Mica composite part for CCS lithium battery cell current-conducting plate and preparation method of mica composite part

Through the design of mica composite parts, combined with surface modified mica and compound silicone resin, the problem of insufficient flame retardant performance of CCS lithium battery modules in high temperature environments is solved, and high safety and low dielectric loss are achieved. Effect, suitable for power battery packs of new energy vehicles.

CN118970382AActive Publication Date: 2024-11-15浙江荣泰电工器材股份有限公司
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411436796.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-15
Publication Date
2024-11-15
Estimated Expiration
2044-10-15

AI Technical Summary

Technical Problem

The epoxy resin binder and electronic grade glass cloth used in the existing CCS lithium battery signal acquisition components are insufficient in high temperature and high heat environments, and the epoxy resin will produce toxic combustion-stimulating gas, which cannot meet the new energy. Thermal runaway safety performance requirements of automotive power battery packs.

Method used

Using mica composite parts, CCS lithium battery electric power with improved thermal runaway safety performance, low dielectric loss, high reliability and high insulation thermal conductivity are prepared by combining surface-modified mica composition and composite silicone resin. The core conductive plate uses nano-scale modified particles and toughened fillers to improve material performance, and prepares the finished product through a four-step hot pressing method.

Benefits of technology

It effectively improves the thermal runaway safety performance of CCS lithium battery modules, reduces dielectric loss, improves reliability and insulation thermal conductivity, meets the high-quality development needs of new energy vehicles, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of CCS lithium battery assemblies, in particular to a mica composite part for a CCS lithium battery cell current-conducting plate and a preparation method of the mica composite part. The mica composite part for the CCS lithium battery cell current-conducting plate comprises a mica composite substrate, electronic-grade glass cloth compounded in the mica composite substrate and copper foil compounded on the surface of the mica composite substrate, the mica composite substrate is prepared from the following raw materials in parts by weight: 80-90 parts of a surface modified mica composition, 0.5-5 parts of a toughening filler and 20-32 parts of compound organic silicon resin, the toughening filler is formed by matching nano aramid fibers with at least one of nano carbon fibers, carbon nanotubes and inorganic whiskers. The signal acquisition assembly used for manufacturing the CCS lithium battery can effectively improve the thermal runaway safety performance of the CCS lithium battery module, has the advantages of low dielectric loss, high reliability and high insulation and heat conduction, and is beneficial to high-quality development of the new energy automobile industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of CCS lithium battery components, and in particular to a mica composite component for a CCS lithium battery cell conductive plate and a preparation method thereof. Background Art

[0002] The lithium battery module CCS is an electrical connection structure within the lithium battery module. It is installed in the lithium battery module by integrating information acquisition components, plastic structural parts, aluminum bars and other components into an electronic control module to achieve functions such as high-voltage series and parallel connection of battery cells, battery temperature sampling, battery cell voltage sampling and over-current fusing. It is part of the BMS battery management system.

[0003] At present, the mature design solutions for CCS signal acquisition components include wiring harnesses, PCBs, FPCs, and FFCs. The signal acquisition components industrially applied to new energy battery pack modules are mainly PCB boards. Compared with wiring harnesses, PCB boards as signal acquisition components have more advantages in product integration, lightweight, and regular structure. They are conducive to better utilization of the internal space of the battery, facilitate automated assembly, and are suitable for large-scale mass production.

[0004] As the core component for energy storage and output, the power battery pack of new energy vehicles determines the driving comfort, endurance stability and thermal runaway safety of new energy vehicles. The thermal runaway safety performance of the power battery pack determines the life and personal protection of car users when abnormal problems occur in the battery module, which is one of the hot issues that consumers are most concerned about. How to improve the thermal runaway safety performance of the power battery pack of new energy vehicles is a key R&D breakthrough project for every car company.

[0005] The PCB board traditionally used in the signal acquisition component of CCS lithium batteries is an electronic-grade glass cloth dipped in epoxy resin adhesive and baked to form a semi-cured sheet. Several semi-cured sheets are stacked on each other to form a substrate, and then one or both sides are covered with copper foil to obtain a semi-finished product. The semi-finished product is hot-pressed, cured, and cut to obtain a finished PCB board. Finally, an integrated circuit is formed based on the finished PCB board.

[0006] However, the flame retardant safety performance of the finished PCB board formed by the existing epoxy resin adhesive + electronic grade glass cloth is average, and the signal acquisition component of the CCS lithium battery is assembled at the upper end of the electrode of the lithium battery cell. When the lithium battery cell has an abnormal accident and explodes, the flame and high temperature of the finished PCB board produced by the explosion are the first to be affected. The flame retardant performance of the finished PCB board under high temperature and high heat is relatively average, and even the epoxy resin adhesive can no longer meet the thermal runaway safety performance requirements of the power battery pack of new energy vehicles because of the toxic and combustion-supporting gases produced at high temperature. For this reason, the inventor provides a mica composite component for the conductive plate of a CCS lithium battery cell and a preparation method thereof. Summary of the invention

[0007] In order to solve the problem that the flame retardancy of the above-mentioned prior art is relatively general, and even the epoxy resin adhesive can no longer meet the thermal runaway safety performance requirements of the power battery pack of new energy vehicles due to the generation of toxic and combustion-supporting gases at high temperatures, the inventors provide a mica composite component for the conductive plate of a CCS lithium battery cell and a preparation method thereof.

[0008] The present application provides a mica composite component for a CCS lithium battery cell conductive plate, which is realized by the following scheme: A mica composite component for a CCS lithium battery cell conductive plate comprises a mica composite substrate, at least one electronic-grade glass cloth composited inside the mica composite substrate, and a copper foil composited on the surface of the mica composite substrate. The mica composite substrate comprises the following raw materials in parts by weight: 80-90 parts of a surface-modified mica composition, 0.5-5 parts of a toughening filler, and 20-32 parts of a compounded silicone resin with a solid content of 40-55wt%; the surface-modified mica composition comprises a mica matrix and nanoscale modified particles loaded on the surface of the mica matrix, the nanoscale modified particles comprise at least one of aluminum oxide, silicon dioxide, titanium dioxide, aluminum nitride, silicon nitride, graphene, carbon nanotubes, and fullerenes; the toughening filler is composed of at least one of nano-aramid fibers, nano-carbon fibers, carbon nanotubes, and inorganic whiskers.

[0009] Preferably, the mica matrix is ​​1340 mesh sieve material, D 10 0.5-2μm, D 50 3-5.5μm, D 90 7.5-9.5μm.

[0010] The mica composite component for the conductive plate of the CCS lithium battery cell in this application is used to make the signal acquisition component of the CCS lithium battery, which can effectively improve the thermal runaway safety performance of the CCS lithium battery module, and has the advantages of low dielectric loss, high reliability, and high insulation and thermal conductivity, which is conducive to the high-quality development of the new energy vehicle industry.

[0011] Preferably, the nano-scale modified particles are aluminum oxide and carbon nanotubes, the aluminum oxide is loaded and fixed on the surface of the mica substrate by a sol-gel method; the carbon nanotubes are fixed on the surface of the mica substrate by sintering with nano-silver or nano-copper.

[0012] By adopting the above technical solution, the overall high insulation thermal conductivity of the mica composite parts can be improved while ensuring the thermal runaway safety performance, low dielectric loss and high reliability performance, and heat can be effectively released, which can better meet the use requirements of power battery packs.

[0013] Preferably, the toughening filler is composed of nano-aramid fiber and inorganic whisker in a mass ratio of (3-7):1; the inorganic whisker is composed of at least one of zinc oxide whisker, aluminum nitride whisker, aluminum oxide whisker, boron nitride whisker and silicon carbide whisker.

[0014] By adopting the above technical solution, the overall impact toughness can be effectively improved, which is not only beneficial to improving the overall processing performance and mechanical strength, but also can improve the overall high insulation and thermal conductivity, which can better meet the use requirements of power battery packs.

[0015] Preferably, the mica composite substrate is made of the following raw materials in parts by weight: 81.4-83.2 parts of a surface-modified mica composition, 2.8-3.6 parts of a toughening filler, and 28-30 parts of a compounded silicone resin with a solid content of 50wt%.

