Preparation method and application of core-shell structure electrode material
By preparing NiMoO4@MnCo2O4/CC core-shell structure electrode material by hydrothermal reaction and cyclic voltammetry on a carbon cloth substrate, the problem of unsatisfactory electrochemical characteristics of mixed transition metal oxide materials is solved, and high conductivity and large The surface area improves the electrochemical performance and application efficiency of supercapacitors.
Patent Information
- Application Number
- CN202411078746.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art has problems with poor electrochemical characteristics in the use of mixed transition metal oxide materials and core-shell structure design, resulting in poor conductivity and low application efficiency.
The NiMoO4 one-dimensional nanomaterial was grown on the carbon cloth substrate by hydrothermal reaction, and the MnCo2O4 electrochemical deposition by cyclic voltammetry was prepared to prepare the NiMoO4@MnCo2O4/CC core-shell structure electrode material, combining the advantages of transition metal oxides of each unit. Overcome poor conductivity and design core-shell structures to achieve high conductivity and large surface area.
Achieve superior transmission channels and lower charge transfer resistance of nanosheet-nanosheet structure, improve the electrochemical performance of supercapacitors, provide more Faraday reaction sites and accelerated electroactivity, and is safe in process and low in cost. .
Smart Images

Figure CN118942922A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrode materials, and specifically relates to a preparation method and application of a core-shell structure electrode material. Background Art
[0002] Since the 21st century, the energy crisis has been gradually spreading, and the consumption of traditional fossil energy has been increasing, which poses a serious threat to the sustainable energy supply of human society. Humans need to search for cleaner and more efficient renewable energy, but at the same time, energy conversion and storage technologies also need to be developed. Supercapacitors have shown great potential in transportation, industrial production, smart wearable textiles and other fields due to their high power density, good cycle stability, and fast charge and discharge rates.
[0003] Transition metal oxides are common pseudocapacitor materials with good pseudocapacitive properties. They can also be well combined with conductive flexible substrates (carbon paper, carbon cloth, etc.) as flexible electrodes for supercapacitors. However, poor conductivity is one of the reasons that hinder its practical application. In order to overcome this difficulty, the advantages of each unit transition metal oxide can be combined to make a mixed transition metal oxide. In addition, designing a suitable core-shell structure is also an effective way to achieve high conductivity and large surface area to provide more Faraday reaction sites and accelerate electrical activity.
[0004] However, the existing technology is lacking in the use of mixed transition metal oxide materials and the design of core-shell structures, and has problems such as unsatisfactory electrochemical properties. Summary of the invention
[0005] The present invention aims to solve the problems that the prior art is deficient in the use of mixed transition metal oxide materials and the design of core-shell structures, and has unsatisfactory electrochemical properties.
[0006] The present invention provides a method for preparing a NiMoO4@MnCo2O4 / CC core-shell structure electrode material, wherein a NiMoO4 one-dimensional nanomaterial is first grown on a carbon cloth substrate by a hydrothermal reaction, and then MnCo2O4 is electrochemically deposited by cyclic voltammetry to obtain a NiMoO4@MnCo2O4 / CC core-shell composite material with excellent supercapacitor performance.
[0007] Among the materials used in the present invention, NiMoO4 is a naturally abundant pseudocapacitive metal oxide, which is considered to be a good candidate material for core materials due to its natural abundance, low cost, excellent redox reaction and wide electrochemical potential window in cyclic voltammetry. Among various binary metal oxides, MnCo2O4 has attracted much attention due to its low cost, high availability, high capacitance value, superior electrochemical performance and environmental protection properties. Manganese can transfer more electrons, and cobalt exhibits a higher oxidation potential. The large oxidation potential of cobalt and the fast electron transfer rate of manganese will increase the entire electrochemical reaction and bring about a better capacitance value.
[0008] The technical solution adopted by the present invention includes:
[0009] 1. A method for preparing a core-shell structure electrode material
[0010] The preparation method comprises the following steps:
[0011] 1) placing the raw carbon cloth in a mixed solution of concentrated sulfuric acid and concentrated nitric acid for water bath activation, and cutting the carbon cloth after the water bath activation is completed;
[0012] 2) The cut carbon cloth is subjected to hydrothermal treatment with a mixed metal solution to load two mixed metals, and then annealed and electrochemically reacted in sequence to deposit another two mixed metals;
[0013] 3) The carbon cloth obtained in step 2) is washed and dried in sequence, and then placed in a muffle furnace for annealing to obtain a carbon cloth loaded with NiMoO4@MnCo2O4 / CC, i.e., a NiMoO4@MnCo2O4 / CC core-shell structure electrode material.
