Battery pole piece and preparation method thereof, battery and power utilization device

By using polyvinylidene fluoride resin and crosslinking agent in the preparation of battery electrode sheets, the limitation of the molecular weight of the adhesive on the performance of the electrode sheets is solved, the bonding strength and uniformity of the electrode sheets are improved, and the Production cost and process complexity.

CN118943284AInactive Publication Date: 2024-11-12BYD CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410994676.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing battery electrode sheet preparation process, high molecular weight binders lead to large viscosity of the slurry and difficult to mix evenly, while low molecular weight binders lead to insufficient bonding strength, making it difficult to meet the uniformity and conductivity requirements of the electrode sheet.

Method used

Polyvinylidene fluoride resin is used as the adhesive component, and a crosslinking agent is added during the drying process to make the adhesive and the crosslinking agent crosslinking reaction, improve the bonding strength and uniformity of the electrode sheet. Low viscosity adhesives increase the amount of active materials and increase the solid content.

Benefits of technology

The high bonding strength and uniformity of the electrode sheet are achieved, the production cost and process complexity are reduced, and the solid content and conductivity of the slurry are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004960194640000101
    Figure BDA0004960194640000101
  • Figure BDA0004960194640000111
    Figure BDA0004960194640000111
  • Figure FDA0004960194420000011
    Figure FDA0004960194420000011
Patent Text Reader

Abstract

The invention discloses a battery pole piece and a preparation method thereof, a battery and an electric device. The battery pole piece comprises a current collector and an active material layer. The active material layer is attached to at least one side of the current collector. The active material layer comprises an active material and an adhesive polymer, the adhesive polymer comprises a part obtained by cross-linking an adhesive component and a cross-linking agent component, the adhesive component comprises polyvinylidene fluoride resin, and the cross-linking agent component has an amino group. According to the battery pole piece disclosed by the invention, the cross-linking agent is added in the stage of preparing the slurry, and the adhesive and the cross-linking agent are subjected to cross-linking reaction by utilizing high temperature during drying, so that low viscosity brought to the slurry by the adhesive before cross-linking can be utilized, the use amount of the active material can be increased, and the solid content of the slurry can be increased; and high bonding strength can be brought to the pole piece after the adhesive is crosslinked, and particularly, the bonding strength between the pole piece and the current collector is proper.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of new energy technology, and more specifically to a battery pole piece and a preparation method thereof, a battery and an electrical device. Background Art

[0002] Binder is an important component in manufacturing battery electrode materials, which is used to bind active materials, conductive agents, etc. together.

[0003] At present, the commercial battery pole piece preparation process often adopts the method of dissolving the binder in the solvent and then mixing it with other components. However, this method needs to balance multiple requirements, such as ensuring the bonding strength of the pole piece and maintaining the appropriate slurry viscosity for production and processing. In the process of preparing slurry and pole pieces, the following issues are involved:

[0004] (1) Using high molecular weight adhesives to reduce the amount of additives and maintain bonding strength, however, high molecular weight will cause the viscosity of the mixed slurry to be very high, making it difficult to fully mix and disperse the slurry, resulting in a decrease in the surface density and uniformity of the electrode after drying;

[0005] (2) Using a high molecular weight adhesive to increase the viscosity, the viscosity is reduced by adding more solvent. This method requires the addition of a large amount of solvent, resulting in a decrease in the efficiency of the subsequent drying process and an increase in cost;

[0006] (3) Use a low molecular weight adhesive and add a small amount of solvent to maintain the appropriate slurry viscosity. However, the low molecular weight of the adhesive will lead to insufficient bonding strength after the electrode is dried, and it is difficult to meet the requirements by increasing the amount of adhesive.

[0007] Therefore, it is necessary to design a method that can improve the electrode peeling force under the condition of using a low molecular weight binder to keep the slurry configuration process simple, and have low requirements on the polymer molecular weight and a simpler synthesis process. Summary of the invention

[0008] A series of simplified concepts are introduced in the Summary of the Invention section, which will be further described in detail in the Detailed Description of the Invention section. The Summary of the Invention section of this application does not mean to attempt to define the key features and essential technical features of the claimed technical solution, nor does it mean to attempt to determine the scope of protection of the claimed technical solution.