[0016] By optimizing the design of the mica composite substrate formula, the overall thermal runaway safety performance, low dielectric loss, high reliability, and high insulation thermal conductivity can be improved while reducing the overall production cost, and it is also convenient to improve the quality stability of the same batch of products.

[0017] Preferably, the preparation method of the surface modified mica composition is as follows: Step 1: loading and fixing nano-scale modified particles A on the surface of a mica substrate by a sol-gel method, wherein the nano-scale modified particles A are at least one of aluminum oxide, silicon dioxide, titanium dioxide, aluminum nitride, and silicon nitride; Step 2: Add polyvinyl pyrrolidone and nano-scale modified particles B to the prepared Ag(2E4MI)2Ac complex solution, wherein the nano-scale modified particles AB are at least one of graphene, carbon nanotubes, and fullerene, and add the mica matrix material with the surface loaded with nano-scale modified particles A in step 1 after ultrasonic dispersion for 1-4 hours, and then ultrasonic dispersion for 0.5-2 hours; Step 3, the dispersion obtained in step 2 is subjected to reduced pressure distillation to remove the organic solvent in the Ag(2E4MI)2Ac complex solution, and the obtained solid is subjected to high temperature sintering for 2-4 hours, and the high temperature sintering temperature is 200-220°C; Step 4, rolling and grinding the solid obtained in step 3, wet-milling the obtained powder at a ball mill speed of 60-80 rpm for 15-40 min, and then filtering, drying and sieving to obtain a semi-finished surface-modified mica composition; Step 5, placing the semi-finished surface-modified mica composition obtained in step 4 in an aminosilane aqueous solution for ultrasonic dispersion treatment for 30-90 minutes, wherein the concentration of aminosilane in the aminosilane aqueous solution is 0.5-6wt%, and the aminosilane includes at least one of KH550, KH540, KH554, and KH590, filtering and drying to obtain a finished surface-modified mica composition.

[0018] By adopting the above technical scheme, a finished surface-modified mica composition having good compatibility and bonding with the compounded silicone resin can be obtained, thereby improving the overall thermal runaway safety performance, low dielectric loss, high reliability, and high insulation thermal conductivity.

[0019] Preferably, the compound silicone resin with a solid content of 40-55wt% is made of the following raw materials in parts by weight: 200 parts of KR-242A silicone resin, 50-100 parts of KR-271 silicone resin, 20-40 parts of a toughening composition with a molecular weight ≥1000, 20-60 parts of xylene, 20-60 parts of isopropanol, 0.20-0.30 parts of diethylenetriamine, and 0.10-0.20 parts of 1H-benzimidazole-1,5,6-triamine; the toughening composition is at least one of end-side chain epoxy silicone oil chain extender IOTA105-3, double-terminal alcohol hydroxyl silicone oil IOTA 2110, double-terminal alcohol hydroxyl long-chain alkyl silicone oil IOTA-8865H, hydroxyl-terminated methyl vinyl silicone oil IOTA 1203V, carbon hydroxyl silicone oil IOTA 2122, and carbon hydroxyl silicone oil IOTA 2140.

[0020] Preferably, the preparation method of the compound silicone resin with a solid content of 40-55wt% is as follows: 0.05-0.10 parts of diethylenetriamine, 200 parts of KR-242A silicone resin, 50-100 parts of KR-271 silicone resin, and 20-40 parts of a toughening composition with a molecular weight ≥1000 are pre-reacted at 68-70°C for 100-200s, cooled to 0-4°C in an ice water bath, 40-60 parts of xylene and 20-60 parts of isopropanol are added, and stirred at 80-160rpm for 10-30min, the remaining diethylenetriamine and 0.10-0.20 parts of 1H-benzimidazole-1,5,6-triamine are added, and stirred at 60-80rpm for 100-200s to obtain the silicone resin, which is stored at low temperature for standby use.

[0021] By adopting the above technical solution, the overall flame retardant fire safety, high temperature resistance and impact toughness can be given good.

[0022] The present application provides a method for preparing a mica composite component for a CCS lithium battery cell conductive plate, which is achieved through the following technical solutions: A method for preparing a mica composite component for a CCS lithium battery core conductive plate comprises the following steps: Step 1, preparing a surface-modified mica composition and a compounded silicone resin with a solid content of 40-55wt% respectively; Step 2: Evenly mix the accurately measured surface-modified mica composition in step 1, the toughening filler, and the compounded silicone resin with a solid content of 40-55wt% in step 1 to obtain a mica composite substrate slurry; pour the obtained mica composite substrate slurry into a molding mold; heat to remove the organic solvent and then adopt a four-step hot pressing method to obtain a semi-finished mica composite substrate; the obtained semi-finished mica composite substrate is heated to 50-55°C at a heating rate of 1-2°C / min and kept warm for 200-300s; then heated to 80-88°C at a heating rate of 1-2°C / min and kept warm for 60-120min; and naturally cooled to obtain a finished mica composite substrate; At the same time, the surface of the copper foil is subjected to low temperature plasma treatment, and ammonia treatment is used for 5-30 minutes at 0-4°C. The surface of the copper foil after the low temperature plasma treatment is coated with 0.5-1 g / dm of the compound silicone resin with a solid content of 40-55 wt% in step 1. 2 After the organic solvent is removed by heating, an organic silica gel film is formed on the surface of the copper foil after low-temperature plasma treatment; Step three, stacking an electronic grade glass cloth between adjacent finished mica composite substrates to preheat and press to form a mica substrate, and pressing the copper foil in step two on the surface of the mica substrate, so that the organic silicone film on the surface of the copper foil is in contact with the surface of the mica substrate, and finally hot pressing and curing are performed. The mica composite component for the conductive plate of the CCS lithium battery cell can be obtained by hot pressing at a pressure of 2-4MPa and a temperature of 160-240°C for 2-4min, and naturally cooling to room temperature.

[0023] Preferably, the four-step hot pressing molding method in step 2 is as follows: the hot pressing conditions in the first step of hot pressing molding are a platen temperature of 80±2°C, a pressure of 0.25±0.05Mpa, and a duration of 60-80s; the hot pressing conditions in the second step of hot pressing molding are a platen temperature of 130-135°C, a pressure of 0.5-0.6Mpa, and a duration of 100-120s; the hot pressing conditions in the third step of hot pressing molding are a platen temperature of 175-180°C, a pressure of 0.8-1.0Mpa, and a duration of 120-160s; the hot pressing conditions in the fourth step of hot pressing molding are a platen temperature of 115-120°C, a pressure of 0.4-0.6Mpa, and a duration of 60-80s to obtain a semi-finished mica composite substrate.

[0024] The preparation method provided in this application is relatively simple, has low implementation difficulty, and is easy to implement for industrial mass production.

[0025] In summary, this application has the following advantages: 1. This application is used to manufacture signal acquisition components for CCS lithium batteries, which can effectively improve the thermal runaway safety performance of CCS lithium battery modules, and has the advantages of low dielectric loss, high reliability, and high insulation and thermal conductivity, which is conducive to the high-quality development of the new energy vehicle industry.

[0026] 2. This application optimizes the design of the mica composite substrate formula, and the glue content is preferably controlled to 14-15w%, which can not only improve the overall thermal runaway safety performance, low dielectric loss, high reliability, and high insulation thermal conductivity, but also reduce the overall production cost, and is also convenient for improving the quality stability of the same batch of products.

[0027] 3. The finished surface-modified mica composition obtained by surface modification of the mica composition in the present application has good compatibility and bonding with the compounded silicone resin. The mica composite parts for CCS lithium battery cell conductive plates prepared by using the mica composite parts have good thermal runaway safety performance, low dielectric loss, high reliability, and high insulation and thermal conductivity.

[0028] 4. The preparation method provided in this application is relatively simple, has low implementation difficulty, and is easy to implement for industrial mass production. DETAILED DESCRIPTION

[0029] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples and comparative examples.

