Polymer material as well as preparation method and application thereof

By designing polymer materials containing anionic, cationic, and hydrophobic groups on the molecular chain, the problem of poor adaptability to cementing loss in existing technologies has been solved. This has achieved intelligent anti-leakage effect for different types of loss formations, with strong adaptability and high pressure-bearing sealing capability.

CN118994480AActive Publication Date: 2024-11-22CHINA NAT PETROLEUM CORP +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202310570170.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-22
Estimated Expiration
2043-05-19

AI Technical Summary

Technical Problem

Existing technologies struggle to effectively address well cementing loss issues in unconventional oil and gas extraction, particularly due to poor adaptability to formations with varying types of loss. Furthermore, existing anti-loss materials are complex to prepare, costly, and lack intelligent response capabilities.

Method used

A polymer material with anionic, cationic, and hydrophobic groups on its molecular chain is used to prepare a leak-proof material that can adapt to different types of leakage in the formation, and has temperature sensitivity and high pressure-bearing sealing capability.

Benefits of technology

It achieves intelligent leakage prevention for formations with various types of leakage, such as fractures and pores. It is highly adaptable and can effectively seal under different temperature and pressure conditions, reduce rheological effects, form a dense structure, and meet the cementing needs of complex deep wells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004238230240000021
    Figure BDA0004238230240000021
  • Figure BDA0004238230240000081
    Figure BDA0004238230240000081
  • Figure BDA0004238230240000181
    Figure BDA0004238230240000181
Patent Text Reader

Abstract

The invention discloses a polymer material as well as a preparation method and application thereof. The polymer material is a polymer with an anionic group, a cationic group and a hydrophobic group on a molecular chain at the same time; the polymer is a straight-chain polymer, and the anionic group, the cationic group and the hydrophobic group are randomly distributed on a main chain of the polymer through covalent bonds. According to the polymer material prepared by the invention, an anionic group is introduced through the 2-alkenyl amido-2-methylpropanesulfonic acid and the unsaturated carboxylic acid monomer, a cationic group and a hydrophobic group are introduced through the amphiphilic unsaturated cationic monomer, and the three groups are utilized to realize a specific effect, so that the purpose of intelligent leakage prevention can be achieved, and a plugging effect can be effectively exerted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a polymer material and a preparation method and application thereof. Background Art

[0002] According to OPEC's World Oil Outlook 2020, oil will continue to be the largest contributor to the energy structure, accounting for more than 27% by 2045, followed by natural gas (25%). With the increase in oil and gas demand, global resource exploration is gradually turning to unconventional oil and gas resources. However, fracture leakage, porosity leakage, and high permeability leakage have become a key problem restricting the efficient exploitation of unconventional oil and gas. At this stage, research on leak prevention and plugging of leaky formations, especially in drilling fluids, has made great progress. In the cementing process, in order to ensure the displacement efficiency, the design density of cement slurry is often higher than that of drilling fluid. Therefore, cement slurry has higher requirements for formation pressure, which leads to fractured and high permeability formations. There is still a risk of cementing leakage after the drilling fluid is leak-proof and plugged. In addition, the friction and collision between the casing and the well wall during the casing process may cause the plugging layer structure to fail and the cracks to expand further, further increasing the risk of cementing leakage. Cementing leakage can cause cement slurry to invade the formation and cause pollution. At the same time, serious leakage can cause insufficient return and affect the sealing quality.

[0003] At present, there are three main methods to reduce cementing leakage. One is to reduce the density of the cementing fluid slurry column to reduce the slurry column pressure. The second is to improve the thixotropy of the cement slurry. The third is to add leak-proof and plugging materials to the cementing fluid. Since the cementing fluid needs to bear the role of stabilizing the formation and replacing the drilling fluid, the density range of its slurry column is often limited. To ensure safe construction, the rheology of the slurry also needs to be controlled within a reasonable range. Therefore, the first two methods are not suitable for cementing and leak prevention in complex deep wells. The third method is currently a more common and universal method to solve cementing leakage. Cementing leak-proof and plugging materials usually use a combination of polymers, gels, fiber materials and solid-phase granular materials. Summary of the invention

[0004] In order to increase the selectivity of the raw materials of cementing and plugging materials, the present invention provides a polymer material that can overcome the problems of poor adaptability to different types of leakage in the prior art, as well as the preparation method of the current adaptive cementing and plugging materials and complex components, so as to achieve industrial production and large-scale promotion and application.