[0009] In order to at least partially solve the above problems, the first aspect of the present application provides a battery electrode sheet, the battery electrode sheet comprising:

[0010] current collector;

[0011] an active material layer, the active material layer being attached to at least one side of the current collector, the active material layer comprising an active material and a binding polymer;

[0012] The adhesive polymer includes a portion obtained by cross-linking an adhesive component and a cross-linking agent component;

[0013] The adhesive component includes polyvinylidene fluoride resin;

[0014] The crosslinker component has an amine group.

[0015] According to the battery pole piece of the present application, a cross-linking agent is added in the stage of preparing the slurry, and the high temperature during drying is used to cause a cross-linking reaction between the adhesive and the cross-linking agent. This can not only utilize the low viscosity of the slurry brought by the adhesive before cross-linking, thereby increasing the amount of active material and improving the solid content of the slurry, but also achieve high bonding strength for the pole piece after the adhesive is cross-linked, especially the bonding strength between the pole piece and the current collector is appropriate, and the pole piece has good uniformity and conductivity.

[0016] In an optional embodiment, the weight average molecular weight of the polyvinylidene fluoride resin is 400,000 g / mol to 1,070,000 g / mol.

[0017] Preferably, the weight average molecular weight of the polyvinylidene fluoride resin is 520,000 g / mol to 780,000 g / mol.

[0018] In an optional implementation, the mass ratio of the cross-linking agent component to the adhesive component is 1:8 to 1:12.

[0019] In an alternative embodiment, the crosslinker component comprises a substance having Formula I or Formula II;

[0020] Wherein, the general formula I is The molecular formula of R is C a H b O c N d , where 2≤a≤100, 4≤b≤200, 0≤c≤100, 0≤d≤100;

[0021] The general formula II is, R' is an alkyl group, preferably, the alkyl group is selected from ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, 1-pentyl, 2-pentyl, neopentyl, benzyl, phenyl, cyclopentyl, cyclohexyl, 1-hexyl, 2-hexyl, 3-hexyl, 1-octyl, 2-octyl, 2-ethylhexyl, 3-octyl, n-decyl, 1-dodecyl, and norbornyl.

[0022] In an optional embodiment, the monomer of the polyvinylidene fluoride resin includes vinylidene fluoride, and the polyvinylidene fluoride resin further includes:

[0023] At least one of perfluoropropylene, chlorotrifluoroethylene, trifluoroethylene and tetrafluoroethylene; and / or a non-fluorine-containing monomer.

[0024] In an optional embodiment, the vinylidene fluoride accounts for 75% to 99% of the polyvinylidene fluoride resin main chain.

[0025] Preferably, the vinylidene fluoride accounts for 90% to 95% of the main chain of the polyvinylidene fluoride resin.

[0026] In an alternative embodiment, the adhesive polymer comprises a substance having the general formula III,

[0027] Wherein, the general formula III is wherein R is an alkyl group, and m and n are positive integers.

[0028] The second aspect of the present application provides a method for preparing the battery electrode sheet described in the first aspect, comprising:

[0029] mixing an active material, a binder component, and a cross-linker component to form an electrode slurry;

[0030] The electrode slurry is applied to at least one side surface of the current collector and subjected to a heat treatment so as to form the active material layer on at least one side surface of the current collector to obtain the battery electrode sheet.

[0031] In an optional embodiment, the heating temperature is greater than or equal to 100°C.

[0032] Preferably, the heating temperature is greater than or equal to 130°C.

[0033] In an optional implementation, the viscosity of the electrode slurry is 800 mPa·s to 3000 mPa·s.

[0034] A third aspect of the present application provides a battery, comprising the battery electrode sheet described in the first aspect or a battery electrode sheet prepared by the method for preparing the battery electrode sheet described in the second aspect.

[0035] A fourth aspect of the present application provides an electrical device, wherein the electrical device comprises the battery described in the third aspect. DETAILED DESCRIPTION

[0036] In the following description, a large number of specific details are provided to provide a more thorough understanding of the present application. However, it is apparent to those skilled in the art that the present application can be implemented without one or more of these details. In other examples, in order to avoid confusion with the present application, some technical features well known in the art are not described.

