Method for coating paper substrate by using modified cutin extract
By heat treatment of raw keratin extracts, it is used to prepare water-based barrier coating compositions, and the problem of insufficient barrier properties of paper substrates in the prior art is solved, and the water resistance and oil resistance of paper substrates are realized Significantly improved.
Patent Information
- Application Number
- CN202380032872.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-01
- Filing Date
- 2023-03-31
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, the failure to effectively utilize modified keratin extracts in the preparation of aqueous barrier coating compositions for paper substrates leads to insufficient barrier properties of paper substrates.
By heat treatment of the raw keratin extract, a modified keratin extract is formed and used to prepare an aqueous barrier coating composition with a solid content of 10 to 60 wt%, applied to a paper substrate, the modified keratin extract is passed through Heat treatment was obtained at a temperature of 40 to 120°C.
The water and oil resistance of the paper substrate is significantly improved, providing excellent barrier properties, similar to the effect of using synthetic polymers, while avoiding adverse effects on the performance of the paper substrate.
Abstract
Description
Technical Field
[0001] The present invention relates to a method for coating a paper substrate so as to provide improved barrier properties to the paper substrate. Background Art
[0002] In the paper and packaging industry, barrier coating compositions are used to improve the barrier properties (such as water resistance and / or oil resistance) of paper substrates.Traditionally, barrier coating compositions are based on film-forming polymers derived from fossil resources.
[0003] In recent years, there has been a growing interest in replacing the synthetic polymers traditionally used in barrier coating compositions without adversely affecting the barrier properties of the coated paper substrate. This can be achieved by incorporating compounds derived from renewable resources.
[0004] In this context, compounds extracted from plant matter and their derivatives may be an attractive alternative.
[0005] Cutin is a support biopolyester involved in the waterproofing of leaves and fruits of higher plants. Cutin is the main component (40% to 85 wt%) of the plant cuticle, a continuous lipid outer cell membrane covering the aerial parts of plant leaves, fruits and non-lignified stems.
[0006] From a chemical point of view, cutin is composed of polyhydroxylated C 16 and C 18 Polymeric network of fatty acids. However, when extracted from plant matter (e.g. by the methods described in WO2015 / 028299 or WO2016 / 187581), keratin undergoes depolymerization. Thus, raw keratin extracts consist mainly of hydroxy fatty acids and fatty esters and their oligomers.
[0007] G. Tedeschi et al., ACS Sustainable Chem. Eng., 2018, 6, 11, pp. 14955-14966, describe a method for preparing a composite self-supporting film inspired by plant cuticle, which consists of a blend of sodium alginate, unsaturated polyhydroxy fatty acids derived from agricultural waste generated in the tomato peeling industrial process, beeswax in water and ethanol, and subsequent heat treatment.
[0008] However, in the prior art, there is no mention of using modified keratin extracts in preparing aqueous barrier coating compositions for paper substrates. Summary of the invention
[0009] Therefore, an object of the present invention is a method for coating a paper substrate, said method comprising: i) providing a paper substrate;
[0010] ii) applying an aqueous barrier coating composition having a solid content of 10 to 60 wt% (weight %) and comprising 20 to 100 wt% of a modified keratin extract obtained by heat treating a raw keratin extract at a temperature of 40 to 120°C to a paper substrate.
[0011] "Modified keratin extract" refers to raw keratin extract that has been modified by heat treatment. Without being bound by any theory, it is believed that heat treatment allows the formation of polyesters derived from hydroxy fatty acids, which are the main components of raw keratin extract. DETAILED DESCRIPTION OF THE INVENTION
[0013] A method for coating a paper substrate may include:
[0014] i) providing a paper substrate;
[0015] ii) applying an aqueous barrier coating composition having a solid content of 10 to 60 wt% (weight %) and comprising 50 to 100 wt% of a modified keratin extract obtained by heat treating a raw keratin extract at a temperature of 60 to 100°C to a paper substrate.
[0016] Preferably, a method for coating a paper substrate comprises:
[0017] i) providing a paper substrate;
[0018] ii) applying an aqueous barrier coating composition having a solid content of 10 to 60 wt% (weight %) and comprising 50 to 100 wt% of a modified keratin extract obtained by heat treating a raw keratin extract at a temperature of 80 to 100°C to a paper substrate.