[0030] Preparation Example 1: The preparation method of the surface modified mica composition is as follows: Step 1: load and fix rutile nano-TiO2 on the surface of mica matrix by sol-gel method. The specific preparation method is as follows: 5g of 1340-mesh sifted phlogopite powder (325-mesh phlogopite is crushed by ball milling and sieved with 1340-mesh sieve, and the sieved material is the 1340-mesh sifted phlogopite powder), 14.5g of titanyl sulfate and 49.1g of deionized water are mixed and stirred for about 4h until clear and transparent, then 1.7g of polyvinyl pyrrolidone (average molecular weight is 54,000) is added and stirred for 5h until clear and transparent, and then 1 7.3g of propylene glycol and 17.3g of dimethylformamide were stirred for 10min, and then aged for 24h to obtain titanium dioxide / phlogopite binary colloid. The binary colloid was washed three times with distilled water, and the solid powder was filtered and dried in a vacuum drying oven at 125°C for 12h, and then calcined in a transposed atmosphere tube furnace. The temperature was raised to 980°C at 20°C / min in an air atmosphere and calcined for 3h. After ball milling at 60rpm for 30min, 1340 mesh sieve was used to obtain rutile nano-TiO2 / phlogopite. 10 1.38μm, D 50 3.87μm, D90 8.31μm; Meanwhile, prepare Ag(2E4MI)2Ac complex solution: add 0.02 mol of 2-ethyl-4-methylimidazole 2E4MI and 0.01 mol of silver acetate AgAc into 400 mL of dichloromethane at room temperature, stir magnetically at a speed of 240 r / min until the AgAc particles completely disappear, to obtain Ag(2E4MI)2Ac complex solution; Step 2: Add 0.3g polyvinyl pyrrolidone and 0.2g carbon nanotubes (CNTs, TNGM2, Chengdu Institute of Organic Chemistry, Chinese Academy of Sciences) to the prepared Ag(2E4MI)2Ac complex solution, and then add 5g of rutile nano-TiO2 / phlogopite prepared in step 1 at an ultrasonic frequency of 40kHz / 800W for 2h, and then ultrasonically disperse at an ultrasonic frequency of 40kHz / 800W for 1h to obtain a finished dispersion; Step 3, removing dichloromethane from the finished dispersion obtained in step 2 by vacuum distillation, and then transferring the obtained solid to a muffle furnace and heating it to 210° C. for high-temperature sintering for 3 hours to obtain a solid; Step 4: Place the solid obtained in step 3 in a three-roll mill (the roller spacing of the three-roll mill is 10 μm) for three times of grinding and crushing, and transfer the obtained powder to a planetary ball mill for wet ball milling (ethanol to powder solid-liquid ratio of 1:3) at a ball mill speed of 60-80 rpm for 30 minutes, and then filter and dry, and sieve with 1340 mesh to obtain a semi-finished surface-modified mica composition; Step 5: Place 5 g of the semi-finished surface-modified mica composition obtained in step 4 in 200 mL of KH540 aqueous solution (KH540 concentration 2 wt%) at an ultrasonic frequency of 40 kHz / 800 W for 60 min, filter, and dry to obtain a finished surface-modified mica composition.

[0031] The difference between Preparation Example 2 and Preparation Example 1 is that: Step 1, ZnO is loaded and fixed on the surface of the mica substrate by a sol-gel method. The specific preparation method is as follows: 12.6 g of zinc acetate is dissolved in 1 L of distilled water and magnetically stirred for 0.5 h, and then 40 g of 1340 mesh sifted phlogopite powder and 0.25 g of polyethylene glycol PEG-400 are added, and magnetic stirring is continued for 0.5 h, and then 3 wt% concentration of ammonia water is added until Zn is completely precipitated and magnetic stirring is continued for 1 h, and the mixture is allowed to stand for 5 minutes. The ZnOH / phlogopite binary colloid was treated for 24 hours, and the obtained binary colloid was washed three times with distilled water and filtered to obtain a solid powder, which was transferred to a vacuum drying oven and dried at 125°C for 12 hours and then transferred to an atmosphere tube furnace for calcination. The temperature was increased to 720°C at 20°C / min in an air atmosphere and calcined for 3 hours to obtain ZnO / phlogopite powder, which was wet-milled at 60rpm for 30 minutes and then sieved through a 1340-mesh sieve to obtain nano ZnO / phlogopite. 10 1.24μm, D 50 3.76μm, D 90 It is 8.09μm.

[0032] The difference between Preparation Example 3 and Preparation Example 1 is that: Step 1, Al2O3 is loaded and fixed on the surface of the mica substrate by a sol-gel method. The specific preparation method is as follows: 18g of aluminum nitrate nonahydrate is dissolved in 1L of distilled water and magnetically stirred for 0.5h, then 40g of 1340-mesh sifted phlogopite powder is added, and magnetic stirring is continued for 0.5h, and then a 3wt% concentration of sodium hydroxide aqueous solution is added until Al is completely precipitated, and magnetic stirring is continued for 1h, and the product is obtained by standing and aging for 24h. Al(OH)3 / phlogopite binary colloid was washed three times with distilled water and then filtered to obtain solid powder, which was transferred to a vacuum drying oven and dried at 125°C for 12 hours and then transferred to an atmosphere tube furnace for calcination. The temperature was raised to 600°C at 20°C / min in an air atmosphere and calcined for 4 hours to obtain Al2O3 / phlogopite powder. The powder was wet-milled at 60rpm for 30 minutes and then sieved through a 1340 mesh sieve to obtain nano-Al2O3 / phlogopite. D 10 1.43 μm, D 50 3.94μm, D 90 It is 8.39μm.

[0033] Preparation Example 4 is different from Preparation Example 1 in that: Step 1, AlN is loaded and fixed on the surface of the mica substrate by a sol-gel method. The specific preparation method is as follows: 0.1 mol of aluminum nitrate nonahydrate and 0.3 mol of glucose are dissolved in 1 L of distilled water and magnetically stirred for 0.5 h, and then 40 g of 1340 mesh sifted phlogopite powder and 0.25 g of polyethylene glycol PEG-400 are added, and then 5 g of urea is added to a 75°C constant temperature water bath, and a 3 wt% concentration of ammonia solution is added dropwise while stirring to obtain an alumina sol, and then the temperature is increased to evaporate most of the water to obtain a gel, which is freeze-dried to form AlN The precursor / phlogopite powder is placed in a closed vacuum carbon tube furnace, and the temperature is increased while vacuuming, so that the organic matter in the precursor is gradually dehydrated and carbonized in the absence of oxygen, and forms a uniformly mixed and loose porous substance with the aluminum oxide generated by the decomposition of aluminum hydroxide. By controlling the nitrogen flow rate and continuously increasing the temperature, it is finally nitrided at 1550°C for 3h to obtain carbon-containing AlN, and placed in a decarburization furnace for 800°C / 2h in a reducing atmosphere of H2 to obtain nano-AlN / phlogopite. After wet ball milling at 60rpm for 30min, it is sieved with a 1340 mesh screen to obtain nano-grade AlN / phlogopite. D 10 1.47μm, D 50 3.82μm, D 90 It is 7.95μm.

[0034] The difference between Preparation Example 5 and Preparation Example 1 is that the preparation method of the surface-modified mica composition is as follows: Step 1: load and fix rutile nano-TiO2 on the surface of mica matrix by sol-gel method. The specific preparation method is as follows: 5g of 325 mesh phlogopite powder, 14.5g of titanyl sulfate and 49.1g of deionized water are mixed and stirred for about 4h until clear and transparent, then 1.7g of polyvinyl pyrrolidone with an average molecular weight of 54,000 is added and stirred for 5h until clear and transparent, then 17.3g of glycerol and 17.3g of dimethylformamide are added and stirred for 10min, and then the mixture is stirred for 10min. After aging for 24 hours, titanium dioxide / phlogopite binary colloid can be obtained, and then the prepared binary colloid is washed three times with distilled water, and the solid powder is filtered and placed in a vacuum drying oven at 125°C for 12 hours, and then calcined in a transposed atmosphere tube furnace, and heated to 980°C at 20°C / min in an air atmosphere for calcination for 3 hours. The obtained solid is placed in a three-roll mill (the roller spacing of the three-roll mill is 45μm) and ground and crushed three times to obtain rutile nano-TiO2 / phlogopite; Meanwhile, prepare Ag(2E4MI)2Ac complex solution: add 0.02 mol of 2-ethyl-4-methylimidazole 2E4MI and 0.01 mol of silver acetate AgAc into 400 mL of dichloromethane at room temperature, stir magnetically at a speed of 240 r / min until the AgAc particles completely disappear, to obtain Ag(2E4MI)2Ac complex solution; Step 2: Add 0.3 g of polyvinyl pyrrolidone and 0.2 g of carbon nanotubes CNTs, TNGM2 to the prepared Ag(2E4MI)2Ac complex solution, and then add 5 g of rutile nano-TiO2 / phlogopite prepared in step 1 at an ultrasonic frequency of 40 kHz / 800 W for 2 h, and then ultrasonically disperse at an ultrasonic frequency of 40 kHz / 800 W for 1 h to obtain a finished dispersion; Step 3, removing dichloromethane from the finished dispersion obtained in step 2 by vacuum distillation, and then transferring the obtained solid to a muffle furnace and heating it to 210° C. for high-temperature sintering for 3 hours to obtain a solid; Step 4, placing the solid obtained in step 3 on a three-roll mill (the roller distance of the three-roll mill is 45 μm) for three times of grinding and crushing to obtain a semi-finished surface-modified mica composition; Step 5: Place 5 g of the semi-finished surface-modified mica composition in 200 mL of 2 wt% KH540 aqueous solution at an ultrasonic frequency of 40 kHz / 800 W for 1 hour, filter, and dry to obtain a finished surface-modified mica composition. Example