[0037] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should also be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of the features, wholes, steps, operations, elements and / or components, but does not exclude the presence or addition of one or more other features, wholes, steps, operations, elements, components and / or combinations thereof.

[0038] The first aspect of the present application provides a battery electrode, in particular a positive electrode. In another aspect, a battery and an electric device are provided. The battery has the battery electrode provided in the present application. The electric device uses the battery provided in the present application. Exemplarily, the electric device can be a new energy vehicle.

[0039] The battery pole piece includes a current collector and an active material layer, the active material layer is attached to at least one side of the current collector, the active material layer includes an active material and an adhesive polymer, the adhesive polymer includes a part obtained by cross-linking an adhesive component and a cross-linking agent component, the adhesive component includes a polyvinylidene fluoride resin, and the cross-linking agent component has an amine group.

[0040] According to the battery pole piece of the present application, a cross-linking agent is added in the stage of preparing the slurry, and the high temperature during drying is used to cause a cross-linking reaction between the adhesive and the cross-linking agent. This can not only utilize the low viscosity of the slurry brought by the adhesive before cross-linking, thereby increasing the amount of active material and improving the solid content of the slurry, but also achieve high bonding strength for the pole piece after the adhesive is cross-linked, especially the bonding strength between the pole piece and the current collector is appropriate, and the pole piece has good uniformity and conductivity.

[0041] In addition, a crosslinking agent with an amine group is selected, which has suitable reaction conditions and reaction speed. Specifically, the amine-based crosslinking agent and the polyvinylidene fluoride resin will not crosslink quickly after mixing, resulting in difficulty in processing, and will undergo a crosslinking reaction synchronously with the evaporation of the solvent as the temperature rises, and can react completely after the solvent evaporates, having good production and processing adaptability.

[0042] The positive electrode active material includes one or more of a lithium transition metal oxide, a lithium-containing phosphate and their respective modified compounds. For example, the lithium transition metal oxide may include: lithium nickel oxide, lithium cobalt oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium manganese cobalt oxide, lithium nickel cobalt oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese oxide and their respective modified compounds. The lithium-containing phosphate may include one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon and their respective modified compounds.

[0043] As an implementation form, the polyvinylidene fluoride resin can be a copolymer, that is, it has other monomers, such as other fluorine-containing monomers. Exemplarily, other fluorine-containing monomers include at least one of perfluoropropylene, chlorotrifluoroethylene, trifluoroethylene and tetrafluoroethylene. The polyvinylidene fluoride resin can also include non-fluorine-containing monomers. Among them, the non-fluorine-containing monomer can be acrylate and its derivatives, etc.

[0044] As an example, the proportion of vinylidene fluoride monomer in the main chain is 75% to 99%, such as 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98% or 99%, etc. Preferably, the proportion of vinylidene fluoride monomer in the main chain is 90% to 95%.

[0045] The polyvinylidene fluoride resin of the above-mentioned adhesive component has a moderate molecular weight, for example, its weight average molecular weight is 400000g / mol~1070000g / mol. Preferably, the weight average molecular weight of the polyvinylidene fluoride resin is 520000g / mol~780000g / mol. In this weight average molecular weight range, the polyvinylidene fluoride resin has better solubility in the solvent, so that the electrode slurry obtained by the configuration has a smaller viscosity, thereby allowing more solid active materials to be added. In addition, the polyvinylidene fluoride resin with a moderate molecular weight does not need to be excessively modified, the synthesis conditions are mature, the requirements for the modified monomer are low, and the synthesis process is simple.

[0046] As an example, the polyvinylidene fluoride resin of the above-mentioned adhesive component can be prepared by the following process.

[0047] In a nitrogen atmosphere at 50-70°C, vinylidene fluoride monomer (1,1-difluoroethylene monomer) is introduced into a reaction kettle containing water. Then, an emulsifier, paraffin wax, and a portion of the initiator (40% of the total amount of the initiator) and a portion of the chain transfer agent (40% of the total amount of the chain transfer agent) are added.

