Perovskite solar cell, preparation method and electronic device
By forming a hole transport layer with high coverage in a perovskite solar cell, the problem of low coverage of SAM layer is solved, device performance and stability is improved, and photoelectric conversion is achieved efficiency.
Patent Information
- Application Number
- CN202411040355.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
The coverage of self-assembled single-molecular layer (SAM layer) in existing perovskite solar cells is low, resulting in direct contact between the perovskite layer and the metal oxide layer, causing perovskite decomposition and carrier recombination, affecting device performance.
By performing self-assembly and removal operations on the transparent conductive oxide film multiple times, the anchor layer and self-assembled single molecule layer form a high coverage hole transport layer, which improves the coverage of the SAM layer and isolates the perovskite layer and metal Contact of oxides to optimize device performance.
It significantly improves the coverage of the SAM layer and device performance, and enhances the stability of the device and photoelectric conversion efficiency.
Smart Images

Figure CN118984629A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of solar cells, and in particular to a perovskite solar cell, a preparation method and an electronic device. Background Art
[0002] Organic-inorganic metal halide perovskite solar cells have excellent optoelectronic properties and potential low-cost manufacturing characteristics, making them a very promising type of solar cell. In addition, the band gap of perovskite materials is adjustable and can be stacked with perovskite materials themselves or other photovoltaic materials to form a stacked solar cell, thereby achieving higher photoelectric conversion efficiency.
[0003] Because the inverted device has less parasitic absorption, good stability, and requires a lower temperature in the preparation process, and can also be used in crystalline silicon to form stacked cells, it has attracted extensive attention from researchers and related industry personnel. However, the positive device is not suitable for practical applications due to the irreplaceability of spiro-OmeTAD and strong parasitic absorption. Therefore, the inverted structure is often used to prepare single-junction perovskite solar cells or perovskite crystalline silicon stacked cells.
[0004] At present, inversion devices often use the method of metal oxide plus self-assembled monolayer (SAM layer) to prepare the hole selective transport layer. The SAM layer can effectively isolate the direct contact between the metal oxide and the perovskite layer to avoid the decomposition of the perovskite layer and the metal oxide layer. At the same time, the synthesis method of the hole selective transport layer is relatively simple, and the raw materials used to prepare the hole selective transport layer consume little and have low cost, making it a very promising hole selective transport layer material.
[0005] The solubility of self-assembled monolayer materials (SAM materials) in ethanol or isopropanol is low, and they will spontaneously aggregate into cluster structures in the solution, resulting in a low coverage of the formed SAM layer. The coverage of the SAM layer on the substrate surface greatly affects the performance of the device. The lower the coverage, the larger the direct contact area between the perovskite layer and the metal oxide, which will lead to a large amount of perovskite decomposition and a large amount of carrier recombination, which is not conducive to the performance of the device. Summary of the invention
[0006] The present application aims to solve one of the technical problems in the related art at least to a certain extent. To this end, one object of the present application is to provide a perovskite solar cell, a preparation method and an electronic device.
[0007] The first aspect of the present application provides a method for preparing a perovskite solar cell, characterized in that it comprises the following operations:
[0008] Performing a monomolecular material self-assembly operation: attaching a self-assembled monomolecular material to one side of the transparent conductive oxide film, allowing the self-assembled monomolecular material to react to form a self-assembled monolayer on the transparent conductive oxide film, so as to complete the self-assembly of a single monolayer;
[0009] Performing a removal operation: removing the self-assembled monomolecular material that is not anchored on the transparent conductive oxide film;
[0010] Repeating the single-molecule material self-assembly operation and the removal operation, and independently performing the second single-molecule material self-assembly to the (n-1)th single-molecule material self-assembly; wherein n is a preset number of single-molecule material self-assemblies;
[0011] After the (n-1)th self-assembly of the single molecule material, the self-assembly operation of the single molecule material is repeated to perform the nth self-assembly of the single molecule material to obtain a hole transport layer on the transparent conductive oxide film.
[0012] In the first aspect of the present application, multiple depositions and reactions are performed on a transparent conductive oxide film to prepare a SAM layer. The self-assembled monomolecular material is easily chemically bonded with the active groups (hydroxyl and carboxyl groups, etc.) on the surface of the conductive oxide, and then anchored on the surface of the transparent conductive oxide film. After a single deposition and reaction, the self-assembled monomolecular material not anchored on the transparent conductive oxide film is removed, so that the unanchored transparent conductive oxide film surface is exposed, and then the unanchored surface is filled through multiple depositions and reactions, thereby increasing the coverage of the SAM layer on the transparent conductive oxide film through multiple deposition reactions, thereby optimizing the device performance. This method is universal and easy to promote and apply on a large scale.