[0005] As one aspect of the present invention, it relates to a polymer material, which refers to a polymer having anionic groups, cationic groups and hydrophobic groups on its molecular chain; the polymer is a straight-chain polymer, and the anionic groups, the cationic groups and the hydrophobic groups are randomly distributed on the main chain of the polymer through covalent bonds.

[0006] In a specific embodiment, the polymer material comprises the following components by weight: 15 to 22 parts of 2-enamide-2-methylpropanesulfonic acid, 0.8 to 1.8 parts of amphiphilic unsaturated cationic monomer, and 2.5 to 4 parts of unsaturated carboxylic acid monomer.

[0007] Furthermore, the polymer material comprises the following components by weight: 15 to 22 parts of 2-enamide-2-methylpropanesulfonic acid, 0.8 to 1.8 parts of amphiphilic unsaturated cationic monomers, 2.5 to 4 parts of unsaturated carboxylic acid monomers, and 10 to 20 parts of unsaturated amide monomers.

[0008] In a specific embodiment, the amphiphilic unsaturated cationic monomer is as shown in formula (I):

[0009]

[0010] In the formula, R is H or a C1-C4 alkyl group, and n is 11, 13, 15, 17 or 19.

[0011] In a specific embodiment, the unsaturated carboxylic acid monomer is selected from one of maleic acid, itaconic acid or acrylic acid.

[0012] In a specific embodiment, the unsaturated amide monomer is selected from diacetone acrylamide, N,N-dimethyl acrylamide or N,N-diethyl acrylamide.

[0013] In a specific embodiment, the polymer material further includes an initiator.

[0014] Furthermore, the mass of the initiator accounts for 0.15-0.5% of the total mass of the four substances including the 2-enamide-2-methylpropane sulfonic acid, the amphiphilic unsaturated cationic monomer, the unsaturated carboxylic acid monomer and the unsaturated amide monomer.

[0015] In a specific embodiment, the initiator adopts an oxidant-reducing agent initiation system.

[0016] Furthermore, the oxidizing agent is selected from ammonium persulfate and / or potassium persulfate; the reducing agent is selected from sodium bisulfite and / or sodium hydroxide.

[0017] Specifically, the molar ratio of the oxidizing agent to the reducing agent is 1:(0.5-1).

[0018] As another aspect of the present invention, it relates to a method for preparing the above-mentioned polymer material. When preparing the polymer material, the method simultaneously uses anionic groups introduced by 2-enamide-2-methylpropanesulfonic acid and unsaturated carboxylic acid monomers, and cationic groups and hydrophobic groups introduced by amphiphilic unsaturated cationic monomers.

[0019] In a specific embodiment, the method comprises the following steps:

[0020] S1. Preparation of mixture M1

[0021] adding water to dissolve the amphiphilic unsaturated cationic monomer to prepare a mixture M1;

[0022] S2. Preparation of mixture M2

[0023] Add 2-enamide-2-methylpropanesulfonic acid, unsaturated amide monomer and unsaturated carboxylic acid monomer to water in sequence, stir to dissolve, and adjust the pH value of the solution to obtain a mixture M2;

[0024] S3. Preparation of polymer solution

[0025] S1 is heated in a water bath to obtain a mixture M1, and the mixture M2 obtained by S2 and an aqueous solution of an initiator are simultaneously added dropwise under stirring. After the addition is completed, the temperature is raised to react to obtain a polymer solution.

[0026] In a specific embodiment, in S2, the pH value of the solution is adjusted to 6-7.

[0027] In a specific embodiment, in S3, the water bath temperature is set to 40-50°C.

[0028] In a specific embodiment, in S3, the stirring speed is set to 50-150 rpm.

[0029] In a specific embodiment, in S3, the dropping time is controlled to be 3 to 5 hours.

[0030] In a specific embodiment, in S3, the temperature is raised to 50-55° C. and the reaction is carried out for 4-6 hours.

[0031] As another aspect of the present invention, it relates to a leakage-proof material, which uses the above-mentioned polymer material.

[0032] As another aspect of the present invention, it relates to a cementing leak-proof pre-fluid, and the cementing leak-proof pre-fluid comprises the above-mentioned leak-proof material.