[0048] The pressure is then maintained at 6 to 10 MPa for 6 to 10 hours. The pressure is maintained by continuously introducing 1,1-difluoroethylene.

[0049] After the reaction starts, part of the initiator (10% of the total amount of the initiator) and part of the chain transfer agent (10% of the total amount of the chain transfer agent) are added in batches every hour. After the monomer conversion rate is high, the reaction is stopped and post-processing is performed to obtain the above-mentioned vinylidene fluoride polymer. The post-processing step includes repeated washing until the conductivity of the filtrate drops below 0.08 and then vacuum drying at 40-50°C for 20-30 hours.

[0050] Wherein, non-fluorine-containing monomers can be added while the vinylidene fluoride monomer is introduced into the reaction kettle. The mass ratio of vinylidene fluoride (1,1-difluoroethylene monomer) to comonomer (non-fluorine-containing monomer) is 100:(0.03-10).

[0051] As an implementation form, when the vinylidene fluoride monomer is introduced into the reaction kettle, other fluorine-containing monomers are also added, wherein the amount of the other fluorine-containing monomers added is less than 10.00% of the total molar amount of the fluorine-containing monomers.

[0052] As an optional embodiment, the above-mentioned emulsifier can be a perfluorocarboxylic acid ammonium compound or a perfluorocarboxylic acid metal salt or a perfluoropolyether compound. Preferably, the emulsifier is at least one of ammonium perfluorohexanoate, sodium perfluorohexanoate, potassium perfluorohexanoate, ammonium perfluorooctanoate, sodium perfluorooctanoate, potassium perfluorooctanoate, ammonium perfluorodecanoate, sodium perfluorodecanoate, potassium perfluorodecanoate, ammonium perfluorooctanoate, sodium perfluorooctanoate, and potassium perfluorooctanoate.

[0053] As an optional embodiment, the above-mentioned initiator is an organic peroxide initiator, a sulfate initiator or a persulfate / sodium bisulfite initiator. The organic peroxide initiator can be at least one of di-n-propyl peroxydicarbonate, diisopropyl peroxydicarbonate, diethyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, dicyclopentyl peroxydicarbonate, tert-butyl peroxypivalate, tert-amyl peroxypivalate, diisobutyryl peroxide, benzoyl peroxide, tert-butyl hydroperoxide, di-tert-butyl peroxide or N,N-azobisisobutyronitrile. The persulfate initiator is ammonium persulfate or potassium persulfate. Wherein, the amount of the initiator added is 0.01 to 0.4% of the mass of the 1,1-difluoroethylene monomer.

[0054] As an optional embodiment, the chain transfer agent is at least one of ethyl acetate, diethyl malonate, diethyl carbonate, dimethyl carbonate, methanol, ethanol, n-propanol, isopropanol, acetone or butanone. Preferably, the mass of the chain transfer agent accounts for 0.01% to 2.0% of the total mass of the 1,1-difluoroethylene monomer and the sulfonic acid compound.

[0055] The crosslinking agent component has an amine group. As an implementation form, it contains a substance having the general formula I.

[0056] Wherein, the general formula I is The molecular formula of R is C a H b O c N d , where 2≤a≤100, 4≤b≤200, 0≤c≤100, 0≤d≤100.

[0057] As another implementation form, the crosslinking agent component comprises a substance having the general formula II: wherein the general formula II is, and R' is an alkyl group.

[0058] Illustratively, the alkyl group can be selected from ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, 1-pentyl, 2-pentyl, neopentyl, benzyl, phenyl, cyclopentyl, cyclohexyl, 1-hexyl, 2-hexyl, 3-hexyl, 1-octyl, 2-octyl, 2-ethylhexyl, 3-octyl, n-decyl, 1-dodecyl, and norbornyl.

[0059] As an example, the mass ratio of the cross-linking agent component to the adhesive component is 1:8 to 1:12. Preferably, the mass ratio of the cross-linking agent component to the adhesive component is 1:10.