[0019] Raw keratin extracts suitable for use in preparing the modified keratin extracts of the present invention may be obtained by any extraction method known in the art for extracting keratin from plant materials.
[0020] As used herein, "plant matter" refers to any part of a plant that contains cutin, including, for example, fruits (in the botanical sense, the peel and juice sacs), leaves, stems, bark, seeds, flowers, or any other part of a plant.
[0021] According to the present invention, plant matter may include agricultural waste, such as tomato skins, grape skins, apple skins, pepper skins, lemon skins, lemon leaves, lime skins, lime leaves, orange skins, orange leaves, orange fruit, clementine leaves, clementine fruit, mandarin leaves, mandarin fruit, pea seeds, grapefruit skins, grapefruit leaves, grapefruit seeds, papaya skins, cherry fruit, cranberry skins, grass clippings.
[0022] The raw keratin extract of the present invention is preferably obtained from tomatoes, more preferably from waste tomato skins.
[0023] According to the present invention, the raw keratin extract extracted from waste tomato skin is a complex mixture of long-chain ω-hydroxy acids and their oligomers, usually with a 16 or 18 carbon backbone, the major component of which is 10,16-dihydroxyhexadecanoic acid.
[0024] According to the invention, the raw keratin extract is water-based and generally has a dry content of 30 to 95% by weight, preferably 50 to 80% by weight. Furthermore, the pH of the raw keratin extract is generally 3 to 6. The Brookfield viscosity of the raw keratin extract ( The viscosity (measured in a 31 wt% aqueous solution at 25° C. and pH=9) is 10 to 500 mPa*s, preferably 50 to 200 mPa*s.
[0025] The method for preparing the modified keratin extract of the present invention comprises heat treatment at a temperature of 40 to 120°C, preferably 80 to 100°C.
[0026] Advantageously, the process for preparing the modified keratin extract of the invention comprises a heat treatment at a temperature ranging from 60°C (which is approximately equal to the melting temperature of the dry raw keratin extract) to 100°C.
[0027] As used herein, "heat treatment" refers to applying heat to the raw keratin extract. Heat can be applied by conduction (e.g., heating coils), convection (e.g., heat transfer through a fluid such as water or air), and / or radiation (e.g., heat transfer using electromagnetic waves).
[0028] In the method for preparing the modified keratin extract of the present invention, a solvent selected from water, an organic solvent or a mixture thereof may be added. Preferably, the solvent that may be added is water.
[0029] The solvent used in this process can be removed by distillation under reduced pressure.
[0030] The heat treatment for preparing the modified keratin extract of the present invention is carried out at atmospheric pressure or at reduced pressure (generally 0.001 to 0.6 bar). Preferably, the heat treatment is carried out at atmospheric pressure.
[0031] The heat treatment for preparing the modified keratin extract of the present invention can be carried out in the presence of a catalyst. Non-limiting examples of catalysts that can be used include, for example, tetraisopropoxytitanium, dibutyltin oxide, tin octoate, aluminum isopropoxide, zirconium acetylacetonate, tetrabutoxyzirconium, tin (II) n-octoate, tin (II) 2-ethylhexanoate, tin (II) laurate, dibutyltin dichloride, dibutyltin diacetate, dibutyltin dilaurate, dibutyltin dimaleate, dioctyltin diacetate, antimony triethoxide or a boric acid derivative (such as pyridineboric acid). Preferably, the catalyst is zirconium acetylacetonate.
[0032] The heat treatment for preparing the modified keratin extract of the present invention can be carried out under acidic conditions (i.e., pH 2 to 7, preferably 3 to 7) or alkaline conditions (i.e., pH 7 to 12, preferably 7 to 11). Preferably, the heat treatment is carried out under acidic conditions.
[0033] When the heat treatment is carried out under acidic conditions, the heat treatment starts immediately because the raw keratin extract usually already has an acidic pH value (3 to 6). After the heat treatment is completed, the modified keratin extract obtained is treated with a base until the pH value reaches 7 to 11. The base is preferably ammonia, an inorganic base or an amine. More preferably, the base is ammonia.
