All-solid-state post-processing technology of perovskite quantum dots and application of all-solid-state post-processing technology
Through all-solid-state post-treatment technology, the size of perovskite luminescent is reduced and its surface is passivated by reacting HF gas with silicon oxide, which solves the problems of large size and photoinduced defects in high-temperature solid-state synthesis methods and improves perovskite luminescence light stability and application of the body.
Patent Information
- Application Number
- CN202411040282.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The perovskite luminescent materials prepared by existing high-temperature solid-state synthesis methods are large in size and are susceptible to photoinduced defects, which limits their development in applications such as LED, inkjet printing and photoconverting films.
Using all-solid-state post-treatment technology, the perovskite luminescent and the post-treatment additive are mixed, and the HF gas reacts with silicon oxide through heating, reduces the particle size and passivates the surface of perovskite quantum dots, and uses the pore channels of mesoporous silicon oxide. Adsorb HF gas to reduce template agent clustering and bonding.
Effectively reduce the size of perovskite luminescents and improve their light stability, making them suitable for a wider range of applications, including inkjet printing and Micro LED.
Smart Images

Figure BDA0004972202710000081
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of post-processing of perovskite quantum dots, and in particular relates to a full-solid-state post-processing technology of perovskite quantum dots and an application thereof. Background Art
[0002] As a new type of luminescent material, metal halide perovskite (hereinafter referred to as perovskite) luminescent body has the characteristics of excellent luminescence efficiency, narrow emission half-peak width, high color purity, adjustable visible light band, etc., and is simple to prepare, low cost, and easy to scale up production. It is expected to become a key luminescent layer material in the future display field and has broad application prospects in the fields of light-emitting diodes (LEDs), solar cells, lasers, etc. However, since perovskite is a soft lattice ionic compound, high humidity, high temperature and strong light irradiation in the external environment can easily induce perovskite defects, thereby damaging its luminescence performance.
[0003] High-temperature solid-state synthesis methods are often used to prepare perovskite luminophores, which have the advantages of being suitable for large-scale synthesis, high controllability, and simple processes. The existing high-temperature solid-state synthesis method is mainly divided into two steps: 1) mixing the perovskite precursor and the template; 2) calcining the precursor mixture, reacting and melting the perovskite precursor at high temperature, and supercooling and crystallizing in the template to form a perovskite luminophore. Due to the coating effect of the template, these perovskite luminophores can isolate water, oxygen, and external high temperatures, showing stability against water and high temperatures.
[0004] However, strong external light irradiation can still easily cause irreversible photoinduced defects in these perovskite luminescent bodies, which hinders the further development of perovskite luminescent bodies in applications such as LEDs and light conversion coatings that require external light excitation. At the same time, since high-temperature calcination (at least 400°C) can easily cause templates to cluster and bond, the perovskite luminescent bodies obtained by the existing high-temperature calcination preparation technology are relatively large in size, usually in the order of tens to hundreds of microns, which limits the further application of these perovskite luminescent bodies in inkjet printing, Micro LEDs, and light conversion films. Therefore, it is necessary to develop a post-processing technology to improve the photostability of solid-state synthetic perovskite luminescent bodies, while reducing the size of the perovskite luminescent bodies prepared by high-temperature calcination, so that they can be used in a wider range of applications. Summary of the invention
[0005] The purpose of the present invention is to provide a full solid-state post-processing technology for perovskite quantum dots and its application, which can reduce the size of high-temperature solid-state synthesized perovskite luminescent bodies on the one hand, and improve the photostability of perovskite luminescent bodies on the other hand.
[0006] To achieve the above object, the technical solution adopted by the present invention is: a full solid-state post-processing technology of perovskite quantum dots, comprising the following steps:
[0007] S1. Mixing a perovskite luminescent body and a post-processing additive to obtain a mixed powder; the perovskite luminescent body includes a template and perovskite quantum dots located in the pores of the template, and the template retains pores used as a post-processing mass transfer path;
[0008] S2, placing the mixed powder in a reaction container and heating it to decompose the post-treatment additive to generate HF gas, and the HF gas then reacts with silicon oxide to reduce the particle size, and at the same time, the HF gas diffuses into the template pores to passivate the surface of the perovskite quantum dots;
[0009] The template agent is at least one of mesoporous silica and microporous silica.