[0060] The second aspect of the present application provides a method for preparing a battery electrode sheet as described in the first aspect, comprising:

[0061] mixing an active material, a binder component, and a cross-linker component to form an electrode slurry;

[0062] The electrode slurry is coated on at least one side of the surface of the current collector and subjected to a heat treatment so as to form an active material layer on at least one side of the surface of the current collector to obtain a battery electrode.

[0063] The active material layer is formed by applying the positive electrode slurry to the surface of the current collector and heating it. In other words, the electrode slurry is applied to at least one side of the current collector and heated to form the above-mentioned active material layer on at least one side of the current collector to obtain the battery pole sheet.

[0064] As an implementation form, the viscosity of the electrode slurry is 800 mPa·s to 3000 mPa·s. The viscosity in this range is in a suitable range, which is convenient for subsequent stirring processing and allows the addition of more active materials.

[0065] Specifically, the positive electrode slurry also includes active materials, conductive agent components, adhesive components, crosslinking agent components and solvent components. After the above components are mixed evenly to form the positive electrode slurry, it is coated on the positive electrode collector and heated and dried to form the positive electrode sheet.

[0066] The conductive agent component may include one or more of conductive graphite, carbon black, acetylene black, carbon dots, carbon nanotubes, Ketjen black, carbon nanofibers, activated carbon, and graphene.

[0067] The positive electrode current collector may be a metal foil current collector or a composite current collector. As an example, the metal foil may be aluminum foil or the like.

[0068] As another example, the composite current collector may include a polymer material base metal layer, wherein the metal layer is disposed on at least one surface of a polymer material substrate. The metal material may be copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, silver alloy, etc. The polymer material substrate may be polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.

[0069] The monomer of the polyvinylidene fluoride resin of the adhesive component mainly includes vinylidene fluoride. As an implementation form, the polyvinylidene fluoride resin can be a homopolymer. For example, the monomers are all vinylidene fluoride.

[0070] The solvent used was N-methylpyrrolidone.

[0071] The heating temperature is greater than or equal to 100° C. Preferably, the heating temperature is greater than or equal to 130° C.

[0072] Among them, since the preparation of the pole piece requires the solvent to be volatilized, and the solvent needs to be above 100°C to be completely dried, the heating temperature is greater than or equal to 100°C. Preferably, the heating temperature is greater than or equal to 130°C to increase the speed and degree of the cross-linking reaction, thereby ensuring that the cross-linking reaction can be completed after the solvent evaporates.

[0073] According to the electrode pole piece of the present application, the electrode slurry used includes an adhesive component and a cross-linking agent component. The polyvinylidene fluoride resin as the adhesive component does not need to be modified too much, the synthesis conditions are mature, the requirements for modified monomers are low, and the synthesis process is simple. Compared with the existing adhesive polymers, the present application adopts the method of adding a cross-linking agent and fully stirring during the slurry configuration process, and the polyvinylidene fluoride resin requires a small molecular weight before cross-linking, so it has better solubility in the solvent. Due to the small molecular weight of the polymer, the time required for the dissolution process is shorter, and the solid content of the slurry can be further increased, saving production costs. Since the polyvinylidene fluoride resin is added in a reduced amount and is not cross-linked during the pulping process, the slurry viscosity is lower, and other components are easier to be evenly dispersed on the surface of the pole piece. In addition, the cross-linking agent component of the present application is widely available, the addition amount is low, and the impact on cost and process is small.

[0074] Compared with traditional straight-chain and branched-chain adhesives, the cross-linked polymer of the present application can form a network space structure, thereby further enhancing the bonding force; in addition, the structure can better wrap the metal ions in the active substance in the polymer, thereby enhancing the ion conduction rate of the positive electrode plate.

[0075] In one embodiment of the present invention, the adhesive polymer comprises a substance having the general formula III,

[0076] Wherein, the general formula III is Wherein R is an alkyl group, and m and n are positive integers. The substance having this general formula forms a cross-linked network structure and has great strength to achieve the bonding function.

[0077] In a third aspect, the present application provides a battery, comprising the battery electrode sheet described in the first aspect or a battery electrode sheet prepared by the method for preparing the battery electrode sheet described in the second aspect.

[0078] The battery according to the present application has a technical effect similar to that of the battery pole piece described in the first aspect.

