thickness of the printed layer is, for example, 3 μm to 30 μm, preferably 5 μm to 20 μm, and more preferably 10 μm to 15 μm. When the thickness of the printed layer is within this range, a seamless effect between the display area and the non-display area can be preferably obtained.
[0104] A-5. Surface base material layer
[0105] The surface substrate layer 50 can function as the front panel of the image display device. Thus, when the optical laminate is configured on the visible side of the display element, it is preferred that the surface substrate layer is configured to become the most superficial position. The surface substrate layer includes a substrate film, and as required, it can further include functional layers such as an anti-reflection layer, an anti-fouling layer, and a hard coat layer. The surface substrate layer preferably includes an anti-reflection layer. As an anti-reflection layer, for example, a thin layer type that prevents reflection by eliminating the reflected light based on the interference of light as disclosed in Japanese Patent Publication No. 2005-248173, a surface structure type that exhibits low reflectivity by giving a fine structure to the surface as disclosed in Japanese Patent Publication No. 2011-2759, etc. The functional layer can be used in combination with one or more than two kinds. As required, the functional layer can be laminated on the substrate film via an adhesive layer (for example, an adhesive layer, an adhesive layer) in a state formed on a support film, or it can be directly formed on the substrate film without an adhesive layer.
[0106] As the base film, a glass film (inorganic glass film) or a resin film can be used.
[0107] As the glass constituting the glass film, according to the classification based on the composition, for example, soda lime glass, boric acid glass, aluminosilicate glass, and quartz glass can be cited. In addition, according to the classification based on the alkali component, for example, alkali-free glass and low-alkali glass can be cited. The thickness of the glass film is preferably 100 μm to 2000 μm, and more preferably 200 μm to 1000 μm.
[0108] As the resin constituting the resin film, polyethylene terephthalate resin, polyethylene naphthalate resin, acetate resin, polyethersulfone resin, polycarbonate resin, polyamide resin, polyimide resin, polyamideimide resin, polyolefin resin, (meth) acrylic resin, polyvinyl chloride resin, polyvinylidene chloride resin, polystyrene resin, polyvinyl alcohol resin, polyarylate resin, polyphenylene sulfide resin, etc. can be cited. Among them, polyamide resin, polyimide resin, polyamideimide resin, polyethylene naphthalate resin, polycarbonate resin are preferred, and polyimide resin is more preferred. These resins can be used alone or in combination of two or more. The thickness of the resin film is preferably 100 μm to 2000 μm, and more preferably 200 μm to 1000 μm.
[0109] A-6. Adhesive layer
[0110] As the adhesive layer, any appropriate adhesive layer or adhesive layer that can be applied to optical purposes can be used. The total light transmittance of the adhesive layer is preferably 85% or more, more preferably 88% or more. In addition, the haze of the adhesive layer is preferably 1.0% or less, more preferably 0.8% or less. In one embodiment, the bonding of the first phase difference layer 20 and the second polarizer 30 is performed via an adhesive layer. The adhesive layer can appropriately fill the height difference of the end of the printed layer 40 provided between the first phase difference layer 20 and the second polarizer 30.
[0111] As the adhesive composition constituting the adhesive layer, any appropriate adhesive composition can be used. For example, adhesive compositions such as rubber, acrylic, silicone, urethane, vinyl alkyl ether, polyvinyl alcohol, polyvinyl pyrrolidone, polyacrylamide, and cellulose can be cited. Among them, acrylic adhesive compositions can be preferably used from the perspective of excellent optical transparency, and also from the perspective of excellent adhesive properties, weather resistance, heat resistance, etc.
[0112] The thickness (thickness in the display region) of the adhesive layer used for laminating the first retardation layer 20 and the second polarizer 30 is, for example, 50 μm to 1000 μm, preferably 200 μm to 750 μm, and more preferably 250 μm to 500 μm. The thickness of the adhesive layer that can be used for laminating any other constituent member can be, for example, 1 μm to 300 μm, preferably 5 μm to 100 μm, and more preferably 10 μm to 50 μm.
[0113] As the adhesive composition constituting the adhesive layer, any appropriate adhesive composition can be used. For example, water-based adhesives, solvent-based adhesives, emulsion-based adhesives, solvent-free adhesives, active energy ray-curable adhesives, and thermosetting adhesives can be mentioned. As active energy ray-curable adhesives, electron beam-curable adhesives, ultraviolet-curable adhesives, and visible light-curable adhesives can be mentioned. Preferably, a thermosetting adhesive or an ultraviolet-curable adhesive can be used.