[0035] A mica composite product for a CCS lithium battery core conductive plate comprises a mica composite substrate, at least one electronic grade glass cloth composited inside the mica composite substrate, and a copper foil composited on the surface of the mica composite substrate.

[0036] The mica composite substrate comprises the following raw materials in parts by weight: 80-90 parts of a surface-modified mica composition, 0.5-5 parts of a toughening filler, and 20-32 parts of a compounded organic silicon resin with a solid content of 40-55wt%.

[0037] Preferably, the mica composite substrate is made of the following raw materials in parts by weight: 81.4-83.2 parts of a surface-modified mica composition, 2.8-3.6 parts of a toughening filler, and 28-30 parts of a compounded silicone resin with a solid content of 50 wt%.

[0038] The toughening filler is composed of at least one of nano-aramid fiber and nano-carbon fiber, carbon nanotube, and inorganic whisker. Preferably, the toughening filler is composed of nano-aramid fiber and inorganic whisker in a mass ratio of (3-7):1. The inorganic whisker is composed of at least one of zinc oxide whisker, aluminum nitride whisker, aluminum oxide whisker, boron nitride whisker, and silicon carbide whisker. Further preferably, the toughening filler is composed of nano-aramid fiber and boron nitride whisker in a mass ratio of 4:1.

[0039] The surface modified mica composition comprises a mica matrix and nano-scale modified particles loaded on the surface of the mica matrix, wherein the mica matrix is ​​a 1340 mesh sieve material, D 10 0.5-2μm, D 50 3-5.5μm, D 90 The nano-scale modified particles include at least one of aluminum oxide, silicon dioxide, titanium dioxide, aluminum nitride, silicon nitride, graphene, carbon nanotubes, and fullerene. Preferably, the nano-scale modified particles are aluminum oxide and carbon nanotubes, the aluminum oxide is loaded and fixed on the surface of the mica substrate by a sol-gel method, and the carbon nanotubes are fixed on the surface of the mica substrate by sintering nano-silver or nano-copper.

[0040] The preparation method of the surface modified mica composition is as follows: Step 1: loading and fixing nano-scale modified particles A on the surface of a mica substrate by a sol-gel method, wherein the nano-scale modified particles A are at least one of aluminum oxide, silicon dioxide, titanium dioxide, aluminum nitride, and silicon nitride; Step 2: Add polyvinyl pyrrolidone and nano-scale modified particles B to the prepared Ag(2E4MI)2Ac complex solution, wherein the nano-scale modified particles AB are at least one of graphene, carbon nanotubes, and fullerene, and add the mica matrix material with the surface loaded with nano-scale modified particles A in step 1 after ultrasonic dispersion for 1-4 hours, and then ultrasonic dispersion for 0.5-2 hours; Step 3, the dispersion obtained in step 2 is subjected to reduced pressure distillation to remove the organic solvent in the Ag(2E4MI)2Ac complex solution, and the obtained solid is subjected to high temperature sintering for 2-4 hours, and the high temperature sintering temperature is 200-220°C; Step 4, rolling and grinding the solid obtained in step 3, wet-milling the obtained powder at a ball mill speed of 60-80 rpm for 15-40 min, and then filtering, drying and sieving to obtain a semi-finished surface-modified mica composition; Step 5, placing the semi-finished surface-modified mica composition obtained in step 4 in an aminosilane aqueous solution for ultrasonic dispersion treatment for 30-90 minutes, wherein the concentration of aminosilane in the aminosilane aqueous solution is 0.5-6wt%, and the aminosilane includes at least one of KH550, KH540, KH554, and KH590, filtering and drying to obtain a finished surface-modified mica composition.

[0041] The compound silicone resin with a solid content of 40-55wt% in the mica composite substrate formula is made of the following raw materials in parts by weight: 200 parts of KR-242A silicone resin, 50-100 parts of KR-271 silicone resin, 20-40 parts of a toughening composition with a molecular weight ≥1000, 20-60 parts of xylene, 20-60 parts of isopropanol, 0.20-0.30 parts of diethylenetriamine, and 0.10-0.20 parts of 1H-benzimidazole-1,5,6-triamine.

[0042] The toughening composition is at least one of the end-side chain epoxy silicone oil chain extender IOTA 105-3, double-terminal alcohol hydroxy silicone oil IOTA 2110, double-terminal alcohol hydroxy long-chain alkyl silicone oil IOTA-8865H, hydroxyl-terminated methyl vinyl silicone oil IOTA 1203V, carbon hydroxy silicone oil IOTA 2122, and carbon hydroxy silicone oil IOTA 2140 of Anhui Aiyota Silicone Oil Co., Ltd.

[0043] Necessity of compound silicone resin: When the mica composite parts for CCS lithium battery cell conductive plates were prepared using Japan's Shin-Etsu's KR-242A silicone resin as the silicone resin, it was found during the subsequent machining, stamping and cutting that obvious cracks appeared at the edges of the stamping and cutting of the mica composite parts for CCS lithium battery cell conductive plates, affecting the overall quality of the mica composite parts for CCS lithium battery cell conductive plates, unable to meet its later processing requirements, and limiting its production and application. The inventor conducted an optimization design study on the compound silicone resin: a toughening composition and 1H-benzimidazole-1,5,6-triamine curing agent were introduced into the formula to improve the impact toughness of the mica composite parts for CCS lithium battery cell conductive plates, while also having good bending strength and insulation and thermal conductivity safety performance, meeting the thermal runaway protection requirements of the signal acquisition components of CCS lithium batteries.

[0044] The preparation method of the compound silicone resin with a solid content of 40-55wt% is as follows: 0.05-0.10 parts of diethylenetriamine, 200 parts of KR-242A silicone resin, 50-100 parts of KR-271 silicone resin, and 20-40 parts of a toughening composition with a molecular weight of ≥1000 are pre-reacted at 68-70°C for 100-200s, cooled to 0-4°C in an ice water bath, 40-60 parts of xylene and 20-60 parts of isopropanol are added, and stirred at 80-160rpm for 10-30min, the remaining diethylenetriamine and 0.10-0.20 parts of 1H-benzimidazole-1,5,6-triamine are added, and stirred at 60-80rpm for 100-200s to obtain the silicone resin, which is stored at low temperature for standby use.