[0079] In a fourth aspect, the present application provides an electrical device, comprising the battery described in the third aspect.

[0080] The electrical device according to the present application has a technical effect similar to that of the battery of the third aspect.

[0081] The technical solution of the present application will be described in more detail below in combination with embodiments and comparative examples.

[0082] Example 1

[0083] First, the linear polymer is prepared (preparation of the adhesive component).

[0084] A horizontal reactor with a stirring blade of high suction and low shear force and a volume of 50L was selected. First, 20kg of pure water, 250g of 4% potassium perfluorooctanoate solution and 40g of paraffin (melting point: 60°C) were put into the reactor, and nitrogen was filled and vacuumed to deoxygenate until the oxygen content in the reactor was less than 20ppm. The stirring speed was adjusted to 130rpm / min, the reactor temperature was raised to 60°C, and vinylidene fluoride monomer was added until the reactor pressure reached 5.0MPa. 24g of diisopropyl peroxydicarbonate and 12g of ethyl acetate were added to the reactor through an auxiliary pump, and the addition time was controlled to be 0.5 hours (addition of the auxiliary pump and reaction of the reactor were carried out to ensure uniform reaction), and the reaction pressure was maintained at 5.0MPa by continuously adding vinylidene fluoride monomer, and 6g of initiator and 3g of chain transfer agent ethyl acetate were added in batches every hour. A total of 5 kg of vinylidene fluoride monomer was added to the reaction. When the pressure dropped to 3.0 MPa, the gas was released and the material was collected. The reaction time was 8 hours. The polymer was filtered to remove wax, coagulated and demulsified, washed, dehydrated, and then dried. The linear polyvinylidene fluoride polymer obtained by drying was sampled and dissolved in N,N-dimethylformamide to test its molecular weight and dispersity.

[0085] Then prepare the positive electrode sheet. Add 20g of the linear polymer prepared in the above steps to 700g of the solvent N-methylpyrrolidone to form a glue solution, and test the viscosity of the glue solution. Then weigh 1kg of positive electrode active material lithium iron phosphate, 10g of positive electrode conductive agent carbon nanotubes, and 2g of cross-linking agent 1,3-propylenediamine, and add them, then stir in a mixer for 200min to form a positive electrode slurry, and measure the viscosity of the positive electrode slurry.

[0086] The positive electrode slurry was evenly coated on the surface of the positive electrode current collector aluminum foil, and then placed in an oven and dried at 130° C. to obtain a positive electrode sheet, and the bonding strength of the sheet was tested.

[0087] The molecular weight was tested by liquid chromatography using DMF as the mobile phase and PMMA as the standard sample on an Agilent liquid chromatograph 1290.

[0088] After the glue solution is prepared, the viscosity of the glue solution is tested before adding the conductive slurry and the positive electrode active material, and the viscosity of the positive electrode slurry is tested after adding the conductive slurry and the positive electrode active material.

[0089] The adhesion is tested by 180° peeling force test method with a tensile speed of 50 mm / min and with reference to GB / T2792.

[0090] Example 2

[0091] The steps are the same as those in Example 1, except that 1,6-hexanediamine is used as the cross-linking agent.

[0092] Example 3

[0093] First, the linear polymer is prepared (preparation of the adhesive component).

[0094] A horizontal reactor with a stirring blade of high suction and low shear force and a volume of 50L was selected. First, 20kg of pure water, 250g of 4% potassium perfluorooctanoate solution and 40g of paraffin (melting point: 60°C) were put into the reactor, and nitrogen was filled and vacuumed to deoxygenate until the oxygen content in the reactor was less than 20ppm. The stirring speed was adjusted to 130rpm / min, and the reactor temperature was raised to 60°C. Vinylidene fluoride (VDF) and hexafluoropropylene (HFP) were added until the reactor pressure reached 5.0MPa (VDF:HFP=19:1). 24g of diisopropyl peroxydicarbonate and 12g of ethyl acetate were added to the reactor through an auxiliary pump, and the addition time was controlled to be 0.5 hours (addition of the auxiliary pump and reaction of the reactor were carried out to ensure uniform reaction), and the reaction pressure was maintained at 5.0MPa by continuously adding vinylidene fluoride monomer, and 6g of initiator and 3g of chain transfer agent ethyl acetate were added in batches every hour. A total of 5 kg of vinylidene fluoride monomer was added to the reaction. When the pressure dropped to 3.0 MPa, the gas was released and the material was collected. The reaction time was 8 hours. The polymer was filtered to remove wax, coagulated and demulsified, washed, dehydrated, and then dried. The linear polyvinylidene fluoride polymer obtained by drying was sampled and dissolved in N,N-dimethylformamide to test its molecular weight and dispersity.