[0034] When the heat treatment is carried out under alkaline conditions, before starting the heat treatment, the raw keratin extract is treated with a base until the pH reaches 7 to 11. The base is preferably ammonia, an inorganic base or an amine. More preferably, the base is ammonia.
[0035] The method for preparing the modified keratin extract of the present invention involves a heat treatment which may last from 2 to 72 hours.
[0036] The method for preparing the modified keratin extract of the present invention comprises a heat treatment preferably lasting from 2 to 24 hours, more preferably from 3 to 15 hours.
[0037] The modified keratin extract of the present invention is water-based, has a dry content of 10 to 60 wt%, preferably 20 to 40 wt%, and a pH of 6 to 11, preferably 7 to 10. The Brookfield viscosity of the modified keratin extract ( The viscosity (measured in a 31 wt% aqueous solution at 25° C. and pH=9) is 100 to 3000 mPa*s, preferably 300 to 1500 mPa*s.
[0038] The aqueous barrier coating composition of the present invention may further contain additives commonly used in the field of paper coatings, such as pigments, adhesives, waxes, thickeners, anti-caking agents, dyes, flow control agents or defoamers.
[0039] Suitable pigments include, for example, metal salt pigments such as calcium sulfate, calcium aluminum sulfate, barium sulfate, magnesium carbonate and calcium carbonate. Calcium carbonate can be natural ground calcium carbonate (GCC), precipitated calcium carbonate (PCC), lime or chalk. Other suitable pigments include, for example, silicon oxide (silica), aluminum oxide, hydrated aluminum, silicates, titanium dioxide, zinc oxide, kaolin, clay, talc or silicon dioxide.
[0040] Suitable adhesives include synthetic adhesives and natural adhesives. Suitable synthetic adhesives include, but are not limited to, (meth) acrylic acid (copolymer) polymers, ethylene-(meth) acrylic acid copolymers, styrene-(meth) acrylic acid copolymers, and polyvinyl alcohol. Suitable natural adhesives include, but are not limited to, carboxymethyl cellulose, starch, and starch derivatives.
[0041] Suitable starches include natural starches such as potato, wheat, corn, rice or tapioca starch.
[0042] Suitable starch derivatives include, but are not limited to, chemically modified starches such as hydroxyethyl starch, hydroxypropyl starch or phosphate starch.
[0043] Preferred starch and starch derivatives include degraded starch and degraded starch derivatives with a molecular weight Mn of 500 to 30000 Da, more preferably 500 to 20000 Da. The degraded starch is obtained by degradation of natural starch or chemically modified starch.
[0044] Suitable waxes include, but are not limited to, polyethylene, polypropylene, paraffin wax, amides, waxes of vegetable origin, carnauba wax, or mixtures thereof.
[0045] The aqueous barrier coating composition of the present invention can be applied to the paper substrate by, for example, roller coating, spray coating, curtain coating, knife coating, dip coating, gravure roller coating, reverse direct gravure coating, rod coating, soft tip knife coating, jet coating and / or a combination thereof.
[0046] The present invention is further described by the following examples. Example
[0047] The raw keratin extract used in the examples was from waste tomato skins and had a Brookfield viscosity (measured on a 31 wt% aqueous solution at 25°C and pH=9) of 100 mPa*s.
[0048] Example 1
[0049] Polymerization under reduced pressure
[0050] In a four-necked round-bottom reactor equipped with a mechanical IKA stirrer, a thermometer and equipped with a Dean-Stark adapter and a condenser for reflux, the polymerization of raw keratin extract (50-80 wt% dry content, pH 3-6) was carried out under vacuum evaporation (100-300 mbar). The reaction was carried out at 90°C until a very high viscosity product (>50000 mPas) with a dry content of up to 99.9% was obtained. The polymerization was stopped when the product began to rise along the impeller (6 hours after all the water was evaporated). The modified keratin extract obtained was cooled and an ammonia solution was added until a modified keratin extract aqueous solution with a dry content of 25-35 wt% and a pH of 7-9 was obtained. Filtering was performed using a 100 μm filter cloth. Brookfield viscosity of the modified keratin extract (31 wt% aqueous solution at 25°C and pH 9): 700 mPa*s.
