Method for preparing metallized pellets from high-silicon low-grade magnetite concentrate
By using stepped grinding, step beneficiation, and rotary kiln reduction roasting to prepare high-silicon, low-grade iron concentrate, the problem of the uneconomical utilization of high-silicon, low-grade iron ore resources has been solved. This has enabled the efficient preparation of metallized pellets with high compressive strength, thereby improving blast furnace capacity and resource utilization efficiency.
Patent Information
- Application Number
- CN202411195731.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-15
AI Technical Summary
High-silicon, low-grade iron ore resources cannot be economically utilized due to problems such as high beneficiation ratio, fine concentrate particle size, difficult grinding, and high SiO2 content, making them difficult to develop and utilize effectively.
High-silicon, low-grade iron concentrate was prepared by a stepped grinding and separation method. Green pellets were prepared by a drum dryer, pre-consolidated by an oxide pelletizing vertical furnace, and then combined with rotary kiln reduction roasting and magnetic separation to prepare acid metallized pellets with high compressive strength.
This enables the efficient utilization of high-silicon, low-grade magnetite concentrate, increases blast furnace capacity, reduces coke ratio, alleviates the shortage of acidic furnace materials, reduces grinding and beneficiation costs, increases mineral processing capacity, and achieves economical utilization of resources.
Smart Images

Figure FT_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy and mineral engineering, and specifically relates to a technology for efficiently utilizing high-silicon low-quality magnetite concentrate. Background Art
[0002] Iron ore resources are abundant in the earth, with iron accounting for about 4.75% of the mass of the earth's crust, and the world's proven iron ore reserves are 170 billion tons. Although the world's iron ore resources are very rich, their distribution is extremely uneven. The iron ore reserves of Australia, Brazil and Russia account for 60% of the world's total reserves. Although my country has relatively rich resources, with a basic reserve of 20 billion tons, ranking fourth in the world, its ore endowment is poor and the iron grade is low, only 34.5%, about 13 percentage points lower than the world average iron grade. Rich ores with an iron grade greater than 50% only account for 2.7%.
[0003] my country's iron ore resources generally present the following characteristics: First, the grade of iron ore resources is low, with an average grade of about 34.5%, which is much lower than that of Brazil, Russia, India and other countries, and also lower than the world average iron ore grade; second, there are more lean mines and fewer rich mines, and the reserves of lean ore resources account for 80% of the total reserves; third, there are more small and medium-sized mines and fewer large and extra-large mines; fourth, the ore types are complex, and there are many iron ores that are difficult to utilize.
[0004] High-silicon ore is a typical type of iron ore that is difficult to select and utilize. It is widely distributed in China. However, this type of resource has problems such as high selection ratio, fine concentrate particle size, difficulty in grinding and high SiO2 content when processed using conventional mineral processing methods. It cannot be used economically, which is also an important reason why this type of iron ore has not been effectively developed for a long time.
[0005] There are a lot of such iron ore resources in China. If such resources can be prepared into metallized pellets and supplied to blast furnaces in a stable manner, it will effectively activate the existing high-silicon, low-grade and difficult-to-select resources, increase blast furnace capacity, reduce coke ratio, and achieve low-cost utilization of the above resources. It can also make full use of SiO2 in the iron material and turn harm into benefit, alleviate the problem of shortage of acidic furnace charges in some domestic steel companies, greatly improve my country's self-sufficiency level of iron ore resources, and provide resource guarantee for the future development of my country's steel industry. Summary of the invention
[0006] The present invention provides a method for efficiently utilizing high-silicon low-quality magnetite concentrate to prepare metallized pellets, aiming to solve the problem that the current high-silicon low-quality iron ore resources cannot be economically utilized.
