Multilayer structured surfaces for anti-glare applications and associated methods
By setting multiple discrete, height-distributed diffractive surface regions on the main surface of the display product, the specular reflectivity is reduced by utilizing far-field scattering patterns, thus solving the problems of glare and excessive reflectivity in existing technologies and achieving a display effect with low reflectivity and high contrast.
Patent Information
- Application Number
- CN202380030959.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-16
- Publication Date
- 2024-11-15
AI Technical Summary
Existing anti-reflective coatings and anti-glare technologies are insufficient to effectively reduce reflections across the entire visible spectrum, leading to glare problems. Furthermore, excessively large angles of reflection can reduce the contrast of displayed images.
By employing a diffractive surface region design, multiple discrete height-distributed regions are set on the main surface of the display product. The far-field scattering pattern is used to reduce specular reflectivity and control the light scattering angle, thereby achieving a reduction of specular reflectivity by at least 10 times while maintaining low haze.
It significantly reduces specular reflectivity, minimizes glare interference, maintains display image contrast, and provides excellent anti-glare and anti-haze performance.
Smart Images

Figure CN118973974A_ABST
Abstract
Description
[0001] priority
[0002] This application claims the benefit of priority under 35 USC §119 to U.S. Provisional Application Serial No. 3 / 325,280 filed on March 30, 2022, the contents of which are the basis of this application and are incorporated herein by reference in their entirety. Technical Field
[0003] The present disclosure relates to anti-glare articles, and more particularly, to display articles including a surface having a diffractive surface region including a plurality of regions disposed in a discrete height distribution and arranged in a pattern based on a target scattering pattern. Background Art
[0004] A display of a display article covered with a substrate that is transparent to visible light. Such display articles include smartphones, tablet computers, televisions, computer monitors, vehicle interior displays, etc. The display is typically a liquid crystal display and an organic light emitting diode, etc. The substrate protects the display, while the transparency of the substrate allows the user of the device to view the display. Glare is a phenomenon associated with a degradation of the viewing experience in the presence of a bright light source. In addition, reflected images from the environment rather than from the bright light source can also contribute to a degradation of the viewing of the display. For example, a visually distinct reflected image of the user himself or light from the surrounding environment can cause distraction, reduced readability, and visual fatigue.
[0005] Several techniques have been used to reduce glare, including anti-reflective coatings and anti-glare techniques. Anti-reflective coatings can reduce glare by directly reducing the total amount of reflection. However, some existing anti-reflective coatings may not reduce reflections to a large enough extent across the entire visible spectrum so that users will not notice such reflections. Anti-glare technology attempts to extend the reflection of light to a large angle range to reduce the peak intensity of the reflection and make the distracting reflected image less noticeable to the user. However, reflections at too large an angle can result in relatively high haze, which can reduce the contrast of the displayed image.
[0006] Therefore, an alternative to existing anti-glare and anti-reflective coating technologies that allows the angular distribution of scattered light to be advantageously controlled would be beneficial. Summary of the invention
[0007] Aspect (1) of the present disclosure relates to a display article comprising: a first major surface; a second major surface opposite the first major surface; and a diffractive surface region formed in the first major surface. Within the diffractive surface region, the first major surface comprises a plurality of regions arranged in a discrete height distribution, the discrete height distribution being measured relative to an imaginary reference plane extending through the display article and parallel to the first major surface. The plurality of regions are arranged so that at a wavelength greater than or equal to a minimum wavelength λ min and less than or equal to the maximum wavelength λ max The incident angle range on the first major surface is the minimum incident angle within the wavelength range of interest. To maximum incident angle When , the specular reflectivity of light incident on the first major surface is reduced by at least a factor of 10 compared to a non-textured version of the first major surface that does not include the diffractive surface region. The difference between the heights in the discrete height distribution is Within 5% of an integer multiple of λ′ min =λ min / cosθ min , and λ′ max =λ max / cosθ max .
[0008] Aspect (2) of the present disclosure relates to a display article according to aspect (1), wherein the diffractive surface region scatters light in a far-field scattering pattern having a peak scattering angle less than or equal to 1.5° in the wavelength range of interest.
[0009] Aspect (3) of the present disclosure relates to a display article according to aspect (2), wherein the peak scattering angle is less than or equal to 0.5° within at least a portion of the wavelength range of interest.
[0010] Aspect (4) of the present disclosure relates to a display article according to aspect (2), wherein the far-field scattering pattern approximates a Laguerre-Gaussian mode.
[0011] Aspect (5) of the present disclosure relates to a display article according to any one of aspects (1) to (4), wherein: min Greater than or equal to 380nm and λ max Less than or equal to 1200nm, and Greater than or equal to 0° and Less than or equal to 75°.
[0012] Aspect (6) of the present disclosure relates to a display article according to any one of aspects (1) to (5), wherein λ min =400nm and λ max=800nm.
[0013] Aspect (7) of the present disclosure relates to a display article according to any of aspects (1)-(6), wherein the specular reflectivity is reduced by at least 100 times compared to a non-textured version of the first major surface.
[0014] Aspect (8) of the present disclosure relates to a display article according to any one of aspects (1) to (8), wherein the plurality of regions have a minimum feature size greater than or equal to 1 μm.
[0015] Aspect (9) of the present disclosure relates to the display article according to any one of aspects (1) to (8), wherein the plurality of regions are arranged in a pattern that is periodic in two directions perpendicular to each other.
[0016] Aspect (10) of the present disclosure relates to a display article according to aspect (9), wherein the pattern includes at least one enclosed area, the at least one enclosed area being completely surrounded by a plurality of areas having a height different from that of the enclosed area relative to an imaginary reference plane.
[0017] Aspect (11) of the present disclosure relates to a display article according to any one of aspects (1) to (10), wherein the transmission haze of light incident on the first major surface is less than or equal to 4% over the entire wavelength range of 400 nm to 800 nm.
[0018] Aspect (12) of the present disclosure relates to a display article according to any of aspects (1)-(11), wherein the regions in a plurality of regions at each height of a discrete height distribution occupy a combined surface area percentage of the diffractive surface area that is predetermined to minimize the specular reflectivity.
[0019] Aspect (13) of the present disclosure relates to the display article according to aspect (12), wherein the discrete height distribution comprises three or more heights.
[0020] Aspect (14) of the present disclosure relates to a display article according to aspect (13), wherein the discrete height distribution includes at least four heights, the at least four heights including a minimum height h min ,exist The second height within 5% min ,exist The third height within 5% and The fourth height within 5% of the.
[0021] Aspect (15) of the present disclosure relates to a display product according to aspect (14), wherein: a first plurality of regions having a minimum height occupy a first combined surface area percentage of the diffractive surface area, and the first combined surface area percentage is less than a second combined surface area percentage occupied by a second plurality of regions having a second height.
[0022] Aspect (16) of the present disclosure relates to a display product according to aspect (15), wherein: a third plurality of regions having a third height occupy a third combined surface area percentage of the diffractive surface area, a fourth plurality of regions having a fourth height occupy a fourth combined surface area percentage of the diffractive surface area, the first combined surface area percentage is within 5% of the fourth combined surface area percentage, and the second combined surface area percentage is within 5% of the third combined surface area percentage.
[0023] Aspect (17) of the present disclosure relates to a display article according to aspect (13), wherein the combined surface area percentage associated with each height is less than or equal to 40%.
[0024] Aspect (18) of the present disclosure relates to a glass display product, the glass display product comprising: a first major surface; a second major surface opposite the first major surface; and a diffractive surface region formed in the first major surface, wherein within the diffractive surface region, the first major surface comprises: a first plurality of regions, the first plurality of regions comprising a first plurality of heights, the first plurality of heights having a maximum height h max Within 5% of the average of the first plurality of heights, the maximum height h max is measured from an imaginary reference plane extending through the display article and parallel to the first major surface, the first plurality of regions occupying a first combined surface area percentage of the diffractive surface area; and a second plurality of regions, the second plurality of regions comprising a second plurality of heights having a minimum height h measured from the imaginary reference plane min The second plurality of regions occupy a second combined surface area percentage of the diffractive surface area, wherein: the first plurality of regions and the second plurality of regions are arranged in a predetermined pattern, the predetermined pattern being based on a wavelength greater than or equal to a minimum wavelength λ min and less than or equal to the maximum wavelength λ max The incident angle range on the first major surface is the minimum incident angle within the wavelength range of interest. To maximum incident angle The predicted specular reflectance of light incident on the first major surface when max -h min exist Within 5% of an integer multiple of λ′ min =λ min / cosθmin , and λ′ max =λ max / cosθ max , and the average measured specular reflectivity of the first major surface is less than or equal to 2.5% within the range of incident angles and wavelengths of interest.
[0025] Aspect (19) of the present disclosure relates to a glass display article according to aspect (18), wherein the diffractive surface region scatters light in a far-field scattering pattern having a peak scattering angle less than or equal to 1.5° in the wavelength range of interest.
[0026] Aspect (20) of the present disclosure relates to a glass display article according to aspect (19), wherein the peak scattering angle is less than or equal to 0.5° in the wavelength range of interest.
[0027] Aspect (21) of the present disclosure relates to a glass display article according to any one of aspects (19)-(20), wherein the far-field scattering pattern approximates a Laguerre-Gaussian mode.
[0028] Aspect (22) of the present disclosure relates to a display article according to any one of aspects (18) to (21), wherein: min Greater than or equal to 380nm and λ max Less than or equal to 1200nm, and Greater than or equal to 0° and Less than or equal to 75°.
[0029] Aspect (23) of the present disclosure relates to a glass display article according to any one of aspects (18)-(22), wherein, within the diffractive surface region, the first major surface includes a third plurality of regions, the third plurality of regions including a third plurality of heights, the third plurality of heights being within 5% of an average of the third plurality of heights at a height h1 measured from a reference plane, the third plurality of regions occupying a third combined surface area percentage of the diffractive surface region, wherein the height h1 is within 5% of an average of the third plurality of heights. within 5%.
[0030] Aspect (24) of the present disclosure relates to a glass display article according to aspect (23), wherein, within the diffractive surface region, the first major surface includes a fourth plurality of regions, the fourth plurality of regions including a fourth plurality of heights, the fourth plurality of heights being within 5% of an average of the fourth plurality of heights at a height h2 measured from the reference plane, the fourth plurality of regions occupying a fourth combined surface area percentage of the diffractive surface region, wherein the height h2 is within 5% of an average of the fourth plurality of heights. within 5%.
