Preparation method of nanoscale metal filtering material based on 3D printing

By combining 3D printing technology with binders and interfacial catalysts and controlling the sintering temperature, nanoscale metal filter materials can be prepared, solving the problem that traditional methods are difficult to use to prepare nanoscale filter materials. This achieves efficient control of nanoscale pore size and uniform interconnected structure.

CN118951017APending Publication Date: 2024-11-15LUOYANG INST OF SCI & TECH +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411022572.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing technologies make it difficult to prepare nanoscale filter materials, and traditional methods are prone to causing environmental pollution.

Method used

By using 3D printing technology combined with binders and interfacial catalysts, and controlling the sintering temperature through local melting and sintering, nanoscale metal filter materials are prepared. The binders and interfacial catalysts are used to purify the oxide film on the surface of metal particles, achieving ultra-clean sintering of metal particles.

Benefits of technology

Precise control of nanoscale pores was achieved, forming a uniform and interconnected pore structure, which improved the anti-clogging performance of the filter material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004967720700000021
    Figure BDA0004967720700000021
  • Figure FDA0004967720690000011
    Figure FDA0004967720690000011
  • Figure HDA0004967720710000011
    Figure HDA0004967720710000011
Patent Text Reader

Abstract

A preparation method of a nanoscale metal filter material based on 3D printing relates to the field of filter material preparation, and comprises the following steps: S1, mixing a premix with metal balls with uniform particle size to obtain a metal blank; s2, the metal blank is placed in a 3D printer to be printed into a filter material green body in a preset shape; s3, degreasing the filter material green body in a vacuum environment to obtain a filter material intermediate, and locally melting and sintering the filter material intermediate to obtain the filter material. Nano-scale regulation and control of sintering sieve pores are realized by controlling the sintering temperature, filtering stacking layers with different pore diameters are formed by controlling the sintering size, space pipelines of the stacking layers are three-dimensional channels, and in terms of the topology principle, the anti-blocking performance of the channels is superior to that of traditional two-dimensional channels.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of filter material preparation, and in particular to a method for preparing a nano-scale metal filter material based on 3D printing. Background Art

[0002] Filter materials are materials specially used for filtering, separation, purification, etc. There are many types of them, and they can be divided into many types according to different classification standards. According to the material classification, filter materials can be divided into metal filter materials, ceramic filter materials, cellulose filter materials, synthetic filter materials, etc. Among them, metal filter materials such as stainless steel filters and copper mesh filters have the characteristics of high strength, high temperature resistance, corrosion resistance, etc., and are widely used.

[0003] Some methods for preparing metal filter materials are also disclosed in the prior art: for example, Chinese invention patent with application number CN201610461318.9 discloses a porous metal high-efficiency filter material and a preparation method thereof. The porous metal high-efficiency filter material has uniform pore size distribution, large porosity, good air permeability, and good pressure resistance. It is a porous filter material with excellent performance. However, the method for preparing the porous metal high-efficiency filter material of the invention uses a large number of chemical raw materials, which is easy to cause pollution to the environment, and the pore size of the prepared filter material is generally at the micron level, and nano-level filter materials cannot be obtained. Summary of the invention

[0004] The present invention aims to provide a method for preparing a nano-scale metal filter material based on 3D printing, so as to prepare a filter material with a nano-scale sieve aperture.

[0005] In order to solve the above technical problems, the specific solution adopted by the present invention is: a method for preparing a nanoscale metal filter material based on 3D printing, comprising the following steps:

[0006] S1: Mix the premix and metal balls of uniform particle size to obtain metal blanks

[0007] S2: placing the metal blank in a 3D printer to print out a filter material blank of a preset shape;

[0008] S3: Degreasing the filter material embryo under vacuum to obtain a filter material intermediate, and then partially melting and sintering the filter material intermediate to obtain the filter material.

[0009] As a further optimization of the above technical solution, in the process of partially melting and sintering the filter material intermediate in step S3, the method for determining the sintering temperature includes:

[0010] Determine the target value of the mesh aperture of the filter material;

[0011] Calculate the sintering temperature influencing factor based on the target value of the sieve aperture;

[0012] The sintering temperature is calculated by combining the sintering temperature influencing factors with the material of the metal ball.

[0013] As a further optimization of the above technical solution, the method for calculating the sintering temperature influencing factor based on the target value of the sieve aperture is:

[0014]

[0015] Among them, x is the sintering temperature influence factor, r is the target value of the sieve aperture, b is the correction coefficient, and R is the radius of the metal ball.

