Sputtering target, method for manufacturing laminated film, laminated film, and magnetic recording medium

By using Nb2O5 and TiO2 as dispersions in the magnetic layer and intermediate layer of the hard disk drive, a uniform grain boundary is formed, which solves the problem of insufficient exchange coupling between magnetic particles, improves magnetic separation and maintains high magnetic Anisotropy realizes the high density of hard disk drivers.

CN118979229APending Publication Date: 2024-11-19JX NIPPON MINING & METALS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410943183.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2017-09-21
Filing Date
2018-08-16
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In a hard disk drive, the exchange coupling between magnetic particles in the magnetic layer is relatively firm, resulting in insufficient magnetic separation. Increasing metal oxides will lead to deterioration of the crystallinity of magnetic particles, reducing saturated magnetization Ms and magnetic anisotropy Ku.

Method used

Using Nb2O5 as a metal oxide of a non-magnetic material, combined with TiO2 as a dispersion in the Co-Pt magnetic layer, a uniform grain boundary is formed in the magnetic layer and the intermediate layer through sputtering target technology, thereby improving the magnetic separation between magnetic particles. and maintain high saturation magnetization Ms and magnetic anisotropy Ku.

Benefits of technology

The magnetic separation between magnetic particles is significantly improved, and the magnetic anisotropy is maintained, which avoids the magnetic properties of the magnetic layer and realizes the density of the hard disk driver.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004944821770000091
    Figure BDA0004944821770000091
  • Figure HDA0004944821780000011
    Figure HDA0004944821780000011
  • Figure HDA0004944821780000012
    Figure HDA0004944821780000012
Patent Text Reader

Abstract

The invention relates to a sputtering target, a method for manufacturing a laminated film, a laminated film, and a magnetic recording medium. Specifically, the sputtering target contains Co and Pt as metal components, the molar ratio of the Pt content to the Co content is 5 / 100 to 45 / 100, and Nb2O5 is contained as a metal oxide component.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the PCT patent application entered into China with Chinese patent application number 2018800035543, invention name “Sputtering target, method for manufacturing laminated film, laminated film and magnetic recording medium”, and application date August 16, 2018. Technical Field

[0002] The present invention relates to a sputtering target containing Co and Pt as metal components and suitable for forming a magnetic layer on an intermediate layer of a perpendicular magnetic recording medium, for example, a method for manufacturing a laminated film, a laminated film and a magnetic recording medium, and in particular proposes a technology that can contribute to the high density of hard disk drives. Background Art

[0003] In hard disk drives, a perpendicular magnetic recording method that performs magnetic recording in a direction perpendicular to a recording surface has been put into practical use. Compared with the previous in-plane magnetic recording method, this method can perform higher-density recording and is therefore widely adopted.

[0004] The magnetic recording medium of the perpendicular magnetic recording method is generally composed of a bonding layer, a soft magnetic layer, a seed layer, a base layer such as a Ru layer, an intermediate layer, a magnetic layer, and a protective layer, which are stacked in order on a substrate such as aluminum or glass. Among them, the magnetic layer has a grain (グラニュラ) film of SiO2 or other metal oxides dispersed in a Co-Pt alloy with Co as the main component at the bottom, which has a high saturation magnetization Ms and magnetic anisotropy Ku. In addition, the intermediate layer stacked on the lower side of the magnetic layer is composed of a structure in which the same metal oxides are dispersed in a Co-Cr-Ru alloy, and sometimes contains relatively more Ru or Cr to become non-magnetic.

[0005] In such magnetic layers and intermediate layers, the metal oxides serving as nonmagnetic materials are precipitated at grain boundaries of magnetic grains such as Co alloys oriented in a perpendicular direction, thereby reducing magnetic interactions between magnetic grains, thereby achieving improved noise characteristics and higher recording density.

[0006] In general, each layer such as a magnetic layer or an intermediate layer is formed by sputtering a sputtering target having a specific composition or structure on a substrate. As such a technique, there is a prior art such as that described in Patent Document 1.

[0007] Background Art Literature

[0008] Patent Literature

[0009] Patent document 1: Japanese Patent No. 5960287. Summary of the invention

[0010] Problem that the invention aims to solve

[0011] Furthermore, in order to realize a higher density of hard disk drives, it is required to increase the magnetic anisotropy Ku to ensure thermal stability and to have higher magnetic separation of magnetic particles to improve resolution.