[0031] Aspect (25) of the present disclosure relates to a glass display article according to aspect (24), wherein: the first combined surface area percentage is within 5% of the fourth second combined surface area percentage, and the third combined surface area percentage is within 5% of the fourth combined surface area percentage.
[0032] Aspect (26) of the present disclosure relates to a glass display article according to aspect (24), wherein each of the first combined surface area percentage, the second combined surface area percentage, the third combined surface area percentage, and the fourth combined surface area percentage is less than or equal to 40%.
[0033] Aspect (27) of the present disclosure relates to a glass display article according to any one of aspects (18)-(26), wherein the first plurality of regions and the second plurality of regions each have a characteristic size greater than or equal to 1 μm.
[0034] Aspect (28) of the present disclosure relates to the glass display article according to any one of aspects (18) to (27), wherein the predetermined pattern is periodic in two directions perpendicular to each other.
[0035] Aspect (29) of the present disclosure relates to a glass display product according to any one of aspects (18)-(28), wherein the predetermined pattern includes at least one enclosed area, which is completely surrounded by a plurality of areas having a height different from that of the enclosed area relative to an imaginary reference plane.
[0036] Aspect (30) of the present disclosure relates to a glass display article according to any one of aspects (18) to (29), wherein the transmission haze of light incident on the first major surface is less than or equal to 4% over the entire wavelength range of 400 nm to 800 nm.
[0037] Aspect (31) of the present disclosure relates to a method for forming a diffractive surface region of a substrate for a display article, the method comprising: determining a pattern of multiple regions on a first major surface of the substrate, wherein each region in the multiple regions includes a surface region disposed at a height measured relative to an imaginary reference plane extending through the display article and parallel to the first major surface, wherein the multiple regions include discrete height distributions; disposing one or more etching masks on the first major surface, the one or more etching masks allowing etching to be performed only on selected regions of the first major surface to form at least some of the multiple regions; and after disposing each of the one or more etching masks on the first major surface, contacting the display article with an etchant for a period of time to form multiple regions including discrete height distributions in the substrate, such that the difference between the heights in the discrete height distributions is within a range of 0.1% to 0.1%. Within 5% of an integer multiple of λmin is the minimum wavelength of the wavelength range of interest, λ max is the maximum wavelength in the wavelength range of interest, Define the range of incident angles within which it is desired to minimize the specular reflectivity of the display article, λ′ min =λ max cosθ min , and λ′ max =λ min cosθ max .
[0038] Aspect (32) of the present disclosure relates to a method according to aspect (31), wherein determining the pattern of the plurality of regions comprises determining an ideal combined surface area percentage for each height in a discrete height distribution using the following relationship FA=1, where A is a vector having N entries, where N corresponds to the number of heights in the discrete height distribution, 1 is an identity row vector having N entries, and F is an NxN matrix, where each value F ij is calculated as
[0039] Aspect (33) of the present disclosure relates to a method according to aspect (32), wherein determining the patterns of the plurality of regions comprises: generating an initial pattern of the plurality of regions; calculating an estimated far-field scattering pattern by approximating the incident light as a uniform field and approximating the diffractive surface regions as causing only phase shifts in the reflected light; and use an optimization algorithm to update the initial pattern to reduce The difference between the target scattering pattern u(λ).
[0040] Aspect (34) of the present disclosure relates to a method according to aspect (33), wherein the optimization algorithm minimizes the following objective function of the pattern P: where K is an integer value that samples the wavelength range of interest, and i and j are the range of incident angles. An integer value for uniform sampling, A i is the percentage of surface area associated with the heights in the discrete height distribution associated with the initial pattern, is the ideal combined surface area percentage in vector A, and w is a weighting factor.
[0041] Aspect (35) of the present disclosure relates to the method according to aspect (33), wherein the target far-field scattering pattern approximates a Laguerre-Gaussian pattern.
[0042] Aspect (36) of the present disclosure relates to a method according to any one of aspects (33)-(35), wherein the target scattering pattern comprises a peak scattering angle less than or equal to 1.5° in the wavelength range of interest.
[0043] Aspect (37) of the present disclosure relates to a method according to any one of aspects (33)-(36), wherein the peak scattering angle is less than or equal to 0.5° in the wavelength range of interest.
[0044] Aspect (38) of the present disclosure relates to a method according to any one of aspects (31)-(37), wherein the one or more etching masks include at least two etching masks such that the discrete height distribution includes at least 4 heights.
[0045] Aspect (39) of the present disclosure relates to a method according to aspect (38), wherein: after exposing the substrate to an etchant via a first etching mask, a second etching mask of at least two etching masks is disposed on a first main surface, and the second etching mask exposes an area of the first main surface etched via the first etching mask, so that the area is etched via both the first etching mask and the second etching mask.
[0046] Aspect (40) of the present disclosure relates to a method according to any one of aspects (31)-(39), wherein the pattern comprises a minimum feature size greater than or equal to 1 μm.
[0047] Aspect (41) of the present disclosure relates to a method according to any one of aspects (31) to (40), wherein the pattern is periodic in at least two directions that are perpendicular to each other.
[0048] It should be understood that both the foregoing general description and the following detailed description are merely illustrative and are intended to provide an overview or framework for understanding the nature and character of the claims. The accompanying drawings are included to provide a further understanding and are incorporated into and constitute a part of this specification. The drawings illustrate one or more embodiments and, together with the detailed description, serve to explain the principles and operation of the various embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate several aspects of the present invention and, together with the description, serve to explain the principles of the present invention. In the drawings:
[0050] Figure 1 depicts a perspective view of a display article according to one or more embodiments of the present disclosure;
[0051] Figure 2 Schematically depicting one or more embodiments of the present disclosure Figure 1 a plurality of regions of a diffractive surface area of the display article;
[0052] Figure 3 Schematically depicting one or more embodiments of the present disclosure Figure 2Height profile of the diffractive surface area depicted in;
[0053] Figure 4A a two-dimensional intensity graph depicting a Laguerre-Gaussian pattern according to one or more embodiments of the present disclosure;
[0054] Figure 4B Describes one or more embodiments of the present disclosure. Figure 4A One-dimensional intensity plot of the Laguerre-Gaussian pattern depicted in ;
[0055] Figure 5A depicts a calculated optimal specular suppression associated with a pattern of regions at multiple heights as a function of the number of heights in a discrete height distribution in accordance with one or more embodiments of the present disclosure;
[0056] Figure 5B depicts calculated optimal specular suppression associated with a pattern of regions at multiple heights for multiple discrete height distributions as a function of bandwidth of light in accordance with one or more embodiments of the present disclosure;
[0057] Figure 5C depicts calculated specular reflectance associated with a pattern of regions at multiple heights as a function of bandwidth of light for multiple discrete height distributions in accordance with one or more embodiments of the present disclosure;
[0058] Fig. 6A A flow chart depicting a method of identifying a pattern of multiple regions of a diffractive surface area according to one or more embodiments of the present disclosure;
[0059] Figure 6B Schematically depicts a method for implementing one or more embodiments of the present disclosure. Fig. 6A A computing system for the method described in;
[0060] Figure 7 A flow chart depicting a method of making a diffractive surface region of a display article according to one or more embodiments of the present disclosure;
[0061] Fig. 8A schematically depicts a pattern of a first etching mask for forming a plurality of regions in a diffractive surface region according to one or more embodiments of the present disclosure;
[0062] Figure 8B schematically depicts a pattern of a second etching mask for forming a plurality of regions in a diffractive surface region according to one or more embodiments of the present disclosure;
[0063] Fig. 9 Describes the use of one or more embodiments according to the present disclosure Fig. 8A and Figure 8B a plurality of calculated far-field scattering patterns of the diffraction region formed by the first mask and the second mask depicted in;
[0064] Fig. 10A Describes the use of one or more embodiments according to the present disclosure Fig. 8A and Fig. 9 A histogram of surface heights in a diffractive surface region formed by the first mask and the second mask depicted in B;
[0065] Fig. 10B Describes the use of one or more embodiments according to the present disclosure Fig. 8A and Figure 8B A graph of calculated reflectance and haze properties of a diffractive region formed by a first mask and a second mask depicted in FIG.
[0066] Fig.11A depicts a measured far-field scattering pattern associated with a first example article having a diffractive surface region according to one or more embodiments of the present disclosure;
[0067] Fig. 11B a graph depicting measured reflected intensity of a first example article according to one or more embodiments of the present disclosure; and
[0068] Fig. 11C Graph depicting azimuthally averaged scattered intensity at multiple wavelengths for a first example article according to one or more embodiments of the present disclosure. DETAILED DESCRIPTION
[0069] With general reference to the figures, display articles are described herein that include diffractive regions that are designed to significantly reduce specular reflections throughout the wavelength range of interest while still providing relatively low scattering intensities at high scattering angles. Such diffractive surface regions beneficially prevent noticeable reflected images from interfering with a user viewing experience of the display while still providing favorable image contrast characteristics. This favorable performance is achieved by structuring a major surface of the display article to include a plurality of regions, wherein each of the regions includes a region of the major surface that is disposed at a height relative to an imaginary reference plane. The plurality of regions are structured such that the heights associated with the regions form a discrete height distribution. The differences between the heights in the discrete height distribution are in the range of Within 5% of an integer multiple of The range of incident angles on the main surface over which the specular reflectivity is attempted to be reduced ( to ) and the wavelength range of interest (λ min To max )according to Defined as follows, where λ′min =λ min / cosθ min , and λ′ max =λ max / cosθ max The plurality of regions are arranged in a pattern identified based on a target far-field scattering pattern associated with a relatively low scattering amplitude at scattering angles above 2°. It has been discovered that, when so arranged, such a height distribution associated with the regions of the diffractive surface regions reduces specular reflectance by at least 10 times (e.g., at least 100 times, at least 1000 times) as compared to a non-textured article without the diffractive surface regions while providing advantageous haze performance.
[0070] As used herein, the term "specular reflectance" refers to the percentage of light reflected from an article at an angle of reflection equal to the light's angle of incidence.