[0010] By adopting the above method: In the present application, the perovskite light emitter can be any perovskite quantum dot coated with silicon oxide in the prior art, and the pores of the silicon oxide are not collapsed or not completely collapsed, so as to retain the pores as the post-processing mass transfer path.
[0011] During the heating process of the mixed powder, the post-treatment additive decomposes to produce HF gas. HF gas is a corrosive gas that can react with silicon dioxide to form silicon tetrafluoride (SiF4). It can etch the large particles originally formed by silicon oxide clusters and bonding to reduce the overall particle size. At the same time, due to the adsorption effect of many pores on silicon oxide, HF gas and silicon tetrafluoride (SiF4) can be adsorbed into the pores to passivate the surface of perovskite quantum dots.
[0012] In addition, the difference between the mesoporous silica and microporous silica mentioned above is only the difference in the pore size of the silica.
[0013] Further, the preparation method of the perovskite luminescent body can refer to the perovskite nanocrystalline fluorescent material and its preparation method and application previously applied and disclosed by our company (publication number: CN118165723A), or other related methods disclosed in the prior art. At the same time, the present invention also provides the following methods as examples:
[0014] A method for preparing a perovskite luminescent body comprises the following steps:
[0015] Step 1: Grind and mix perovskite precursors such as cesium halide and lead halide and a template agent to obtain a mixture.
[0016] Step 2: Heat the mixture to allow the precursors to react in the template to form a perovskite emitter.
[0017] The above methods are merely examples and do not constitute a limitation on the method for preparing perovskite light emitters.
[0018] Further, the post-treatment additive is at least one or more of NH4F, NH4HF2, KHF2, and NaHF2. In the present invention, the post-treatment additive is solid, and the HF gas is generated by the thermal decomposition process at the sintering temperature. The HF gas reacts with the template to reduce the clustering and bonding of the template, thereby achieving the purpose of reducing the size of the perovskite luminescent body prepared by high-temperature calcination. At the same time, the HF gas can effectively diffuse into the pores of the template.
[0019] Furthermore, the template agent is MCM-41 molecular sieve, which is a type of silicon oxide, more specifically, a silicon dioxide material with a mesoporous structure.
[0020] Furthermore, the perovskite quantum dots have an ABX3 structure, wherein the molar ratio of A, B and X is 1:1:3, and A is Cs, B is Pb, and X is at least one of Cl, Br or I.
[0021] Furthermore, the reaction container is a closed reactor to prevent HF gas leakage.
[0022] Furthermore, the heating temperature in step S2 is 100-300°C.
[0023] Furthermore, the mass ratio of the perovskite luminescent body to the post-treatment additive in step S1 is (1-6): 1. By specifically limiting the ratio of the two, it is ensured that the generated HF gas can simultaneously meet the requirements of corroding silicon dioxide to reduce the particle size and diffusing into the template pores to passivate the perovskite quantum dots.
[0024] Furthermore, the heating and heat preservation time of step S2 is at least 30 minutes. By limiting the heat preservation time, it is ensured that enough HF gas can be adsorbed in the pores with the template.
[0025] A fully solid-state post-processing technology for perovskite quantum dots is applied in perovskite diffuser plates, inkjet printing, wavelength conversion films, quantum dot films or Micro LEDs.
[0026] The beneficial effects of the present invention are mainly reflected in:
[0027] (1) The post-processing technology of this application is targeted at: Perovskite quantum dots that have been synthesized. At the same time, all the materials used in the post-processing process of this application are solid, which is suitable for the post-processing of quantum dots in the industrial scale-up stage. In other words, this application essentially provides a full solid-state Perovskite quantum dot post-processing technology.