[0033] As another aspect of the present invention, it relates to a cementing process, in which the cementing anti-leakage pre-fluid mentioned above is used.

[0034] The present invention introduces hydrophobic groups by using amphiphilic unsaturated cationic monomers with good water solubility, thereby ensuring that the amphiphilic unsaturated cationic monomers can better participate in the polymerization reaction; and because the amphiphilic unsaturated cationic monomers can be dissolved in an aqueous solution, they can be more evenly distributed on the polymer chain during synthesis, ensuring that the distribution of the hydrophobic groups in the polymer is more random, which is beneficial to improving the hydrophobic association of the polymer; and the conversion rate of monomers with a large molecular weight and a large polymerization steric hindrance, such as surfactant monomers, can be improved through the specific monomer mixing sequence in the present invention.

[0035] The special molecular structure designed by the present invention introduces anionic groups through 2-enamide-2-methylpropanesulfonic acid and unsaturated carboxylic acid monomers, introduces cationic groups and hydrophobic groups through amphiphilic unsaturated cationic monomers, and utilizes the three groups to achieve specific effects, thereby achieving the purpose of intelligent leakage prevention and playing a blocking role.

[0036] The preparation method of the present invention adopts a solution polymerization method, has a simple process flow, is green, safe and environmentally friendly, has readily available raw materials and low production cost, and can realize industrial production and large-scale promotion and application;

[0037] The invention adopts a specific order of adding ingredients, which is beneficial to increasing the conversion rate of macromolecular monomers and effectively controlling the molecular structure and molecular weight of polymers.

[0038] The leakproof material prepared by the invention has a simple composition, strong adaptability to different types of pre-fluids, and good compatibility with the pre-fluids.

[0039] The intelligent polymer leak-proof material for cementing pre-fluid prepared by the present invention has strong adaptability to cracks and voids, can adapt to voids and cracks of various shapes and types, and plays a role of intelligent leak-proofing.

[0040] The intelligent polymer anti-leakage material for cementing pre-fluid of the present invention has strong adaptability and can be used to deal with various leakage problems such as fracture leakage, porosity leakage, high permeability leakage, etc., and meets the cementing technical requirements of fractured formations, high permeability formations and other leaky formations.

[0041] The polymer material prepared by the present invention undergoes intramolecular association at room temperature through the electrostatic effect of ionic groups and the hydrophobic association of hydrophobic groups, thereby reducing the hydrodynamic radius of the polymer and reducing the influence on the rheology of the pre-fluid. As the temperature rises, the molecular chain extends and gradually begins to form intermolecular association. When the minimum critical temperature of association is reached, a large amount of hydrophobic association occurs between polymer molecules. As the polymer concentration increases, the contact probability of hydrophobic groups between polymer molecules increases, and a large amount of hydrophobic association also occurs between different polymers. Based on the property that the self-assembled polymer undergoes hydrophobic association after reaching a specific temperature and concentration, ionic groups are introduced into the polymerization to adsorb solid phase particles, forming a deformable polymer-solid phase particle composite structure, which adaptively flows into cracks and pores of different types and openings under the action of pressure difference. The polymer concentration in the crack space is further increased, the association structure is enlarged and dense, and finally a structure of "rigid material bridging + flexible material filling" is formed, thereby realizing intelligent leakage prevention of a set of system plugging applicable types of formations.

[0042] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention are realized and obtained by the structures particularly pointed out in the description, claims and drawings. DETAILED DESCRIPTION

[0043] With the increasing requirements for leak prevention and plugging efficiency and success rate, leak prevention and plugging materials are gradually given more performance requirements, such as the need to have adaptability to cracks, temperature sensitivity, and sufficient pressure-bearing plugging capabilities. Therefore, the design of polymers and compound material systems has become more complicated. The inventors found during material exploration that:

[0044] CN 105062440 B discloses a plugging and leak-proofing material, which includes fibers, polymer microspheres, polymer powder, and blast furnace slag. The polymer microspheres and fibers are entangled with each other, and the polymer powder can bond the polymer microspheres, fibers, and blast furnace slag to ensure the pressure bearing capacity of the plugging and leak-proofing material. The method can meet the plugging requirements of cementing of fracture-type, pore-type, and seepage-type formations, and has high temperature resistance. However, the inventor believes that the synthesis method of preparing leak-proof materials with polymer microspheres is complicated, the size of the microspheres is difficult to control, and the application cost is high.