[0071] As used herein, the term "haze" or "transmission haze" refers to the percentage of transmitted light scattered outside an approximately ±2.5° angular cone according to ASTM D1003, entitled "Standard Test Method for Haze and Luminous Transmittance of Transparent Plastics," the contents of which are incorporated herein by reference in their entirety. Note that while the title of ASTM D1003 refers to plastics, the standard is equally applicable to substrates including glass materials. For optically smooth surfaces, the transmission haze is approximately close to zero.
[0072] Reference now Figure 1 , a display article 10 is depicted according to an example embodiment. Display article 10 includes substrate 12. In an embodiment, display article 10 further includes housing 14 to which substrate 12 is coupled and display 16 within housing 14. In such embodiments, substrate 12 at least partially covers display 16 such that light emitted by display 16 can be transmitted through substrate 12.
[0073] Substrate 12 includes a first major surface 18, a second major surface 19, a diffractive surface region 20 defined on first major surface 18, and a thickness 21 partially bounded by first major surface 18 (e.g., representing the minimum distance between first major surface 18 and second major surface 19 at a particular point on first major surface 18). In the depicted embodiment, the shape of substrate 12 is generally planar, such that first major surface 18 and second major surface 19 are generally flat (except for the transition between heights of first major surface 18, as described herein). Embodiments in which substrate 12 includes a curved shape (e.g., via suitable hot forming and cold forming techniques) are also contemplated and within the scope of the present disclosure. First major surface 18 generally faces an external environment 24 surrounding display article 10 and faces away from display 16. In an embodiment, display 16 emits visible light, which is transmitted through thickness 22 of substrate 12, exits first major surface 18, and enters external environment 24.
[0074] The diffractive surface region 20 is structured to scatter light originating from the external environment 24 in a scattering pattern designed to suppress specular reflectivity while also having a scattering angle greater than or equal to 2.0° (e.g., greater than or equal to 2.5°, greater than or equal to 3.0°). In an embodiment, the diffractive surface region 20 is structured to have a far-field scattering pattern that is uniform over the entire wavelength range of interest [λ min ,λ max ], within the incident angle range The diffractive surface region 20 has a maximum scattering amplitude at a scattering angle of less than or equal to 2.0° (e.g., less than or equal to 1.5°, less than or equal to 1.0°, less than or equal to 0.9°, less than or equal to 0.8°, less than or equal to 0.7°, less than or equal to 0.6°, less than or equal to 0.5°). In an embodiment, the diffractive surface region 20 is structured to reduce the specular reflectivity by at least 10 times (e.g., at least 100 times, at least 1000 times, at least 1000 times) relative to a smooth, non-textured version of the first major surface 18. By reducing the specular reflectivity of the substrate 12 while controlling the scattering amplitude at relatively high scattering angles, the structure of the diffractive surface region 20 provides advantageous anti-glare and haze performance compared to certain existing display articles.
[0075] As used herein, when used to describe the specular reflectivity performance of the articles described herein, the term "non-textured version" refers to the specular reflectivity predicted using the Fresnel coefficients associated with the optically smooth surface of the material comprising substrate 12. For example, if substrate 12 is composed of a material having a refractive index n1 (e.g., glass or a suitable polymeric material) and the external environment includes a refractive index n2 (e.g., air), the specular reflectivity of the non-textured version of substrate 12 can be calculated using the following equation:
[0076]
[0077]
[0078] in is the angle of incidence on the first major surface 18, is the transmission angle immediately after the first major surface (determined using Snell's law), R s is the intensity reflectivity of s-polarized light, R p is the intensity reflectivity of p-polarized light.
[0079] Figure 2 Schematically depicting an example embodiment according to the present disclosure Figure 1 1 shows a plan view of region II of a diffractive surface region 20 of the display article 10. In an embodiment, within the diffractive surface region 20, the first major surface 18 includes a non-uniform structure such that the first major surface 18 includes a surface height deviation measured relative to an imaginary reference plane, the surface height deviation being greater than the maximum surface roughness value (e.g., Sa value) of a portion of the first major surface 18 extending within 2° parallel to the second major surface 19. The first major surface 18 includes a surface height deviation outside the range associated with the inherent roughness of the material forming the substrate 12. Due to such surface height deviations, within the diffractive surface region 20, the first major surface 18 includes a plurality of regions 22. Each of the plurality of regions 22 constitutes a portion of the first major surface 18 and extends substantially parallel to the second major surface 19, while it should be understood that each of the plurality of regions 22 may be tilted relative to the second major surface 19 due to the formation process for the plurality of regions 22 described herein. In an embodiment, each of the plurality of regions 22 represents a continuous portion of the first major surface 18 that does not include a surface height deviation outside the range associated with the surface roughness of the first major surface 18. Each of the plurality of regions 22 includes a portion of the first major surface 18 disposed at a common height relative to an imaginary reference plane extending through the substrate 12 (e.g., within a tolerance associated with a formation process). Each of the plurality of regions 22 is adjacent to at least one other region of the plurality of regions 22, the at least one other region including a portion of the first major surface 18 disposed at a height relative to the imaginary reference plane different from that of the region. Regions of the plurality of regions 22 that include the same height relative to the imaginary reference plane may be separated from each other by at least one other region of the plurality of regions disposed at a different height relative to the imaginary reference plane. The boundaries of each of the plurality of regions 22 are delineated by a contour at which an abrupt change in surface height (e.g., greater than 50 nm) is observed on the first major surface 18.
[0080] As described herein, the plurality of regions 22 forming the diffractive surface region 20 are arranged in a predetermined pattern, the predetermined pattern being calculated based on a target far-field scattering pattern exhibiting a low specular reflectivity amplitude for light incident on the first major surface 18 from the external environment 24 and a low scattering amplitude at a scattering angle greater than 2° (e.g., greater than 5°, greater than 10°). The predetermined pattern is generally not distinguishable via observation with the naked eye, but is identified via the method described herein using an optimization algorithm. The size and shape of the plurality of regions 22 may vary significantly across the diffractive surface region 20. For example, in an embodiment, the maximum linear dimension of the plurality of regions 22 (the length of the longest line segment connecting multiple portions of the perimeter of the region to each other without intersecting another portion of the perimeter) may vary from tens of micrometers to hundreds of micrometers.
[0081] Figure 3 Schematically depicting the passage Figure 2 Simplified cross-sectional view of the diffractive surface region 20 along line III-III depicted in FIG. Figure 3 The cross-sectional views depicted in are conceptual and simplified for discussion purposes and do not correspond to Figure 2 The actual pattern depicted in Figure 3 As shown, the plurality of regions 22 include portions of the first major surface 18 disposed at discrete height distributions measured relative to an imaginary reference plane 25 extending through the substrate 12 and parallel to the first major surface 18 (each region includes a portion of the first major surface 18 extending substantially parallel to the imaginary reference plane 25, thereby allowing for manufacturing tolerances). In an embodiment, the plurality of regions 22 include: a first plurality of regions 22a, wherein the first major surface 18 is disposed at a maximum height h max At maximum height h max is measured as a distance in a direction perpendicular to the imaginary reference plane 25; and a second plurality of regions 22b in which the first major surface 18 is disposed at a minimum height h min At minimum height h min is a distance measured in a direction perpendicular to an imaginary reference plane 25. The imaginary reference plane 25 is not a physical component of the substrate 12, but rather is an imaginary reference plane extending through the substrate 12. In an embodiment, the imaginary reference plane 25 extends through the geometric center of the substrate 12. In the depicted embodiment, the first plurality of regions 22a of the first major surface 18 represent points on the first major surface 18 that are disposed at a maximum distance from the imaginary reference plane 25, such that the thickness 21 has a maximum value when measured within the first plurality of regions 22a. Each of the first plurality of regions 22a may be related to h max There is a slight deviation. In the embodiment, h max represents the average measured height of the first plurality of regions 22a and the height of each of the first plurality of regions 22a is within h maxThe same is true for other heights in the discrete height distribution.
[0082] In an embodiment, the discrete height distribution at which the first major surface 18 is located relative to the imaginary reference plane 25 may include any number of heights (e.g., 2 heights, 3 heights, 4 heights, 5 heights, 6 heights, 7 heights, 8 heights, 9 heights, 10 heights, or even a greater number of heights). In an embodiment, the plurality of regions 22 include: a third plurality of regions 22c, in which the first major surface 18 is disposed at a height h1 relative to the imaginary reference plane 25; and a fourth plurality of regions 22d, in which the first major surface 18 is disposed at a height h2 relative to the imaginary reference plane 25. The heights in the discrete height distribution are evenly spaced such that the difference between adjacent heights is within a spacing constant (e.g., h max -h2=h2–h1=h1-h min ). The heights in the discrete height distribution may differ from each other by an integer multiple of the spacing constant. Values of the spacing constant, which can be used to achieve favorable anti-glare and haze performance attributes, are described in more detail herein.
[0083] like Figure 3 As shown, the plurality of regions 22 of the first major surface 18 are separated from each other by transition surfaces 26 of the substrate 12. The transition surfaces 26 represent portions of the outer surface of the substrate 12 that extend at a large angle (e.g., greater than 20°) relative to the imaginary reference plane 25. The transition surfaces 26 represent points where the surface height of the first major surface 18 deviates from a range associated with the surface roughness of the first major surface 18. The length of each of the transition surfaces 26 depends on the pattern of the plurality of regions 22 (i.e., which heights in the discrete height distributions are disposed adjacent to each other). In an embodiment, at least some of the transition surfaces 26 extend perpendicular to (or within 10° of perpendicular to) the imaginary reference plane 25. Such transition surfaces 26 extending perpendicular to the imaginary reference plane 25 may have differences (e.g., h < 0.05) between the heights corresponding to the discrete height distributions. max -h min 、h max -h2,h max -h1) length.