[0114] The thickness of the adhesive layer is preferably 0.01 μm to 3.0 μm, more preferably 0.1 μm to 2.5 μm, and even more preferably 0.5 μm to 1.5 μm.
[0115] A-7. Second phase difference layer
[0116] The second phase difference layer 60 functions as a circular polarizer together with the first polarizer, for example. The second phase difference layer preferably includes a phase difference film (hereinafter referred to as "λ / 4 plate") that functions as a λ / 4 plate. The λ / 4 plate has, for example, Re(550) of 120nm to 160nm, preferably 135nm to 155nm. The λ / 4 plate may have, for example, a refractive index characteristic of nx>ny≥nz. The Nz coefficient of the λ / 4 plate is preferably 0.9 to 1.5, more preferably 0.9 to 1.3. The λ / 4 plate may be configured in such a way that the angle between its slow axis direction and the absorption axis direction of the first polarizer is, for example, 45°±10°, preferably 45°±5°, and more preferably 45°. The λ / 4 plate preferably exhibits a reverse dispersion wavelength characteristic in which the phase difference value increases in accordance with the wavelength of the measurement light. The Re(450) / Re(550) of the λ / 4 plate is, for example, greater than 0.75 and less than 1, and may be 0.8 to 0.95.
[0117] In addition to the λ / 4 plate, the second phase difference layer may also include a phase difference film that functions as a λ / 2 plate (hereinafter referred to as "λ / 2 plate"). The λ / 2 plate has, for example, Re(550) of 210nm~280nm, preferably 230nm~240nm. The λ / 2 plate may have, for example, a refractive index characteristic of nx>ny≥nz. The Nz coefficient of the λ / 2 plate is preferably 0.9~1.5, more preferably 0.9~1.3. The λ / 2 plate can be arranged between the first polarizer and the λ / 4 plate. The angle formed by the absorption axis of the first polarizer and the slow axis of the λ / 4 plate is preferably 65°~85°, more preferably 72°~78°, and further preferably about 75°. The angle formed by the absorption axis of the first polarizer and the slow axis of the λ / 2 plate is preferably 10°~20°, more preferably 13°~17°, and further preferably about 15°.
[0118] When the optical laminate including the second phase difference layer is used in combination with an organic EL element, in addition to seamlessness, it can also exert an excellent anti-reflection function. The λ / 4 plate and the λ / 2 plate can be composed of, for example, a stretched film of a resin film or an oriented solidified layer of a liquid crystal compound. Such λ / 4 plates and λ / 2 plates are well known to those skilled in the art, so their detailed description is omitted.
[0119] B. Image display device
[0120] The image display device of the embodiment of the present invention comprises, in order toward the visible side, a display element and the optical laminate described in item A, wherein the optical laminate is arranged so that the second polarizer is closer to the visible side than the first polarizer. The image display device of such a configuration has good seamlessness when viewed from the front direction and the oblique direction, and thus has excellent appearance design.
[0121] In the L*a*b* color space of the SCI method in the display area when the display is not displayed, for example, L* is preferably 15 or less, more preferably 10 or less, a* is preferably -10 to +10, more preferably -5 to +5, and b* is preferably -10 to +10, more preferably -5 to +5. In addition, in the L*a*b* color space of the SCE method in the display area when the display is not displayed, L* is preferably 10 or less, more preferably 5 or less, a* is preferably -10 to +10, more preferably -5 to +5, and b* is preferably -10 to +10, more preferably -5 to +5.
[0122] The SCI method L*a*b* color difference (CIE 1976) ΔE*ab between the display area and the non-display area when not displaying is preferably less than 20, more preferably less than 15, and further preferably less than 10. In addition, the SCE method L*a*b* color difference (CIE1976) ΔE*ab is preferably less than 5, more preferably less than 3, and further preferably less than 1. In addition, the L*a*b* color difference (CIE 1976) ΔE*ab when measured (receiving light) at a polar angle of 45° is preferably less than 5, more preferably less than 3, and further preferably less than 1. If ΔE*ab is within the above range, it is a state in which it is difficult to recognize the difference in appearance between the display area and the non-display area when not displaying. In addition, the L*a*b* color difference (CIE 1976) ΔE*ab is a value calculated by the following formula (wherein L* represents brightness, a* represents chromaticity a*, and b* represents chromaticity b*).