[0045] CN 115029926 A provides the composition and preparation method of fiber grafted expandable resin plugging material and its cementing leak prevention and plugging application. The fiber grafted expandable resin plugging material is obtained by grafting copolymerization of modified polypropylene fiber with acrylic acid, acrylamide, 2-acrylamide-2-methylpropanesulfonic acid and N,N-methylenebisacrylamide under certain conditions. It can be deformed and squeezed into the pores formed by the bridging material, and effectively plugs the cracks of 1 to 5 mm under the temperature condition of 20 to 120°C. However, the inventor believes that: in the preparation process of this method, it is necessary to ensure the control of the water absorption and expansion rate of the expandable resin material to avoid the problem of premature expansion.

[0046] CN 114426818 A provides a cementing and leak-proof plugging cement slurry system based on thermosensitive memory polymer, comprising oil well cement, thermosensitive memory expansion balls, thermosensitive memory expansion nets, rigid particles, high-temperature suspension stabilizers, and water. The density of the cement slurry system is 1.20-1.50 g / cm 3 Adjustable, the application temperature is 90-150℃, and the 0.5-6mm crack pressure is not less than 6MPa. However, the inventor believes that the current manufacturing process of temperature-sensitive memory materials is complex and costly, and its intelligent response factor is mainly temperature, and its intelligent adaptability to different types of leakage formations is insufficient.

[0047] CN 110002798 A discloses a leak-proof cement slurry for cementing, comprising the following components: water, oil well cement, bridging particles, quartz sand, microsilica powder, and cement admixture; the median particle size of the oil well cement is 10 μm to 30 μm; the particle size of the bridging particles is 1 / 2 to 2 / 3 of the average pore throat diameter or average crack width of the target formation; the particle size of the quartz sand is 180 μm to 425 μm; the particle size of the microsilica powder is 0.1 μm to 0.3 μm. The leak-proof cement slurry forms a bridge plug through the reasonable grading between granular materials of different particle sizes, thereby effectively plugging porous formations prone to leakage and induced fracture formations caused by pressure difference, and has high pressure bearing capacity. However, the inventor believes that the system needs to consider the formation pore throat diameter or crack width when selecting components, and its adaptive ability to different types of leakage is insufficient.

[0048] In summary, in view of the fact that the existing technologies are not as good as the inventors' expectations, the inventors made the present invention through further research and development.

[0049] The present invention is further described below in conjunction with specific embodiments, and the protection scope of the present invention is not limited by the following embodiments. The sources of the materials mainly involved in the embodiments are shown in Table 1 below, and other materials not shown are conventional commercial products.

[0050] Table 1 Material source description

[0051]

[0052]

[0053] Through a large number of experimental studies, the inventors have made the following optimization selections on the constituent raw materials of the polymer material and the preparation method thereof, and provided Examples 1 to 9.

[0054] Example 1

[0055] The polymer material of this embodiment includes the following components by weight: 20 g of 2-enamido-2-methylpropanesulfonic acid, 15 g of N,N-dimethylacrylamide, 3 g of itaconic acid, 1.2 g of an amphiphilic unsaturated cationic monomer (wherein, in the structure of the amphiphilic unsaturated cationic monomer, R is a methyl group and n is 13), 0.12 g of ammonium persulfate (oxidation initiator), and 0.07 g of sodium bisulfite (reduction initiator);

[0056] The polymer material of this embodiment is prepared by the following steps:

[0057] S1. Preparation of mixture M1

[0058] Dissolve 1.2 g of an amphiphilic unsaturated cationic monomer in 140 g of deionized water to prepare a mixture M1;

[0059] S2. Preparation of mixture M2

[0060] 20 g of 2-enamido-2-methylpropanesulfonic acid, 15 g of N,N-dimethylacrylamide, and 3 g of itaconic acid were dissolved in 25 g of deionized water, and 4.4 g of NaOH was added to adjust the pH value to 6 to prepare a mixture M2;

[0061] S3. Preparation of polymer materials

[0062] The mixture M1 prepared by S1 was transferred to a three-necked flask, placed in a 50°C water bath for heating, and stirred with a magnetic stirrer at a stirring speed of 50 rpm; then, a metering pump was used to simultaneously drip the mixture M2 and the aqueous solution of the initiator into the three-necked flask containing the mixture M1, and the dripping time was controlled to be 5h. After the dripping was completed, the temperature was raised to 55°C for reaction for 5h. The polymer material SSL1 was obtained;

[0063] The aqueous solution of the initiator refers to 0.12 g of ammonium persulfate and 0.07 g of sodium bisulfite dissolved in 10 g of deionized water.