[0084] As will be appreciated, due to manufacturing tolerances, each region of the first plurality of regions 22a may be disposed at a position approximately equal to h. max At a slightly different height, each of the second plurality of regions 22 may be disposed at a height corresponding to h min Each of the third plurality of regions 22c may be disposed at a height slightly different from h1, and each of the fourth plurality of regions 22d may be disposed at a height slightly different from h2. max 、h min, h1, and h2 may represent manufacturing targets for forming the diffractive surface region 20 using any of the methods described herein. In an embodiment, each of the first plurality of regions 22a, the second plurality of regions 22b, the third plurality of regions 22c, and the fourth plurality of regions 22d is disposed at a height within 5% of its target value. In an embodiment, if the average surface height of each of the first plurality of regions 22a, the second plurality of regions 22b, the third plurality of regions 22c, and the fourth plurality of regions 22d is measured, and each group of average values associated with each height in the discrete height distribution is averaged, the average value of each group may be within 5% of the manufacturing target value. In an embodiment, such average values of each group may differ from each other within 5% of an integer multiple of a spacing constant that establishes the height spacing described herein.
[0085] In an embodiment, the combined surface area of each of the plurality of regions 22 at each height in the discrete height distribution occupies a predetermined combined surface area percentage of the diffractive surface area 20. In the depicted example, the first plurality of regions 22a occupies a first combined surface area percentage of the diffractive surface area 20, the second plurality of regions 22b occupies a second combined surface area percentage of the diffractive surface area 20, the third plurality of regions 22c occupies a third combined surface area percentage of the diffractive surface area 20, and the fourth plurality of regions 22d occupies a fourth combined surface percentage of the diffractive surface area 20. In an embodiment, the first combined surface area percentage is within 5% of the second combined surface area percentage, and the third combined surface area percentage is within 5% of the fourth combined surface area percentage. In an embodiment, the second combined surface area percentage and the third combined surface area percentage are greater than the first combined surface area percentage or the second combined surface area percentage. In an embodiment, each of the first combined surface area percentage, the second combined surface area percentage, the third combined surface area percentage, and the fourth combined surface area percentage is less than 40%.
[0086] The pattern in which the plurality of regions 22 are arranged and the combined surface area percentages associated with each height in the discrete height distribution may be determined using scalar diffraction theory and a suitable optimization algorithm, as described herein. Figure 3 As shown, the incident radiation from the external environment 24 can be approximated as a uniform plane wave, which is approximately
[0087]
[0088] where I0 represents the uniform intensity of the incident radiation, and k x0 and k y0 represents the wave vector associated with the wavelength of the radiation and the angle of incidence on the first major surface 18 (for example, the angle of incidence can be decomposed into components in the x and y directions, such as Figure 1In this case, the scalar near field of the outgoing radiation (after interacting with the first major surface 18) can be approximated by
[0089] u near (x,y)=ρu0(x,y)·e iφ(x,y) (4)
[0090] where ρ is the Fresnel coefficient of the interface (polarization of the incident radiation, calculated using Equation 1 or Equation 2), and is the local phase accumulated via a dual channel at a distance H(x, y) from the first major surface 18, where H(x, y) represents the pattern in which the plurality of regions 22 are arranged (H(x, y) represents the local phase at a height h max The height distribution measured by the imaginary plane 28 extending at and parallel to the imaginary reference plane 25, but with respect to the height h max 、h min , h1 and h2 are related). In this example, the incident radiation is approximated to have a uniform intensity distribution, and the interface between the substrate 12 and the external environment 24 is approximated to apply only a spatially varying phase, so that the outgoing radiation in the near field also has a uniform intensity distribution.
[0091] exist Figure 3 In this example depicted in , the far-field scattering pattern associated with the outgoing radiation can be represented in reciprocal k-space and, via Fourier transformation, compared to the near-field u calculated using Equation 4 near (x,y) is related and is expressed as
[0092]
[0093] In an embodiment, the pattern in which the plurality of regions 22 are arranged is selected so that H(x, y) approximately matches a target far-field distribution when input into Equation 5. In an embodiment, the target far-field distribution is selected to provide a relatively low level of specular reflection and a low scattering amplitude at angles greater than 2.0°. A set of target far-field distributions can be mathematically described by a Laguerre-Gaussian ("LG") pattern, represented as
[0094]
[0095] Where l is the azimuth index, k max is the wave number associated with the maximum scattering intensity, and c l is a normalization factor. The LG mode advantageously provides (l-1 th ) order zero, where larger values of l are associated with a flatter distribution of the scattering amplitude at about the specular reflectivity. The LG mode also decays beneficially exponentially at large wave numbers (associated with large scattering angles).
[0096] Figure 4A and Figure 4B An example LG mode scattering distribution with azimuthal index l equal to 2 is depicted in FIG. Figure 4A Depicts the two-dimensional scattering function, and Figure 4B Draw through line k y A graphical view of the scattering amplitude at k0 = 0 (representing the scattering amplitude when the incident radiation is incident on a single incident plane at different incident angles). As shown, the scattering pattern provides very low specular reflection, with the scattering maximum occurring at k0 = 0. X / k0=0.008, corresponding to a maximum scattering angle of 0.5 degrees. Although the LG pattern is one possible target far-field scattering distribution, it should be understood that a variety of target far-field scattering distributions are contemplated and within the scope of the present disclosure. The target far-field scattering distribution can be used in a suitable optimization algorithm to determine the pattern of the plurality of regions 22, as described herein.
[0097] In an embodiment, the target of reducing specular reflection occurs at a wavelength greater than or equal to the minimum wavelength of interest λ min and is less than or equal to the maximum wavelength λ of interest max The wavelength range of interest. min and λ max can vary depending on the application. For example, one application may aim to minimize specular reflectance in the visible to near-infrared range so that λ min =380nm and λ max = 1200 nm. In another example, it may be desirable to limit the specular reflectivity only within the visible spectrum, so that λ min =380nm and λ max = 730 nm. Any suitable wavelength range of interest may be used.
[0098] In an embodiment, the target of reducing specular reflection occurs at various incident angles θ i (See Figure 3 ). That is, for a specific display application, over a wide range of incident angles θ i It may be advantageous to provide an anti-glare function within the display to prevent the reflected image from being noticed by the user from a variety of different angles. For example, in an embodiment, it may be desirable to have a range of θ min to θ max In an embodiment, θ min =0°, 5°, 10° or 20°. In an embodiment, θ max =70°, 60°, 50°, 45°, 40°, 35° or 30°. Given the above, the goal of reducing the specular reflectivity can be understood as min ,λ max ], in the range [θ min ,θmax ] (square brackets indicate the boundaries of the inclusive range) to minimize specular reflection at multiple incident angles. This problem can be simplified in inverse k space to minimize k′ min and k′ max That is, the goal of minimizing the specular reflectivity can be understood as minimizing k′ min and k′ max The specular reflectivity between and
[0099] refer to Figure 3 , each height h in the height distribution of the plurality of regions 22 i The combined surface area percentage can be expressed as the value A j , where j is a reference integer. Constraints can also be provided The plurality of regions 22 occupy 100% of the surface area of the first major surface 18 in the diffractive surface region 20. In such a case, and in view of equations 3-5, it can be determined that the goal of minimizing the specular reflectivity can be mathematically expressed as minimizing a function proportional to f(A, h), expressed as
[0100]
[0101] Among them A j and h j is a free parameter in the optimization, and g(k) is the spectral weight function. In an embodiment, g(k)=k -1 , so that g(k)dk = d(log(k)), corresponding to the entire wavelength range of interest [λ min ,λ max ] and the incident angle range [θ min ,θ max ] uniformly samples k on an intrinsic logarithmic scale. In this case, under the constraint It can be shown that Equation 7 has an analytical solution
[0102]
[0103] where h0 is a constant, and is λ′ min and λ′ max The harmonic mean of
[0104]
[0105] where λ′ min =λ min / cosθ min , and λ′ max =λmax / cosθ max Therefore, in the embodiments, as described above with respect to Figure 3 As described above, the difference between the heights in the discrete height distributions of the plurality of regions 22 in the diffractive surface region 20 is ideally The manufacturing method used to form the plurality of regions 22 may result in the actual heights of the plurality of regions being slightly different from the heights calculated using equations 8-9. Thus, the differences between the heights in the discrete height distributions may differ from each other by Therefore, Figure 3 In the example depicted in and
[0106] Refer to equations 7-9, and for each height h j The associated ideal combined surface area percentage A j Satisfies the linear equation system represented by the following matrix equation
[0107] FA=1 (10)
[0108] Where A is the ideal area A j , 1 is an identity column vector with N elements (N corresponds to the number of heights in the discrete height distribution), and F is an NxN matrix, each element in F is calculated as
[0109]
[0110] Use equations 10-11 to calculate each height h calculated using equation (9) j The ideal combined surface area percentage A j , the optimal local phase accumulation function can be calculated This function is used for the wavelength range of interest [λ min ,λ max ] and the incident angle range [θ min ,θ max ], for λ min , max ,θ min and θ max . minimizes the specular reflection (determined using Equations 4 and 5). min =400nm,λ max =800nm,θ min = 0°, and θ max = 60°, λ′ can be calculated min ,λ′ max and substitute it into Equation 9 to calculate = 150 nm. Use in Equation 11 With this value, the area vector A can be calculated as (0.178, 0.322, 0.322, 0.178), with the first value corresponding to λ min The second and third values are at heights h1 and h2, respectively, and the fourth value is at height h max Place.
[0111] Figure 5A , Figure 5B and Figure 5C Plotting the wavelengths of interest for a number of different wavelength ranges (expressed in octave units as = log2(λ max / λ min )), ideal specular reflection and reduction calculated for a plurality of height distributions for a plurality of regions 22 (compared to a non-textured version of first major surface 18) (each distribution containing a different number of heights). Figure 5B As shown, for the wavelength range of interest from 400 nm to 800 nm (corresponding to 1 octave), two discrete heights reduce the specular reflection by about 10 dB, while four discrete heights reduce the specular reflection by about 30 dB compared to the non-textured version. Figure 5C As shown, over the wavelength range of interest of 400 nm to 800 nm, two discrete heights provide a specular reflectance of slightly less than 1%, while four discrete heights provide a specular reflectance of less than 0.01%. The results of this analysis are summarized in Table 1 below, which provides the reduction in specular reflectance (in dB) compared to a non-textured version of first major surface 18 for various wavelength ranges of interest (values represent the average reduction over the wavelength range of interest).