[0028] (2) Compared with the existing high-temperature solid-state synthetic perovskite luminophores, the all-solid-state post-processing technology provided by the present invention makes these perovskite luminophores not only resistant to water, oxygen, and heat, but also resistant to the generation of light-induced defects. The post-processing technology provided by the present invention makes it possible for perovskite luminophores to be used in inkjet printing, Micro LED, light conversion film, light conversion coating and other application fields that require external light excitation. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific implementation methods described herein are only used to explain the present invention and are not used to limit the present invention.
[0030] Embodiment 1:
[0031] This embodiment provides a full solid-state post-processing technology for perovskite quantum dots, including the following steps:
[0032] Step 1: Grind and mix 1.064 g of cesium halide, 1.835 g of lead halide and 3.2 g of template MCM-41 molecular sieve for 2 h.
[0033] Step 2: Heat the mixed powder of step 1 to 580°C and maintain for 60 minutes, then cool naturally to obtain a perovskite light emitter.
[0034] Step 3: Weigh 300 mg of the perovskite luminescent material obtained after calcination in step 2, add 0.15 g of NH4F, and grind and blend.
[0035] Step 4: Take the perovskite luminescent body obtained after grinding in step 3, place it in a closed reactor and heat it to 180 degrees Celsius, maintain it for 60 minutes and then cool it naturally to obtain a post-treated product (perovskite luminescent body).
[0036] In the above, the cesium halide is cesium bromide; and the lead halide is lead bromide.
[0037] Experimental analysis: The perovskite luminescent body obtained by the above post-treatment was analyzed by Bettersize2600 laser particle size analyzer. The results showed that the D50 of the luminescent body was 0.862 μm and the D97 was 5.326 μm. In comparison, the D50 of the perovskite luminescent body without post-treatment provided in Comparative Example 1 was 4.665 μm and the D97 was 75.67 μm. By comparing before and after post-treatment, it can be seen that all-solid-state post-treatment can reduce the size of the perovskite luminescent body.
[0038] The powder obtained by the sintering was tested for fluorescence quantum yield (PLQY), as shown in Table 1, and the PLQY of the sample was 86%. In comparison, the PLQY of the perovskite luminescent material without post-treatment provided in Comparative Example 1 was 32%. The improvement of PLQY indicates that the all-solid-state post-treatment can passivate the defects of the perovskite CsPbBr3 luminescent material.
[0039] The stability of the perovskite luminescent material obtained by the above post-treatment was tested under strong blue light irradiation environment. See Table 1 for details. 2 After continuous irradiation of blue light (450nm) for 100 hours, the luminous intensity of the luminophore can maintain 85% of the original intensity. In contrast, the luminous intensity of the perovskite luminophore provided in Comparative Example 1 without post-treatment under the same blue light test conditions dropped to 28% of the initial intensity after 100 hours. The blue light stability proves that post-treatment is beneficial to improving the light stability of CsPbBr3 luminophores.
[0040] Embodiment 2:
[0041] This embodiment provides a full solid-state post-processing technology for perovskite quantum dots, including the following steps:
[0042] Step 1: Grind and mix 1.064 g of cesium halide, 1.835 g of lead halide and 3.2 g of template MCM-41 molecular sieve for 2 h.
[0043] Step 2: Heat the mixed powder of step 1 to 580°C and maintain for 60 minutes, then cool naturally to obtain a perovskite light emitter.
[0044] Step 3: Weigh 300 mg of the perovskite luminescent material obtained after calcination in step 2, add 0.15 g of NH4HF2, and grind.
[0045] Step 4: Take the perovskite luminescent body obtained after grinding in step 3, place it in a reaction kettle and heat it to 180 degrees Celsius, maintain it for 60 minutes and then cool it naturally to obtain a post-treated product (perovskite luminescent body).
[0046] In the above, the cesium halide is cesium bromide; and the lead halide is lead bromide.