[0007] For this reason, the present invention adopts the following technical scheme: A method for efficiently using high-silicon low-quality magnetite concentrate to prepare metallized pellets comprises the following steps: (1) High-silicon refractory ore is graded and ground to produce high-silicon low-grade iron ore concentrate: High-silicon refractory magnetite is graded and ground. In the first stage, the iron ore is finely ground to -200 mesh, accounting for 60-70%. The tailings are magnetically separated by a weak magnetic separator. The coarse concentrate after tailings is then subjected to the second stage of grinding, finely ground to -200 mesh, accounting for 90-95%. The concentrate is then separated by a weak magnetic separator to obtain high-silicon low-grade iron ore. The iron grade of high-silicon difficult-to-select magnetite is 25-27%, and the SiO2 content is 47%-42%. The high-silicon low-grade iron concentrate obtained by step grinding and step selection has an iron grade of 48-54% and a SiO2 content of 25-15%.
[0008] (2) Preparation of green balls: Use a drum dryer to dry the high-silicon low-grade iron ore concentrate to a water content of less than 6%, mix the iron ore concentrate and bentonite in a mass ratio of 100: (2-3.5), and use a ball-making disk to add water to prepare green balls to obtain 8-16 mm wet balls with a water content of 10-12%.
[0009] (3) Preparation of pre-consolidated pellets: The wet pellets are evenly distributed to the drying bed of the oxidized pellet vertical furnace through a distribution belt, and roasting is started. The grate temperature is controlled at 450-500°C and the combustion chamber temperature is controlled at 1060±10°C to produce pre-consolidated pellets with a compressive strength of >500N / ball.
[0010] (4) Reduction of pre-consolidated pellets: The pre-consolidated pellets are mixed with the residual carbon and added to the rotary kiln from the feed end, and high-volatile granular coal is sprayed from the discharge end for reduction roasting. The feed end temperature is controlled at 650-800°C, the high temperature section temperature is 1050-1150°C, and the discharge temperature is 950-1100°C. Acidic metallized pellets with a metallization rate of more than 85% and a compressive strength of more than 2500N / ball are produced.
[0011] (5) Cooling of high-temperature materials: The high-temperature materials of 1050-1150℃ discharged from the discharge end of the rotary kiln are cooled in an oxygen-free cooling device and discharged after being cooled to room temperature.
[0012] (6) Cooling of magnetic and non-magnetic materials: The discharged room temperature materials are separated into magnetic and non-magnetic materials by a dry magnetic separator to obtain acid metallized pellets and residual carbon; the residual carbon is returned to the feed section for utilization, and the metallized pellets are supplied to the blast furnace.
[0013] The beneficial effects of the present invention are: 1. High-efficiency utilization technology of high-silicon low-quality magnetite concentrate can solve the problem of rotary kiln ring formation After the high silicon iron ore concentrate is pelletized, it is pre-consolidated in an oxidation pelletizing vertical furnace. By optimizing the grate temperature of the oxidation pelletizing vertical furnace at 450-550℃ and the combustion chamber temperature at 1060±10℃, pre-consolidated pellets with a compressive strength of >500N / ball are produced. The pre-consolidated pellets do not produce powder during the reduction process in the rotary kiln, which can effectively solve the problem of rotary kiln ringing due to powder entering the kiln.
[0014] 2. High-silicon low-quality magnetite concentrate efficient utilization technology can achieve efficient utilization of high-silicon resources The acidic metallized pellets prepared by this technology have a compressive strength of more than 2500N / ball and can be used as high-quality acidic charge for blast furnaces. Such metallized pellets can be stably supplied to blast furnaces, increase blast furnace production capacity, reduce coke ratio, and make full use of SiO2 in iron materials, turning harm into benefit, thus alleviating the shortage of acidic materials for blast furnaces.
[0015] 3. High-silicon low-quality magnetite concentrate efficient utilization technology can effectively activate high-silicon difficult-to-dress ore resources This technology can reduce the iron grade of high-silicon low-quality magnetite concentrate to about 50%. Relatively coarse grinding particle size can be used in the beneficiation process of high-silicon difficult-to-select ore, and its selection ratio can be greatly reduced. Therefore, it can effectively reduce grinding costs, increase beneficiation capacity, and will be able to effectively activate existing high-silicon difficult-to-select resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a process flow chart of a high-silicon low-quality magnetite concentrate efficient utilization technology of the present invention; DETAILED DESCRIPTION
[0017] The present invention is further explained below in conjunction with specific implementation modes.