[0016] As a further optimization of the above technical solution, the method for calculating the sintering temperature based on the sintering temperature influencing factor is: when the material of the metal ball is 316L, b = 1.26, T = 0.0004935*x 3 -0.1051*x 2 +9.792*x+986, T is the sintering temperature.

[0017] As a further optimization of the above technical solution, the method for calculating the sintering temperature based on the sintering temperature influence factor is: when the material of the metal ball is TC4, b = 1.4, T = 0.0005629*x 3 -0.1219*x 2 +10.22*x+984.6, T is the sintering temperature.

[0018] As a further optimization of the above technical solution, the degreasing conditions are vacuum pressure 0.1-5 Pa and temperature 200-500°C.

[0019] As a further optimization of the above technical solution, the premix includes 96% polyethylene, 0.5-1.2% polyvinyl chloride and the balance polytetrafluoroethylene according to mass fraction.

[0020] As a further optimization of the above technical solution, the volume ratio of the premix to the metal balls is: 38-40%: 60-62%.

[0021] As a further optimization of the above technical solution, the premix includes a binder and an interfacial catalyst, the binder is polyethylene, and the interfacial catalyst is a mixture of polyvinyl chloride and polytetrafluoroethylene.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The present invention controls the sintering temperature to precisely control the surface energy and the sintering contact melting area, thereby achieving nano-level regulation of the sintering sieve holes. The control of the sintering size forms a filtering stacking layer with different pore sizes. The spatial pipeline of the stacking layer is a three-dimensional channel. From a topological principle, the anti-clogging performance of this channel is better than that of a traditional two-dimensional channel.

[0024] The present invention selects nano-scale metal particles for 3D printing, and uses a binder and a surfactant to purify the metal surface. The oxide film layer on the surface of the metal particles decomposes and disappears due to the action of the interface catalyst, and the interface of the metal particles is purified. The metal particles are ultra-cleanly sintered and fused, which makes it easier for the metal ball surface to contact and be subjected to high temperature. The metal surface energy is uniformly increased, and the atoms on the metal surface will be uniformly diffused and rearranged, so that the prepared filter material has uniformly connected sieve holes. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is an electron microscope image of the filter material prepared in Example 1;

[0026] Figure 2 is the relationship curve between the sintering temperature of the metal ball and the sintering temperature influencing factor when the material of the metal ball is 316L, y is the sintering temperature, and x is the sintering temperature influencing factor;

[0027] Figure 3 is the relationship curve between the sintering temperature of the metal ball and the sintering temperature influencing factor when the material of the metal ball is TC4, y is the sintering temperature, and x is the sintering temperature influencing factor;

[0028] Figure 4 It is a schematic diagram of the structure of the filter material mesh;

[0029] Figure 5 It is a schematic diagram of the structure of a metal sphere before sintering;

[0030] Figure 6 This is a schematic diagram of the structure of a metal ball with a diameter of 20 μm before sintering;

[0031] Figure 7 Schematic diagram of the structure of a metal ball with a diameter of 20 μm after sintering. DETAILED DESCRIPTION

[0032] The technical solution of the present invention is further elaborated in detail below in conjunction with specific embodiments. The parts of the present invention that are not described and disclosed in detail in the following embodiments should be understood as the prior art known or should be known to those skilled in the art.

[0033] The present invention discloses a method for preparing a nano-scale metal filter material based on 3D printing, comprising the following steps:

[0034] S1: mixing the premix and metal balls of uniform particle size to obtain a metal blank;

[0035] Specifically, a binder, an interfacial catalyst and metal balls are mixed, and the obtained mixture is injection molded into a metal wire as a metal blank. The injection molding pressure is 70-80 MPa and the temperature is 140-180°C; the metal balls with uniform particle size refer to the metal balls having the same diameter;

[0036] The premix includes a binder and an interface catalyst, the binder is polyethylene, and the interface catalyst is a mixture of polyvinyl chloride and polytetrafluoroethylene. Specifically, according to the mass fraction, the premix includes 96% PE polyethylene particles, 0.5-1.2% polyvinyl chloride particles and the remainder polytetrafluoroethylene particles, and the volume ratio of the premix to the metal ball is: 38-40%: 60-62%;

[0037] S2: placing the metal blank in a 3D printer to print out a filter material blank of a preset shape;

[0038] S3: degreasing the filter material embryo under vacuum to obtain a filter material intermediate, and partially melting and sintering the filter material intermediate to obtain the filter material;

[0039] The degreasing treatment conditions are vacuum pressure 0.1-5 Pa and temperature 200-500°C;