[0013] Furthermore, the method for preparing the perovskite solar cell also includes:
[0014] An anchoring layer is deposited on one side of the transparent conductive oxide film to obtain a hole transport layer including the anchoring layer and a self-assembled monolayer; wherein the self-assembled monolayer formed by the first self-assembly is located on the side of the anchoring layer away from the transparent conductive oxide film; and the material of the anchoring layer includes a conductive metal oxide. Thus, an anchoring layer is deposited on the transparent conductive oxide film, and the anchoring layer has more active sites, which is more conducive to the anchoring of the self-assembled monolayer, thereby improving production efficiency.
[0015] The second aspect of the present application provides a perovskite solar cell, which is prepared according to the preparation method described in the first aspect. Thus, due to the high coverage of the SMA layer, the device performance is improved.
[0016] In some embodiments, an inverted single-junction perovskite solar cell and a crystalline silicon perovskite tandem solar cell are included. Thus, multiple types of solar cells are obtained.
[0017] A third aspect of the present application provides an electronic product, whose power supply device includes the perovskite solar cell described in the second aspect.
[0018] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0020] Figure 1 This is a diagram of the structure of an inverted perovskite solar cell;
[0021] Figure 2 This is a diagram of the structure of an inverse perovskite and crystalline silicon stacked solar cell;
[0022] Figure 3 are flow diagrams of some embodiments.
[0023] Figure numerals: 100 - first transparent conductive oxide film; 110 - HTL layer; 120 - PVK layer; 130 - electron transport layer; 131 - hole blocking layer; 140 - protective layer; 150 - third transparent conductive oxide film; 160 - first metal gate line layer; 170 - anti-reflection layer; 180 - second transparent conductive oxide film; 190 - second metal gate line layer; 200 - N-type silicon wafer; 210 - first intrinsic amorphous silicon layer; 220 - n-type amorphous silicon; 230 - second intrinsic amorphous silicon layer; 240 - p-type amorphous silicon layer. DETAILED DESCRIPTION
[0024] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present application, and should not be construed as limiting the present application.
[0025] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of the application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the description of the present application, the meaning of "several" is at least one, such as one, two, etc., unless otherwise clearly and specifically defined.
[0026] As used herein, "includes," "comprising," "including," "containing," "having," or other variations are intended to encompass non-closed inclusions, and no distinction is made between these terms. The term "comprising" means that other steps and ingredients that do not affect the end result may be added. The term "comprising" also includes the terms "consisting of" and "consisting essentially of." The compositions and methods / processes of the present application include, consist of, and consist essentially of the essential elements and limitations described herein, as well as any additional or optional ingredients, components, steps, or limitations described herein. As used herein, no distinction is made between the terms "efficacy," "performance," "effect," and "efficacy."
[0027] The words "preferably", "more preferably" and the like in this application refer to embodiments of the present application that may provide certain beneficial effects in certain circumstances. However, other embodiments may also be preferred under the same circumstances or in other circumstances. In addition, the statement of one or more preferred embodiments does not imply that other embodiments are not available, nor is it intended to exclude other embodiments from the scope of this application.
[0028] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0029] Explanation of the name:
[0030] Self-Assembled Monolayer (SAM) is an ordered monolayer that is spontaneously formed on a solid surface through intermolecular interactions. The SAM layer can be composed of molecules with specific active groups that can spontaneously self-assemble on a solid surface (such as a metal, oxide, or semiconductor material) to form a highly ordered monolayer structure.
[0031] The inventors have learned that there are the following improvement measures for preparing a SAM layer with high coverage on a transparent conductive glass or anchoring layer: 1. Use a mixed SAM material to mix SAM materials of different molecular sizes, and small SAM materials fill the gaps caused by large SAM materials, thereby improving the overall coverage; 2. Adjust the solubility of the SAM material to increase the solubility of the SAM material in the solution and reduce the clustering phenomenon, so that the SAM layer prepared on the metal oxide is more uniform; 3. Adjust the structure of the SAM material to obtain a SAM material with a greater intermolecular force in the parallel direction, thereby increasing the density of the SAM layer prepared on the metal oxide; 4. Use a mixed solvent to add a solvent with a greater solubility for the SAM material to the ethanol or isopropanol solution of the SAM material to reduce the clustering phenomenon of the SAM material in the alcohol solution, thereby obtaining a denser SAM layer. Among the above improvement measures, adjusting the structure of the SAM material requires designing a specific SAM structure, and the universality is not strong; and for mixed SAM materials and mixed solvents, the coverage of the SAM is improved to a certain extent, but the coverage improvement is not significant.