[0012] However, in the magnetic layer with a high saturation magnetization Ms as described above, the magnetic separation between the magnetic particles is insufficient because the exchange coupling between the magnetic particles is relatively strong. Here, if a large amount of metal oxide is added to improve the magnetic separation, the metal oxide enters the magnetic particles and causes the crystallinity of the magnetic particles to deteriorate, thereby reducing the saturation magnetization Ms and the magnetic anisotropy Ku.

[0013] The present invention aims to solve the problems existing in the prior art and aims to provide a sputtering target, a method for manufacturing a laminated film, a laminated film and a magnetic recording medium that can improve the magnetic separation between magnetic particles without significantly reducing the magnetic anisotropy of the magnetic layer of the magnetic recording medium.

[0014] Technical means of solving problems

[0015] The inventors have made great efforts to study and have obtained the following insights, that is, as a metal oxide of a non-magnetic material dispersed in the magnetic material of the magnetic layer and the intermediate layer, namely the Co alloy, in addition to or instead of SiO2, etc. used previously, Nb2O5 is used, thereby significantly improving the magnetic separation between magnetic particles even if the content of the metal oxide is not increased that much. In addition, it is found that the higher saturation magnetization Ms and higher magnetic anisotropy Ku of the magnetic layer with Co-Pt as the main body can be maintained. Furthermore, it is found that if both Nb2O5 and TiO2 are contained, the magnetic separation can be maintained and higher Ms and Ku can be obtained.

[0016] The reason is believed to be that the wettability of Nb2O5 and Co is moderate, and even if a part of O is missing, it can form a stable oxide, so the oxide will not enter the magnetic particles and can form grain boundaries with a uniform width around the magnetic particles, but the present invention is not limited to this theory.

[0017] Based on this knowledge, the sputtering target of the present invention contains Co and Pt as metal components, the molar ratio of the Pt content to the Co content is 5 / 100 to 45 / 100, and contains Nb2O5 as a metal oxide component.

[0018] The sputtering target of the present invention preferably further contains TiO 2 as a metal oxide component.

[0019] Here, in the sputtering target of the present invention, the content of Nb2O5 is preferably 0.5 mol% to 5 mol%. When TiO2 is contained, the content of TiO2 is preferably 0.5 mol% to 15 mol%.

[0020] Moreover, in the sputtering target of the present invention, it is preferable to have all phases containing Ti, Nb, and O.

[0021] In the sputtering target of the present invention, it is preferred that the sputtering target further contains at least one metal oxide of SiO2 and B2O3 as a metal oxide component, and the total content of the metal oxide including Nb2O5 is 20 vol% to 40 vol%.

[0022] Furthermore, in the sputtering target of the present invention, the molar ratio of the content of Pt to the content of Co is preferably 15 / 100 to 35 / 100.

[0023] The sputtering target of the present invention preferably contains Pt in an amount of 2 mol % to 25 mol %.

[0024] Furthermore, the sputtering target of the present invention may further contain 0.5 mol % to 20 mol % of Cr and / or Ru as a metal component.

[0025] The method for manufacturing a laminated film of the present invention includes: forming a magnetic layer on a base layer or an intermediate layer by sputtering using any of the sputtering targets described above, wherein the base layer contains Ru, and the intermediate layer is formed on the base layer by sputtering using a sputtering target containing Co and one or more metals selected from a group consisting of Cr and Ru as metal components.

[0026] The laminated film of the present invention comprises: a base layer containing Ru; and a magnetic layer directly formed on the base layer, or indirectly formed on the base layer via an intermediate layer containing Co and one or more metals selected from the group consisting of Cr and Ru as metal components, containing Co and Pt as metal components, and the molar ratio of Pt content to Co content is 5 / 100 to 45 / 100; the magnetic layer contains Nb2O5, and preferably contains TiO2 as a metal oxide component in addition to Nb2O5.

[0027] The magnetic recording medium of the present invention comprises the above-mentioned laminated film.