[0123] ΔE*ab=[(ΔL*) 2 +(Δa*) 2 +(Δb*) 2 ] 1 / 2
[0124] The reflectivity of the SCI method in the display area when not displaying is preferably less than 5%, more preferably less than 3%, and further preferably less than 1%. The reflectivity in the non-display area is preferably less than 3%, more preferably less than 2%, and further preferably less than 1%. The reflectivity difference between the two areas is preferably less than 3%, and more preferably less than 1%.
[0125] The reflectivity of the SCE method in the display area when not displaying is preferably 3% or less, more preferably 2% or less, and further preferably 1% or less. The reflectivity in the non-display area is preferably 3% or less, more preferably 2% or less, and further preferably 1% or less. The reflectivity difference between the two areas is preferably 3% or less, and more preferably 1% or less.
[0126] In the display area when not displaying, the reflectivity when measured (receiving light) at a polar angle of 45° is preferably 5% or less, more preferably 3% or less, and further preferably 1% or less. The reflectivity in the non-display area is preferably 3% or less, more preferably 2% or less, and further preferably 1% or less. The reflectivity difference between the two areas is preferably 3% or less, and more preferably 1% or less.
[0127] As the above-mentioned display element, a liquid crystal cell, an organic EL element, an inorganic EL element, etc. can be cited. In addition, the display element can further include a touch panel. These display elements are well known to those skilled in the art, so their detailed description is omitted.
[0128] Figure 2A It is a schematic cross-sectional view of an image display device (liquid crystal display device) including a liquid crystal unit as a display element. The image display device 200A includes, in order toward the visible side: a backlight unit 110, a third polarizer 120 including a third polarizer, a liquid crystal unit 130, and an optical laminate 100A. Preferably, the optical laminate 100A has an adhesive layer (not shown) on the outside of the first polarizer 10, and is bonded to the liquid crystal unit 130 via the adhesive layer. In addition, the optical laminate 100A is typically configured in a manner such that the absorption axis direction of the first polarizer 10 (first polarizer 12) is substantially orthogonal to the absorption axis direction of the third polarizer 120 (third polarizer), and the first polarizer 10, the liquid crystal unit 130, and the third polarizer 120 constitute a liquid crystal panel.
[0129] Figure 2B 200B includes an organic EL element 140 and an optical laminate 100B in order toward the visible side. The optical laminate 100B is bonded to the organic EL element 140 via an adhesive layer (not shown) provided on the outside of the second phase difference layer 60, for example.
[0130] Figure 2C It is a schematic cross-sectional view of an image display device (organic EL display device) including a touch panel and an organic EL element as a display element. The image display device 200C has, in sequence toward the visible side: an organic EL element 140, a touch panel 150, and an optical laminate 100B. These components are preferably bonded via an adhesive layer (not shown). In the example shown in the figure, the touch panel is configured as an out-cell on the visible side of the display element, but the touch panel can also be introduced into the display element in an on-cell or in-cell manner.
[0131] Example
[0132] Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to these examples. In addition, the measuring methods of each characteristic are as follows.
[0133] (1) Thickness
[0134] The measurement was performed using a digital gauge (manufactured by Ozaki Seisakusho Co., Ltd., product name: "PEACOCK").
[0135] (2) Single-unit transmittance and polarization degree of polarizer
[0136] The single transmittance Ts, parallel transmittance Tp, and orthogonal transmittance Tc obtained by measuring the polarizer (protective layer / polarizer / protective layer) using an ultraviolet visible near-infrared spectrophotometer (V-7100 made by JASCO Corporation) are set as Ts, Tp, and Tc of the polarizer, respectively. These Ts, Tp, and Tc are the Y values obtained by measuring the 2-degree field of view (C light source) of JIS Z8701 and correcting the visibility. The polarization degree is calculated using the following formula based on the obtained Tp and Tc.
[0137] Polarization degree (%) = {(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100
[0138] (3) Refractive index (nx, ny, nz), Re (λ), and Rth (λ)
[0139] The measurement was performed using "Axoscan" manufactured by Axometrics Co., Ltd. The measurement wavelength was 550 nm and the measurement temperature was 23°C.
[0140] [Manufacturing Example 1A: Phase Difference Film A (Negative B Plate) Having Refractive Index Characteristics of nx>ny>nz]
[0141] As a retardation film A having a refractive index characteristic of nx>ny>nz, a commercially available retardation film (a stretched film of a cyclic olefin resin film, "Zeonor Film" manufactured by Zeon Co., Ltd.) was prepared. (R) ZB", thickness: 75 μm). The Re(550) and Rth(550) of the retardation film A are 55 nm and 275 nm.