[0032] Accordingly, in a first aspect of the present application, a method for preparing a perovskite solar cell is proposed.
[0033] In some embodiments, see Figure 3 , a method for preparing a perovskite solar cell, comprising the following operations:
[0034] S1. providing a transparent conductive oxide film;
[0035] S2, performing a monomolecular material self-assembly operation: attaching a self-assembled monomolecular material to one side of the transparent conductive oxide film, allowing the self-assembled monomolecular material to react to form a self-assembled monolayer on the transparent conductive oxide film, so as to complete the self-assembly of a single monolayer;
[0036] S3, performing a removal operation: removing the self-assembled monomolecular material that is not anchored on the transparent conductive oxide film;
[0037] S4, repeating the single molecule material self-assembly operation and the removal operation, and independently performing the second single molecule material self-assembly to the (n-1)th single molecule material self-assembly; wherein n is a preset number of single molecule material self-assembly;
[0038] S5. After the (n-1)th self-assembly of the single molecule material, repeat the self-assembly operation of the single molecule material to perform the nth self-assembly of the single molecule material to obtain a hole transport layer located on the transparent conductive oxide film.
[0039] In the first aspect of the present application, multiple depositions and reactions are performed on a transparent conductive oxide film to prepare a SAM layer. Since the transparent conductive oxide film contains conductive oxides, the self-assembled monomolecular material is easy to chemically bond with the active groups (hydroxyl and carboxyl groups, etc.) on the surface of the conductive oxide, and then anchored on the surface of the transparent conductive oxide film. After a single deposition and reaction, the self-assembled monomolecules not anchored on the transparent conductive oxide film are removed, so that the unanchored transparent conductive oxide film surface is exposed, and then the unanchored surface is filled through multiple depositions and reactions, thereby increasing the coverage of the SAM layer on the transparent conductive oxide film through multiple deposition reactions, thereby better isolating the contact between the perovskite layer and the transparent conductive oxide film, avoiding the decomposition of the perovskite and the recombination of the carriers, and optimizing the device performance. The method has universal applicability, is easy to promote and apply on a large scale, effectively increases the coverage of the SAM layer on the transparent conductive oxide film, and can significantly improve the device performance and stability.
[0040] In some embodiments, the method for preparing the perovskite solar cell further comprises:
[0041] An anchor layer is deposited on one side of the transparent conductive oxide film to obtain a hole transport layer including the anchor layer and a self-assembled monolayer; wherein the self-assembled monolayer formed by the first self-assembly is located on the side of the anchor layer away from the transparent conductive oxide film; the material of the anchor layer includes a conductive metal oxide. In this embodiment, an anchor layer is deposited on the transparent conductive oxide film, and the anchor layer has more active groups, which is more conducive to the anchoring of the self-assembled monolayer and improves production efficiency.
[0042] Furthermore, the conductive metal oxide comprises NiO x , Al2O3, CuO2, CuO, CuAlO2, CuCrO2, WO3, MoO c 、V2O5、VO d CrO e One or more of. It is understood that the above metal oxides all refer to metal oxides with conductivity. When the metal oxide itself does not have conductivity, it can be modified by doping to obtain a conductive metal oxide. Preferably, 1≦x≦2. Thus, NiO x Has good electrical conductivity.
[0043] In some embodiments, the hole transport layer may include a self-assembled monolayer, and may also include a self-assembled monolayer and an anchoring layer. Further, the thickness of the hole transport layer is 0.1nm to 300nm, for example, it can be 3nm, 5nm, 50nm, 100nm, 150nm, 200nm, 250nm, 300nm, etc. Further, when the hole transport layer is a SAM layer, the thickness is 0.1nm to 10nm; and when the hole transport layer is an anchoring layer and a SAM layer, the thickness is 1nm to 300nm. This is conducive to the transmission and collection of holes.
[0044] In some embodiments, in the method for preparing the perovskite solar cell, a deposition method is used in S2 to attach the self-assembled monomolecular material to the transparent conductive oxide film. Specifically, the deposition method includes at least one of a solution method and an evaporation method. Thus, the self-assembled monomolecular material or a solution containing the self-assembled monomolecular material is attached to the transparent conductive oxide film or the anchoring layer, which facilitates subsequent anchoring.
[0045] Furthermore, the solution method includes one or more of spin coating, blade coating, printing, spray coating, spray pyrolysis, slit coating, and evaporation. Thus, the solution containing the self-assembled monomolecular material is attached to the transparent conductive oxide film or the anchoring layer. Exemplarily, a spin coating method can be used to first cover the solution containing the self-assembled monomolecular material on the substrate (transparent conductive oxide film or anchoring layer) for 30 seconds, and then rotate at a speed of 4000 rpm for 10 seconds to complete the attachment of the solution containing the self-assembled monomolecular material.