[0014] The step 1) is specifically as follows:
[0015] 1.1) Mix 90-98% concentrated sulfuric acid and 60-70% concentrated nitric acid in a volume ratio of (2-3):1 to form a mixed solution;
[0016] 1.2) placing the raw carbon cloth in the mixed solution obtained in step 1.1) for activation treatment in a water bath at a temperature of 65 to 70° C. for 2 to 3 hours;
[0017] 1.3) After water bath activation, the carbon cloth is cut.
[0018] The step 2) is specifically as follows:
[0019] 2.1) Dissolve nickel salt, molybdenum salt, ammonium fluoride and urea in deionized water and stir magnetically to obtain a uniform and transparent light green mixed solution;
[0020] 2.2) pouring the mixed solution obtained in step 2.1) into a polytetrafluoroethylene reactor, and then placing the carbon cloth obtained in step 1) upright into the polytetrafluoroethylene reactor for hydrothermal reaction, and cooling to room temperature after the reaction is complete to obtain a carbon cloth loaded with a precursor;
[0021] 2.3) The carbon cloth loaded with the precursor obtained in step 2.2) is taken out, cleaned and dried, and then placed in a muffle furnace for annealing to obtain a carbon cloth loaded with NiMoO4 nanosheets (NiMoO4 / CC);
[0022] 2.4) The NiMoO4 / CC obtained in step 2.3) is used as a working electrode, a platinum wire electrode is used as a counter electrode, an Ag / AgCl electrode is used as a reference electrode, and a mixed metal salt is used as an electrolyte. Cyclic voltammetry is used for deposition. After the deposition is completed, a carbon cloth with deposited mixed metals and loaded NiMoO4 nanosheets is obtained.
[0023] In the step 2.1), the nickel salt is one or more of nickel chloride, nickel sulfate and nickel nitrate, the molybdenum salt is one or more of ammonium molybdate, potassium molybdate and sodium molybdate, the molar ratio of the nickel salt, the molybdenum salt, ammonium fluoride and urea is (1-2 mmol): (1-2 mmol): (4-6 mmol): (5-7 mmol), and the volume of deionized water is 35-45 mL.
[0024] In the step 2), the stirring speed is 400-500 rpm / min, and the stirring time is 30-60 min.
[0025] In the step 2.2), the hydrothermal reaction temperature is 140-160° C., and the hydrothermal insulation time is 6-8 hours.
[0026] In the step 2.3), the cleaning solutions are deionized water and anhydrous ethanol, the cleaning times are 2 to 3 times, the drying temperature is 60 to 70°C, the drying time is 8 to 10 hours, the annealing temperature is 350 to 400°C, the annealing time is 2 to 4 hours, and the heating rate is 5 to 6°C / min.
[0027] In the step 2.4), the mixed metal salt is a mixture of cobalt salt and manganese salt, the molar concentration of the electrolyte is 0.075 mol / L to 0.15 mol / L, the deposition potential is -1.2 to 0.2 V, the deposition cycle is 4 to 7 cycles, and the deposition rate is 5 mV / s.
[0028] In the step 3), the cleaning solutions are deionized water and anhydrous ethanol in sequence, the cleaning times are 2 to 3 times, the drying temperature is 60 to 70°C, the drying time is 8 to 10 hours, the annealing temperature is 350 to 400°C, the annealing time is 2 to 4 hours, and the heating rate is 5 to 6°C / min.
[0029] The cobalt salt is one or more of cobalt nitrate and cobalt chloride;
[0030] The manganese salt is one or more of manganese sulfate, manganese nitrate and manganese chloride.
[0031] 2. Application of a core-shell structure electrode material
[0032] Application of electrode materials for energy conversion and storage, specifically in the preparation of capacitor materials and core-shell structures.
[0033] The electrode material prepared by the present invention overcomes the disadvantage of poor conductivity by combining the advantages of each unit transition metal oxide. The designed core-shell structure realizes high conductivity and large surface area, provides more Faraday reaction sites and accelerates electrical activity.