[0142] [Manufacturing Example 1B: Phase Difference Film B (Positive C Plate) Having Refractive Index Characteristics of nz>nx=ny]
[0143] A liquid crystal coating liquid was prepared by dissolving 20 parts by weight of a side chain liquid crystal polymer represented by the following chemical formula (1) (the numbers 65 and 35 in the formula represent the molar % of the monomer unit, and for convenience, it is expressed as a block polymer: weight average molecular weight 5000), 80 parts by weight of a polymerizable liquid crystal showing a nematic liquid crystal phase (manufactured by BASF: trade name Paliocolor LC242) and 5 parts by weight of a photopolymerization initiator (manufactured by Ciba Specialty Chemicals: trade name Irgacure 907) in 200 parts by weight of cyclopentanone. Then, the coating liquid was applied to a PET substrate subjected to a vertical alignment treatment by a wire bar coater, and then heated and dried at 80°C for 4 minutes to align the liquid crystal. The liquid crystal layer was irradiated with ultraviolet rays to cure the liquid crystal layer, thereby forming a liquid crystal alignment solidified layer (thickness 3 μm) on the substrate. The liquid crystal alignment solidified layer had a refractive index characteristic of nz>nx=ny, Re(550) was 0 nm, and Rth(550) was -135 nm.
[0144] [Chemical formula 1]
[0145]
[0146] [Manufacturing Example 1C: Phase Difference Film C (Z Plate) Having Refractive Index Characteristics of nx>nz>ny]
[0147] A shrinkable film with a thickness of 60 μm (manufactured by Toray Industries, trade name "TORAYFAN BO2873") was attached to both sides of a commercially available cyclic olefin resin film (manufactured by JSR, trade name "Arton (R5000)", thickness: 130 μm, Tg: 137°C) via an acrylic adhesive layer (thickness of 15 μm), and the film was subjected to uniaxial stretching at the free end to obtain a retardation film C having a refractive index characteristic of nx>nz>ny. The stretching temperature was set to 146°C, and the stretching ratio was set to 1.38 times. The obtained retardation film C had a Re (550) of 270 nm and a Rth (550) of 135 nm.
[0148] [Manufacturing Example 1D: Phase Difference Film D (Positive A Plate) Having Refractive Index Characteristics of nx>ny=nz]
[0149] As a retardation film D having a refractive index characteristic of nx>ny=nz, a commercially available retardation film ("UTZ-film #270" manufactured by KANEKA Corporation, thickness: 33 μm) was prepared. The retardation film D had Re(550) of 270 nm and Rth(550) of 270 nm.
[0150] [Manufacturing Example 2: Polarizing Plate A]
[0151] 1. Preparation of polarizer
[0152] A polyvinyl alcohol film having an average degree of polymerization of 2400, a saponification degree of 99.9 mol % and a thickness of 45 μm was prepared. The polyvinyl alcohol film was immersed in a swelling bath (water bath) at 20°C between rollers having different peripheral speed ratios for 30 seconds to swell, and stretched 2.2 times in the conveying direction (swelling process), and then immersed in a dyeing bath (an aqueous solution having an iodine concentration of 0.1 wt % and a potassium iodide concentration of 0.9 wt %) at 30°C for 30 seconds to dye, and stretched 3.3 times in the conveying direction based on the original polyvinyl alcohol film (a polyvinyl alcohol film that was not stretched at all in the conveying direction) (dyeing process). Next, the dyed polyvinyl alcohol film was immersed in a crosslinking bath (an aqueous solution having a boric acid concentration of 3.0 wt % and a potassium iodide concentration of 3.0 wt %) at 40°C for 28 seconds, and stretched to 3.6 times in the conveying direction based on the original polyvinyl alcohol film (crosslinking process). In addition, the obtained polyvinyl alcohol film was immersed in a stretching bath (aqueous solution with a boric acid concentration of 4.0 wt% and a potassium iodide concentration of 5.0 wt%) at 61°C for 60 seconds, stretched to 6.0 times in the conveying direction based on the original polyvinyl alcohol film (stretching process), and then immersed in a cleaning bath (aqueous solution with a potassium iodide concentration of 2.0 wt%) at 20°C for 10 seconds (cleaning process). The cleaned polyvinyl alcohol film was dried at 40°C for 30 seconds to prepare a polarizer. The thickness of the polarizer was 18 μm.