[0046] Furthermore, the solvent used in the solution method can be selected by those skilled in the art as needed. As some examples, the solvent used in the solution method includes one or more of isopropanol, ethanol, chlorobenzene, n-butanol, ethyl acetate, acetone, benzyl chloroformate, methyl nylonate, acetonitrile, tetramethylsilane, N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), and acetonitrile.
[0047] In some embodiments, in S2 of the method for preparing the perovskite solar cell, the self-assembly condition includes annealing at a temperature of 80°C to 200°C for 10 min to 100 min. For example, the annealing temperature is 50°C, 100°C, 150°C, 200°C, etc., and the annealing time is 10 min, 30 min, 50 min, 60 min, 100 min, etc. Under the reaction conditions, the self-assembled monomolecular material can be chemically bonded to the surface of the transparent conductive oxide film or the anchoring layer to form a tightly arranged two-dimensional ordered monomolecular layer.
[0048] In some embodiments, the operation of removing the self-assembled monomolecules not anchored on the transparent conductive oxide film in S2 of the method for preparing a perovskite solar cell includes: washing with a solvent, followed by spin coating and drying to remove the washing solvent. For example, ethanol may be used for washing.
[0049] In some embodiments, in the method for preparing the perovskite solar cell, in S2, the number of self-assembly n is greater than or equal to 2 to improve the coverage of the self-assembled monolayer. Preferably, 2≦n≦5, for example, it can be 2 times, 3 times, 4 times, 5 times, after 2 to 5 times of self-assembly, the coverage of the self-assembled monolayer is significantly improved, and the coverage improvement is relatively limited when the number of self-assembly is increased.
[0050] In some embodiments, in the preparation method of the perovskite solar cell, the chemical formula of the perovskite in the perovskite layer described in S2 is ABX3, A is a monovalent cation, including but not limited to a mixture of one or several monovalent cations of cesium (Cs), rubidium (Rb), methylamine (CH3NH3), and guanidine (CH2(NH2)2); B is a divalent cation, including but not limited to a mixture of one or several divalent cations of lead (Pb), copper (Cu), zinc (Zn), gallium (Ga), tin (Sn), and calcium (Ca); X is a monovalent anion, including but not limited to a mixture of one or several monovalent anions of iodine (I), bromine (Br), chlorine (Cl), fluorine (F), and thiocyanate ion (SCN).
[0051] It is understood that the above self-assembled monomolecular materials refer to organic, inorganic molecules or ions in solution or gas phase through chemical bonds to form a tightly arranged two-dimensional ordered monolayer formed by spontaneous adsorption on a solid surface, with a thickness of about several nanometers, a simple preparation method and high stability. In some embodiments, the self-assembled monomolecular materials used for at least two monomolecular material self-assemblies are the same, that is, the self-assembled monomolecular materials used for the first self-assembly to the nth self-assembly can have the same materials used twice, the same materials used three times, ..., and the materials used for n times are the same. In other embodiments, the self-assembled monomolecular materials used for at least two monomolecular material self-assemblies are different, that is, the self-assembled monomolecular materials used for the first self-assembly to the nth self-assembly can have different materials used twice, different materials used three times, ..., and different materials used for n times. Thus, the self-assembled monomolecular materials used for each self-assembly are independently selected, and those skilled in the art can select as needed. Further, the self-assembled monomolecular materials include at least one of the self-assembled monomolecular materials containing phosphonic acid groups, self-assembled monomolecular materials of hydroxyl groups, and self-assembled monomolecular materials of carboxylic acid groups. As some examples, the self-assembled monomolecular materials containing phosphonic acid groups include one or more of [2-(9H-carbazole-9-yl)ethyl]phosphonic acid (2PACz), [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid (MeO-2PACz), and [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACz); and the self-assembled monomolecular materials containing carboxylic acid groups include one or more of benzoic acid and 4-[bis(2,4-dimethoxybiphenyl-4-yl)amino]-biphenyl-4-carboxylic acid [MC-43]; the self-assembled monomolecular materials containing hydroxyl groups include one or more of dopamine (CAS No.: 62-31-7) and diethanolamine (CAS No.: 111-42-2). Furthermore, the self-assembled monomolecular material deposited each time can be a single self-assembled monomolecular material or a combination of multiple self-assembled monomolecular materials. For example, the self-assembled monomolecular material used in the first deposition may be 2PACz, and the self-assembled monomolecular material used in the second self-assembly may be at least one of Me-4PACz, MeO-2PACz, and 2PACz.