[0028] Effects of the Invention

[0029] According to the present invention, by containing at least Nb2O5, preferably Nb2O5 and TiO2 as metal oxide components, good magnetic separation between magnetic particles and high magnetic anisotropy Ku can be achieved at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic diagram showing the layer structure of the laminated film produced in the example.

[0031] Figure 2It is a graph showing the change of saturation magnetization Ms with respect to the Pt / Co ratio in Examples.

[0032] Figure 3 It is a graph showing the change of the magnetic anisotropy Ku with respect to the Pt / Co ratio in the example.

[0033] Figure 4 This is a graph showing the change in the slope α of the magnetization curve with respect to the Pt / Co ratio in the example.

[0034] Figure 5 This is a SEM / EDS mapping diagram of the target in the example.

[0035] Figure 6 This is a graph showing the results of identification of the crystal structure of the target in the example using XRD. DETAILED DESCRIPTION

[0036] Hereinafter, embodiments of the present invention will be described in detail.

[0037] A sputtering target according to one embodiment of the present invention is characterized in that it contains Co and Pt as metal components, the molar ratio of the Pt content to the Co content is 5 / 100 to 45 / 100, and contains Nb2O5 or Nb2O5 and TiO2 as metal oxide components.

[0038] More specifically, it has a structure in which a metal oxide containing Nb2O5 is dispersed in an alloy of Co and Pt. In the case of containing both TiO2 and Nb2O5, it has a structure in which a solid solution of TiO2 and Nb2O5 is dispersed as a metal oxide.

[0039] The sputtering target is particularly preferably used for forming a magnetic layer located on an intermediate layer of a magnetic recording medium in a perpendicular magnetic recording method. In this case, in the magnetic layer formed by sputtering using the sputtering target, the above-mentioned metal component constitutes magnetic particles, and the metal oxide containing Nb2O5 becomes a non-magnetic material and is uniformly distributed around the magnetic particles oriented in the perpendicular direction, effectively reducing the magnetic interaction between the magnetic particles.

[0040] (composition)

[0041] The metal component of the sputtering target is mainly composed of Co, and also contains Pt. The metal component is particularly a Co alloy containing Pt.

[0042] The content of Pt is preferably 2 mol% to 25 mol%. If the total content of Pt is too large, the magnetic anisotropy may be reduced or the crystallinity of the magnetic particles may be reduced. On the other hand, if the total content of Pt is too small relative to the ratio of Co, the magnetic anisotropy may become insufficient.

[0043] Pt is contained in an amount of 5 / 100 to 45 / 100 in a molar ratio relative to the content of Co. The reason is that, if the molar ratio of the content of Pt to the content of Co is less than 5 / 100 or exceeds 45 / 100, the magnetic anisotropy decreases. From this point of view, the molar ratio of the content of Pt to the content of Co is more preferably 15 / 100 to 35 / 100. Furthermore, if there is too much Co, there is a concern that the magnetic anisotropy decreases. On the other hand, if there is too little Co, there is a possibility that the saturation magnetization and the magnetic anisotropy decrease.

[0044] The sputtering target of the embodiment of the present invention may further contain Cr and / or Ru as metal components at 0.5 mol% to 20 mol%. By further containing such metals, there is an advantage that the saturation magnetization and magnetic anisotropy can be adjusted while maintaining the crystallinity of the magnetic particles. In addition, most of such metals are usually contained in the form of metal components, but there are also cases where a part of them is contained in the form of metal oxides due to oxidation during sintering during the following production.

[0045] Moreover, the sputtering target of the present invention contains at least Nb2O5 as a metal oxide component. Compared with SiO2 and the like, which are the main metal oxides in existing sputtering targets, Nb2O5 has moderately good wettability with Co and becomes a stable oxide even if a part of oxygen is missing. Therefore, by containing Nb2O5, magnetic anisotropy can be maintained and the separability of magnetic particles can be improved. Furthermore, by containing both Nb2O5 and TiO2, magnetic separability can be maintained and higher Ms and Ku can be obtained.

[0046] The content of Nb2O5 is preferably 0.5 mol% to 5 mol%. The reason is that, when the content of Nb2O5 is small, the above-mentioned effect may not be fully obtained, and on the other hand, when the content of Nb2O5 is large, there is a concern that the magnetic anisotropy is reduced. Therefore, the content of Nb2O5 is more preferably 0.5 mol% to 3 mol%.