[0047] Experimental analysis: The perovskite luminescent body obtained by the above post-treatment was analyzed by Bettersize2600 laser particle size analyzer. The results showed that the D50 of the luminescent body was 0.754 μm and the D97 was 4.958 μm. In comparison, the D50 of the perovskite luminescent body without post-treatment provided in Comparative Example 1 was 4.665 μm and the D97 was 75.67 μm. By comparing before and after post-treatment, it can be seen that all-solid-state post-treatment can reduce the size of the perovskite luminescent body.
[0048] The powder obtained by the sintering was tested for fluorescence quantum yield (PLQY), as shown in Table 1, and the PLQY of the sample was 91%. In comparison, the PLQY of the perovskite luminescent body without post-treatment provided in Comparative Example 1 was 32%. The improvement of PLQY indicates that post-treatment can passivate the defects of the perovskite CsPbBr3 luminescent body.
[0049] The stability of the perovskite luminescent material obtained by the above post-treatment was tested under strong blue light irradiation environment. See Table 1 for details. 2 After continuous irradiation of blue light (450nm) for 100 hours, the luminous intensity of the luminophore can maintain 83% of the original intensity. In contrast, the luminous intensity of the perovskite luminophore provided in Comparative Example 1 without post-treatment under the same blue light test conditions dropped to 28% of the initial intensity after 100 hours. The blue light stability proves that post-treatment is beneficial to improving the photostability of CsPbBr3 luminophores.
[0050] Comparative Example 1:
[0051] Compared with Examples 1 and 2, this comparative example does not have a post-processing step, and comprises the following steps:
[0052] Step 1: Grind and mix 1.064 g of cesium halide, 1.835 g of lead halide and 3.2 g of template MCM-41 molecular sieve for 2 h.
[0053] Step 2: Heat the mixed powder of step 1 to 580°C and maintain for 60 minutes, then cool naturally to obtain a perovskite light emitter.
[0054] In the above, the cesium halide is cesium bromide; and the lead halide is lead bromide.
[0055] Experimental analysis: The perovskite luminescent body obtained by the above sintering was subjected to particle size analysis using a Bettersize 2600 laser particle size analyzer. The results showed that the D50 of the luminescent body was 4.665 μm and the D97 was 75.67 μm.
[0056] The powder obtained by the sintering was taken to test the fluorescence quantum yield (PLQY). As shown in Table 1, the PLQY of the sample was 32%.
[0057] The stability of the perovskite luminescent material obtained above was tested under strong blue light irradiation. See Table 1 for details. 2 After continuous irradiation with blue light (450nm) for 100 hours, the luminous intensity of the luminescent body can maintain 28% of the original intensity.
[0058] Comparative Example 2:
[0059] The difference from Example 1 is that the post-treatment additive (NH4F) is replaced by HF liquid.
[0060] Experimental analysis: The sample obtained after the above treatment is whitish and does not emit light. This indicates that the strong acid solution will damage the structure of the perovskite quantum dots and degrade their performance. It should be noted that the intermediate product HF gas in Example 1 of the present invention is not directly acidic. However, when HF gas is dissolved in water, it forms hydrofluoric acid (HF aqueous solution), which is an acidic solution. Hydrofluoric acid solution can release hydrogen ions (H+), thereby showing acidity.
[0061] Comparative Example 3:
[0062] This comparative example provides a full solid-state post-processing technology for perovskite quantum dots, comprising the following steps:
[0063] Step 1: Grind and mix 1.064 g of cesium halide and 1.835 g of lead halide for 2 h.
[0064] Step 2: Heat the mixed powder of step 1 to 580°C and maintain for 60 minutes, then cool naturally to obtain a CsPbBr3 perovskite light emitter (without template coating).
[0065] Step 3: Weigh 300 mg of the perovskite luminescent material obtained after calcination in step 2, and place the perovskite luminescent material in a hydrogen fluoride vapor environment in a closed reactor for 60 minutes.