[0052] In addition, the method for preparing the perovskite solar cell, when used to prepare an inverted single-junction perovskite solar cell, also includes the necessary steps in the preparation process of the perovskite solar cell, such as preparing a perovskite layer, an electron transport layer, and an electrode. When used to prepare a laminated crystalline silicon perovskite solar cell, it also includes the necessary steps in the preparation process of the perovskite solar cell, such as preparing amorphous silicon, a perovskite layer, an electron transport layer, and a metal grid line layer. Those skilled in the art can also add some optimization measures according to needs, such as introducing a perovskite passivation layer, an anti-reflection layer on the top of the device, etc.
[0053] In some embodiments, the method for preparing a perovskite solar cell further includes the following operations after S5:
[0054] Prepare a perovskite layer on a side of the hole transport layer away from the transparent conductive oxide film;
[0055] Depositing an electron transport layer on a side of the perovskite layer away from the hole transport layer;
[0056] Wherein, the perovskite layer is a pin inversion structure.
[0057] Optionally, the electron transport layer material includes n-type single crystal silicon, n-type polycrystalline silicon, n-type amorphous silicon, TiO2, SnO2, ZnO, ZrO2, gallium zinc oxide (GZO), indium zinc oxide (IZO), fluorine-doped SnO2 (FTO), indium tin oxide (ITO), BaSnO3, TiSnO a SnZnO b , fullerenes and their derivatives or more.
[0058] Preferably, TiSnO a a in SnZnO is 1 to 4; b Where b is 1 to 3.
[0059] Furthermore, the fullerene and its derivatives include one or more of C60, C70, and PCBM.
[0060] Optionally, the thickness of the electron transport layer is 1 nm to 300 nm, for example, 5 nm, 50 nm, 100 nm, 200 nm, 300 nm, etc. This facilitates the transport and collection of electrons.
[0061] Regardless of inverted single-junction perovskite solar cells or stacked crystalline silicon perovskite solar cells, they both contain a SAM layer. The first aspect of the present application is applicable to inverted single-junction perovskite solar cells and stacked crystalline silicon perovskite solar cells to increase the coverage of the SAM layer therein and improve device performance.
[0062] See also Figure 1 , Figure 1 It is a structural diagram of an inverted perovskite solar cell. The inverted perovskite solar cell includes an HTL layer (hole transport layer) 110, a PVK layer (perovskite layer) 120, an electron transport layer 130 and a hole blocking layer 131 which are stacked in sequence on one side of a first transparent conductive oxide film 100. A first metal grid line layer 160 is provided on a side of the hole blocking layer 131 away from the electron transport layer 130, and a second metal grid line layer 190 is provided on a side of the first transparent conductive oxide film 100 away from the hole blocking layer 131.
[0063] See also Figure 2 , Figure 2 The invention is a structural diagram of an inverted perovskite and crystalline silicon stacked solar cell, which includes an N-type silicon wafer 200. A first intrinsic amorphous silicon layer 210, an n-type amorphous silicon layer 220, a first transparent conductive oxide film 100, an HTL layer 110, a PVK layer 120, an electron transport layer 130, a protective layer 140 and a third transparent conductive oxide film 150 are sequentially stacked on one side of the N-type silicon wafer 200. A first metal grid line layer 160 and an anti-reflection layer 170 are provided on a side of the third transparent conductive oxide film 150 away from the protective layer 140. A second intrinsic amorphous silicon layer 230, a p-type amorphous silicon layer 240 and a second transparent conductive oxide film 180 are sequentially stacked on the other side of the N-type silicon wafer 200. A second metal grid line layer 190 is provided on a side of the second transparent conductive oxide film 180 away from the p-type amorphous silicon layer 240. The materials of the first transparent conductive oxide film 100 , the second transparent conductive oxide film 180 , and the third transparent conductive oxide film 150 may be completely the same or may not be completely the same, for example, they may be ITO, FTO, indium-doped cadmium oxide (ICO), etc.
[0064] The above HTL layer 110 may include a self-assembled monolayer, and may also include a self-assembled monolayer and an anchor layer.
[0065] The second aspect of the present application provides a perovskite solar cell, which is prepared according to the preparation method described in the first aspect. As a result, the self-assembled monolayer has a high coverage on the substrate (transparent conductive oxide film or anchoring layer), so that the device has good performance, and the fill factor and photoelectric conversion efficiency are improved.
[0066] Specifically, the perovskite solar cell includes an inverted single-junction perovskite solar cell and a crystalline silicon perovskite stacked solar cell.
[0067] In a third aspect of the present application, an electronic product is provided, wherein the power supply device comprises the perovskite solar cell described in the second aspect. The electronic product may be, but is not limited to, a watch, a smart phone, a telephone, a television, a video player (VCD, SVCD, DVD), a video recorder, a camcorder, a radio, a radio recorder, a combination speaker, a laser player (CD), a computer, a game console, and a mobile communication product.