[0034] The beneficial effects of the present invention are:
[0035] 1. The NiMoO4@MnCo2O4 / CC core-shell structure electrode material was synthesized by hydrothermal method and cyclic voltammetry electrodeposition method. The nanosheet-nanosheet structure has a more superior transmission channel and lower charge transfer resistance, which can reduce the dendrite growth of the electrode material and provide a more uniform electric field distribution, thereby improving the electrochemical performance of the supercapacitor.
[0036] 2. The present invention uses carbon cloth with high specific surface area and reactive sites after water bath activation as a flexible substrate to directly grow active materials in situ, thus avoiding the use of a binder.
[0037] 3. The present invention has the obvious advantages of safe and mild reaction process, simple operation, low process cost and good process flexibility. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 The high-magnification and low-magnification SEM images of the activated carbon cloth, NiMoO4 / CC, MnCo2O4 / CC and NiMoO4@MnCo2O4 / CC in the embodiments and comparative examples of the present invention are shown;
[0039] Figure 2 XRD diagrams of activated carbon cloth, NiMoO4 / CC, MnCo2O4 / CC and NiMoO4@MnCo2O4 / CC in the embodiments and comparative examples of the present invention;
[0040] Figure 3 1 is a pore size distribution diagram of NiMoO4 / CC, MnCo2O4 / CC and NiMoO4@MnCo2O4 / CC in the embodiments and comparative examples of the present invention.
[0041] Figure 4It is a constant current charge-discharge (GCD) curve of NiMoO4 / CC, MnCo2O4 / CC and NiMoO4@MnCo2O4 / CC in the embodiments and comparative examples of the present invention as working electrodes in 2 mol / L potassium hydroxide aqueous solution.
[0042] Figure 5 The cyclic voltammetry (CV) curves of NiMoO4 / CC, MnCo2O4 / CC and NiMoO4@MnCo2O4 / CC in the embodiments and comparative examples of the present invention as working electrodes in 2 mol / L potassium hydroxide aqueous solution are shown.
[0043] Figure 6 : EIS impedance diagram of NiMoO4 / CC, MnCo2O4 / CC and NiMoO4@MnCo2O4 / CC in the embodiments and comparative examples of the present invention as working electrodes in 2 mol / L potassium hydroxide aqueous solution.
[0044] Figure 7 This is a constant current charge and discharge (GCD) curve of NiMoO4@MnCo2O4 / CC as a working electrode in an embodiment of the present invention at different current densities in a 2 mol / L potassium hydroxide aqueous solution.
[0045] Figure 8 This is a constant current charge-discharge (GCD) curve of NiMoO4@MnCo2O4 / CC as a working electrode in a 2 mol / L potassium hydroxide aqueous solution at different deposition cycle times in an embodiment of the present invention.
[0046] Fig. 9 This is the EIS impedance diagram of NiMoO4@MnCo2O4 / CC as a working electrode in a 2 mol / L potassium hydroxide aqueous solution at different deposition cycle times in an embodiment of the present invention. DETAILED DESCRIPTION
[0047] The present invention is described in more detail below in conjunction with the accompanying drawings and embodiments, but the present invention is not limited thereto. For those skilled in the art, several improvements and modifications can be made without departing from the principles of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention. The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in the field.
[0048] The specific embodiments of the present invention are as follows:
[0049] Embodiment 1:
[0050] This embodiment provides a preparation method of a NiMoO4@MnCo2O4 / CC composite material, and the specific steps are as follows:
[0051] 1) Take a cleaned 2×3cm 2 The carbon cloth was placed upright in a 100 mL beaker;
[0052] 2) Add 30 mL of 98% concentrated H2SO4 and 10 mL of 68% concentrated HNO3 into the beaker, stirring with a glass rod.