[0018] Example 1 A method for preparing metallized pellets from high-silicon low-quality magnetite concentrate comprises the following steps: (1) Preparation of high-silicon low-grade iron ore concentrate by step grinding and step selection of high-silicon refractory ore: A high-silicon refractory magnetite with an iron grade of 25-27% and a SiO2 content of 47%-42% is used. The iron ore is finely ground to -200 mesh, accounting for 60-70%, and then magnetically separated by a weak magnetic separator. The coarse concentrate after separation is then subjected to a second grinding stage and finely ground to -200 mesh, accounting for 90-95%. The concentrate is then separated by a weak magnetic separator to obtain a high-silicon low-grade iron ore with an iron grade of 48-54% and a SiO2 content of 25-15%.
[0019] (2) Preparation of green balls: Use a drum dryer to dry the high-silicon low-grade iron ore concentrate to a water content of less than 6%, mix the ingredients according to the mass ratio of iron ore concentrate: bentonite = 100:2, and use a ball-making disk to add water to prepare green balls to obtain 8-16 mm wet balls with a moisture content of 10-12%.
[0020] (3) Preparation of pre-consolidated pellets: The wet pellets are evenly distributed to the drying bed of the oxidation pellet vertical furnace through a distribution belt, and roasting begins. The grate temperature is controlled at 450-500°C and the combustion chamber temperature is controlled at 1060±10°C to produce pre-consolidated pellets with a compressive strength of 500-1800N / ball.
[0021] (4) Reduction of pre-consolidated pellets: The pre-consolidated pellets are mixed with the residual carbon and added to the rotary kiln from the feed end, and high-volatile granular coal is sprayed from the discharge end for reduction roasting. The feed end temperature is controlled at 650-700°C, the high temperature section temperature is 1050-1120°C, and the discharge temperature is 950-1050°C. Acidic metallized pellets with a metallization rate of more than 85% and a compressive strength of more than 2500N / ball are produced.
[0022] (5) Cooling of high-temperature materials: The high-temperature materials of 1050-1150℃ discharged from the discharge end of the rotary kiln are cooled in an oxygen-free cooling device and discharged after being cooled to room temperature.
[0023] (6) Cooling of magnetic and non-magnetic materials: The discharged room temperature materials are separated into magnetic and non-magnetic materials by a dry magnetic separator to obtain acid metallized pellets and residual carbon. The residual carbon is returned to the feed section for utilization, and the metallized pellets are supplied to the blast furnace.
[0024] (5) Flue gas treatment: The high-temperature flue gas discharged from the rotary kiln is recycled through a waste heat boiler to recover waste heat, and the heated steam is used for the steam turbine generator; the low-temperature flue gas from the waste heat boiler is dedusted by a bag filter before being discharged.
[0025] Example 2 A method for preparing metallized pellets from high-silicon low-quality magnetite concentrate comprises the following steps: (1) Preparation of high-silicon low-grade iron ore concentrate by step grinding and step selection of high-silicon refractory ore: A high-silicon refractory magnetite with an iron grade of 25-27% and a SiO2 content of 47%-42% is used. The iron ore is finely ground to -200 mesh, accounting for 60-70%, and then magnetically separated by a weak magnetic separator. The coarse concentrate after separation is then subjected to a second grinding stage and finely ground to -200 mesh, accounting for 90-95%. The concentrate is then separated by a weak magnetic separator to obtain a high-silicon low-grade iron ore with an iron grade of 48-54% and a SiO2 content of 25-15%.
[0026] (2) Preparation of green balls: Use a drum dryer to dry the high-silicon low-quality iron ore concentrate to a water content of less than 6%, mix the ingredients according to the mass ratio of iron ore concentrate: bentonite = 100:3.5, and use a ball-making disk to add water to prepare green balls to obtain 8-16 mm wet balls with a moisture content of 10-12%.
[0027] (3) Preparation of pre-consolidated pellets: The wet pellets are evenly distributed to the drying bed of the oxidation pellet vertical furnace through a distribution belt, and roasting begins. The grate temperature is controlled at 480-550°C and the combustion chamber temperature is controlled at 1060±10°C to produce pre-consolidated pellets with a compressive strength of 1000-1800N / ball.