[0068] The present application is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present application in any way.
[0069] Example 1
[0070] A method for preparing an inverted single-junction perovskite solar cell
[0071] (1) providing an ITO glass substrate with a substrate size of 2.5 cm×2.5 cm, cleaning, drying, and UV-ozone treatment for 20 min, i.e., a first transparent conductive oxide film 100;
[0072] (2) Deposition of NiO on the front side of the ITO glass substrate by magnetron sputtering x , with a thickness of 15 nm, which is the anchoring layer;
[0073] (3) NiO was prepared by one-step spin coating in a nitrogen glove box. x A self-assembled SAM layer was deposited on the NiO layer. A 0.5 mg / mL Me-4PACz solution (volume ratio of ethanol:DMF=97:3) was covered on the NiO x The substrate was placed on the substrate for 30 seconds, then rotated at 4000 rpm for 10 seconds, annealed at 100°C for 10 minutes, and washed with ethanol after cooling. Specifically, ethanol was dripped on the substrate, then rotated at 4000 rpm for 20 seconds, and dried at 100°C for 5 minutes. The above operation was repeated once without washing to obtain an HTL layer 110 consisting of an anchor layer and a SAM layer (about 1 nm);
[0074] (4)With FA 0.8 Cs 0.2 Pb(I 0.8 Br 0.2 )3 is a chemical formula, CsI, FAI (iodoformamide), PbI2 and PbBr2 are dissolved in a mixed solvent of DMF and DMSO (the volume ratio of DMF and DMSO is 4:1) at a concentration of 1.5 M of Pb, and then methyl ammonium chloride (MACl) is added at a concentration of 60 mg / mL, and stirred for 6 hours to obtain a perovskite precursor solution;
[0075] (5) in a nitrogen glove box, the perovskite precursor solution is dropped onto the substrate, and then spin-coated. Specifically, the substrate is firstly rotated at 500 rpm for 5 s, then at 4000 rpm for 50 s, and then at 5000 rpm for 40 s, chlorobenzene is flushed onto the surface of the substrate, and finally annealed at 120° C. for 20 min to form a perovskite layer, i.e., a PVK layer 120;
[0076] (6) dissolving 1,3-propylenediamine hydroiodide in IPA (isopropyl alcohol) to prepare a 0.5 mg / mL solution, and spin-coating the solution on the perovskite surface at 4000 rpm for 30 s in a nitrogen glove box, followed by annealing on a hot plate at 100° C. for 2 min to complete the passivation of the PVK layer 120 ;
[0077] (7) A C60 layer is formed by thermal evaporation, with a total thickness of 30 nm, which is the electron transport layer 130;
[0078] (8) a BCP layer using a thermal evaporation method with a total thickness of 6 nm, i.e., a hole blocking layer 131;
[0079] (9) A Ag metal electrode layer with a thickness of 200 nm is prepared by thermal evaporation, a first metal grid line layer 160 is prepared on the hole blocking layer 131, and a second metal grid line layer 190 is prepared on the first transparent conductive oxide film 100, thereby completing the preparation of an inverted single-junction perovskite solar cell.
[0080] Example 2
[0081] A method for preparing a laminated crystalline silicon perovskite solar cell
[0082] (1) Providing an N-type silicon wafer 200 with a size of 2.5 cm×2.5 cm and a velvet thickness of less than 1 um;
[0083] (2) using PECVD to sequentially prepare a 10 nm thick first intrinsic amorphous silicon 210 and a 15 nm thick n-type amorphous silicon 220 on the front side of the N-type silicon wafer;
[0084] (3) using PECVD to sequentially prepare a 10 nm thick second intrinsic amorphous silicon 230 and a 10 nm thick p-type amorphous silicon 240 on the back side of the N-type silicon wafer 200;
[0085] (4) preparing a transparent conductive oxide film of TCO on the front side by sputtering, i.e., a first transparent conductive oxide film 100, with a thickness of 10 nm;
[0086] (5) Preparation of NiO on the front side by magnetron sputtering x , i.e. the anchoring layer, with a thickness of 15 nm;