[0040] Local melt sintering refers to a sintering process at a high temperature but not reaching the melting point of the metal. Before sintering, channels are formed between the stacked metal balls. When the surfaces of the metal balls are in contact and subjected to high temperature, the metal surface energy increases. At this time, the atoms on the metal surface diffuse and rearrange, resulting in the enhancement of the intermolecular force between the metal surfaces, thereby causing the surfaces of the metal balls to adhere together. Since only the surface layer of the metal ball melts during local melt sintering, the melted part of the volume is filled into the channel. When the flow of the melted part of the volume affects the shape of the internal channel, under the action of surface tension, the melted parts of adjacent metal balls adhere to each other, and the aperture of the middle channel is approximately spherical. The channels of many metal balls are connected, thus forming connected sieve holes.

[0041] Next, the process of using metal surface energy to melt and reduce the mesh size is further described. Figure 5 , 6 As shown in ,7, taking a metal ball with a diameter of 20μm as an example, when the ball is not melted, Figure 6As shown in the figure, the maximum ball diameter allowed to pass through the middle pore is 3.09 μm. When the ball is exposed to high temperature, it will partially melt due to the effect of surface energy and then shrink, resulting in a decrease in internal pores, such as Figure 7 As shown, when the melted part does not affect the inscribed circle when the three balls meet, the maximum ball diameter allowed to pass through the intermediate pores is 1.09 μm.

[0042] When performing local melting and sintering treatment, the target value of the sieve aperture of the filter material is first determined, and then the sintering temperature influencing factor is calculated based on the target value of the sieve aperture. The sintering temperature influencing factor is combined with the material of the metal ball to calculate the sintering temperature.

[0043] When the metal balls of the present invention are stacked, four adjacent metal balls are stacked in a regular tetrahedron. During the calculation process, it is necessary to calculate the maximum ball diameter that can pass through the gap between the metal balls (that is, the ball diameter that can be accommodated in the middle gap when three balls are stacked in a plane). In the prepared nano-level filter material, the small ball passes through the stacking gap. Only when the small ball is smaller than or equal to the minimum cross-section of the stacking gap, can the small ball pass through the sieve hole. The ball diameter that can be accommodated in the middle gap when three balls are stacked in a plane is the minimum cross-section.

[0044] like Figure 4 , 5 As shown, the metal balls that fit together can enclose a space, which can be defined as the inscribed space. When the surface of the metal ball melts, the molten part can flow into the inscribed space under the action of surface tension, thereby shrinking the inscribed space. After the melted material cools, the reduced inscribed space can form the required sieve hole. The sintering temperature influence factor is calculated based on the target value of the sieve hole diameter, and then the sintering temperature influence factor is combined with the material of the metal ball to calculate the sintering temperature.

[0045] The calculation method of sintering temperature influence factor is:

[0046] Where r is the sieve radius, R is the metal ball radius, x is the sintering temperature influence factor, and b is the correction coefficient. The correction coefficient ranges from 1.2 to 1.5, and the correction coefficient is related to the material of the metal ball.

[0047] The method for calculating the sintering temperature based on the sintering temperature influencing factor is:

[0048] When the material of the metal ball is 316L, the correction coefficient b = 1.26, T = 0.0004935*x 3 -0.1051*x 2 +9.792*x+986, T is the sintering temperature.

[0049] When the material of the metal ball is TC4, the correction coefficient b = 1.4, T = 0.0005629*x3 -0.1219*x 2 +10.22*x+984.6, T is the sintering temperature.

[0050] Next, taking metal balls made of 316L and TC4 as examples, filter materials are prepared using the preparation method provided by the present invention:

[0051] 1. A filter material with a target mesh size of 1 nm was prepared using metal balls made of 316L material. The particle size of the metal balls was 8.5 nm, and the sintering temperature during the local melting sintering treatment was 1017°C.

[0052] The specific preparation method of the filter material is as follows:

[0053] S1: Mixing a premix with metal balls, wherein the material of the metal balls is 316L and the particle size is 8.5 nm, and then injection molding the obtained mixture into metal wires under the conditions of a pressure of 70 MPa and a temperature of 180° C.; wherein the premix includes 96% PE polyethylene particles, 1.2% polyvinyl chloride particles and 2.8% polytetrafluoroethylene particles, and the volume ratio of the premix to the metal balls is 2:3;

[0054] S2: placing the metal wire in a 3D printer to print out a filter material embryo of a preset shape;

[0055] S3: The filter material embryo is subjected to degreasing treatment and partial melting and sintering treatment in a vacuum environment in sequence. The degreasing treatment conditions are a vacuum pressure of 5Pa and a temperature of 300°C. The sintering temperature during the partial melting and sintering treatment is 1017°C. After the partial melting and sintering treatment, the filter material is obtained.