[0045] A method for preparing a mica composite component for a CCS lithium battery core conductive plate comprises the following steps: Step 1, preparing a surface-modified mica composition and a compounded silicone resin with a solid content of 40-55wt% respectively; Step 2: Evenly mix the accurately measured surface-modified mica composition in step 1, the toughening filler, and the compounded silicone resin with a solid content of 40-55wt% in step 1 to obtain a mica composite substrate slurry; pour the obtained mica composite substrate slurry into a molding mold; heat to remove the organic solvent and then adopt a four-step hot pressing method to obtain a semi-finished mica composite substrate; the obtained semi-finished mica composite substrate is heated to 50-55°C at a heating rate of 1-2°C / min and kept warm for 200-300s; then heated to 80-88°C at a heating rate of 1-2°C / min and kept warm for 60-120min; and naturally cooled to obtain a finished mica composite substrate; Preferably, the four-step hot pressing molding method is as follows: in the first step of hot pressing molding, the hot pressing conditions are a platen temperature of 80±2°C, a pressure of 0.25±0.05Mpa, and a duration of 60-80s; in the second step of hot pressing molding, the hot pressing conditions are a platen temperature of 130-135°C, a pressure of 0.5-0.6Mpa, and a duration of 100-120s; in the third step of hot pressing molding, the hot pressing conditions are a platen temperature of 175-180°C, a pressure of 0.8-1.0Mpa, and a duration of 120-160s; in the fourth step of hot pressing molding, the hot pressing conditions are a platen temperature of 115-120°C, a pressure of 0.4-0.6Mpa, and a duration of 60-80s, to obtain a semi-finished mica composite substrate; At the same time, a surface of the copper foil is subjected to low-temperature plasma treatment, treated with ammonia gas at 0-4°C for 5-30 minutes, and the surface of the copper foil after the low-temperature plasma treatment is coated with 0.5-1 g / dm2 of the compounded organic silicone resin with a solid content of 40-55 wt% in step 1, and an organic silicone film is formed on the surface of the copper foil after the low-temperature plasma treatment after heating to remove the organic solvent; Step three, stacking an electronic grade glass cloth between adjacent finished mica composite substrates to preheat and press to form a mica substrate, and pressing the copper foil in step two on the surface of the mica substrate, so that the organic silicone film on the surface of the copper foil is in contact with the surface of the mica substrate, and finally hot pressing and curing are performed. The mica composite component for the conductive plate of the CCS lithium battery cell can be obtained by hot pressing at a pressure of 2-4MPa and a temperature of 160-240°C for 2-4min, and naturally cooling to room temperature.

[0046] In the preparation method of the above-mentioned mica composite parts for the conductive plates of CCS lithium battery cells, attention should be paid to the design of the molding mold. The molding mold is a simple and low-cost plate-type molding mold, and the final finished mica composite parts for the conductive plates of CCS lithium battery cells are mica composite plates with a thickness of 0.30±0.02mm, which need to be stamped and cut as the signal acquisition components of the CCS lithium battery. The inventors found in actual processing that the mica and glass fiber will be exposed and protruding at the cut surface of the mica composite plate after stamping and cutting, and the stamping and cutting surface will also be affected by the workpiece clamping friction due to processing requirements, that is, the impurities generated by friction during the processing and assembly process will affect the electrode conductivity of the lithium battery and will also affect the current circuit etched on the copper foil, affecting the quality of the finally assembled CCS lithium battery cells. To this end, before stamping and cutting the mica composite panel, the release film needs to be attached to the upper and lower surfaces of the mica composite panel, and then the corresponding stamping and cutting treatment is carried out. After the stamping and cutting are completed, the slot section formed is coated with a layer of titanium dioxide wet gel through a gluing process (for the sol-gel method, see Preparation Example 1), and then placed in a vacuum drying oven for drying at 125°C for 12 hours, and then the slot section is laser sintered in an air atmosphere to form a nano titanium dioxide wear-resistant layer by laser sintering on the slot section, thereby improving the quality of the CCS lithium battery cell.

[0047] Assuming a standardized mica composite part for the conductive plate of a CCS lithium battery cell, the design of the molding mold has a preset notch, that is, the final finished mica composite substrate is integrally formed with a preset slot, and the electronic-grade glass fiber mesh needs to be punched to form the corresponding slot in the subsequent processing process to meet the preset slot design of the mica composite part for the conductive plate of the CCS lithium battery cell. There are two slot section treatment schemes for the mica composite part for the conductive plate of the CCS lithium battery cell prepared by this method: the first is to coat a layer of titanium dioxide wet gel on the slot section through the gluing process mentioned above (the sol-gel method is prepared in Preparation Example 1), and then place it in a vacuum drying oven at 125°C for 12 hours, and then perform laser sintering on the slot section in an air atmosphere, and laser sinter the slot section to form a nano titanium dioxide wear-resistant layer. The second scheme is: to coat the slot section with a compounded silicone resin through a gluing process to form an elastic silicone protective film layer.

[0048] Example 1: A mica composite component for a CCS lithium battery cell conductive plate includes a mica composite substrate, an electronic grade glass cloth composited inside the mica composite substrate, and a copper foil composited on the surface of the mica composite substrate. The mica composite substrate is made of 82 parts of the surface modified mica composition in Preparation Example 1, 3 parts of a toughening filler, and 30 parts of a compound silicone resin with a solid content of 50wt%. The toughening filler is composed of nano-aramid fiber and boron nitride whisker in a mass ratio of 4:1.

[0049] Preparation method of nano-aramid fiber: Aramid nanofiber dispersion U51 is prepared by a proton donor-assisted deprotonation method. Specifically, 2 g of para-aramid (DuPont Teijin para-aramid chopped PPTA, equivalent diameter 1 μm, length 1 mm) fiber is weighed and placed in a mixed solution of 3 g KOH, 1 L DMSO and 40 mL deionized water. The solution is stirred in a water bath at 60 ° C for 3 h to obtain a deep red ANFS dispersion with a mass concentration of 2 g / L. Aramid nanofiber ANFS powder is obtained by nanofiltration. 50 g of aramid nanofiber ANFS powder is ultrasonically dispersed in 1 L of isopropanol for use.

[0050] Boron nitride whiskers were from Shanghai Xiangtian Nanomaterials Co., Ltd., XT-BN-X2, with a diameter of 0.5-1 μm and a length of 10-20 μm.

[0051] The compound silicone resin with a solid content of 50wt% in the mica composite substrate formula is prepared from 200g of KR-242A silicone resin, 60g of KR-271 silicone resin, 25g of end-side chain epoxy silicone oil chain extender IOTA 105-3, 15g of double-terminal alcohol hydroxyl long-chain alkyl silicone oil IOTA-8865H, 20.4g of xylene, 20g of isopropanol, 0.20g of diethylenetriamine, and 0.20g of 1H-benzimidazole-1,5,6-triamine.

[0052] A method for preparing a mica composite component for a CCS lithium battery core conductive plate comprises the following steps: Step 1, preparing a surface-modified mica composition and a compounded silicone resin with a solid content of 50 wt % respectively; The preparation of the surface modified mica composition is shown in Preparation Example 1; The preparation method of a compound silicone resin with a solid content of 50 wt% is as follows: 0.08 g of diethylenetriamine, 200 g of KR-242A silicone resin, 60 g of KR-271 silicone resin, 25 g of end-side chain epoxy silicone oil chain extender IOTA 105-3, and 15 g of double-end alcohol hydroxyl long-chain alkyl silicone oil IOTA-8865H are pre-reacted at 70°C for 180 s, and then 20.4 g of xylene and 20 g of isopropanol are added after cooling to 0-4°C in an ice water bath, and stirred at 120 rpm for 30 min, and 0.12 g of diethylenetriamine and 0.20 g of 1H-benzimidazole-1,5,6-triamine are added, and stirred at 60 rpm for 180 s to obtain a compound silicone resin with a solid content of 50 wt%; Step 2: Evenly mix 720 g of the surface-modified mica composition accurately measured in step 1, 30 g of the toughening filler, and 300 g of the compounded silicone resin with a solid content of 50 wt% in step 1 to obtain a mica composite substrate slurry; pour the obtained mica composite substrate slurry into a molding mold; heat to remove the organic solvent (xylene and isopropanol); and then adopt a four-step hot pressing method to obtain a semi-finished mica composite substrate. The four-step hot pressing method is as follows: In the first step of hot pressing, the hot pressing conditions are as follows: the pressing plate temperature is 80°C, the pressure is 0.25 MPa, and the duration is 60 s; in the second step of hot pressing, the hot pressing conditions are as follows: the pressing plate temperature is 135°C, the pressure is 0.6Mpa, duration is 120s, the hot pressing conditions in the third step of hot pressing molding are a platen temperature of 180°C, a pressure of 1Mpa, and a duration of 150s; the hot pressing conditions in the fourth step of hot pressing molding are a platen temperature of 120°C, a pressure of 0.6Mpa, and a duration of 80s, and naturally cooled to room temperature to obtain a semi-finished mica composite substrate, the obtained semi-finished mica composite substrate is heated to 50°C at a heating rate of 1°C / min and kept warm for 300s, and then heated to 85°C at a heating rate of 2°C / min and kept warm for 100min, and naturally cooled to obtain a finished mica composite substrate with a thickness of 0.30±0.02mm; At the same time, the surface of the copper foil is treated with low-temperature plasma, and then treated with ammonia gas at 0°C for 15 minutes. The surface of the copper foil after the low-temperature plasma treatment is coated with 0.6 g / dm of the compound silicone resin with a solid content of 50 wt% in step 1. 2 , after heating to remove the organic solvent (xylene and isopropyl alcohol), an organic silica gel film is formed on the surface of the copper foil after the low-temperature plasma treatment; Step three, take three finished mica composite substrates with a thickness of 0.30±0.02mm, stack an electronic grade glass cloth between adjacent finished mica composite substrates, preheat and press to form a mica substrate, the preheat and press conditions are as follows: the pressing plate temperature is 150°C, the pressure is 0.8Mpa, and the duration is 120s; the copper foil in the stacking step 2 is pressed on the surface of the mica substrate formed by preheating and pressing, and the organic silicone film on the surface of the copper foil is in contact with the surface of the mica substrate, and finally hot pressing and curing are performed, hot pressing treatment is performed at a pressure of 3.2MPa and a temperature of 220°C for 4min, and naturally cooled to room temperature to obtain a mica composite component for a conductive plate of a CCS lithium battery cell.