[0066] In the above, the cesium halide is cesium bromide; and the lead halide is lead bromide.
[0067] Experimental analysis: Since there is no template (silicon oxide), there is no basis for hydrofluoric acid gas to react with silicon oxide, and the particle size has no change; at the same time, it will not react with silicon oxide to form silicon tetrafluoride. Hydrofluoric acid gas can only effectively fill the defect sites on the surface of perovskite, and only has a passivation effect.
[0068] Comparative Example 4:
[0069] The difference from Comparative Example 3 is that there is no post-treatment step of HF gas in Step 3.
[0070] Table 1 shows the particle size test results of the samples obtained in Examples 1-2 of the present invention and Comparative Example 1, the PLQY test results and the ratio of the luminous intensity after 100 hours of blue light aging to the initial intensity.
[0071] Table 1
[0072]
[0073] The present invention illustrates the detailed preparation method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed preparation method, that is, it does not mean that the present invention must rely on the above-mentioned products and detailed preparation methods to be implemented. It should be clear to those skilled in the art that any improvement of the present invention, the combination or equivalent replacement of the raw materials of the product of the present invention, all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A full solid-state post-processing technology for perovskite quantum dots, characterized in that: The steps include: S1. Mixing a perovskite luminescent body and a post-processing additive to obtain a mixed powder; the perovskite luminescent body includes a template and perovskite quantum dots located in the pores of the template, and the template retains pores used as a post-processing mass transfer path; S2, placing the mixed powder in a reaction container and heating it to decompose the post-treatment additive to generate HF gas, and the HF gas then reacts with silicon oxide to reduce the particle size, and at the same time, the HF gas diffuses into the template pores to passivate the surface of the perovskite quantum dots; The template is silicon oxide.
2. The all-solid-state post-processing technology of perovskite quantum dots according to claim 1, characterized in that: The post-treatment additive is at least one or more of NH4F, NH4HF2, KHF2, and NaHF2.
3. The all-solid-state post-processing technology of perovskite quantum dots according to claim 1, characterized in that: The template agent is MCM-41 molecular sieve.
4. The all-solid-state post-processing technology of perovskite quantum dots according to claim 1, characterized in that: The perovskite quantum dots have an ABX3 structure, wherein the molar ratio of A, B and X is 1:1:3, and A is Cs, B is Pb, and X is at least one of Cl, Br or I.
5. The all-solid-state post-processing technology of perovskite quantum dots according to claim 2, characterized in that: The reaction vessel is a closed reactor to prevent HF gas leakage.
6. The all-solid-state post-processing technology of perovskite quantum dots according to claim 2, characterized in that: The heating temperature in step S2 is 100-300°C.
7. The all-solid-state post-processing technology of perovskite quantum dots according to claim 2, characterized in that: The mass ratio of the perovskite light emitter to the post-treatment additive in step S1 is (1-6):
1.
8. The all-solid-state post-processing technology of perovskite quantum dots according to claim 6, characterized in that: The heating and heat preservation time of step S2 is at least 30 minutes.
9. Application of the all-solid-state post-processing technology of perovskite quantum dots according to any one of claims 1 to 8 in perovskite diffuser plates, inkjet printing, wavelength conversion films, quantum dot films or Micro LEDs.
Citation Information
Patent Citations
Method for growing halide perovskite nanocrystals through in-situ chemical vapor deposition
CN116752116A
Perovskite nanocrystalline fluorescent material and preparation method and application thereof
CN118165723A
Method for improving illumination stability of perovskite through post-treatment and application
CN120718648A
Cited By
Solid-liquid mixed packaged perovskite quantum dot and preparation method thereof
CN119875618A
Post-processing technology of perovskite illuminant and application thereof
CN119899656A
Preparation method of mesoporous silica
CN120463207A
Surface post-treatment process of perovskite quantum dots
CN121628614A
Solid-liquid mixed packaged perovskite quantum dot and preparation method thereof
CN121825545A