[0064] Example 2

[0065] The polymer material of this embodiment includes the following components by weight: 15 g of 2-enamido-2-methylpropanesulfonic acid, 10 g of diacetone acrylamide, 2.5 g of itaconic acid, 0.8 g of an amphiphilic unsaturated cationic monomer (wherein, in the structure of the amphiphilic unsaturated cationic monomer, R is methyl and n is 13), 0.08 g of ammonium persulfate (oxidation initiator), and 0.048 g of sodium bisulfite (reduction initiator);

[0066] The polymer material of this embodiment is prepared by the following steps:

[0067] S1. Preparation of mixture M1

[0068] Dissolve 0.8 g of an amphiphilic unsaturated cationic monomer in 120 g of deionized water to prepare a mixture M1;

[0069] S2. Preparation of mixture M2

[0070] 15 g of 2-enamido-2-methylpropanesulfonic acid, 10 g of diacetone acrylamide, and 2.5 g of itaconic acid were dissolved in 25 g of deionized water, and 3.2 g of NaOH was added to adjust the pH value to 6.5 to prepare a mixture M2;

[0071] S3. Preparation of polymer materials

[0072] The mixture M1 prepared by S1 was transferred to a three-necked flask, placed in a 50°C water bath for heating, and stirred with a magnetic stirrer at a stirring speed of 100 rpm; then, a metering pump was used to simultaneously drip the mixture M2 and the aqueous solution of the initiator into the three-necked flask containing the mixture M1, and the dripping time was controlled to be 4 hours. After the dripping was completed, the temperature was raised to 55°C for reaction for 4 hours. The polymer material SSL2 was obtained;

[0073] The aqueous solution of the initiator refers to 0.08 g of ammonium persulfate and 0.048 g of sodium bisulfite dissolved in 10 g of deionized water.

[0074] Example 3

[0075] The polymer material of this embodiment includes the following components by weight: 22 g of 2-enamido-2-methylpropanesulfonic acid, 20 g of N,N-diethylacrylamide, 4 g of itaconic acid, 1.8 g of an amphiphilic unsaturated cationic monomer (wherein, in the structure of the amphiphilic unsaturated cationic monomer, R is a methyl group and n is 11), 0.12 g of ammonium persulfate (oxidation initiator), and 0.07 g of sodium bisulfite (reduction initiator);

[0076] The polymer material of this embodiment is prepared by the following steps:

[0077] S1. Preparation of mixture M1

[0078] Dissolve 1.8 g of an amphiphilic unsaturated cationic monomer in 180 g of deionized water to prepare a mixture M1;

[0079] S2. Preparation of mixture M2

[0080] 22 g of 2-enamido-2-methylpropanesulfonic acid, 20 g of N,N-diethylacrylamide, and 4 g of itaconic acid were dissolved in 40 g of deionized water, and 4.5 g of NaOH was added to adjust the pH value to 6.5 to prepare a mixture M2;

[0081] S3. Preparation of polymer materials

[0082] The mixture M1 prepared by S1 was transferred to a three-necked flask, placed in a 50°C water bath for heating, and stirred with a magnetic stirrer at a stirring speed of 150rpm; then, a metering pump was used to simultaneously drip the mixture M2 and the aqueous solution of the initiator into the three-necked flask containing the mixture M1, and the dripping time was controlled to be 3h. After the dripping was completed, the temperature was raised to 55°C for reaction for 5h. The polymer material SSL3 was obtained;

[0083] The aqueous solution of the initiator refers to 0.12 g of ammonium persulfate and 0.07 g of sodium bisulfite dissolved in 10 g of deionized water.