[0095] Then prepare the positive electrode sheet. Add 20g of the linear polymer prepared in the above steps to 700g of the solvent N-methylpyrrolidone to form a glue solution, and test the viscosity of the glue solution. Then weigh 1kg of positive electrode active material lithium iron phosphate, 10g of positive electrode conductive agent carbon nanotubes, and 2g of cross-linking agent 1,3-propylenediamine, and add them, then stir in a mixer for 200min to form a positive electrode slurry, and measure the viscosity of the positive electrode slurry.

[0096] The positive electrode slurry was evenly coated on the surface of the positive electrode current collector aluminum foil, and then placed in an oven and dried at 130° C. to obtain a positive electrode sheet, and the bonding strength of the sheet was tested.

[0097] The molecular weight was tested by liquid chromatography using DMF as the mobile phase and PMMA as the standard sample on an Agilent liquid chromatograph 1290.

[0098] After the glue solution is prepared, the viscosity of the glue solution is tested before adding the conductive slurry and the positive electrode active material, and the viscosity of the positive electrode slurry is tested after adding the conductive slurry and the positive electrode active material.

[0099] The adhesion is tested by 180° peeling force test method with a tensile speed of 50 mm / min and with reference to GB / T2792.

[0100] Example 4

[0101] The steps are the same as those in Example 3, except that 1,6-hexanediamine is used as the cross-linking agent.

[0102] Example 5

[0103] The steps are the same as those in Example 3, except that 1,8-octanediamine is used as the cross-linking agent.

[0104] Example 6

[0105] The steps are the same as those in Example 3, except that methacrylamide is used as the cross-linking agent.

[0106] Example 7

[0107] The steps are the same as those in Example 1, except that n-propylamine is used as the cross-linking agent.

[0108] Comparative Example 1

[0109] The steps are the same as those in Example 3, except that 1,3-propylene glycol is used as the cross-linking agent.

[0110] Comparative Example 2

[0111] The steps are the same as those in Example 1, except that no cross-linking agent is added.

[0112] The results of Examples 1-7 and Comparative Examples 1-2 are shown in the table below.

[0113]

[0114]

[0115] Examples 1, 2 and 7 use the same homopolymer adhesive component, and Examples 3, 4, 5 and 6 use the same copolymer adhesive component. From the comparison of the results of the above two types of adhesive components, it can be seen that whether it is a homopolymer adhesive component or a copolymer adhesive component, its molecular weight is within the range specified in this application, and can achieve a lower viscosity of the glue and slurry, and has a higher bonding force after cross-linking.

[0116] Comparing Example 3 with Comparative Example 1, it can be seen that although Comparative Example 1 has a suitable viscosity without using an amine-containing crosslinking agent, the adhesion after crosslinking is poor.

[0117] Comparing Example 1 with Comparative Example 2, no crosslinking agent was added in Comparative Example 2, resulting in a significant difference in adhesion between the comparative example 2 and Example 1.

[0118] The processes and steps described in all the above preferred embodiments are only examples. Unless adverse effects occur, various processing operations can be performed in a sequence different from the sequence of the above processes. The sequence of steps in the above processes can also be increased, merged or deleted according to actual needs.

[0119] Unless otherwise defined, the technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present application. The terms used herein are only for describing specific implementation purposes and are not intended to limit the present application. The features described herein in one embodiment may be applied to another embodiment individually or in combination with other features, unless the feature is not applicable or otherwise specified in the other embodiment.