[0047] When TiO2 is contained, it is preferably 0.5 mol% to 15 mol%. This is because, when the content of TiO2 is small, the above-mentioned effect may not be fully obtained, while when the content of TiO2 is large, the volume of the oxide increases, which may reduce the magnetic anisotropy.

[0048] Furthermore, the sputtering target more preferably has a phase containing all of Ti, Nb, and O. Examples of such a phase include a solid solution phase in which Nb is mixed in TiO2, or a solid solution phase in which Ti is mixed in Nb2O5, or a solid solution phase in which TiNb2O5 is mixed. 7、 TiNb6O 17 In addition, a part of oxygen may be missing at this time. The phase of mixed Ti, Nb, and O can be confirmed by, for example, element mapping using SEM / EDS, based on the intensity signals of Nb, Ti, and O from the same part. In addition, the solid solution phase or the composite oxide phase can also be confirmed by XRD evaluation using X-rays.

[0049] Furthermore, the sputtering target according to the embodiment of the present invention may contain metal oxides such as SiO2 and B2O3 as metal oxide components in addition to Nb2O5 and TiO2.

[0050] In the case of containing the above-mentioned metal oxides other than Nb2O5, the total content of all metal oxides including Nb2O5 is preferably 20vol% to 40vol%. If the total content of the metal oxides is less than 20vol%, there is a concern that the separation of the magnetic particles may become insufficient. On the other hand, if it exceeds 40vol%, there is a possibility that the saturation magnetization may decrease. For this reason, the total content of the metal oxides is further preferably 25vol% to 35vol%.

[0051] (Method for Manufacturing Sputtering Target)

[0052] The sputtering target can be produced by using a powder sintering method, and a specific example thereof is as follows.

[0053] First, as metal powder, Co powder, Pt powder, and other metal powders as described above are prepared as needed. The metal powder may be not only a powder of a single element but also a powder of an alloy, and preferably has a particle size in the range of 1 μm to 10 μm in order to be able to be uniformly mixed and prevent segregation and coarse crystallization. When the particle size of the metal powder is greater than 10 μm, the oxide particles described below may not be uniformly dispersed, and when the particle size is less than 1 μm, there is a concern that the sputtering target may deviate from the desired composition due to the influence of oxidation of the metal powder.

[0054] In addition, as oxide powder, at least Nb2O5 powder and at least one powder selected from the group consisting of TiO2 powder, SiO2 powder and B2O3 powder are prepared as needed. The oxide powder is preferably set to a particle size in the range of 1μm to 30μm. Thus, when mixed with the above-mentioned metal powder and pressure sintered, the oxide particles can be more uniformly dispersed in the metal phase. When the particle size of the oxide powder is greater than 30μm, coarse oxide particles may be generated after pressure sintering. On the other hand, when the particle size is less than 1μm, the oxide powders may agglomerate with each other.

[0055] Then, the metal powder and oxide powder are weighed so as to obtain a desired composition, mixed and crushed using a known method such as a ball mill. At this time, it is preferable to fill the inside of the container for mixing and crushing with an inert gas to suppress oxidation of the raw material powder as much as possible. In this way, a mixed powder in which a specific metal powder and oxide powder are uniformly mixed can be obtained.

[0056] Thereafter, the mixed powder obtained in this manner is pressurized and sintered in a vacuum environment or an inert gas environment to be formed into a specific shape such as a disk. Here, various pressure sintering methods such as hot pressing sintering, hot isostatic sintering, and plasma discharge sintering can be used. Among them, hot isostatic sintering is effective from the perspective of increasing the density of the sintered body.

[0057] The holding temperature during sintering is preferably set to a temperature range of 700 to 1500° C., and particularly preferably set to 800 to 1400° C. The time for holding the temperature in this range is preferably set to 1 hour or more.

[0058] The pressure applied during sintering is preferably 10 MPa to 40 MPa, more preferably 25 MPa to 35 MPa.

[0059] This allows the oxide particles to be dispersed more uniformly in the metal phase.