[0053] The difference between Example 2 and Example 1 is that the mica composite substrate is made of 80 parts of the surface-modified mica composition in Preparation Example 1, 5 parts of toughening filler, and 30 parts of a compound silicone resin with a solid content of 50 wt%.

[0054] The difference between Example 3 and Example 1 is that the mica composite substrate is made of 89 parts of the surface-modified mica composition in Preparation Example 1, 0.5 parts of a toughening filler, and 21 parts of a compound silicone resin with a solid content of 50 wt%.

[0055] The difference between Example 4 and Example 1 is that the mica composite substrate is made of 83 parts of the surface-modified mica composition in Preparation Example 1, 3 parts of toughening filler, and 28 parts of a compound silicone resin with a solid content of 50 wt%.

[0056] The difference between Example 5 and Example 4 is that the mica composite substrate is made of 83 parts of the surface-modified mica composition in Preparation Example 2, 3 parts of toughening filler, and 28 parts of a compound silicone resin with a solid content of 50 wt%.

[0057] The difference between Example 6 and Example 4 is that the mica composite substrate is made of 83 parts of the surface-modified mica composition in Preparation Example 3, 3 parts of toughening filler, and 28 parts of a compound silicone resin with a solid content of 50 wt%.

[0058] The difference between Example 7 and Example 4 is that the mica composite substrate is made of 83 parts of the surface-modified mica composition in Preparation Example 4, 3 parts of a toughening filler, and 28 parts of a compound silicone resin with a solid content of 50 wt%.

[0059] The difference between Example 8 and Example 4 is that the surface-modified mica composition in Preparation Example 1 is replaced by a 1340-mesh screen-out material - rutile nano-TiO2 / phlogopite - obtained by screening with a 1340-mesh screen.

[0060] The difference between Example 9 and Example 4 is that the surface-modified mica composition in Preparation Example 1 is replaced by a 1340-mesh screen outlet material - nano ZnO / phlogopite - obtained by screening with a 1340-mesh screen.

[0061] The difference between Example 10 and Example 4 is that the surface-modified mica composition in Preparation Example 1 is replaced by a 1340-mesh screen-out material obtained by screening with a 1340-mesh screen - nano-Al2O3 / phlogopite.

[0062] The difference between Example 11 and Example 4 is that the surface-modified mica composition in Preparation Example 1 is replaced by a 1340-mesh screen outlet material - nano-scale AlN / phlogopite - obtained by screening with a 1340-mesh screen.

[0063] The difference between Example 12 and Example 4 is that the toughening filler is composed of nano-aramid fiber and alumina whisker in a mass ratio of 4: 1. The alumina whisker is purchased from Hubei Xinyuhong Biomedical Technology Co., Ltd., with specifications of 0.5-1.0 μm in diameter, 10 μm in length, and aspect ratio of 15.

[0064] The difference between Example 13 and Example 4 is that the toughening filler is composed of nano-aramid fiber and boron nitride whisker in a mass ratio of 2:1.

[0065] The difference between Example 14 and Example 4 is that the toughening filler is composed of nano-aramid fiber and boron nitride whisker in a mass ratio of 7:1.

[0066] The difference between Example 15 and Example 4 is that the toughening filler is composed of nano-aramid fiber and boron nitride whisker in a mass ratio of 9:1.

[0067] The difference between Example 16 and Example 4 is that the toughening filler is only nano-aramid fiber.

[0068] The difference between Example 17 and Example 4 is that the compound silicone resin with a solid content of 50 wt% in the mica composite substrate formula is prepared from 200 g of KR-242A silicone resin, 80 g of KR-271 silicone resin, 10 g of end-side chain epoxy silicone oil chain extender IOTA 105-3, 10 g of double-end alcohol hydroxyl long-chain alkyl silicone oil IOTA-8865H, 20.4 g of xylene, 20 g of isopropanol, 0.20 g of diethylenetriamine, and 0.20 g of 1H-benzimidazole-1,5,6-triamine.

[0069] The difference between Example 18 and Example 4 is that the compound silicone resin with a solid content of 50 wt% in the mica composite substrate formula is prepared from 200 g of KR-242A silicone resin, 50 g of KR-271 silicone resin, 20 g of end-side chain epoxy silicone oil chain extender IOTA 105-3, 10 g of double-end alcohol hydroxyl long-chain alkyl silicone oil IOTA-8865H, 20.4 g of xylene, 20 g of isopropanol, 0.20 g of diethylenetriamine, and 0.20 g of 1H-benzimidazole-1,5,6-triamine.

[0070] The difference between Example 19 and Example 4 is that the compound silicone resin with a solid content of 50 wt% in the mica composite substrate formula is prepared from 200 g of KR-242A silicone resin, 60 g of KR-271 silicone resin, 25 g of end-side chain epoxy silicone oil chain extender IOTA 105-3, 15 g of hydroxyl-terminated methyl vinyl silicone oil IOTA 1203V, 20.4 g of xylene, 20 g of isopropanol, 0.20 g of diethylenetriamine, and 0.20 g of 1H-benzimidazole-1,5,6-triamine.

[0071] The difference between Example 20 and Example 4 is that the compound silicone resin with a solid content of 50 wt% in the mica composite substrate formula is prepared from 200 g of KR-242A silicone resin, 60 g of KR-271 silicone resin, 25 g of end-side chain epoxy silicone oil chain extender IOTA 105-3, 15 g of carbon hydroxy silicone oil IOTA 2140, 20.4 g of xylene, 20 g of isopropanol, 0.20 g of diethylenetriamine, and 0.20 g of 1H-benzimidazole-1,5,6-triamine.

[0072] The difference between Comparative Example 1 and Example 1 is that the mica composite substrate is made of 85 parts of the surface-modified mica composition in Preparation Example 1 and 30 parts of a compounded silicone resin with a solid content of 50 wt%. When the mica composite parts for CCS lithium battery cell conductive plates prepared above are subsequently machined, punched and cut, it is found that the mica substrate at the punching and cutting edges has fine cracks, which affects the overall quality of the mica composite parts for CCS lithium battery cell conductive plates.

[0073] The difference between Comparative Example 2 and Example 1 is that the mica composite substrate is made of 82 parts of a common surface-modified mica composition, 3 parts of a toughening filler, and 30 parts of a compounded silicone resin with a solid content of 50 wt%. The preparation method of the common surface-modified mica composition is as follows: 5 g of phlogopite powder sieved through a 1340 mesh is placed in 200 mL of a 2 wt% KH540 aqueous solution at an ultrasonic frequency of 40 kHz / 800 W, ultrasonically dispersed for 60 min, filtered, and dried to obtain the result.

[0074] The difference between Comparative Example 3 and Example 1 is that the mica composite substrate is made of 82 parts of the surface-modified mica composition in Preparation Example 5, 3 parts of toughening filler, and 30 parts of a compound silicone resin with a solid content of 50 wt%.