[0087] (6) NiO was prepared by one-step spin coating in a nitrogen glove box. xA self-assembled SAM layer was deposited on the substrate, and a 0.5 mg / mL Me-4PACz solution (the solvent was ethanol:DMF=97:3 by volume) was covered on the substrate for 30 seconds, and then rotated at a speed of 4000 rpm for 10 seconds, annealed at 100°C for 10 minutes, and washed with ethanol after cooling. During washing, ethanol was dripped on the substrate, and the substrate was rotated at a speed of 4000 rpm for 20 seconds, and annealed at 100°C for 5 minutes. The above operation was repeated twice, and the last time was not washed, to obtain a HTL layer 110 consisting of an anchor layer and a SAM layer (1 nm);
[0088] (7)With FA 0.8 Cs 0.2 Pb(I 0.8 Br 0.2 )3 is a chemical formula, CsI, FAI, PbI2 and PbBr2 are dissolved in a mixed solvent of DMF and DMSO with a volume ratio of 4:1 according to a Pb concentration of 1.5 M, and then methyl ammonium chloride (MACl) is added at a concentration of 60 mg / mL, and stirred for 6 hours to prepare a perovskite precursor solution;
[0089] (9) In a nitrogen glove box, the perovskite precursor solution was dropped onto the substrate for spin coating, first at 500 rpm for 5 s, then at 4000 rpm for 50 s, and then at 5000 rpm for 40 s, chlorobenzene was flushed onto the surface of the substrate, and then annealed at 120° C. for 20 min to form a perovskite layer, i.e., PVK layer 120;
[0090] (10) 1,3-Propylenediamine hydroiodide was dissolved in IPA to prepare a 0.5 mg / mL solution, and the solution was spin-coated on the perovskite surface at a speed of 4000 rpm for 30 s in a nitrogen glove box, followed by annealing on a hot plate at 100 °C for 2 min to prepare a passivation layer;
[0091] (11) A C60 layer is formed by thermal evaporation, with a total thickness of 15 nm, which is the electron transport layer 130;
[0092] (12) SnO2 is prepared by atomic layer deposition with a thickness of 12 nm, i.e., the protective layer 140;
[0093] (13) preparing IZO by sputtering method with a thickness of 40 nm, i.e., the third transparent conductive oxide film 150;
[0094] (14) preparing a transparent conductive oxide film of ITO on the back side by sputtering, i.e., the second transparent conductive oxide film 180, with a thickness of 10 nm;
[0095] The top Ag metal gate line layer and the bottom Ag metal gate line layer are prepared by thermal evaporation method, and the thickness of the first metal gate line layer 160 and the second metal gate line layer 190 are 400 nm respectively;
[0096] (15) A 100 nm thick MgF2 layer is prepared on the top by thermal evaporation as an anti-reflection layer 170 to complete the preparation of the stacked crystalline silicon perovskite solar cell.
[0097] Example 3
[0098] The other operations are the same as those in Example 1, except that there is no step (2).
[0099] Comparative Example 1
[0100] The other operations are the same as those in Example 1, except that step (3) is: a one-step spin coating method is used in a nitrogen glove box to coat NiO x A self-assembled SAM layer was deposited on the NiO layer. A 0.5 mg / mL Me-4PACz solution (volume ratio of ethanol:DMF=97:3) was covered on the NiO x The film was layered for 30 s, then spun at 4000 rpm for 20 s and annealed at 100 °C for 20 min.
[0101] Comparative Example 2
[0102] The other operations are the same as those in Example 2, except that step (6) is: a one-step spin coating method is used in a nitrogen glove box to coat NiO x A self-assembled SAM layer was deposited on the layer, and a 0.5 mg / mL Me-4PACz solution (solvent volume ratio of ethanol:DMF=97:3) was covered on the substrate for 30 s, then rotated at 4000 rpm for 30 s and annealed at 100°C for 30 min.
[0103] Comparative Example 3
[0104] The other operations are the same as those in Example 3, except that step (3) is as follows: a self-assembled SAM layer is deposited on the ITO layer by a one-step spin coating method in a nitrogen glove box, and a 0.5 mg / mL Me-4PACz solution (volume ratio of ethanol:DMF=97:3) is covered on the NiO x The film was layered for 30 s, then spun at 4000 rpm for 20 s and annealed at 100 °C for 20 min.
[0105] Test methods and test results
[0106] The current-voltage curves of the batteries prepared in the above embodiments and comparative examples were tested to obtain photovoltaic data. The specific testing method was to place the battery under a light source of 100 mW / cm 2The results were obtained by connecting the source meter using the four-wire method under AM 1.5G simulated sunlight at 25°C. See Table 1.