[0056] After testing, the pore size of the prepared filter material was found to be 1 nm, which was consistent with the target pore size.

[0057] 2. A filter material with a target mesh aperture of 2 nm was prepared using metal balls made of TC4 material. The particle size of the metal balls was 18.5 nm, and the sintering temperature during the local melting sintering treatment was 998°C.

[0058] The specific preparation method of the filter material is as follows:

[0059] S1: mixing a premix with metal balls, wherein the material of the metal balls is TC4 and the particle size is 18.5 nm, and then injection molding the obtained mixture into metal wires under the conditions of a pressure of 70 MPa and a temperature of 180° C.; wherein the premix includes 96% PE polyethylene particles, 1.2% polyvinyl chloride particles and 2.8% polytetrafluoroethylene particles, and the volume ratio of the premix to the metal balls is 2:3;

[0060] S2: placing the metal wire in a 3D printer to print out a filter material embryo of a preset shape;

[0061] S3: The filter material embryo is subjected to degreasing treatment and partial melting and sintering treatment in a vacuum environment in sequence. The degreasing treatment conditions are a vacuum pressure of 5Pa and a temperature of 300°C. The sintering temperature during the partial melting and sintering treatment is 998°C. After the partial melting and sintering treatment, the filter material is obtained.

[0062] After testing, the pore size of the prepared filter material was found to be 2 nm, which was consistent with the target pore size.

[0063] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a nanoscale metal filter material based on 3D printing, characterized in that: The following steps are involved: S1: mixing the premix and metal balls of uniform particle size to obtain a metal blank; S2: placing the metal blank in a 3D printer to print out a filter material blank of a preset shape; S3: Degreasing the filter material embryo under vacuum to obtain a filter material intermediate, and then partially melting and sintering the filter material intermediate to obtain the filter material.

2. The method for preparing a nanoscale metal filter material based on 3D printing according to claim 1, characterized in that: In the process of partially melting and sintering the filter material intermediate in step S3, the method for determining the sintering temperature includes: Determine the target value of the mesh aperture of the filter material; Calculate the sintering temperature influencing factor based on the target value of the sieve aperture; The sintering temperature is calculated by combining the sintering temperature influencing factors with the material of the metal ball.

3. The method for preparing a nanoscale metal filter material based on 3D printing according to claim 2, characterized in that: The method for calculating the sintering temperature influencing factor based on the target value of the sieve aperture is: Among them, x is the sintering temperature influence factor, r is the target value of the sieve aperture, R is the radius of the metal ball, b is the correction coefficient, and 1.2 <b<1.5。 4. The method for preparing a nanoscale metal filter material based on 3D printing according to claim 3, characterized in that: The method for calculating the sintering temperature based on the sintering temperature influencing factor is: when the material of the metal ball is 316L, b = 1.26, T = 0.0004935*x 3 -0.1051*x 2 +9.792*x+986, T is the sintering temperature.

5. The method for preparing a nanoscale metal filter material based on 3D printing according to claim 3, characterized in that: The method for calculating the sintering temperature based on the sintering temperature influence factor is: when the material of the metal ball is TC4, b = 1.4, T = 0.0005629*x 3 -0.1219*x 2 +10.22*x+984.6, T is the sintering temperature.

6. The method for preparing a nanoscale metal filter material based on 3D printing according to claim 1, characterized in that: The degreasing conditions are vacuum pressure 0.1~5Pa and temperature 200~500℃.

7. The method for preparing a nanoscale metal filter material based on 3D printing according to claim 1, characterized in that: According to the mass fraction, the premix includes 96% polyethylene, 0.5-1.2% polyvinyl chloride and the balance polytetrafluoroethylene.

8. The method for preparing a nano-scale metal filter material based on 3D printing according to claim 7, characterized in that: The volume ratio of the premix to the metal balls is: 38-40%: 60-62%.

9. The method for preparing a nanoscale metal filter material based on 3D printing according to claim 7, characterized in that: The premix comprises a binder and an interface catalyst, wherein the binder is polyethylene and the interface catalyst is a mixture of polyvinyl chloride and polytetrafluoroethylene.

Citation Information

Patent Citations

  • Efficient porous metal filtering material and preparation method thereof

    CN105925867A