[0053] 3) placing the solution obtained in step 2) in a water bath and heating it to 65° C., and maintaining the constant temperature for 2 h;
[0054] 4) washing the acidified carbon cloth obtained in step 3) with anhydrous ethanol and deionized water in turn, and drying the washed carbon cloth in a drying oven at 60° C. for 8 h to obtain an activated carbon cloth;
[0055] 5) Dissolve 1mmol Ni(NO3)2·6H2O, 1mmol Na2MoO4·4H2O, 4mmol NH4F, and 5mmol CO(NH2)2 in 40mL deionized water and stir magnetically at 500rpm / min for 30min to form a uniform, transparent, light green solution;
[0056] 6) Transfer the transparent solution to a 50 mL polytetrafluoroethylene reactor and place a piece of activated carbon cloth 2×3 cm 2 ;
[0057] 7) The reactor was sealed and heated to 150°C for 8 hours. After the reaction was completed and cooled to room temperature, the carbon cloth loaded with the precursor was taken out and washed repeatedly in deionized water and anhydrous ethanol for 2 to 3 times;
[0058] 8) drying the precursor obtained in step 7) in a drying oven at 60° C. for 8 h;
[0059] 9) placing the precursor obtained in step 8) in a muffle furnace and annealing in an air atmosphere at a temperature of 350° C., an annealing time of 2 h, and a heating rate of 5° C. / min to obtain NiMoO4 nanosheets supported on carbon cloth;
[0060] 10) 1 mmol MnSO4·H2O, 2 mmol Co(NO3)2·6H2O, and 1 mmol Na2SO4 were dissolved in 40 mL of deionized water, and magnetically stirred at 500 rpm / min for 30 min to form a uniform, transparent magenta solution as an electrodeposition solution;
[0061] 11) The product NiMoO4 / CC obtained in step 9) is used as a working electrode, a platinum wire electrode is used as a counter electrode, and an Ag / AgCl electrode is used as a reference electrode. A three-electrode system is used. Cyclic voltammetry is performed at a rate of 5 mV / s in a potential range of -1.2 to 0.2 V using an electrochemical workstation to perform electrodeposition for 5 cycles. The carbon cloth loaded with the precursor is taken out and washed in deionized water and anhydrous ethanol for 2 to 3 times respectively;
[0062] 12) placing the sample obtained in step 11) in a drying oven at 60° C. and drying for 8 h;
[0063] 13) The precursor obtained in step 12) is placed in a muffle furnace and annealed in an air atmosphere at a temperature of 350° C., an annealing time of 2 h, and a heating rate of 5° C. / min to obtain a NiMoO4@MnCo2O4 / CC composite material.
[0064] Embodiment 2:
[0065] In order to explore the effect of different cyclic deposition times on the performance of electrode materials, this example provides the preparation of NiMoO4@MnCo2O4 / CC composite materials with different cyclic deposition times. The other steps are the same as those in Example 1. The specific steps are as follows:
[0066] 1) Take a cleaned 2×3cm 2 The carbon cloth was placed upright in a 100 mL beaker;
[0067] 2) Add 30 mL of 98% concentrated H2SO4 and 10 mL of 68% concentrated HNO3 into the beaker, stirring with a glass rod.
[0068] 3) placing the solution obtained in step 2) in a water bath and heating it to 65° C., and maintaining the constant temperature for 2 h;
[0069] 4) washing the acidified carbon cloth obtained in step 3) with anhydrous ethanol and deionized water in turn, and drying the washed carbon cloth in a drying oven at 60° C. for 8 h to obtain an activated carbon cloth;
[0070] 5) Dissolve 1mmol Ni(NO3)2·6H2O, 1mmol Na2MoO4·4H2O, 4mmol NH4F, and 5mmol CO(NH2)2 in 40mL deionized water and stir magnetically at 500rpm / min for 30min to form a uniform, transparent, light green solution;
[0071] 6) Transfer the transparent solution to a 50 mL polytetrafluoroethylene reactor liner and place a piece of activated carbon cloth 2×3 cm 2 ;
[0072] 7) The reactor was sealed and heated to 150°C for 8 hours. After the reaction was completed and cooled to room temperature, the carbon cloth loaded with the precursor was taken out and washed repeatedly in deionized water and anhydrous ethanol for 2 to 3 times;
[0073] 8) drying the precursor obtained in step 7) in a drying oven at 60° C. for 8 h;
[0074] 9) placing the precursor obtained in step 8) in a muffle furnace and annealing in an air atmosphere at a temperature of 350° C., an annealing time of 2 h, and a heating rate of 5° C. / min to obtain NiMoO4 nanosheets supported on carbon cloth;
[0075] 10) 1 mmol MnSO4·H2O, 2 mmol Co(NO3)2·6H2O, and 1 mmol Na2SO4 were dissolved in 40 mL of deionized water, and magnetically stirred at 500 rpm / min for 30 min to form a uniform, transparent magenta solution as an electrodeposition solution;
[0076] 11) The product NiMoO4 / CC obtained in step 9) was used as a working electrode, a platinum wire electrode was used as a counter electrode, and an Ag / AgCl electrode was used as a reference electrode. A three-electrode system was used. An electrochemical workstation was used to perform cyclic voltammetry electrodeposition at a rate of 5 mV / s in a potential range of -1.2 to 0.2 V for 4, 6, and 7 cycles, respectively. The carbon cloth loaded with the precursor was taken out and washed in deionized water and anhydrous ethanol for 2 to 3 times respectively;
[0077] 12) placing the sample obtained in step 11) in a drying oven at 60° C. and drying for 8 h;
[0078] 13) The precursor obtained in step 12) is placed in a muffle furnace and annealed in an air atmosphere at a temperature of 350° C., an annealing time of 2 h, and a heating rate of 5° C. / min to obtain a NiMoO4@MnCo2O4 / CC composite material.