[0060] The sintered body obtained by the pressure sintering is subjected to mechanical processing such as cutting into a desired shape using a lathe or the like, whereby a sputtering target can be manufactured.

[0061] (Laminated Film)

[0062] The laminated film includes at least a base layer and a magnetic layer formed on the base layer.

[0063] More specifically, the underlayer contains Ru, and is generally composed of Ru, or is a layer having Ru as a main component.

[0064] An intermediate layer may be provided between the base layer and the magnetic layer. The intermediate layer contains Co and one or more metals selected from the group consisting of Cr and Ru as metal components, and the molar ratio of the content of the one or more metals selected from the group consisting of Cr and Ru to the content of Co is 1 / 2 or more. In addition, the intermediate layer preferably contains at least one metal selected from the group consisting of Nb2O5, TiO2, SiO2, B2O3, CoO, Co3O4, Cr2O3, Ta2O5, ZnO and MnO as a metal oxide component, and more preferably contains Nb2O5.

[0065] In addition, the content of Nb2O5 in the intermediate layer may be 5 mol% to 15 mol%, or when other metal oxides are contained, the content of Nb2O5 may be 2 mol% to 5 mol%. The intermediate layer may further contain the above-mentioned metal oxides other than Nb2O5, and the total content of the metal oxides including Nb2O5 may be 30 vol% or more.

[0066] The Co content of the intermediate layer may be 15 mol% to 60 mol%, and the total content of Cr and Ru may be 30 mol% to 60 mol%. In addition, the intermediate layer may further contain 2 mol% to 25 mol% of Pt as a metal component.

[0067] The magnetic layer preferably contains Co and Pt as metal components, the molar ratio of the Pt content to the Co content is 5 / 100 to 45 / 100, preferably 15 / 100 to 35 / 100, and contains Nb2O5 as a metal oxide component. By making the magnetic layer contain Nb2O5, the magnetic separation of the magnetic particles can be improved. Furthermore, if both Nb2O5 and TiO2 are contained, the magnetic separation can be maintained and Ms and Ku can be increased.

[0068] The magnetic layer can be formed by forming a film on the intermediate layer by sputtering using the above-mentioned sputtering target.

[0069] Therefore, similar to the above-mentioned sputtering target, the magnetic film preferably has a Nb2O5 content of 0.5 mol% to 5 mol%, and when containing TiO2, the TiO2 content is 0.5 mol% to 15 mol%. When further containing at least one metal oxide selected from the group consisting of SiO2 and B2O3 as a metal oxide component, the total content of metal oxides including Nb2O5 is 20 vol% to 40 vol%, and contains Pt at 2 mol% to 25 mol%, and further contains Cr and / or Ru as metal components at 0.5 mol% to 20 mol%.

[0070] (Method for producing laminated film)

[0071] Each layer of the laminated film can be formed by forming a film using a magnetron sputtering device or the like, using a sputtering target having a composition and structure corresponding to each layer.

[0072] Here, the intermediate layer of the laminated film is formed by forming a film on the base layer by sputtering using a sputtering target containing Co and one or more metals selected from the group consisting of Cr and Ru as metal components.

[0073] Furthermore, the magnetic layer of the laminated film can be formed on the intermediate layer by sputtering using the above-mentioned sputtering target.

[0074] (Magnetic Recording Media)

[0075] The magnetic recording medium has a laminated film having a base layer, an intermediate layer formed on the base layer, and a magnetic layer formed on the intermediate layer as described above. The magnetic recording medium is usually manufactured by sequentially forming a soft magnetic layer, a base layer, an intermediate layer, a magnetic layer, and a protective layer on a substrate such as aluminum or glass.

[0076] Example

[0077] Next, the sputtering target of the present invention was produced, and the effect of the magnetic layer formed using the sputtering target was confirmed, so the following description is given. However, the description here is for illustrative purposes only and is not intended to be limiting.

[0078] Using various sputtering targets, manufacturing Figure 1 A laminated film having the layer structure shown.

[0079] Here, Figure 1 The magnetic layers indicated by "Mag" in the figure were formed by sputtering targets having different compositions as shown in Table 1, and the saturation magnetization Ms, magnetic anisotropy Ku, and slope α of the magnetization curve of the magnetic layer in the laminated film having the magnetic layers were measured.