[0120] The present application has been illustrated through the above-mentioned embodiments, but it should be understood that the above-mentioned embodiments are only for the purpose of example and explanation, and the present application is not limited to the above-mentioned embodiments. According to the teachings of the present application, more variations and modifications can be made, and these variations and modifications all fall within the scope of protection claimed by the present application.

Claims

1. A battery pole piece, characterized in that: The battery pole piece comprises: current collector; an active material layer, the active material layer being attached to at least one side of the current collector, the active material layer comprising an active material and a binding polymer; The adhesive polymer includes a portion obtained by cross-linking an adhesive component and a cross-linking agent component; The adhesive component includes polyvinylidene fluoride resin; The crosslinker component has an amine group.

2. The battery electrode according to claim 1, characterized in that: The weight average molecular weight of the polyvinylidene fluoride resin is 400000 g / mol to 1070000 g / mol.

3. The battery pole piece according to claim 2, characterized in that: The weight average molecular weight of the polyvinylidene fluoride resin is 520000 g / mol to 780000 g / mol.

4. The battery pole piece according to claim 1, characterized in that: The mass ratio of the cross-linking agent component to the adhesive component is 1:8 to 1:

12.

5. The battery pole piece according to claim 1, characterized in that: The crosslinker component comprises a substance having Formula I or Formula II; Wherein, the general formula I is The molecular formula of R is C a H b O c N d , where 2≤a≤100, 4≤b≤200, 0≤c≤100, 0≤d≤100; The general formula II is R'-HN2, where R' is an alkyl group.

6. The battery pole piece according to claim 5, characterized in that: The alkyl group is selected from ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, 1-pentyl, 2-pentyl, neopentyl, benzyl, phenyl, cyclopentyl, cyclohexyl, 1-hexyl, 2-hexyl, 3-hexyl, 1-octyl, 2-octyl, 2-ethylhexyl, 3-octyl, n-decyl, 1-dodecyl, and norbornyl.

7. The battery pole piece according to claim 1, characterized in that: The monomer of the polyvinylidene fluoride resin includes vinylidene fluoride, and the monomer of the polyvinylidene fluoride resin also includes: At least one of perfluoropropylene, chlorotrifluoroethylene, trifluoroethylene and tetrafluoroethylene; and / or a non-fluorine-containing monomer.

8. The battery pole piece according to claim 7, characterized in that: The vinylidene fluoride accounts for 75% to 99% of the main chain of the polyvinylidene fluoride resin.

9. The battery pole piece according to claim 8, characterized in that: The vinylidene fluoride accounts for 90% to 95% of the main chain of the polyvinylidene fluoride resin.

10. The battery pole piece according to claim 1, characterized in that: The adhesive polymer comprises a substance having the general formula III, Wherein, the general formula III is wherein R is an alkyl group, and m and n are positive integers.

11. A method for preparing a battery electrode according to any one of claims 1 to 10, characterized in that: include: mixing the active material, the binder component and the crosslinker component to form an electrode slurry; The electrode slurry is applied to at least one side surface of the current collector and subjected to a heat treatment so as to form the active material layer on at least one side surface of the current collector to obtain the battery electrode sheet.

12. The method according to claim 11, characterized in that The heating temperature is greater than or equal to 100°C.

13. The method according to claim 12, characterized in that The heating temperature is greater than or equal to 130°C.

14. The method according to claim 11, characterized in that The viscosity of the electrode slurry is 800 mPa·s to 3000 mPa·s.

15. A battery, characterized in that: The battery comprises a battery pole sheet according to any one of claims 1 to 10 or a battery pole sheet prepared by the method for preparing a battery pole sheet according to any one of claims 11 to 14.

16. An electrical device, characterized in that: The electric device comprises the battery according to claim 15.

Citation Information

Patent Citations

  • Conductive carbon slurry, positive electrode slurry, and preparation method and application of conductive carbon slurry and positive electrode slurry

    CN114914402A

  • Nonaqueous electrolyte secondary battery

    JP1995296815A

  • Binder for battery binder solution, electrode mixture, electrode structure and battery

    JP1998298386A

  • Nonaqueous secondary battery and its manufacturing method

    JP2010287470A