[0051] Example 2
[0052] Polymerization under acidic conditions
[0053] The polymerization of raw keratin extract (50-80 wt% dry content, pH 3-6) was carried out at atmospheric pressure in a four-necked round-bottom reactor equipped with a mechanical IKA stirrer, a thermometer and a condenser for reflux. The reaction was carried out at 90° C. for 10 hours. The modified keratin extract was cooled and an ammonia solution was added until an aqueous solution of the modified keratin extract with a dry content of 25-35 wt% and a pH of 7-9 was obtained. Filtration was performed using a 100 μm filter cloth. Brookfield viscosity of the modified keratin extract (31 wt% aqueous solution at 25° C. and pH 9): 850 mPa*s.
[0054] Example 3
[0055] Polymerization under alkaline conditions
[0056] The polymerization of raw keratin extract (50-80 wt% dry content, pH 3-6) was carried out at atmospheric pressure in a four-necked round-bottom reactor equipped with a mechanical IKA stirrer, a thermometer and a condenser for reflux. Before starting the heating, the raw keratin extract was treated with ammonia to a pH of 9.5. The reaction was carried out at 90° C. for 15 hours. The modified keratin extract was cooled and an aqueous solution of the modified keratin extract with a dry content of 25-35 wt% and a pH of 7-9 was obtained. Filtration was carried out using a 100 μm filter cloth. Brookfield viscosity of the modified keratin extract (31 wt% aqueous solution at 25° C. and pH 9): 450 mPa*s.
[0057] Example 4
[0058] Polymerization under acidic conditions
[0059] The polymerization of raw keratin extract (50-80 wt% dry content, pH 3-6) was carried out at atmospheric pressure in a four-necked round-bottom reactor equipped with a mechanical IKA stirrer, a thermometer and a condenser for reflux. The reaction was carried out at 70°C for 15 hours. The modified keratin extract was cooled and an ammonia solution was added until an aqueous solution of the modified keratin extract with a dry content of 25-35 wt% and a pH of 7-9 was obtained. Filtration was performed using a 100 μm filter cloth. Brookfield viscosity of the modified keratin extract (31 wt% aqueous solution at 25°C and pH 9): 800 mPa*s.
[0060] Comparative Example 1
[0061] An acrylic emulsion copolymer derived from ethylhexyl acrylate, methyl methacrylate and methacrylic acid, which is a synthetic polymer commonly used to improve the water resistance of paper substrates.
[0062] Comparative Example 2
[0063] 125HI 12, a dextrin derived from potato starch, commercially available from Avebe, is commonly used to improve the oil resistance of paper substrates.
[0064] Comparative Example 3
[0065] Raw keratin extract obtained from spent tomato skin (50-80 wt% dry content, pH 3-6).
[0066] Application Testing
[0067] The modified keratin extract prepared in the previous examples was used to prepare an aqueous barrier coating composition.
[0068] The obtained water-based barrier coating composition was heated at 5.5 g / m 2 The coating weight is applied at a grammage of 80g / m 2 on paper substrate.
[0069] The coated paper substrates were evaluated for water and oil resistance.
[0070] Liquid water resistance is tested using the Cobb method as described in TAPPI method T 441-om. The test time is 600 seconds. This method determines the amount of liquid water absorbed by paper or paperboard in a specific time under standardized conditions.
[0071] The oil absorption capacity was tested using the KIT method according to TAPPI test method UM 557. In this test, solutions numbered in increasing hydrophobicity (1 to 16) were applied to a paper substrate. The highest numbered solution that did not stain the surface was recorded as the result of the KIT test.
[0072] The heat sealability of the coated paper substrates was also evaluated.
[0073] Heat sealability was evaluated using a Gandus DD 100-200ATR 121-141 (an automatic sealer in accordance with DIN 58953p-7) with a maximum heat seal area of 196 mm x 13 mm and a heat seal temperature range of 50-150 ± 1 °C. The test was performed by contacting two coated paper samples (50 mm x 50 mm) for 1 second at a given temperature. The two seals were then peeled off after cooling at room temperature and the heat seal strength was visually verified. The lowest temperature at which heat sealing occurred was recorded.