[0079] Comparative Example 1:
[0080] This comparative example provides a method for activating a commercial carbon cloth to improve its hydrophilicity, and the specific steps are as follows:
[0081] 1) Take a cleaned 2×3cm 2 The carbon cloth was placed upright in a 100 mL beaker;
[0082] 2) Add 30 mL of 98% concentrated H2SO4 and 10 mL of 68% concentrated HNO3 into the beaker, stirring with a glass rod.
[0083] 3) placing the solution obtained in step 2) in a water bath and heating it to 65° C., and maintaining the constant temperature for 2 h;
[0084] 4) The acidified carbon cloth obtained in step 3) is washed with anhydrous ethanol and deionized water in turn, and the washed carbon cloth is dried in a drying oven at 60° C. for 8 h to obtain an activated carbon cloth.
[0085] Comparative Example 2:
[0086] This comparative example provides a preparation method of a NiMoO4 / CC flexible electrode, and the specific steps are as follows:
[0087] 1) Dissolve 1mmol Ni(NO3)2·6H2O, 1mmol Na2MoO4·4H2O, 4mmol NH4F, and 5mmol CO(NH2)2 in 40mL deionized water and stir magnetically at 500rpm / min for 30min to form a uniform, transparent, light green solution;
[0088] 2) Transfer the transparent solution to a 50mL polytetrafluoroethylene reactor and place an activated 2×3cm 2 Carbon cloth;
[0089] 3) The reactor was sealed and heated to 150°C for 8 hours. After the reaction was completed and cooled to room temperature, the carbon cloth loaded with the precursor was taken out and washed repeatedly in deionized water and anhydrous ethanol for 2 to 3 times;
[0090] 4) drying the precursor obtained in step 3) in a drying oven at 60° C. for 8 h;
[0091] 5) placing the precursor obtained in step 4) in a muffle furnace and annealing it in an air atmosphere at a temperature of 350° C., an annealing time of 2 h, and a heating rate of 5° C. / min to obtain NiMoO4 nanosheets supported on carbon cloth.
[0092] Comparative Example 3:
[0093] This comparative example provides a preparation method of a MnCo2O4 / CC composite material, and the specific steps are as follows:
[0094] 1) 1 mmol MnSO4·H2O, 2 mmol Co(NO3)2·6H2O, and 1 mmol Na2SO4 were dissolved in 40 mL deionized water, and magnetically stirred at 500 rpm / min for 30 min to form a uniform transparent magenta solution as an electrodeposition solution;
[0095] 2) Using the activated carbon cloth as the working electrode, the platinum wire electrode as the counter electrode, and the Ag / AgCl electrode as the reference electrode, a three-electrode system was used, and an electrochemical workstation was used to perform cyclic voltammetry electrodeposition at a rate of 5 mV / s in the potential range of -1.2 to 0.2 V for 5 cycles, and the carbon cloth loaded with the precursor was taken out and washed in deionized water and anhydrous ethanol for 2 to 3 times respectively;
[0096] 3) placing the sample obtained in step 2) in a drying oven at 60° C. and drying for 8 h;
[0097] 4) placing the precursor obtained in step 3) in a muffle furnace and annealing it in an air atmosphere at a temperature of 350° C., an annealing time of 2 h, and a heating rate of 5° C. / min to obtain MnCo2O4 nanosheets supported on carbon cloth.