[0153] 2. Preparation of polarizer A
[0154] As an adhesive, an aqueous solution containing a polyvinyl alcohol resin having an acetoacetyl group (average degree of polymerization of 1200, saponification degree of 98.5 mol%, degree of acetoacetylation of 5 mol%) and methylol melamine in a weight ratio of 3:1 was used. Using this adhesive, a transparent protective film (manufactured by Nippon Shokubai Co., Ltd.) with a thickness of 30 μm formed of a (meth) acrylic resin (modified acrylic polymer having a lactone ring structure) as a protective layer was laminated to one side (display element side) of the polarizer obtained above by a roll laminator, and a transparent protective film with a thickness of 49 μm formed of HC on a triacetylcellulose film (manufactured by Fujifilm Co., Ltd., trade name "TJ40UL") was laminated to the other side (visible side) as a protective layer, and then heated and dried in an oven (temperature of 90°C for 10 minutes) to produce a polarizing plate A having transparent protective films laminated to both sides of the polarizer. The resulting polarizer had a single body transmittance of 41.7% and a polarization degree of 99.9%.
[0155] [Manufacturing Example 3: Printing Layer Forming Composition A]
[0156] A black printing layer-forming composition A was obtained by impregnating the solvent with "HF GV3 RX01" manufactured by Seiko Advance Co., Ltd. as a colorant (black pigment) at a concentration of 10% by weight.
[0157] [Manufacturing Example 4: Adhesive Layer A]
[0158] In a monomer mixture consisting of 60 parts by weight of butyl acrylate (BA), 6 parts by weight of cyclohexyl acrylate (CHA), 26 parts by weight of 4-hydroxybutyl acrylate (4HBA), and 8 parts by weight of hydroxyethyl acrylate (HEA), 0.09 parts by weight of 2,2-dimethoxy-1,2-diphenyl-1-one (trade name "Irgacure 651", manufactured by BASF JAPAN) and 0.09 parts by weight of 1-hydroxy-cyclohexyl-phenyl-ketone (trade name "Irgacure 184", manufactured by BASF JAPAN) were added to a four-necked flask, and the mixture was exposed to ultraviolet rays in a nitrogen atmosphere to be partially photopolymerized, thereby obtaining a partial polymer (monomer syrup) having a polymerization rate of about 10%. To 100 parts by weight of the partial polymer, 0.12 parts by weight of dipentaerythritol hexaacrylate ("KAYARAD DPHA" manufactured by Nippon Kayaku Co., Ltd.) as a multifunctional polymerizable compound and 0.3 parts by weight of 3-glycidoxypropyltrimethoxysilane ("KBM-403" manufactured by Shin-Etsu Chemical) as a silane coupling agent were added and uniformly mixed to prepare an adhesive (adhesive composition). Thus, an adhesive composition A was obtained.
[0159] The adhesive composition A obtained above was applied onto a release liner R1 (MRF#38, manufactured by Mitsubishi Resins Corporation) having a thickness of 38 μm and a release surface on one side of a polyester film, and covered with a release liner R2 (MRE#38, manufactured by Mitsubishi Resins Corporation) having a thickness of 38 μm and a release surface on one side of a polyester film, and the air was blocked and cured by ultraviolet irradiation, thereby forming an adhesive layer A (thickness of 250 μm, total light transmittance of 92.0%, and haze of 0.3%).
[0160] [Manufacturing Example 5: Surface Base Material Layer A]
[0161] An anti-reflection film (manufactured by Nitto Denko Corporation, product name "T-60LA28HCAR6N", thickness 85 μm) having a structure of an anti-reflection layer / TAC film was adhered to one side of a glass film (manufactured by Matsunami Glass Industries, Ltd., product name "Soda Lime Glass") having a thickness of 1 mm via an adhesive layer A to obtain a surface substrate layer A having a structure of [glass film / TAC film / anti-reflection layer].
[0162] [Example 1]
[0163] The above-mentioned polarizer A is cut into a rectangular shape as a second polarizer. By screen printing, the composition A for forming a printed layer is applied along the outer periphery of the side surface of the second polarizer (meth) acrylic resin film into a frame shape with a width of 1.5 mm in a top view, and it is naturally dried to form a black printed layer with a thickness of 5 μm. Next, the printed layer is coated with the composition A for forming a printed layer again by screen printing, and dried at 50 ° C for 1 hour to form a black printed layer with a thickness of 5 μm (the thickness of the printed layer finally formed: 10 μm). Next, the adhesive layer A is transferred from the release liner to the side of the printed layer formed with the second polarizer, and the phase difference film A is further stacked thereon in a manner that the absorption axis direction of the second polarizer is parallel to the slow axis direction of the phase difference film A. At this time, the height difference portion of the boundary between the printed layer and the second polarizer is completely filled with the adhesive layer A, and no gap is generated. Next, the surface substrate layer is bonded to the second polarizer side surface of the obtained laminate via an acrylic adhesive (thickness of 250 μm). Thus, a laminate 1 having a structure of [surface substrate layer A / second polarizer / printed layer A / adhesive layer A / retardation film A] was obtained.