[0080] Here, the saturation magnetization Ms and the slope α of the magnetization curve were measured by a sample vibration type magnetometer (VSM) manufactured by Tamagawa Manufacturing Co., Ltd., and the magnetic anisotropy Ku was measured by a torque magnetometer (TRQ) manufactured by Tamagawa Manufacturing Co., Ltd. In addition, the volume ratio of the oxide was calculated by estimating the volume of the entire target and the volume of the oxide based on the density and weight of the raw material powder, and the ratio of these was calculated.

[0081] In Table 1, "×" in the item of "Effect" means that there is no effect of reducing α, "○" means that there is an effect of reducing α, and "◎" means that there is a significant effect of reducing α.

[0082] Table 1

[0083]

[0084] From the results shown in Table 1, it can be seen that in Invention Examples 1 to 26 containing Nb2O5, relatively high saturation magnetization Ms and magnetic anisotropy Ku are maintained and the slope α of the magnetization curve is effectively reduced. In contrast, in Comparative Examples 1 to 15 not containing Nb2O5, the slope α of the magnetization curve is not reduced.

[0085] In addition, regarding Inventive Examples 1 to 12 and Comparative Examples 1 to 12 in Table 1, the changes in saturation magnetization Ms, magnetic anisotropy Ku, and the slope α of the magnetization curve with respect to the Pt / Co ratio were confirmed. Figures 2 to 4 Each of them is represented by a curve graph.

[0086] Furthermore, two graphs (corresponding to Invention Examples 19 and 18, respectively) showing the SEM / EDS mapping of the target and the identification results of the crystal structure of the target using XRD are shown in FIG. Figure 5 and Figure 6 For reference only.

[0087] As described above, according to the present invention, it is possible to improve the magnetic segregation between magnetic grains without significantly reducing the magnetic anisotropy of the magnetic layer of the magnetic recording medium.

Claims

1. A sputtering target comprising Co and Pt as metal components, wherein the molar ratio of the content of Pt to the content of Co is 5 / 100 to 45 / 100, and comprising Nb2O5 as a metal oxide component, wherein the content of Nb2O5 is 0.5 mol% to 5 mol%, It further contains Cr as a metal component, and the content of Cr is 3.6 mol% or less, or contains no Cr.

2. The sputtering target according to claim 1, further comprising TiO2 as a metal oxide component.

3. The sputtering target according to claim 2, wherein: The content of TiO2 is 0.5mol% to 15mol%. The sputtering target according to claim 2 , comprising a phase containing all of Ti, Nb and O.

5. The sputtering target according to claim 1 or 2, further comprising at least one metal oxide of SiO2 and B2O3 as a metal oxide component, and the total content of the metal oxide including Nb2O5 is 20 vol% to 40 vol%.

6. The sputtering target according to claim 1 or 2, wherein: The molar ratio of the Pt content to the Co content is 15 / 100 to 35 / 100. 7 . The sputtering target according to claim 1 , comprising Pt in an amount of 2 mol % to 25 mol %. 8 . The sputtering target according to claim 1 , further comprising 0.5 mol % to 20 mol % of Cr and / or Ru as a metal component.

9. A method for manufacturing a laminated film, comprising: A magnetic layer is formed on a base layer or an intermediate layer by sputtering using a sputtering target according to any one of claims 1 to 8, wherein the base layer contains Ru, and the intermediate layer is formed on the base layer by sputtering using a sputtering target containing Co and one or more metals selected from the group consisting of Cr and Ru as metal components.

10. A laminated film comprising: Base layer: contains Ru; and A magnetic layer: formed directly on the base layer, or indirectly on the base layer via an intermediate layer containing Co and one or more metals selected from the group consisting of Cr and Ru as metal components, containing Co and Pt as metal components, and the molar ratio of the content of Pt to the content of Co is 5 / 100 to 45 / 100; The magnetic layer contains Nb2O5 as a metal oxide component, and the content of Nb2O5 is 0.5 mol% to 5 mol%.

11. The laminated film according to claim 10, wherein The magnetic layer further contains TiO2 as a metal oxide component.

12. A magnetic recording medium comprising the laminated film according to claim 10 or 11.