[0075] The difference between Comparative Example 4 and Example 1 is that the mica composite substrate is made of 79 parts of the surface-modified mica composition in Preparation Example 1, 3 parts of toughening filler, and 36 parts of a compound silicone resin with a solid content of 50 wt%.

[0076] The difference between Comparative Example 5 and Example 1 is that the mica composite substrate is made of 88 parts of the surface modified mica composition in Preparation Example 1, 3 parts of toughening filler, and 18 parts of a compounded silicone resin with a solid content of 50wt%. When the mica composite parts for CCS lithium battery cell conductive plates prepared above are subsequently machined, punched and cut, it is found that the mica substrate at the punching and cutting edges has fine cracks, which affects the overall quality of the mica composite parts for CCS lithium battery cell conductive plates.

[0077] The difference between Comparative Example 6 and Example 1 is that the compounded silicone resin with a solid content of 50wt% is prepared from 340g of KR-242A silicone resin and 0.25g of diethylenetriamine. When the mica composite parts for CCS lithium battery core conductive plates prepared above are subsequently machined, punched and cut, it is found that obvious cracks appear on the mica substrate at the punching and cutting edges, affecting the overall quality of the mica composite parts for CCS lithium battery core conductive plates.

[0078] The difference between Comparative Example 7 and Example 1 is that the compounded silicone resin with a solid content of 50wt% is prepared from 260g of KR-242A silicone resin, 80g of KR-271 silicone resin, and 0.25g of diethylenetriamine. When the mica composite parts for CCS lithium battery core conductive plates prepared above are subsequently machined, punched and cut, it is found that the mica substrate at the punching and cutting edges has fine cracks, which affects the overall quality of the mica composite parts for CCS lithium battery core conductive plates.

[0079] The difference between Comparative Example 8 and Example 1 is that KR-271 silicone resin is not added to the compound silicone resin formula with a solid content of 50wt%. The compound silicone resin formula with a solid content of 50wt% is made of 260g of KR-242A silicone resin, 25g of end-side chain epoxy silicone oil chain extender IOTA 105-3, 15g of double-terminal alcohol hydroxyl long-chain alkyl silicone oil IOTA-8865H, 20.4g of xylene, 20g of isopropanol, 0.20g of diethylenetriamine, and 0.20g of 1H-benzimidazole-1,5,6-triamine.

[0080] The difference between Comparative Example 9 and Example 1 is that the compound silicone resin with a solid content of 50 wt% in the mica composite substrate formula is prepared from 260 g of KR-271 silicone resin, 25 g of end-side chain epoxy silicone oil chain extender IOTA 105-3, 15 g of double-end alcohol hydroxyl long-chain alkyl silicone oil IOTA-8865H, 20.4 g of xylene, 20 g of isopropanol, 0.20 g of diethylenetriamine, and 0.20 g of 1H-benzimidazole-1,5,6-triamine.

[0081] The difference between Comparative Example 10 and Example 1 is that: Step 2, 720g of the surface-modified mica composition in Step 1, 30g of the toughening filler, and 300g of the compounded silicone resin with a solid content of 50wt% in Step 1 are evenly mixed to obtain a mica composite substrate slurry, and the obtained mica composite substrate slurry is poured into a molding mold, and after heating to remove the organic solvent (xylene and isopropanol), a two-step hot pressing molding method is used to obtain a semi-finished mica composite substrate. The four-step hot pressing molding method is as follows: the first step is hot pressing The hot pressing conditions during the molding process are a platen temperature of 140°C, a pressure of 0.8 MPa, and a duration of 180 s. The hot pressing conditions in the second step of hot pressing molding are a platen temperature of 180°C, a pressure of 1.2 MPa, and a duration of 240 s. The semi-finished mica composite substrate is naturally cooled to room temperature to obtain a semi-finished mica composite substrate. The obtained semi-finished mica composite substrate is heated to 85°C at a heating rate of 2°C / min and kept warm for 105 minutes. It is naturally cooled to obtain a finished mica composite substrate with a thickness of 0.30±0.02 mm.

[0082] The difference between Comparative Example 11 and Example 1 is that: in step 2, the surface of the copper foil is not subjected to low-temperature plasma treatment, and a composite silicone resin with a solid content of 50 wt% is directly added at a temperature of 0.6 g / dm 2 The coating amount is scraped on the surface of the copper foil, and the copper foil with a composite organic silicone film on the surface is obtained after heating to remove the organic solvent (xylene and isopropyl alcohol). When the mica composite parts for CCS lithium battery cell conductive plates prepared above are subsequently machined, punched and cut, it is found that the copper foil at the edges of the punching and cutting has a warping problem, which affects the overall quality of the mica composite parts for CCS lithium battery cell conductive plates. Therefore, it is necessary to perform low-temperature plasma treatment on the surface of the copper foil during the preparation of the mica composite parts for CCS lithium battery cell conductive plates.

[0083] Performance test: 1. Bending strength test: GB / T 5019.2-2009 mica product test method, Article 11 "bending strength and bending elastic modulus" for testing, sample width is about 25mm, test span is 16mm, test speed is 50mm / min, and pressure head radius is 5mm. 2. Electrical strength test: GB / T 5019.2-2009 mica product test method, Article 22 "electrical strength" for testing, sample thickness is 0.39mm-0.41mm, using Φ25mm / Φ75mm cylindrical electrode system, fast voltage rise mode (voltage rise speed is 1.0kV / s), in 25# transformer oil at 23℃±2℃. 3. Thermal conductivity test: Determined in accordance with GB / T10297-1998 "Determination of thermal conductivity of non-metallic solid materials - hot wire method". 4. Dielectric loss factor test method: Measure according to IPC TM-650 2.5.5.5 (50Hz) method.

[0084] Table 1: Test parameter table of mica composite products for CCS lithium battery core conductive plates in Examples 1-20 and Comparative Examples 1-10

[0085] From Examples 1, 4, 12-16 and Comparative Example 1 and Table 1, it can be seen that the nano-aramid fiber combined with the toughening filler composed of inorganic whiskers can improve the overall bending strength, impact toughness, insulation thermal conductivity, and thermal runaway safety performance, while improving the overall processing performance, increasing the yield rate of machining, stamping and cutting, and reducing production costs.

[0086] It can be seen from Examples 1-11 and Comparative Examples 2-3 and Table 1 that the surface-modified mica composition prepared in the present application can improve the overall low dielectric loss, high reliability, high insulation and thermal conductivity, and thermal runaway safety performance.

[0087] It can be seen from Examples 1-3 and Comparative Examples 4-5 and Table 1 that when the toughening filler is added in an amount of 3 parts, the glue content in the mica composite substrate is preferably 10-15wt%. Preferably, the glue content in the mica composite substrate is 13.8-14.0wt%.

[0088] It can be seen from Example 4 and Examples 17-20 and Comparative Examples 6-9 and Table 1 that the use of the self-made compound silicone resin in the present application can ensure the overall bending strength, impact toughness, insulation thermal conductivity, and thermal runaway safety performance, while improving the overall processing performance, improving the yield rate of machining, stamping and cutting, and reducing production costs.

[0089] It can be seen from Example 1 and Comparative Example 9 and Table 1 that the mica composite component for the conductive plate of the CCS lithium battery cell prepared by the preparation method provided in the present application has relatively good bending resistance and low dielectric loss.

[0090] In summary, the mica composite component for the conductive plate of the CCS lithium battery cell in this application is used to make the signal acquisition component of the CCS lithium battery, which can effectively improve the thermal runaway safety performance of the CCS lithium battery module, and has the advantages of low dielectric loss, high reliability, and high insulation and thermal conductivity, which is conducive to the high-quality development of the new energy vehicle industry.

Claims

1. A mica composite component for a CCS lithium battery cell conductive plate, Features: The invention comprises a mica composite substrate, at least one electronic-grade glass cloth compounded inside the mica composite substrate and a copper foil compounded on the surface of the mica composite substrate. The mica composite substrate is made of the following raw materials in parts by weight: 80-90 parts of a surface-modified mica composition, 0.5-5 parts of a toughening filler, and 20-32 parts of a compounded organic silicone resin with a solid content of 40-55wt%; the surface-modified mica composition comprises a mica matrix and nano-scale modified particles loaded on the surface of the mica matrix, the nano-scale modified particles comprise at least one of aluminum oxide, silicon dioxide, titanium dioxide, aluminum nitride, silicon nitride, graphene, carbon nanotubes, and fullerene; the toughening filler is composed of at least one of nano-aramid fibers, nano-carbon fibers, carbon nanotubes, and inorganic whiskers.