[0164] The polarizer A was cut into a rectangular shape as the first polarizer. A reverse dispersed phase difference film (stretched film of polycarbonate resin film, Re (550) = 147 nm) capable of functioning as a λ / 4 plate was bonded to the first polarizer via an adhesive layer so that the slow axis direction and the absorption axis direction of the first polarizer formed an angle of 45°, thereby obtaining a circular polarizer 1.
[0165] A glass plate was bonded to the surface of the laminate 1 obtained above on the side opposite to the surface base material layer A via an acrylic adhesive (thickness: 23 μm), thereby obtaining a laminate 1 with a glass plate.
[0166] The laminate 1 with a glass plate is bonded to the first polarizer side of the circular polarizer 1 via an acrylic adhesive (thickness of 23 μm), and another glass plate is bonded to the λ / 4 plate side via an acrylic adhesive (thickness of 23 μm). At this time, the surface substrate layer A of the laminate 1 with a glass plate is arranged in a manner that makes the surface substrate layer A of the laminate 1 with a glass plate the outermost layer, and in a manner that makes the absorption axis directions of the first polarizer and the second polarizer parallel to each other. Thus, an optical laminate 1 having a structure of [surface substrate layer A / second polarizer / printed layer A / adhesive layer A / phase difference film A / glass plate / first polarizer / λ / 4 plate / glass plate] is obtained. In addition, in the optical laminate 1, the glass plate is provided from the perspective of handling during characteristic evaluation.
[0167] [Example 2]
[0168] A laminate 2 having a structure of [surface substrate layer A / second polarizer / printing layer A / adhesive layer A / phase difference film A / phase difference film B] was obtained in the same manner as in Example 1, except that phase difference film A and phase difference film B were sequentially laminated on adhesive layer A. In addition, the lamination (transfer) of phase difference film B was performed by attaching phase difference film B to phase difference film A via an adhesive and then peeling off the substrate.
[0169] An optical layered body 2 was obtained in the same manner as in Example 1 except that the layered body 2 was used instead of the layered body 1.
[0170] [Example 3]
[0171] Two phase difference films A were laminated on the adhesive layer A via an acrylic adhesive (thickness of 23 μm), and a laminate 3 having a structure of [surface substrate layer A / second polarizer / printed layer A / adhesive layer A / phase difference film A / phase difference film A] was obtained in the same manner as in Example 1. In addition, the slow axis directions of the two phase difference films A were arranged in a manner parallel to the absorption axis direction of the second polarizer.
[0172] Optical layered body 3 was obtained in the same manner as in Example 1 except that layered body 3 was used instead of layered body 1.
[0173] [Example 4]
[0174] A laminate 4 having a structure of [surface substrate layer A / second polarizer / printed layer A / adhesive layer A / phase difference film C] was obtained in the same manner as in Example 1, except that the phase difference film C was laminated on the adhesive layer A. In addition, the phase difference film C was arranged in a manner that the slow axis direction and the absorption axis direction of the second polarizer were parallel to each other.
[0175] Optical layered body 4 was obtained in the same manner as in Example 1 except that layered body 4 was used instead of layered body 1.
[0176] [Example 5]
[0177] Two phase difference films C were laminated on the adhesive layer A via an acrylic adhesive (thickness of 23 μm), and a laminate 5 having a structure of [surface substrate layer A / second polarizer / printed layer A / adhesive layer A / phase difference film C / phase difference film C] was obtained in the same manner as in Example 1. In addition, the slow axis directions of the two phase difference films C were arranged in a manner parallel to the absorption axis direction of the second polarizer.
[0178] Optical layered body 5 was obtained in the same manner as in Example 1 except that layered body 5 was used instead of layered body 1.
[0179] [Example 6]
[0180] A laminate 6 having a structure of [surface substrate layer A / second polarizer / printed layer A / adhesive layer A / retardation film B] was obtained in the same manner as in Example 1 except that the retardation film B was laminated (transferred) on the adhesive layer A.