[0112] Table 1
[0113]
[0114] Table 1 can provide guidance in determining the number of levels that may be required for a particular application, depending on the level of specular reflectivity reduction desired and the applicable wavelength range of interest. In general, a greater bandwidth associated with the wavelength range of interest will increase the number of levels required to achieve a particular amount of reflectivity reduction relative to the reflectivity from a non-textured surface.
[0115] Fig. 6A Flowchart depicting a method 600 of determining a pattern of a plurality of regions of a diffractive surface region according to an example embodiment of the present disclosure. Figure 6BMethod 600 is performed on a computer system 1000 depicted in . In an embodiment, computer system 1000 includes a processing circuit or processor 1002, a main memory 1004 (e.g., read-only memory (ROM), flash memory, dynamic random-access memory (DRAM), such as synchronous DRAM (SDRAM), etc.), and a static memory 1006 (e.g., flash memory, static random-access memory (SRAM), etc.), and the processing circuit or processor and the main memory can communicate with each other via a data bus 1008. Alternatively, processor 1002 can be connected to main memory 1004 and / or static memory 1006 directly or via some other connection means. Computer system 1000 can further include a network interface device 1010. Computer system 1000 can also include an input 1012, which is configured to receive inputs and selections to be transmitted to computer system 1000 when executing instructions. The computer system 1000 may also include outputs 1014, including but not limited to a display, a video display unit (e.g., a liquid crystal display (LCD) or a cathode ray tube (CRT)), an alphanumeric input device (e.g., a keyboard), and / or a cursor control device (e.g., a mouse). The computer system 1000 may also include instructions 1016, which are stored in a computer-readable medium 1018 and / or reside in the main memory 1004 and / or in the processor 1002 during execution by the computer system 1000, the main memory 1004 and the processor 1002 also constituting computer-readable media. The instructions 1016 may further be transmitted or received over the network 1020 via the network interface device 1010. A user may use the computer system to perform the method 600 by providing input via the input 1010 and causing execution of the following processing steps encoded in the instructions 1016 via the processor 1002.
[0116] In an embodiment, method 600 can be used to design various display articles. For example, method 600 can be used to design Figures 1 to 3 The diffractive surface region 20 of the display article 10 is described. Therefore, reference will be made to Figures 1 to 3 The various features depicted in the drawings are used to help describe method 600, with the understanding that the method can be used to design other display articles.
[0117] refer to Fig. 6AAt block 602, a discrete height distribution of the diffractive surface region 20 is identified. In an embodiment, for example, a user may identify a suitable wavelength range of interest [λ min ,λ max ] and the range of incident angles Such values may vary depending on the application. For example, a display article 10 implemented in a television or computer monitor may attempt to reduce specular reflectivity over a different range of incident angles than a display article 10 implemented in an interior automotive display. Once the wavelength range of interest [λ min ,λ max ] and the range of incident angles Once identified and input into the computer system 1000 (eg, via input 1012), the computer system 1000 may execute instructions 1016 that calculate a plurality of graphs, such as those described herein. FIG. 5A to FIG. 5C The diagram depicted in FIG. 1 shows the wavelength range of interest [λ min ,λ max ] and the range of incident angles In one embodiment, the user may select the number of heights based on the indicated specular reflectance reduction performance. In one embodiment, instructions 1016 cause processor 1002 to automatically select the number of levels based on the specular reflectance performance requirements input by the user (e.g., the user may indicate a maximum allowable specular reflectance). The heights in the discrete height distribution are determined via equations (7)-(9) described herein.
[0118] At block 604, an ideal surface area percentage for each height in the discrete height distribution is identified. The ideal surface area percentage may be calculated via equations 10 and 11 described herein. At block 606, an ideal target scattering pattern is identified. In an embodiment, a user may select an ideal target scattering pattern. It can vary depending on the application. For example, the user can define the appropriate orientation index l and k as described in this article with respect to equation 6 max Parameters are used to define suitable LG modes. Other suitable ideal scattering patterns may be used.
[0119] At block 608, an initial pattern of the plurality of regions 22 is generated. In an embodiment, instructions 1016 start the optimization algorithm by inputting a pre-stored initial pattern. It has been determined that the initial pattern does not have a significant impact on the final result of the optimization, so any suitable random pattern of the plurality of regions 22 may be used. Once the initial pattern is generated, instructions 1016 may cause processor 1002 to estimate the far-field scattering pattern u(λ) of the initial pattern. For example, the initial pattern may be used to define the local phase accumulation function in equations 4 and 5 And the estimated far-field scattering pattern u(λ) is calculated.
[0120] At block 610, an optimization algorithm is used to update the initial pattern to minimize a suitable objective function. As described herein, the discrete height distribution and the ideal surface area percentage associated with each height can be based on the wavelength range of interest [λ min ,λ max ] and the incident angle range [θ min ,θ max By comparing the estimated far-field scattering pattern u(λ) with the ideal target scattering pattern By comparison, an objective may be incorporated that provides a relatively low scattering amplitude at high scattering angles (e.g., greater than or equal to 2.0°, greater than or equal to 2.5°, greater than or equal to 3.0°, greater than or equal to 3.5°, greater than or equal to 4.0°, greater than or equal to 4.5°, greater than or equal to 5.0°, or even greater angles). Thus, the objective function may include a scattering term that compares the estimated far-field scattering pattern u(λ) to the ideal target scattering pattern and an area term that compares the actual combined surface area percentage associated with each height in the initial pattern to the ideal value A calculated herein using equations 10-11 j Make a comparison.
[0121] In an embodiment, a suitable objective function can be expressed as
[0122]
[0123] where K is the wavelength range of interest [λ′ min ,λ′ max ] integer value to sample (e.g., the wavelength range of interest [λ min ,λ max ] can be uniformly discretized using integer values of K), i and j are integer values that uniformly sample the range of scattering angles, w is an area weighting factor (determines the weight placed on the pattern that approximates the ideal combined surface area percentage calculated using equations 10-11), A i is the combined surface area percentage of one of the heights in the discrete height distribution associated with the initial pattern, and is the ideal combined surface area percentage associated with that height. It has been found that the value of w can vary depending on the specific application. A value of w of about 10 corresponds roughly to equal weighting of each term in equation 12 and has been found to be a good starting point.
[0124] The initial pattern may be updated using a suitable nonlinear function optimization algorithm, wherein the values of the objective function in each iteration are compared with each other, so that the initial pattern is updated by performing multiple iterations on a converged solution that minimizes the objective function, so that the estimated far-field scattering pattern u(λ) approximates the ideal target far-field scattering pattern And the combined surface area percentage associated with each height in the discrete height distribution is close to the ideal value calculated using equations 10-11. Any suitable optimization algorithm can be used. Some examples are Newton conjugate gradient (Newton CG), Broyden-Fletcher-Goldfarb-Shannon (Broyden-Fletcher-Goldfarb-Shannon, BFGS) algorithm and Sequential Least Squares Programming (SLSQP).
[0125] Reference again Figures 1 to 3 The plurality of regions 22 in first major surface 18 may be formed using any suitable technique. Figure 7 A flowchart depicting an example method 700 of manufacturing a display article 10 according to an example embodiment of the present disclosure will be referred to. Figures 1 to 3 The various components depicted in FIG. 7 are used to help describe method 700. It should be understood that the specific method used to form the diffractive surface region 20 is not particularly limited and any suitable method may be used.
[0126] At block 702, a pattern of a plurality of regions 22 is determined. In an embodiment, the pattern is determined by Fig. 6A The method 600 described is determined. At box 704, a resist is disposed on the first major surface 18 and patterned. The properties of the deposition and patterning of the resist may vary according to the manufacturing technology used. In an embodiment, various nanoimprint or lithography techniques may be used to deposit and pattern the resist layer. In such embodiments, the minimum feature size (e.g., minimum linear dimension) associated with a plurality of regions 22 may be set to at least 1 μm (e.g., greater than or equal to 1.5 μm, greater than or equal to 2.0 μm, greater than or equal to 2.5 μm, greater than or equal to 5.0 μm, greater than or equal to 10 μm) to facilitate the use of existing resist coating and patterning techniques. In an embodiment, for example, the resist may be formed using thermoplastic nanoimprint lithography, and the resist may be formed of a thermoplastic polymer, the polymer may be spin-coated onto the substrate 12 and then embossed via a mold to form a first pattern, the first pattern at least partially corresponding to the pattern of the plurality of regions 22 on the first major surface 18. The resist may then be thermally cured to form an etching mask. Other methods of forming the resist (eg, gravure lithography, other printing techniques) are also contemplated and within the scope of the present disclosure.
[0127] Photolithography (e.g., photoimprint nanolithography, optical lithography) techniques may also be used, and the resist may be deposited onto the first major surface 18 via a suitable coating method (e.g., spin coating). In such embodiments, a mask comprising a first pattern is aligned with the first major surface 18, the first pattern at least partially corresponding to the pattern determined for the plurality of regions 22, and the resist may be exposed to radiation from a suitable light source (e.g., UV radiation) to cause the resist to cure and form an etching mask. The resist may then be developed so that portions of the first major surface 18 are exposed through the cured resist. Any suitable photolithography technique may be used to pattern the resist. In embodiments, the pattern formed in the resist may be such that the areas of the first major surface 18 covered by the resist form a pattern with respect to the first major surface 18. Figure 3 The described setting is at height h max At least some of the first plurality of regions 22a at.
[0128] At frame 706, the exposed area of the first major surface 18 (via the cured and patterned resist) is exposed to a suitable etchant for a suitable etchant cycle determined based on the target etching depth. Each area of the first major surface 18 exposed via the patterned resist formed in frame 704 can be directly contacted with the etchant, which can degrade the substrate and remove material from it to form an area at a reduced height relative to the imaginary reference plane 25 on the first major surface 18 compared to the area of the first major surface 18 covered by the patterned resist. In an embodiment, the etchant contacting the first major surface 18 is a HF / HNO3 etchant. In an embodiment, the etchant is composed of a combination of hydrofluoric acid (HF, 49w / w%) and nitric acid (HNO3, 69w / w%), which has 0.1-5v / v% of HF and 0.1-5v / v% of HNO3. Typical concentrations for achieving the etch depths discussed herein are 0.1 v / v% HF / 1 v / v% HNO3 to 0.5 v / v% HF / 1 v / v% HNO3 solutions. In embodiments, etching may be performed using a dip or spray etching process at room temperature to about 45°C.