[0098] The morphologies of the activated carbon cloth prepared in Comparative Example 1 of the present invention, the NiMoO4 / CC composite material prepared in Comparative Example 2, the MnCo2O4 / CC composite material prepared in Comparative Example 3 and the NiMoO4@MnCo2O4 / CC composite material prepared in Example 1 are as follows: Figure 1 As shown, from Figure 1 (a) shows that the surface of carbon fiber is rough and has many wrinkles after being treated with concentrated acid, which provides a more solid support for the growth of active substances. Figure 1 (b) and Figure 1 (c) It can be seen that uniform and dense NiMoO4 nanosheets are grown on carbon fibers after hydrothermal treatment, which can be used as a substrate for loading other active materials. Figure 1 (d) shows the MnCo2O4 nanosheets with shells electrodeposited on the NiMoO4 / CC electrode, accompanied by the formation of spherical nanoflowers, which further increases the specific surface area of the reaction. Figure 1 (e) and Figure 1 (f) It can be observed at close range that a large number of vertically oriented MnCo2O4 nanosheets are generated by electrodeposition. The size of the nanosheets is slightly larger than that of NiMoO4, and the newly constructed pores are larger, which is conducive to the charge transfer between the electrode and the electrolyte during the charge and discharge process. Compared with the nanosheet-nanoneedle structure, the nanosheet-nanosheet core-shell structure has a more superior transmission channel and lower charge transfer resistance, providing a more uniform electric field distribution, thereby improving the electrochemical performance of the electrode material.
[0099] The structures and crystalline phases of carbon cloth, NiMoO4 / CC, MnCo2O4 / CC and NiMoO4@MnCo2O4 / CC electrodes were studied by XRD. Figure 2As shown. It can be found that all electrodes have a strong diffraction peak at 2Theta = 25°, which belongs to the characteristic peak of C. With C as the background peak, four obvious diffraction peaks are observed at 2Theta = 14.3°, 28.8°, 32.6° and 43.9°, corresponding to the (110), (220), (022) and (330) crystal planes of NiMoO4 (JCPDS No. 00-033-0948), respectively, indicating that NiMoO4 is successfully synthesized on carbon cloth, among which the diffraction peak at (220) overlaps with the (003) crystal plane of CC, increasing the intensity of the peak. When the 2Theta values are 36°, 43.8° and 63.6°, the crystal planes correspond to (311), (400) and (440). The crystal structure is consistent with that of MnCo2O4 (JCPDS No.01-084-0482), indicating that MnCo2O4 was successfully synthesized on carbon cloth. The XRD results of NiMoO4@MnCo2O4 / CC show that the composite material not only has diffraction peaks of MnCo2O4 (311), (400) and (440) crystal planes, but also a diffraction peak of NiMoO4 (110) crystal plane is observed, indicating that NiMoO4@MnCo2O4 was successfully synthesized on carbon cloth.
[0100] The pore size distributions of the NiMoO4 / CC composite material prepared in Comparative Example 2 of the present invention, the MnCo2O4 / CC composite material prepared in Comparative Example 3 and the NiMoO4@MnCo2O4 / CC composite material prepared in Example 1 are as follows: Figure 3 As shown in the figure, the average pore sizes of NiMoO4 / CC, MnCo2O4 / CC and NiMoO4@MnCo2O4 / CC are 5.7nm, 13.2nm and 9.7nm respectively. The average pore size of MnCo2O4 is larger and the average pore size of NiMoO4 is smaller, thus producing a core-shell structure with a funnel-shaped characteristic nanostructure framework. Compared with single NiMoO4 or MnCo2O4, this greatly increases the specific surface area of the material and also provides more electroactive sites.
[0101] The constant current charge and discharge diagrams of the NiMoO4 / CC composite material prepared in Comparative Example 2 of the present invention, the MnCo2O4 / CC composite material prepared in Comparative Example 3 and the NiMoO4@MnCo2O4 / CC composite material prepared in Example 1 in a 2 mol / L potassium hydroxide aqueous solution are shown in FIG. Figure 4 As shown in the figure, it can be clearly seen that the performance of the core-shell composite NiMoO4@MnCo2O4 / CC is better than any single component material. 2 When NiMoO4 / CC, MnCo2O4 / CC and NiMoO4@MnCo2O4 / CC have area specific capacitances of 0.51 F / cm 2, 3.43F / cm 2 , 4.89F / cm 2 , indicating that nanosheet-nanosheet core-shell structure materials can provide more reactive sites and combine the advantages of different single component materials to greatly improve the electrochemical performance of electrode materials.