[0181] Optical layered body 6 was obtained in the same manner as in Example 1 except that layered body 6 was used instead of layered body 1.
[0182] [Example 7]
[0183] A laminate 7 having a structure of [surface substrate layer A / second polarizer / printed layer A / adhesive layer A / phase difference film B / phase difference film B] was obtained in the same manner as in Example 1, except that two phase difference films B were laminated (transferred) on the adhesive layer A via an acrylic adhesive layer (thickness of 23 μm).
[0184] Optical layered body 7 was obtained in the same manner as in Example 1 except that layered body 7 was used instead of layered body 1.
[0185] [Example 8]
[0186] A laminate 8 having a structure of [surface substrate layer A / second polarizer / printed layer A / adhesive layer A / phase difference film B / phase difference film B / phase difference film B] was obtained in the same manner as in Example 1, except that three phase difference films B were stacked (transferred) on the adhesive layer A via an acrylic adhesive layer (thickness of 23 μm).
[0187] Optical layered body 8 was obtained in the same manner as in Example 1 except that layered body 8 was used instead of layered body 1.
[0188] [Example 9]
[0189] A laminate 9 having a structure of [surface substrate layer A / second polarizer / printed layer A / adhesive layer A / phase difference film B / phase difference film B / phase difference film B / phase difference film B] was obtained in the same manner as in Example 1, except that 4 phase difference films B were stacked (transferred) on the adhesive layer A via an acrylic adhesive layer (thickness of 23 μm).
[0190] Optical layered body 9 was obtained in the same manner as in Example 1 except that layered body 9 was used instead of layered body 1.
[0191] [Comparative Example 1]
[0192] Except that the retardation film was not laminated on the adhesive layer A, a laminate C1 having a structure of [surface substrate layer A / second polarizer / printed layer A / adhesive layer A] was obtained in the same manner as in Example 1.
[0193] An optical layered body C1 was obtained in the same manner as in Example 1 except that the layered body C1 was used instead of the layered body 1.
[0194] [Comparative Example 2]
[0195] A laminate C2 having a structure of [surface substrate layer A / second polarizer / printed layer A / adhesive layer A / phase difference film D] was obtained in the same manner as in Example 1, except that the phase difference film D was laminated on the adhesive layer A. In addition, the phase difference film D was arranged in a manner parallel to the absorption axis direction of the second polarizer.
[0196] Optical layered body C2 was obtained in the same manner as in Example 1 except that layered body C2 was used instead of layered body 1.
[0197] [Comparative Example 3]
[0198] Two phase difference films D were laminated on the adhesive layer A via an acrylic adhesive (thickness of 23 μm), and a laminate C3 having a structure of [surface substrate layer A / second polarizer / printed layer A / adhesive layer A / phase difference film D / phase difference film D] was obtained in the same manner as in Example 1. In addition, the slow axis directions of the two phase difference films D were arranged in a manner parallel to the absorption axis direction of the second polarizer.
[0199] Optical layered body C3 was obtained in the same manner as in Example 1 except that layered body C3 was used instead of layered body 1.
[0200] The structures (excluding the glass plate) of the optical layered bodies 1 to 9 and C1 to C3 obtained above, various measurement results, and seamlessness evaluation results are shown in Tables 1 and 2. The display region and the non-display region are regions where the printed layer is not formed and regions where the printed layer is formed, respectively, in plan view.
[0201] <L*a*b* color space, color difference ΔE*ab and reflectivity>
[0202] The optical laminate was bonded to a reflector (manufactured by Toray Film Co., Ltd., trade name "DMS-X42") using an acrylic adhesive to prepare a measurement sample. At this time, the side surface of the glass plate was bonded to the reflector in a manner opposite to the reflector. The spectral reflectance of the measurement sample was measured under the following measurement conditions to obtain L*a*b*. In addition, for the reflectance in the oblique direction (polar angle 45°), the maximum value of the measured values measured in all directions was used.
[0203] (Measurement conditions)
[0204] Front direction: Using a spectrophotometer (CM-2600d manufactured by Konica Minolta Inc.), the measurement sample was illuminated by diffuse illumination and received light by SCI (including regular reflection light) or SCE (excluding regular reflection light).
[0205] Oblique direction: Using a display measurement system (manufactured by Konica Minolta, Inc., “DMS505”), illumination was applied from the normal direction of the main surface of the measurement sample, and light was received at an angle of 45° with respect to the normal line.