[0129] At decision block 708, a determination is made as to whether the target height distribution is achieved. As can be appreciated, it may be desirable for the plurality of regions 22 to be disposed at more than two heights relative to the imaginary reference plane 25. In an embodiment, forming the diffractive surface region 20 having regions disposed at more than two heights relative to the imaginary reference plane 25 may include multiple etching steps utilizing different etching masks and different etching cycles. For example, in an embodiment, an initial etching step is performed utilizing an initial etching mask and an initial etching cycle, the initial etching cycle being determined to etch a portion of the first major surface 18 to a depth of After this etching step (and additional steps such as cleaning), a second resist may be disposed on first major surface 18 and patterned for etching for a second etching cycle. The second resist may expose portions of first major surface 18 that were already etched in the initial etching step. The second resist may also expose portions of first major surface 18 that were not etched in the initial etching step (due to being covered by the initial etching mask). The second etching cycle may be determined to achieve an etching depth of Therefore, as a result, the area of the first main surface 18 that contacts the etchant in both etching steps can be etched to a total height of The areas that are exposed to the etchant only in the first etching step can be etched only to a height of Only the area exposed to the etchant in the second etching step can be etched only to a height of And the areas of the first major surface 18 that are covered by the resist in both the first and second etching steps may not be modified. This example provides a way to achieve four discrete heights in the first major surface 18. Any suitable combination of etching steps may be used, and a variety of different orders are contemplated and within the scope of the present disclosure.
[0130] Thus, the resists disposed on the first major surface 18 and patterned during the method 700 may not (individually) correspond precisely to the desired final pattern of the plurality of regions. Rather, the pattern associated with each resist may be an intermediate pattern designed to form the final pattern in conjunction with the pattern of any other etch mask that may be formed on the substrate 12 via the method 600 described herein. Blocks 704, 706, and 708 may be repeated until the desired number of heights in the discrete height distribution is achieved in the desired pattern, at which point the method 700 may end or additional processing steps (e.g., chemical strengthening) may be performed on the substrate 12.
[0131] Substrate properties
[0132] Various properties of substrate 12 will now be described according to embodiments of the present disclosure.
[0133] In an embodiment, the substrate 12 is a glass substrate or a glass ceramic substrate. In an embodiment, the substrate 12 is a multi-component glass composition having about 40 mol % to 80 mol % of silicon dioxide and the remaining one or more other components (e.g., aluminum oxide, calcium oxide, sodium oxide, boron oxide, etc.). In some embodiments, the main composition of the substrate 12 is selected from the group consisting of aluminosilicate glass, borosilicate glass and phosphosilicate glass. In other embodiments, the main composition of the substrate 12 is selected from the group consisting of aluminosilicate glass, borosilicate glass, phosphosilicate glass, soda-lime glass, alkali aluminosilicate glass and alkali aluminoborosilicate glass. In another embodiment, the substrate 12 is a glass-based substrate, including but not limited to glass ceramic materials including about 90% or more of a glass component and a ceramic component by weight. In other embodiments of the display article 10, the substrate 12 may be a polymer material having durability and mechanical properties suitable for producing and maintaining a diffractive surface region 20.
[0134] In an embodiment, substrate 12 has a host composition including an alkali aluminosilicate glass, which includes aluminum oxide, at least one alkali metal, and in some embodiments includes greater than 50 mol% SiO2, in other embodiments includes at least 58 mol% SiO2, and in other embodiments includes at least 60 mol% SiO2, wherein the ratio (Al2O3 (mol%) + B2O3 (mol%)) / ∑alkali metal modifier (mol%)>1, wherein the modifier is an alkali metal oxide. In particular embodiments, the glass comprises, consists essentially of, or consists of: about 58 mol % to about 72 mol % SiO2; about 9 mol % to about 17 mol % Al2O3; about 2 mol % to about 12 mol % B2O3; about 8 mol % to about 16 mol % Na2O; and 0 mol % to about 4 mol % K2O, wherein the ratio (Al2O3 (mol %) + B2O3 (mol %)) / ∑ alkali metal modifier (mol %)>1, wherein the modifier is an alkali metal oxide.
[0135] In an embodiment, substrate 12 has a bulk composition including an alkali aluminosilicate glass comprising, consisting essentially of, or consisting of: about 61 mol % to about 75 mol % SiO2; about 7 mol % to about 15 mol % Al2O3; 0 mol % to about 12 mol % B2O3; about 9 mol % to about 21 mol % Na2O; 0 mol % to about 4 mol % K2O; 0 mol % to about 7 mol % MgO; and 0 mol % to about 3 mol % CaO.
[0136] In an embodiment, substrate 12 has a bulk composition including an alkali aluminosilicate glass comprising, consisting essentially of, or consisting of: about 60 mol % to about 70 mol % SiO2; about 6 mol % to about 14 mol % Al2O3; 0 mol % to about 15 mol % B2O3; 0 mol % to about 15 mol % Li2O; 0 mol % to about 20 mol % Na2O; 0 mol % to about 10 mol % Na2O; % K2O; 0 mol % to about 8 mol % MgO; 0 mol % to about 10 mol % CaO; 0 mol % to about 5 mol % ZrO2; 0 mol % to about 1 mol % SnO2; 0 mol % to about 1 mol % CeO2; less than about 50 ppm As2O3; and less than about 50 ppm Sb2O3; wherein 12 mol %≦Li2O+Na2O+K2O≦20 mol % and 0 mol %≦MgO+Ca≦10 mol %.
[0137] In an embodiment, substrate 12 has a bulk composition including an alkali aluminosilicate glass comprising, consisting essentially of, or consisting of: about 64 mol % to about 68 mol % SiO2; about 12 mol % to about 16 mol % Na2O; about 8 mol % to about 12 mol % Al2O3; 0 mol % to about 3 mol % B2O3; about 2 mol % to about 5 mol % K2O; about 4 mol % to about 6 mol % MgO; and 0 mol% to about 5 mol% CaO, wherein: 66 mol% ≤ SiO2+B2O3+CaO ≤ 69 mol%; Na2O+K2O+B2O3+MgO+CaO+SrO>10 mol%; 5 mol% ≤ MgO+CaO+SrO ≤ 8 mol%; (Na2O+B2O3)-Al2O3 ≤ 2 mol%; 2 mol% ≤ Na2O-Al2O3 ≤ 6 mol%; and 4 mol% ≤ (Na2O+K2O)-Al2O3 ≤ 10 mol%.
[0138] In an embodiment, the substrate 12 has a host composition including SiO2, Al2O3, P2O5 and at least one alkali metal oxide (R2O), wherein 0.75>[(P2O5 (mol%) + R2O (mol%)) / M2O3 (mol%)]≦1.2, wherein M2O3=AbO3+B2O3. In an embodiment, [(P2O5 (mol%) + R2O (mol%)) / M2O3 (mol%)]=1, and in an embodiment, the glass does not include B2O3 and M2O3=Al2O3. In an embodiment, the substrate 12 includes: about 40 to about 70 mol% SiO2; 0 to about 28 mol% B2O3; about 0 to about 28 mol% Al2O3; about 1 mol% to about 14 mol% P2O5; and about 12 mol% to about 16 mol% R2O. In some embodiments, the glass substrate includes: about 40 to about 64 mol% SiO2; 0 to about 8 mol% B2O3; about 16 to about 28 mol% Al2O3; about 2 to about 12 mol% P2O5; and about 12 to about 16 mol% R2O. The substrate 12 may further include at least one alkaline earth metal oxide, such as, but not limited to, MgO or CaO.
[0139] In some embodiments, substrate 12 has a host composition that is substantially free of lithium; that is, the glass includes less than 1 mol% Li2O, and in other embodiments less than 0.1 mol% Li2O, and in other embodiments 0.01 mol% Li2O, and in still other embodiments 0 mol% Li2O. In some embodiments, such glass is free of at least one of arsenic, antimony, and barium; that is, the glass includes less than 1 mol%, and in other embodiments less than 0.1 mol%, and in still other embodiments 0 mol% As2O3, Sb2O3, and / or BaO.
[0140] In an embodiment, substrate 12 has a bulk composition comprising, consisting essentially of, or consisting of a glass composition, such as Glass, Glass, Glass 2, Glass 3, Glass 4 or Glass 5.
[0141] In an embodiment, the substrate 12 has an ion-exchangeable glass composition that is strengthened by chemical or thermal means known in the art. In an embodiment, the substrate 12 is chemically strengthened by ion exchange. In this process, metal ions at or near the first major surface 18 of the substrate 12 are exchanged for larger metal ions having the same valence as the metal ions in the glass substrate. The exchange is typically performed by contacting the substrate 12 with an ion exchange medium, such as a molten salt bath containing the larger metal ions. The metal ions are typically monovalent metal ions, such as alkali metal ions. In one non-limiting example, chemical strengthening of a substrate 12 containing sodium ions by ion exchange is accomplished by immersing the substrate 12 in an ion exchange bath including a molten potassium salt such as potassium nitrate (KNO3). In a specific embodiment, the ions and larger ions in the surface layer of the substrate 12 adjacent to the first major surface 18 are monovalent alkali metal cations, such as Li + (when present in glass), Na + , K + , Rb + and Cs + Alternatively, the monovalent cations in the surface layer of the substrate 12 may be replaced by monovalent cations other than alkali metal cations, such as Ag. + wait.
[0142] In such embodiments, the replacement of smaller metal ions with larger metal ions during the ion exchange process creates a compressively stressed region in substrate 12 that is compressively stressed, extending from first major surface 18 to a depth (referred to as the "depth of layer"). This compressive stress in substrate 12 is balanced by a tensile stress (referred to as the "central tension") within substrate 12. In some embodiments, first major surface 18 of substrate 12 described herein has a compressive stress of at least 350 MPa when strengthened by ion exchange, and the compressively stressed region extends into thickness 22 to a depth of at least 15 μm below first major surface 18, i.e., the depth of layer.