[0102] The cyclic voltammetry (CV) curves of the NiMoO4 / CC composite material prepared in Comparative Example 2 of the present invention, the MnCo2O4 / CC composite material prepared in Comparative Example 3 and the NiMoO4@MnCo2O4 / CC composite material prepared in Example 1 in 2 mol / L potassium hydroxide aqueous solution are shown in FIG. Figure 5 As shown in the figure, it can be seen that at 20mV s -1 At a scan rate of , the CV curve area of the NiMoO4@MnCo2O4 / CC electrode is significantly larger than that of the other electrodes, which also indicates that its capacitance is excellent.
[0103] The EIS impedance diagrams of the NiMoO4 / CC composite material prepared in Comparative Example 2 of the present invention, the MnCo2O4 / CC composite material prepared in Comparative Example 3 and the NiMoO4@MnCo2O4 / CC composite material prepared in Example 1 in 2 mol / L potassium hydroxide aqueous solution are as follows: Figure 6 As shown in Figure 2, the charge transfer resistance (R ct ) is up to 2.9Ω. However, it is reduced to 1.1Ω when synthesized with NiMoO4 to form a core-shell structure. The NiMoO4@MnCo2O4 / CC electrode has the smallest intercept with the x-axis, indicating the equivalent series resistance (R s ) is the smallest. In addition, the slope in the low-frequency region is also the steepest for NiMoO4@MnCo2O4 / CC, indicating that the charge diffusion rate is the fastest.
[0104] The constant current charge and discharge diagram of the NiMoO4@MnCo2O4 / CC composite material prepared in Example 1 of the present invention in a 2 mol / L potassium hydroxide aqueous solution is shown in FIG. Figure 7 As shown in the figure, it can be seen that at different current densities, the charge and discharge curves of the NiMoO4@MnCo2O4 / CC electrode show an obvious triangular shape, and the discharge and charge times are similar, indicating its excellent electrochemical reversibility.
[0105] The constant current charge and discharge diagram of the NiMoO4@MnCo2O4 / CC composite material prepared in Example 2 of the present invention in a 2 mol / L potassium hydroxide aqueous solution is shown in FIG. Figure 8 As shown in the figure, it can be seen that after 5 cycles of electrodeposition, the prepared electrode has the longest charge and discharge time, indicating that it has the maximum capacitance value at this time.
[0106] The EIS impedance diagram of the NiMoO4@MnCo2O4 / CC composite material prepared in Example 2 of the present invention in 2 mol / L potassium hydroxide aqueous solution is as follows: Fig. 9 As shown in the figure, it can be seen that after 5 cycles of electrodeposition, the electrode material has the steepest slope in the low-frequency region, indicating that the charge diffusion rate is the fastest at this time.
[0107] Combination Figure 8 and Fig. 9 , indicating that the NiMoO4@MnCo2O4 / CC composite material has the maximum specific capacitance in 2 mol / L potassium hydroxide aqueous solution after 5 cycles of electrodeposition. At the beginning, the electrode specific capacitance increases with the increase of electrodeposition time. However, when the covering shell material exceeds a certain limit, the internal resistance of the electrode material also increases, and the influence on the specific capacitance gradually exceeds the influence of the material's own capacitance.
[0108] The present invention provides a binder-free NiMoO4@MnCo2O4 / CC core-shell composite material with good crystal shape, low pollution and low cost. It can be obtained on carbon cloth after hydrothermal and electrodeposition treatment. It is used as an electrode material for characterization testing. The results show that the material is a core-shell structure with a funnel-shaped characteristic nanostructure framework. At the same time, electrochemical tests also show high specific capacitance and excellent electrochemical reversibility, and it has potential application prospects in energy storage.
[0109] The number of devices and processing scales described here are used to simplify the description of the present invention, and the application, modification and variation of the present invention will be obvious to those skilled in the art.
[0110] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.
Claims
1. A method for preparing a core-shell structure electrode material, characterized in that: Methods include: 1) placing the raw carbon cloth in a mixed solution of concentrated sulfuric acid and concentrated nitric acid for water bath activation, and cutting the carbon cloth after the water bath activation is completed; 2) The cut carbon cloth is subjected to hydrothermal treatment with a mixed metal solution to load two mixed metals, and then annealed and electrochemically reacted in sequence to deposit another two mixed metals; 3) The carbon cloth obtained in step 2) is washed and dried in sequence, and then placed in a muffle furnace for annealing to obtain a carbon cloth loaded with NiMoO4@MnCo2O4 / CC, i.e., a NiMoO4@MnCo2O4 / CC core-shell structure electrode material.