[0206] Measurement wavelength range: 360nm-740nm
[0207] Light source: D65
[0208] Determination of the diameter of MAV:
[0209] In addition, the color difference (ΔE*ab) was calculated by the following formula.
[0210] ΔE*ab=[(ΔL*) 2 +(Δa*) 2 +(Δb*) 2 ] 1 / 2
[0211] <Brightness>
[0212] The backlight was taken out from the liquid crystal display device. The optical laminate was placed on the backlight so that the side surface of the glass plate was opposite to the backlight, and the brightness of the backlight when it was turned on was measured using "CONOSCOPE" manufactured by Autonic Melchers. The measurement was performed in two ways: the front direction and the oblique direction (polar angle 45°). For the oblique direction, the minimum value when measuring in all directions was used.
[0213] <Seamlessness>
[0214] A reflective plate (manufactured by Toray Film Co., Ltd., trade name "DMS-X42") was attached to the glass plate side of optical laminates 1 to 9 and C1 to C3 via an acrylic adhesive layer (thickness of 23 μm) as an evaluation sample. The optical laminate was visually observed from the surface substrate layer side at a polar angle of 45° from all directions under fluorescent light, and the visual recognition of the boundary between the display area and the non-display area was evaluated. The evaluation criteria are as follows.
[0215] [Evaluation criteria]
[0216] ×: No change compared to ref
[0217] ○: Slightly improved compared to ref
[0218] ◎: Significantly improved compared to ref
[0219]
[0220] Table 2
[0221]
[0222] *Seamless ΔE*ab: Color difference between display area and non-display area
[0223] *Color shift ΔE00: Color difference in the display area
[0224] As shown in Table 1, the chromatic aberration of the reflected light in the oblique direction between the display area and the non-display area of the optical laminate of the embodiment is smaller than that of the optical laminate of Comparative Example 1, and the seamlessness evaluation result is also excellent. Thus, when the optical laminate of the embodiment is applied to an image display device, the seamlessness when observed from an oblique direction can be improved compared with the case where the optical laminate of Comparative Example 1 is applied. On the other hand, the phase difference value in the thickness direction of the first phase difference layer as a whole of Comparative Examples 2 and 3, in which the first phase difference layer does not include a phase difference film having birefringence in the thickness direction, is the same as that of the first phase difference layer of the embodiment, but the seamlessness improvement effect is not obtained. In addition, with respect to the front direction, the optical laminates of the embodiment and the comparative example both show good seamlessness.
[0225] Industrial Applicability
[0226] The optical layered body of the present invention can be suitably used in an image display device.
Claims
1. An optical laminate, comprising: a first polarizing plate including a first polarizer, a phase difference layer having a phase difference in a thickness direction, a printed layer, and a second polarizing plate including a second polarizer, The phase difference layer includes a phase difference film having birefringence in the thickness direction. The absorption axis direction of the first polarizer is substantially parallel to the absorption axis direction of the second polarizer.
2. The optical layered body according to claim 1, wherein: The absolute value of the retardation value Rth(550) in the thickness direction of the retardation layer is 100 nm or more.
3. The optical layered body according to claim 1, wherein: The phase difference film having birefringence in the thickness direction includes a phase difference film having refractive index characteristics of nx>ny>nz, nx>nz>ny or nz>nx=ny when the refractive index in the slow axis direction is set to "nx", the refractive index in the fast axis direction is set to "ny" and the refractive index in the thickness direction is set to "nz".
4. The optical laminate according to claim 1, wherein: The phase difference film having birefringence in the thickness direction has an in-plane phase difference, The slow axis direction of the phase difference film is substantially parallel to the absorption axis directions of the first polarizer and the second polarizer.
5. The optical layered body according to claim 1, wherein: The thickness of the printing layer is 3 μm to 30 μm.
6. The optical layered body according to claim 1, wherein: The second polarizing plate further includes a surface substrate layer on the side opposite to the side where the retardation layer is arranged.
7. An image display device comprising: a display element and the optical laminate according to any one of claims 1 to 6, in this order toward a viewing side; The optical laminate is arranged such that the second polarizing plate is closer to the viewing side than the first polarizing plate.
8. The image display device according to claim 7, wherein: The display element includes a liquid crystal cell, an organic electronic element or an inorganic electronic element.
9. The image display device according to claim 7, wherein: A touch panel is further included.
10. The image display device according to claim 8, wherein: The display element is a liquid crystal unit, The image display device includes, in order toward the viewing side, a third polarizing plate including a third polarizer, the liquid crystal cell, and the optical laminate.