2. The mica composite component for a CCS lithium battery core conductive plate according to claim 1, Features: The mica matrix is ​​1340 mesh sieve material, D 10 0.5-2μm, D 50 3-5.5μm, D 90 7.5-9.5μm.

3. A mica composite component for a CCS lithium battery core conductive plate according to claim 1 or 2, Features: The nano-scale modified particles are aluminum oxide and carbon nanotubes. The aluminum oxide is loaded and fixed on the surface of the mica matrix by a sol-gel method; the carbon nanotubes are fixed on the surface of the mica matrix by sintering nano-silver or nano-copper.

4. The mica composite component for a CCS lithium battery core conductive plate according to claim 1, Features: The toughening filler is composed of nano-aramid fiber and inorganic whisker in a mass ratio of (3-7):1; the inorganic whisker is at least one of zinc oxide whisker, aluminum nitride whisker, aluminum oxide whisker, boron nitride whisker and silicon carbide whisker.

5. The mica composite component for a CCS lithium battery core conductive plate according to claim 1, Features: The mica composite substrate is made of the following raw materials in parts by weight: 81.4-83.2 parts of a surface-modified mica composition, 2.8-3.6 parts of a toughening filler, and 28-30 parts of a compounded silicone resin with a solid content of 50wt%.

6. The mica composite component for a CCS lithium battery core conductive plate according to claim 5, Features: The preparation method of the surface modified mica composition is as follows: Step 1: loading and fixing nano-scale modified particles A on the surface of a mica substrate by a sol-gel method, wherein the nano-scale modified particles A are at least one of aluminum oxide, silicon dioxide, titanium dioxide, aluminum nitride, and silicon nitride; Step 2: Add polyvinyl pyrrolidone and nano-scale modified particles B to the prepared Ag(2E4MI)2Ac complex solution, wherein the nano-scale modified particles AB are at least one of graphene, carbon nanotubes, and fullerene, and add the mica matrix material with the surface loaded with nano-scale modified particles A in step 1 after ultrasonic dispersion for 1-4 hours, and then ultrasonic dispersion for 0.5-2 hours; Step 3, the dispersion obtained in step 2 is subjected to reduced pressure distillation to remove the organic solvent in the Ag(2E4MI)2Ac complex solution, and the obtained solid is subjected to high temperature sintering for 2-4 hours, and the high temperature sintering temperature is 200-220°C; Step 4, rolling and grinding the solid obtained in step 3, wet-milling the obtained powder at a ball mill speed of 60-80 rpm for 15-40 min, and then filtering, drying and sieving to obtain a semi-finished surface-modified mica composition; Step 5, placing the semi-finished surface-modified mica composition obtained in step 4 in an aminosilane aqueous solution for ultrasonic dispersion treatment for 30-90 minutes, wherein the concentration of aminosilane in the aminosilane aqueous solution is 0.5-6wt%, and the aminosilane includes at least one of KH550, KH540, KH554, and KH590, filtering and drying to obtain a finished surface-modified mica composition.

7. The mica composite component for a CCS lithium battery core conductive plate according to claim 1, Features: The compound silicone resin with a solid content of 40-55wt% is made of the following raw materials in parts by weight: 200 parts of KR-242A silicone resin, 50-100 parts of KR-271 silicone resin, 20-40 parts of a toughening composition with a molecular weight ≥1000, 20-60 parts of xylene, 20-60 parts of isopropanol, 0.20-0.30 parts of diethylenetriamine, and 0.10-0.20 parts of 1H-benzimidazole-1,5,6-triamine; the toughening composition is at least one of end-side chain epoxy silicone oil chain extender IOTA 105-3, double-end alcohol hydroxy silicone oil IOTA 2110, double-end alcohol hydroxy long-chain alkyl silicone oil IOTA-8865H, hydroxyl-terminated methyl vinyl silicone oil IOTA1203V, carbon hydroxy silicone oil IOTA 2122, and carbon hydroxy silicone oil IOTA 2140.

8. The mica composite component for the conductive plate of a CCS lithium battery cell according to claim 7, Features: The preparation method of the compound silicone resin with a solid content of 40-55wt% is as follows: 0.05-0.10 parts of diethylenetriamine, 200 parts of KR-242A silicone resin, 50-100 parts of KR-271 silicone resin, and 20-40 parts of a toughening composition with a molecular weight of ≥1000 are pre-reacted at 68-70°C for 100-200s, and after cooling to 0-4°C in an ice water bath, 40-60 parts of xylene and 20-60 parts of isopropanol are added and stirred at 80-160rpm for 10-30min, and the remaining diethylenetriamine and 0.10-0.20 parts of 1H-benzimidazole-1,5,6-triamine are added, and the silicone resin is stirred at 60-80rpm for 100-200s to obtain the silicone resin, which is stored at low temperature for standby use.

9. A method for preparing a mica composite component for a CCS lithium battery core conductive plate according to any one of claims 1 to 8, Features: The following steps are involved: Step 1, preparing a surface-modified mica composition and a compounded silicone resin with a solid content of 40-55wt% respectively; Step 2: Evenly mix the accurately measured surface-modified mica composition in step 1, the toughening filler, and the compounded silicone resin with a solid content of 40-55wt% in step 1 to obtain a mica composite substrate slurry; pour the obtained mica composite substrate slurry into a molding mold; heat to remove the organic solvent and then adopt a four-step hot pressing method to obtain a semi-finished mica composite substrate; the obtained semi-finished mica composite substrate is heated to 50-55°C at a heating rate of 1-2°C / min and kept warm for 200-300s; then heated to 80-88°C at a heating rate of 1-2°C / min and kept warm for 60-120min; and naturally cooled to obtain a finished mica composite substrate; At the same time, the surface of the copper foil is treated with low temperature plasma, and ammonia is used for treatment at 0-4°C for 5-30 minutes. The surface of the copper foil after the low temperature plasma treatment is coated with 0.5-1g / dm of the compound silicone resin with a solid content of 40-55wt% in step 1. 2 After the organic solvent is removed by heating, an organic silica gel film is formed on the surface of the copper foil after low-temperature plasma treatment; Step three, stacking an electronic grade glass cloth between adjacent finished mica composite substrates to preheat and press to form a mica substrate, and pressing the copper foil in step two on the surface of the mica substrate, so that the organic silicone film on the surface of the copper foil is in contact with the surface of the mica substrate, and finally hot pressing and curing are performed. The mica composite component for the conductive plate of the CCS lithium battery cell can be obtained by hot pressing at a pressure of 2-4MPa and a temperature of 160-240°C for 2-4min, and naturally cooling to room temperature.

10. The preparation method according to claim 9, Features: The four-step hot pressing molding method in step 2 is as follows: the hot pressing conditions in the first step of hot pressing molding are a platen temperature of 80±2°C, a pressure of 0.25±0.05Mpa, and a duration of 60-80s; the hot pressing conditions in the second step of hot pressing molding are a platen temperature of 130-135°C, a pressure of 0.5-0.6Mpa, and a duration of 100-120s; the hot pressing conditions in the third step of hot pressing molding are a platen temperature of 175-180°C, a pressure of 0.8-1.0Mpa, and a duration of 120-160s; the hot pressing conditions in the fourth step of hot pressing molding are a platen temperature of 115-120°C, a pressure of 0.4-0.6Mpa, and a duration of 60-80s to obtain a semi-finished mica composite substrate.

Citation Information

Patent Citations

  • Mixed heat-conductive glue for copper-clad plate and preparation method thereof

    CN109852294A

  • Low-thermal-conductivity and high-insulation mica piece and forming process

    CN113823468A

  • Thermal runaway protection low-thermal-conductivity mica composite part applied between battery cells and preparation method of thermal runaway protection low-thermal-conductivity mica composite part

    CN114361740A

  • CPVC Compositions Having Good Impact Strength And Heat Stability, And Smooth Surfaces

    US20080188608A1

  • Translucent high-temperature powder coatings

    US6248824B1