[0074] Table 1 records the Cobb test and KIT test results of comparing an aqueous barrier coating composition containing the modified keratin extract of the present invention, an aqueous barrier coating composition containing an acrylic emulsion copolymer (Comparative Example 1), an aqueous barrier coating composition containing dextrin derived from potato starch (Comparative Example 2), or an aqueous barrier coating composition containing a raw keratin extract (Comparative Example 3).
[0075] Table 2 records the results of heat sealing tests comparing aqueous barrier coating compositions containing modified keratin extracts of Examples 2 and 3 of the present invention, aqueous barrier coating compositions containing acrylic emulsion copolymers (Comparative Example 1), aqueous barrier coating compositions containing dextrin derived from potato starch (Comparative Example 2), or aqueous barrier coating compositions containing raw keratin extracts (Comparative Example 3).
[0076] Table 1
[0077] Example <![CDATA[Cobb test (g / m 2 )]]> KIT trial Uncoated paper 29 0 CE 1* 8 4 CE 2* nd 6 CE 3* 43 0 1 23 10 2 3 16 3 11 9 4 20 11
[0078] *For comparison
[0079] nd = When the coated paper substrate comes into contact with water, the coating film is completely removed
[0080] The results reported in Table 1 show that while the raw keratin extract (Comparative Example 3) had no significant effect on water and oil resistance, the modified keratin extracts of the present invention (Examples 1-4) provided excellent water and oil resistance to the treated paper substrate.
[0081] Compared to synthetic polymers commonly used as water repellents (Comparative Example 1), the modified keratin extracts of the invention (Examples 1-4) allow to obtain paper substrates with similar water resistance, but significantly improved oil resistance.
[0082] The modified keratin extracts of the invention (Examples 1-4) allow obtaining paper substrates with improved oil resistance and significantly improved water resistance when compared to dextrin derived from potato starch (Comparative Example 2). This result is particularly significant since paper substrates coated with natural polymers such as starch usually suffer from poor water resistance.
[0083] Table 2
[0084] Example Minimum heat sealing temperature (℃) Uncoated paper no CE 1* 80 CE 2* no CE 3* no 2 100 3 100
[0085] *For comparison
[0086] no = not heat sealable
[0087] The results reported in Table 2 show that the modified keratin extracts of the present invention (Examples 2-3) can achieve heat sealable paper substrates just as can be achieved using synthetic polymers (Comparative Example 1).
[0088] In contrast, aqueous barrier coating compositions based on dextrins derived from potato starch (Comparative Example 2) or raw keratin extracts (Comparative Example 3) do not allow obtaining heat-sealable paper substrates.
Claims
1. A method for coating a paper substrate, the method comprising: i) providing a paper substrate; ii) applying an aqueous barrier coating composition having a solid content of 10 to 60 wt% (weight %) and comprising 20 to 100 wt% of a modified keratin extract obtained by heat treating a raw keratin extract at a temperature of 40 to 120°C to a paper substrate.
2. The method for coating a paper substrate according to claim 1, wherein: The aqueous barrier coating composition comprises 50 to 100 wt % of the modified keratin extract.
3. The method for coating a paper substrate according to claim 1, wherein: The heat treatment of the raw keratin extract is carried out at a temperature of 60°C to 100°C.
4. The method for coating a paper substrate according to claim 1, wherein: The heat treatment of the raw keratin extract is carried out at a pH range of 2 to 7.
5. The method for coating a paper substrate according to claim 1, wherein: The heat treatment of the raw keratin extract is carried out at a pH range of 7 to 12.
6. The method for coating a paper substrate according to claim 1, wherein: The dry content of the raw keratin extract is 30 to 95 wt%.
7. The method for coating a paper substrate according to claim 1, wherein: The pH of raw keratin extract is 3 to 6.
8. The method for coating a paper substrate according to claim 1, wherein: The dry content of the modified keratin extract is 10 to 60 wt%.
9. The method for coating a paper substrate according to claim 1, wherein: The pH of the modified keratin extract is between 6 and 11.
10. The method for coating a paper substrate according to claim 1, wherein: The aqueous barrier coating composition may further comprise a pigment, a binder, a wax, a thickener, an anti-caking agent, a dye, a flow control agent or a defoaming agent.