[0028] (4) Reduction of pre-consolidated pellets: The pre-consolidated pellets are mixed with the residual carbon and added to the rotary kiln from the feed end, and high-volatile granular coal is sprayed from the discharge end for reduction roasting. The feed end temperature is controlled at 700-800°C, the high temperature section temperature is 1080-1150°C, and the discharge temperature is 1020-1100°C. Acidic metallized pellets with a metallization rate of more than 85% and a compressive strength of more than 2500N / ball are produced.
[0029] (5) Cooling of high-temperature materials: The high-temperature materials of 1050-1150℃ discharged from the discharge end of the rotary kiln are cooled in an oxygen-free cooling device and discharged after being cooled to room temperature.
[0030] (6) Cooling of magnetic and non-magnetic materials: The discharged room temperature materials are separated into magnetic and non-magnetic materials by a dry magnetic separator to obtain acid metallized pellets and residual carbon. The residual carbon is returned to the feed section for utilization, and the metallized pellets are supplied to the blast furnace.
[0031] (5) Flue gas treatment: The high-temperature flue gas discharged from the rotary kiln is recycled through a waste heat boiler to recover waste heat, and the heated steam is used for the steam turbine generator; the low-temperature flue gas from the waste heat boiler is dedusted by a bag filter before being discharged.
Claims
1. A method for preparing metallized pellets from high-silicon low-quality magnetite concentrate, characterized in that: The following steps are involved: (1) High-silicon refractory ore is graded and ground to produce high-silicon low-grade iron ore concentrate: High-silicon refractory magnetite is graded and ground. In the first stage, the iron ore is finely ground to -200 mesh, accounting for 60-70%. The tailings are magnetically separated by a weak magnetic separator. The coarse concentrate after tailings is then subjected to the second stage of grinding, finely ground to -200 mesh, accounting for 90-95%. The concentrate is then separated by a weak magnetic separator to obtain high-silicon low-grade iron ore. (2) Preparation of green balls: Use a drum dryer to dry the high-silicon low-quality iron ore concentrate to a water content of less than 6%, mix the iron ore concentrate and bentonite in a mass ratio of 100: (2-3.5), and use a ball-making disk to add water to prepare green balls to obtain 8-16 mm wet balls; (3) Preparation of pre-consolidated pellets: The wet pellets are evenly distributed to the drying bed of the oxidized pellet vertical furnace through a distribution belt, and roasting is started. The grate temperature is controlled at 450-500°C and the combustion chamber temperature is controlled at 1060±10°C to produce pre-consolidated pellets with a compressive strength of >500N / ball. (4) Reduction of pre-consolidated pellets: The pre-consolidated pellets are mixed with residual carbon and added to the rotary kiln from the feed end, and high-volatile granular coal is sprayed from the discharge end for reduction roasting. The feed end temperature is controlled at 650-800°C, the high temperature section temperature is 1050-1150°C, and the discharge temperature is 950-1100°C. Acidic metallized pellets with a metallization rate of more than 85% and a compressive strength of more than 2500N / ball are produced. (5) Cooling of high-temperature materials: The high-temperature materials of 1050-1150°C discharged from the discharge end of the rotary kiln are cooled in an oxygen-free cooling device and discharged after being cooled to room temperature; (6) Cooling of magnetic and non-magnetic materials: The discharged room temperature materials are separated into magnetic and non-magnetic materials by a dry magnetic separator to obtain acid metallized pellets and residual carbon; the residual carbon is returned to the feed section for utilization, and the metallized pellets are supplied to the blast furnace.
2. The method for preparing metallized pellets from high-silicon low-quality magnetite concentrate according to claim 1, characterized in that: The high-silicon refractory magnetite in step (1) has an iron grade of 25-27% and a SiO2 content of 47%-42%. The high-silicon low-grade iron concentrate obtained by step grinding and step selection has an iron grade of 48-54% and a SiO2 content of 25-15%.
3. The method for preparing metallized pellets from high-silicon low-quality magnetite concentrate according to claim 1, characterized in that: In the step (2), water is added to the pelletizing plate to prepare 8-16 mm wet pellets, wherein the moisture content of the wet pellets is 10-12%.