[0143] The ion exchange process is typically performed by immersing the substrate 12 in a molten salt bath containing larger ions to be exchanged with smaller ions in the glass. Those skilled in the art will appreciate that the parameters for the ion exchange process, including but not limited to bath composition and temperature, immersion time, number of immersions of the glass in one or more salt baths, use of multiple salt baths, additional steps (such as annealing, cleaning, etc.), are typically determined by the composition of the glass and the desired layer depth and the compressive stress of the glass caused by the strengthening operation. For example, ion exchange of alkali-containing glass can be achieved by immersing in at least one molten bath containing salts of larger alkali metal ions (such as, but not limited to, nitrates, sulfates, and chlorides). The temperature of the molten salt bath is typically in the range of about 380° C. to about 450° C., and the immersion time is in the range of about 15 minutes to about 16 hours. However, temperatures and immersion times different from the above temperatures and immersion times may also be used. Such ion exchange treatment, when used with a substrate 12 having an alkali aluminosilicate glass composition, produces a compressive stress region having a depth (depth of layer) ranging from about 10 μm to at least 50 μm, a compressive stress ranging from about 200 MPa to about 800 MPa, and a central tension less than about 100 MPa.
[0144] Because the etching process that can be used to produce the diffractive surface region 20 of the substrate 12 can remove alkali metal ions from the substrate 12 that would otherwise be replaced by larger alkali metal ions during the ion exchange process, there is a preference for producing compressive stress regions in the display article 10 after forming and producing the diffractive surface region 20.
[0145] Example
[0146] Embodiments of the present disclosure may be further understood in view of the following examples.
[0147] In a first example, the methods described herein were performed on a 2.048 mm x 2.048 mm sample having 4 discrete heights within a design wavelength range of 400 nm to 800 nm. Fig. 6A The process described in the previous section is described in detail. Only normal incidence angles are considered in this case. The etch height is determined using equations 8-9 in this article, and the ideal combined surface area percentage is determined using equations 10-11. Equation 12 is minimized using a suitable optimization algorithm, the target scattering pattern is the LG mode with l=2 and the weighting parameter w is set to 10.
[0148] Fig. 8A and Figure 8B Shows the pattern of the etch mask and the associated etch depth. Fig. 8A Depicted in this example is the first etch depth used FIG. 8 is a plan view of a first etching mask 800 . Figure 8B Depict the depth for the second etch 800 and the second etching mask 802. As shown, the first etching mask 800 and the second etching mask 802 both include worm structures having relatively large continuous areas at the same level (e.g., having a maximum linear dimension of about several hundred microns). The first etching mask 800 and the second etching mask 802 also both include enclosing regions 804, 806, 808, and 810, which are relatively small areas (having a maximum linear dimension of about several tens of microns) that are completely surrounded by multiple areas etched to different levels. The bright areas of each of the first etching mask 800 and the second etching mask 802 (corresponding to areas of the substrate that are not etched during their associated etching steps) may overlap with each other to form a maximum height h relative to an imaginary reference plane. max or overlaps with other dark areas of the etching mask to form Figure 3 The dark regions in each of the first etching mask 800 and the second etching mask 802 (corresponding to the regions of the substrate that are etched to the target etching depth during their associated etching steps) may also overlap with each other to form Figure 3 The minimum height h min area.
[0149] It can be shown that the methods described herein produce a periodic etch pattern (in both the x-direction and the y-direction) such that Fig. 8A and Figure 8B The pattern depicted in can be tiled to cover a larger area. In an embodiment, the minimum tile size associated with the etch mask may be 2 mm 500 μm to allow design flexibility to find a suitable pattern and prevent any visible scattered intensity non-uniformity due to the periodic nature of the pattern.
[0150] Fig. 9 The calculated far-field scattering patterns for several wavelengths within the wavelength range of interest for this example are depicted. All scattering patterns exhibit a characteristic "donut shape" and are very similar to the LG mode with l = 2. The peak scattering angle of the scattering pattern is 0.25°, indicating that the scattering pattern results in relatively low haze.
[0151] Fig. 10A A histogram depicting the etch depth (representing the height h described herein) j The frequency of each of the heights is very consistent with the ideal ratio of 0.147:0.353:0.353:0.147. That is, in the embodiment, the frequency of each of the heights is very consistent with the ideal ratio of 0.147:0.353:0.353:0.147. max The first combined surface area percentage (A1) associated with the first plurality of regions 22a may be substantially equal to the surface area percentage (A2) associated with the first plurality of regions 22a at height h minassociated with a second plurality of regions 22b, a second combined surface area percentage (A2) (see Figure 3 )(e.g., within 5%). In an embodiment, a third combined surface area percentage (A3) associated with a third plurality of regions 22c at a height h1 may be substantially equal to a fourth combined surface area percentage (A4) associated with a fourth plurality of regions 22d at a height h2 (e.g., within 5%). In an embodiment, A4 > A1. In an embodiment, A4 > A2. In an embodiment, A3 > A1. In an embodiment, A3 > A2. In an embodiment, A1 and A2 are less than half of A3 or A4. In an embodiment, A1 + A2 < A3. In an embodiment, A1 + A2 < A4. In an embodiment, when there are four heights in the discrete height distribution, A1, A2, A3, and A4 are all less than 40%. In an embodiment, when there are two heights in the discrete height distribution, A1 (associated with h max ) and A2 (equal to ) are both equal to 50%. In an embodiment, h min is at least 100 nm (e.g., at least 105 nm, at least 110 nm, at least 115 nm, at least 120 nm, at least 125 nm, at least 130 nm, at least 135 nm, at least 140 nm, at least 145 nm, at least 150 nm, at least 200 nm, at least 250 nm, at least 300 nm, at least 350 nm, at least 400 nm, at least 450 nm, at least 500 nm, or even greater) less than h max .
[0152] Fig. 10B Depict a graph 900, which includes a first graph 902 of calculated normalized reflectance (assuming a non-textured version has a reflectance of 1) and a second graph 904 of calculated transmission haze. As shown in graph 902, compared to the textured version, the specular reflectance is greatly reduced, and the maximum specular reflectance appears at the boundary of the wavelength range of interest, but still corresponds to a reduction factor of 0.0035, such that the specular reflectance is 0.35% of the value of the non-textured version. As shown in graph 805, a maximum haze of approximately 3.7% is observed at a wavelength of 400 nm, but the average value is approximately 2.5% over the entire wavelength range of interest. These results indicate that the patterns produced by the methods described herein can provide a beneficial reduction in specular reflectance while providing a relatively low haze.
[0153] A second example is fabricated via method 700 described herein with respect to Figure 7 . The second example includes a diffractive surface region having regions at only two heights relative to a假想 reference plane. The pattern is determined for normal incidence in the wavelength range of interest from 400 nm to 800 nm. The pattern of the region is by Fig. 6A The method 600 described above determines that a single etching mask is placed on a sample. The sample is a 4-inch Gorilla glass having a thickness of 0.7 mm manufactured by Corning. Wafer. After deposition and patterning of the resist, the wafer was exposed to an etchant (0.15% HF / 1% HFNO3) for 175 seconds to achieve an etch depth measured by a stylus of 156.5 nm. Consistent with Example 2, the general sequence of processing steps for a typical photolithography process is as follows: substrate preparation (cleaning and dehydration, followed by an adhesion promoter for spin-coated resist (e.g., hexamethyl disilazane (HMDS)), photoresist spin coating, prebake, exposure (e.g., exposure to high temperature via UV radiation) and development, followed by a wet etching process to transfer the binary image to the glass. The final step is to strip the resist after the resist pattern has been transferred to the underlying layer (e.g., via exposure to a suitable solvent). In some cases, post-bake and post-exposure bake steps are required to ensure resist adhesion during the wet etching process.
[0154] The light from the supercontinuum source is directed via a beam splitter onto the diffractive surface area of the sample, and specular reflectance and scattering are measured at multiple wavelengths. The beam splitter directs the reflected and scattered light onto a camera, and the relative intensity at various scattering angles is measured. Fig.11A An intensity map corresponding to the imaged scattering pattern is depicted. As shown, similarity to the LG pattern is achieved, but the central dot indicating specular reflection is still visible. Fig. 11B A graph depicting the measured spectral reflectance intensity and the calculated spectral reflectance intensity is shown. As shown, good agreement with theory is achieved. Reductions of up to 25 dB (corresponding to a measured specular reflectance of 0.01% at a wavelength of about 620 nm) are achieved relative to a non-textured version of the sample. The observed specular reflectance is less than 4% over the entire wavelength range of 400 nm to 840 nm.
[0155] The azimuthally averaged scattering intensity at various scattering angles is also calculated. Fig. 11C The results are depicted in . Fig. 11C The dashed line 910 in represents a scattering pattern associated with a LG mode target scattering distribution, including a maximum intensity scattering angle of about 0.5°. As shown, a wavelength of about 600 nm closely approximates the target scattering distribution, while wavelengths at the lower end of the wavelength range have a peak scattering angle of less than 0.5°, and wavelengths above 700 nm have a peak scattering angle greater than 0.5° but still less than 2.5°. Such results demonstrate the efficacy of the articles described herein in providing favorable specular reflectance properties while still providing low haze.
[0156] Unless explicitly stated otherwise, any method described herein is in no way intended to be construed as requiring that its steps be performed in a specific order. Thus, if a method claim does not actually recite the order in which its steps are to be followed, or if it is not otherwise specifically stated in the claims or specification that the steps are to be limited to a specific order, no specific order is intended to be inferred. Furthermore, as used herein, "a" is intended to include one or more than one component or element, and is not intended to be construed to mean only one.
[0157] It will be apparent to those skilled in the art that various modifications and variations may be made without departing from the spirit or scope of the disclosed embodiments. Since modifications, combinations, sub-combinations, and variations of these embodiments that include the spirit and substance of the disclosed embodiments may occur to those skilled in the art, the disclosed embodiments should be interpreted as including all within the scope of the appended claims and their equivalents.
Claims
1. A display product, comprising: a first major surface; a second major surface opposite to the first major surface; and a diffractive surface region formed in the first major surface, wherein within the diffractive surface region, the first major surface comprises a plurality of regions arranged in a discrete height distribution, the discrete height distribution being measured relative to an imaginary reference plane extending through the display article and parallel to the first major surface, wherein: The plurality of regions are arranged so that at a wavelength greater than or equal to the minimum wavelength λ min and less than or equal to the maximum wavelength λ max The incident angle range on the first main surface is the minimum incident angle θ within the wavelength range of interest. min To the maximum incident angle θ max When the first major surface is provided with a surface having a surface area of at least 10 Å, the specular reflectivity of light incident on the first major surface is reduced by at least a factor of 10 compared to a non-textured version of the first major surface not including the diffractive surface region, and The difference between the heights in the discrete height distribution is Within 5% of an integer multiple of λ′ min =λ min / cosθ min And λ′ max =λ max / cosθ max .