2. The method for preparing a core-shell structure electrode material according to claim 1, characterized in that: The step 1) is specifically as follows: 1.1) Mix 90-98% concentrated sulfuric acid and 60-70% concentrated nitric acid in a volume ratio of (2-3):1 to form a mixed solution; 1.2) placing the raw carbon cloth in the mixed solution obtained in step 1.1) for activation treatment in a water bath at a temperature of 65 to 70° C. for 2 to 3 hours; 1.3) After water bath activation, the carbon cloth is cut.
3. The method for preparing the core-shell structure electrode material according to claim 1, characterized in that: The step 2) is specifically as follows: 2.1) dissolving nickel salt, molybdenum salt, ammonium fluoride and urea in deionized water and stirring them magnetically to obtain a mixed solution; 2.2) pouring the mixed solution obtained in step 2.1) into a polytetrafluoroethylene reactor, and then placing the carbon cloth obtained in step 1) upright into the polytetrafluoroethylene reactor for hydrothermal reaction, and cooling to room temperature after the reaction is complete to obtain a carbon cloth loaded with a precursor; 2.3) The carbon cloth loaded with the precursor obtained in step 2.2) is taken out, cleaned and dried, and then placed in a muffle furnace for annealing to obtain a carbon cloth loaded with NiMoO4 nanosheets (NiMoO4 / CC); 2.4) The NiMoO4 / CC obtained in step 2.3) is used as a working electrode, a platinum wire electrode is used as a counter electrode, an Ag / AgCl electrode is used as a reference electrode, and a mixed metal salt is used as an electrolyte. Cyclic voltammetry is used for deposition. After the deposition is completed, a carbon cloth with deposited mixed metals and loaded NiMoO4 nanosheets is obtained.
4. The method for preparing the core-shell structure electrode material according to claim 3, characterized in that: In the step 2.1), the nickel salt is one or more of nickel chloride, nickel sulfate and nickel nitrate, the molybdenum salt is one or more of ammonium molybdate, potassium molybdate and sodium molybdate, and the molar ratio of the nickel salt, the molybdenum salt, ammonium fluoride and urea is (1-2 mmol): (1-2 mmol): (4-6 mmol): (5-7 mmol); In the step 2), the stirring speed is 400-500 rpm / min, and the stirring time is 30-60 min.
5. The method for preparing the core-shell structure electrode material according to claim 3, characterized in that: In the step 2.2), the hydrothermal reaction temperature is 140-160° C., and the hydrothermal insulation time is 6-8 hours.
6. The method for preparing a core-shell structure electrode material according to claim 3, characterized in that: In the step 2.3), the cleaning solutions are deionized water and anhydrous ethanol, the cleaning times are 2 to 3 times, the drying temperature is 60 to 70°C, the drying time is 8 to 10 hours, the annealing temperature is 350 to 400°C, the annealing time is 2 to 4 hours, and the heating rate is 5 to 6°C / min.
7. The method for preparing a core-shell structure electrode material according to claim 3, characterized in that: In the step 2.4), the mixed metal salt is a mixture of cobalt salt and manganese salt, the molar concentration of the electrolyte is 0.075 mol / L to 0.15 mol / L, the deposition potential is -1.2 to 0.2 V, the deposition cycle is 4 to 7 cycles, and the deposition rate is 5 mV / s.
8. The method for preparing a core-shell structure electrode material according to claim 1, characterized in that: In the step 3), the cleaning solutions are deionized water and anhydrous ethanol in sequence, the cleaning times are 2 to 3 times, the drying temperature is 60 to 70°C, the drying time is 8 to 10 hours, the annealing temperature is 350 to 400°C, the annealing time is 2 to 4 hours, and the heating rate is 5 to 6°C / min.
9. The method for preparing a core-shell structure electrode material according to claim 7, characterized in that: The cobalt salt is one or more of cobalt nitrate and cobalt chloride; The manganese salt is one or more of manganese sulfate, manganese nitrate and manganese chloride.
10. Application of the core-shell structure electrode material prepared by the preparation method according to any one of claims 1 to 9, characterized in that: Applications in electrode materials for energy conversion and storage.