[0107] Table 1
[0108]
[0109]
[0110] As can be seen from Table 1, compared with Example 1, Example 2 and Comparative Example 2, and Example 3 and Comparative Example 3, it can be seen that the open circuit voltage, fill factor and photoelectric conversion efficiency of the solar cell with the multiple spin-coated self-assembled SAM layer of the present application are better than the corresponding performance of the solar cell with the single spin-coated self-assembled SAM layer, which may be due to the increase in SAM coverage, which reduces leakage and surface carrier recombination. Further, compared with Example 1, Example 3 does not deposit an anchor layer in the preparation method of Example 3, but directly spin-coats and self-assembles on the ITO glass substrate. The open circuit voltage, fill factor and photoelectric conversion efficiency of Example 1 are better than the corresponding performance of Example 3. The reason may be that the anchor layer deposited in Example 1 contains more active groups, which is more conducive to the self-assembly of single molecules, so that it has a higher SAM layer coverage.
[0111] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0112] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.
Claims
1. A method for preparing a perovskite solar cell, characterized in that: The following operations are included: Providing a transparent conductive oxide film; Performing a monomolecular material self-assembly operation: attaching a self-assembled monomolecular material to one side of the transparent conductive oxide film, allowing the self-assembled monomolecular material to react to form a self-assembled monolayer on the transparent conductive oxide film, so as to complete the self-assembly of a single monolayer; Performing a removal operation: removing the self-assembled monomolecular material that is not anchored on the transparent conductive oxide film; Repeating the single-molecule material self-assembly operation and the removal operation, and independently performing the second single-molecule material self-assembly to the (n-1)th single-molecule material self-assembly; wherein n is a preset number of single-molecule material self-assemblies; After the (n-1)th self-assembly of the single molecule material, the self-assembly operation of the single molecule material is repeated to perform the nth self-assembly of the single molecule material to obtain a hole transport layer on the transparent conductive oxide film.
2. The method for preparing a perovskite solar cell according to claim 1, characterized in that: The method further comprises: Depositing an anchor layer on one side of the transparent conductive oxide film to obtain a hole transport layer including the anchor layer and a self-assembled monolayer; Wherein, the self-assembled monolayer formed by the first self-assembly is located on a side of the anchoring layer away from the transparent conductive oxide film; The material of the anchoring layer includes conductive metal oxide.
3. The method for preparing a perovskite solar cell according to claim 2, characterized in that: The conductive metal oxide includes NiO x , Al2O3, CuO2, CuO, CuAlO2, CuCrO2, WO3, MoO c 、V2O5、VO d CrO e One or more of .
4. The method for preparing a perovskite solar cell according to claim 1 or 2, characterized in that: The self-assembled monomolecular material used in at least two monomolecular material self-assemblies is the same; or The self-assembling single molecule materials used in at least two single molecule material self-assemblies are different.
5. The method for preparing a perovskite solar cell according to claim 1 or 2, characterized in that: The self-assembled monomolecular material includes one or more of a self-assembled monomolecular material containing a phosphonic acid group, a self-assembled monomolecular material containing a hydroxyl group, and a self-assembled monomolecular material containing a carboxylic acid group; The self-assembled monomolecular materials containing phosphonic acid groups include [2-(9H-carbazole-9-yl)ethyl]phosphonic acid, [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid, and [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid; The self-assembled monomolecular material containing a carboxylic acid group includes one or more of benzoic acid and 4-[bis(2,4-dimethoxybiphenyl-4-yl)amino]-biphenyl-4-carboxylic acid; The self-assembled monomolecular material containing hydroxyl groups includes one or more of dopamine and diethanolamine.
6. The method for preparing a perovskite solar cell according to claim 1 or 2, characterized in that: The thickness of the hole transport layer is 0.1 nm to 300 nm.
7. The method for preparing a perovskite solar cell according to claim 1 or 2, characterized in that: The self-assembly operation of forming the self-assembled monolayer satisfies at least one of the following operations: (a), 2≦n≦5; (b) The self-assembly conditions include annealing at 80°C to 200°C.
8. The method for preparing a perovskite solar cell according to claim 1 or 2, characterized in that: In the self-assembly operation, a deposition method is used to attach the self-assembled monomolecular material on the transparent conductive oxide film.
9. The method for preparing a perovskite solar cell according to claim 8, characterized in that: The deposition method includes at least one of a solution method and an evaporation method.
10. The method for preparing a perovskite solar cell according to claim 1 or 2, characterized in that: After obtaining the hole transport layer, the following operations are also included: Prepare a perovskite layer on a side of the hole transport layer away from the transparent conductive oxide film; Depositing an electron transport layer on a side of the perovskite layer away from the hole transport layer; Wherein, the perovskite layer is a pin inversion structure; The thickness of the electron transport layer is 1 nm to 300 nm.
11. A perovskite solar cell, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 10.
12. The perovskite solar cell according to claim 11, characterized in that: Including inverted single-junction perovskite solar cells and crystalline silicon perovskite stacked solar cells.
13. An electronic product, characterized in that: The power supply device comprises the perovskite solar cell according to claim 11 or 12.