2. The display article of claim 1 wherein the diffractive surface region scatters the light in a far-field scattering pattern having a peak scattering angle less than or equal to 1.5° in the wavelength range of interest.
3. The display article of claim 2, wherein the peak scattering angle is less than or equal to 0.5° over at least a portion of the wavelength range of interest.
4. The display article of claim 2, wherein the far-field scattering pattern approximates a Laguerre-Gaussian mode.
5. The display article according to any one of claims 1 to 4, wherein: λ min Greater than or equal to 380nm and λ max Less than or equal to 1200nm, and θ min Greater than or equal to 0° and θ max Less than or equal to 75°.
6. The display article according to any one of claims 1 to 5, wherein λ min =400nm and λ max =800nm.
7. The display article of any one of claims 1 to 6, wherein the specular reflectivity is reduced by at least 100 times compared to the non-textured version of the first major surface.
8. The display article of any one of claims 1 to 7, wherein the plurality of regions have a minimum feature size greater than or equal to 1 μm.
9. The display article of any one of claims 1 to 8, wherein the plurality of regions are arranged in a pattern that is periodic in two directions that are perpendicular to each other.
10. The display article of claim 9, wherein the pattern includes at least one enclosed region that is completely surrounded by a plurality of regions having a height relative to the imaginary reference plane different from that of the enclosed region.
11. The display article of any one of claims 1 to 10, wherein a transmission haze of the light incident on the first major surface is less than or equal to 4% over the entire wavelength range of 400 nm to 800 nm.
12. A display article as described in any one of claims 1 to 11, wherein the regions in the multiple regions at each height of the discrete height distribution occupy a percentage of the combined surface area of the diffractive surface area, and the combined surface area percentage is predetermined to minimize the mirror reflectivity.
13. The display article of claim 12, wherein the discrete height distribution comprises three or more heights.
14. The display article of claim 13, wherein the discrete height distribution comprises at least four heights, the at least four heights comprising a minimum height h min ,exist The second height within 5% of The third height within 5% and The fourth height within 5% of the.
15. The display article of claim 14, wherein: a first plurality of regions having said minimum height occupying a first combined surface area percentage of said diffractive surface area, and The first combined surface area percentage is less than a second combined surface area percentage occupied by a second plurality of regions having the second height.
16. The display article of claim 15, wherein: a third combined surface area percentage of the diffractive surface area occupied by a third plurality of regions having the third height, a fourth combined surface area percentage of the diffractive surface area occupied by a fourth plurality of regions having the fourth height, The first combined surface area percentage is within 5% of the fourth combined surface area percentage, and The second combined surface area percentage is within 5% of the third combined surface area percentage.
17. The display article of claim 13 wherein the combined surface area percentage associated with each height is less than or equal to 40%.
18. A glass display product comprising: a first major surface; a second major surface opposite to the first major surface; and a diffractive surface region formed in the first major surface, wherein, within the diffractive surface region, the first major surface comprises: a first plurality of regions, the first plurality of regions comprising a first plurality of heights, the first plurality of heights having a maximum height h max is within 5% of the average of the first plurality of heights, the maximum height h max is a first combined surface area percentage of the diffractive surface area occupied by the first plurality of regions, measured from an imaginary reference plane extending through the display article and parallel to the first major surface; and A second plurality of regions, the second plurality of regions comprising a second plurality of heights, the second plurality of heights having a minimum height h measured from the imaginary reference plane min The second plurality of regions occupy a second combined surface area percentage of the diffractive surface area within 5% of an average of the second plurality of heights, wherein: The first plurality of regions and the second plurality of regions are arranged in a predetermined pattern based on a wavelength greater than or equal to a minimum wavelength λ min and less than or equal to the maximum wavelength λ max The incident angle range on the first main surface is the minimum incident angle θ within the wavelength range of interest. min To the maximum incident angle θ max The predicted specular reflectivity of light incident on the first major surface when h max -h min exist Within 5% of an integer multiple of λ′ min =λ min / cosθ min , and λ′ max =λ max / cosθ max ,and The first major surface has an average measured specular reflectivity of less than or equal to 2.5% over the wavelength range of interest within the incident angle.
19. The glass display article of claim 18, wherein the diffractive surface region scatters the light in a far-field scattering pattern having a peak scattering angle less than or equal to 1.5° in the wavelength range of interest.
20. The glass display article of claim 19, wherein the peak scattering angle is less than or equal to 0.5° over at least a portion of the wavelength range of interest.
21. The glass display article of claim 19, wherein the far-field scattering pattern approximates a Laguerre-Gaussian mode.
22. The glass display article of any one of claims 18 to 21, wherein: λ min Greater than or equal to 380nm and λ max Less than or equal to 1200nm, and θ min Greater than or equal to 0° and θ max Less than or equal to 75°.
23. The glass display article according to any one of claims 18 to 22, wherein: Within the diffractive surface region, the first major surface includes a third plurality of regions, the third plurality of regions including a third plurality of heights, the third plurality of heights being within 5% of an average of the third plurality of heights at a height h1 measured from the reference plane, the third plurality of regions occupying a third combined surface area percentage of the diffractive surface region, wherein the height h1 is within 5% of an average of the third plurality of heights. within 5%.
24. The glass display article of claim 23, wherein: Within the diffractive surface region, the first major surface includes a fourth plurality of regions, the fourth plurality of regions including a fourth plurality of heights, the fourth plurality of heights being within 5% of an average of the fourth plurality of heights at a height h2 measured from the reference plane, the fourth plurality of regions occupying a fourth combined surface area percentage of the diffractive surface region, wherein the height h2 is within 5% of an average of the fourth plurality of heights. within 5%.
25. The glass display article of claim 24, wherein: The first combined surface area percentage is within 5% of the fourth second combined surface area percentage, and The third combined surface area percentage is within 5% of the fourth combined surface area percentage.
26. The glass display article of claim 24, wherein: Each of the first combined surface area percentage, the second combined surface area percentage, the third combined surface area percentage, and the fourth combined surface area percentage is less than or equal to 40%.
27. The glass display article of any one of Claims 18 to 26, wherein the first plurality of regions and the second plurality of regions each have a characteristic dimension greater than or equal to 1 μm.
28. The glass display article of any one of claims 18 to 27, wherein the predetermined pattern is periodic in two directions that are perpendicular to each other.
29. The glass display article of any one of claims 18 to 28, wherein the predetermined pattern includes at least one enclosed region that is completely surrounded by a plurality of regions having a height relative to the imaginary reference plane that is different from that of the enclosed region.
30. The glass display article of any one of claims 18 to 29, wherein the transmission haze of the light incident on the first major surface is less than or equal to 4% over the entire wavelength range of 400 nm to 800 nm.
31. A method of forming a diffractive surface region of a substrate for a display article, the method comprising: determining a pattern of a plurality of regions on a first major surface of the substrate, wherein each region of the plurality of regions comprises a surface region disposed at a height measured relative to an imaginary reference plane extending through the display article and parallel to the first major surface, wherein the plurality of regions comprises a discrete distribution of heights; disposing one or more etching masks on the first major surface, the one or more etching masks allowing etching only on selected areas of the first major surface to form at least some of the plurality of areas; as well as After each of the one or more etching masks is disposed on the first major surface, the display article is contacted with an etchant for a period of time to form the plurality of regions including the discrete height distributions in the substrate such that the differences between the heights in the discrete height distributions are within Within 5% of an integer multiple of λ min is the minimum wavelength of the wavelength range of interest, λ max is the maximum wavelength in the wavelength range of interest, [θ min ,θ max ] defines the range of incident angles within which it is desired to minimize the specular reflectivity of the display article, λ′ min =λ max cosθ min , and λ′ max =λ min cosθ max .
32. The method of claim 31 , wherein determining the pattern of the plurality of regions comprises determining an ideal combined surface area percentage for each height in the discrete height distribution using the following relationship: FA=1, where A is a matrix with N elements, where N corresponds to the number of heights in the discrete height distribution, 1 is an identity row vector with N entries, and F is an NxN matrix with each value in F ij is calculated as:
33. The method of claim 32, wherein determining the pattern of the plurality of regions comprises: generating an initial pattern of the plurality of regions; The estimated far-field scattering pattern is calculated by approximating the incident light as a uniform field and approximating the diffractive surface area as inducing only a phase shift in the reflected light. as well as Use an optimization algorithm to update the initial pattern to reduce The difference between the target scattering pattern u(λ).
34. The method of claim 33, wherein the optimization algorithm minimizes the following objective function of the pattern P: where K is an integer value that samples the wavelength range of interest, and i and j are integer values that sample the incident angle range [θ min ,θ max ] is an integer value for uniform sampling, A i is the percentage of surface area associated with heights in the discrete height distribution associated with the initial pattern, is the ideal combined surface area percentage in the vector A, and w is a weighting factor.
35. The method of any one of claims 33 to 34, wherein the target far-field scattering pattern approximates a Laguerre-Gaussian mode.
36. The method of any one of claims 33 to 35, wherein the target scattering pattern comprises a peak scattering angle less than or equal to 1.5° in the wavelength range of interest.
37. The method of claim 36, wherein the peak scattering angle is less than or equal to 0.5° in the wavelength range of interest.
38. The method of any one of claims 31 to 37, wherein the one or more etch masks include at least two etch masks such that the discrete height distribution includes at least 4 heights.
39. The method of claim 38, wherein: After exposing the substrate to an etchant through a first etch mask, a second etch mask of the at least two etch masks is disposed on the first major surface, and The second etching mask exposes a region of the first main surface etched through the first etching mask so that the region is etched through both the first etching mask and the second etching mask.
40. The method of any one of claims 31 to 39, wherein the pattern comprises a minimum feature size greater than or equal to 1 μm.
41. A method as claimed in any one of claims 31 to 40, wherein the pattern is periodic in at least two directions that are perpendicular to each other.