[0084] Example 4

[0085] The polymer material of this embodiment includes the following components by weight: 20 g of 2-enamido-2-methylpropanesulfonic acid, 15 g of N,N-dimethylacrylamide, 3 g of itaconic acid, 1.2 g of an amphiphilic unsaturated cationic monomer (wherein, in the structure of the amphiphilic unsaturated cationic monomer, R is H and n is 11), 0.12 g of ammonium persulfate (oxidation initiator), and 0.07 g of sodium bisulfite (reduction initiator);

[0086] The polymer material of this embodiment is prepared by the following steps:

[0087] S1. Preparation of mixture M1

[0088] Dissolve 1.2 g of an amphiphilic unsaturated cationic monomer in 140 g of deionized water to prepare a mixture M1;

[0089] S2. Preparation of mixture M2

[0090] 20 g of 2-enamido-2-methylpropanesulfonic acid, 15 g of N,N-dimethylacrylamide, and 3 g of itaconic acid were dissolved in 25 g of deionized water, and 4.4 g of NaOH was added to adjust the pH value to 7 to prepare a mixture M2;

[0091] S3. Preparation of polymer materials

[0092] The mixture M1 prepared by S1 was transferred to a three-necked flask, placed in a 50°C water bath for heating, and stirred with a magnetic stirrer at a stirring speed of 100 rpm; then, a metering pump was used to simultaneously drip the mixture M2 and the aqueous solution of the initiator into the three-necked flask containing the mixture M1, and the dripping time was controlled to be 3 hours. After the dripping was completed, the temperature was raised to 50°C for reaction for 6 hours. The polymer material SSL4 was obtained;

[0093] The aqueous solution of the initiator refers to 0.12 g of ammonium persulfate and 0.07 g of sodium bisulfite dissolved in 10 g of deionized water.

[0094] Example 5

[0095] The polymer material of this embodiment includes the following components by weight: 20 g of 2-enamido-2-methylpropanesulfonic acid, 15 g of N,N-dimethylacrylamide, 3 g of itaconic acid, 1.2 g of an amphiphilic unsaturated cationic monomer (wherein, in the structure of the amphiphilic unsaturated cationic monomer, R is -(CH2)3CH3, and n is 11), 0.12 g of ammonium persulfate (oxidation initiator), and 0.07 g of sodium bisulfite (reduction initiator);

[0096] The polymer material of this embodiment is prepared by the following steps:

[0097] S1. Preparation of mixture M1

[0098] Dissolve 1.2 g of an amphiphilic unsaturated cationic monomer in 140 g of deionized water to prepare a mixture M1;

[0099] S2. Preparation of mixture M2

[0100] 20 g of 2-enamido-2-methylpropanesulfonic acid, 15 g of N,N-dimethylacrylamide, and 3 g of itaconic acid were dissolved in 25 g of deionized water, and 4.4 g of NaOH was added to adjust the pH value to 7 to prepare a mixture M2;

[0101] S3. Preparation of polymer materials

[0102] The mixture M1 prepared by S1 was transferred to a three-necked flask, placed in a 50°C water bath for heating, and stirred with a magnetic stirrer at a stirring speed of 100 rpm; then, a metering pump was used to simultaneously drip the mixture M2 and the aqueous solution of the initiator into the three-necked flask containing the mixture M1, and the dripping time was controlled to be 3 hours. After the dripping was completed, the temperature was raised to 55°C for reaction for 5 hours. The polymer material SSL5 was obtained;

[0103] The aqueous solution of the initiator refers to 0.12 g of ammonium persulfate and 0.07 g of sodium bisulfite dissolved in 10 g of deionized water.

[0104] Example 6

[0105] The polymer material of this embodiment includes the following components by weight: 20 g of 2-enamido-2-methylpropanesulfonic acid, 15 g of N,N-dimethylacrylamide, 3 g of itaconic acid, 1.2 g of an amphiphilic unsaturated cationic monomer (wherein, in the structure of the amphiphilic unsaturated cationic monomer, R is a methyl group and n is 15), 0.12 g of ammonium persulfate (oxidation initiator), and 0.07 g of sodium bisulfite (reduction initiator);

[0106] The polymer material of this embodiment is prepared by the following steps:

[0107] S1. Preparation of mixture M1

[0108] Dissolve 1.2 g of an amphiphilic unsaturated cationic monomer in 140 g of deionized water to prepare a mixture M1;

[0109] S2. Preparation of mixture M2

[0110] 20 g of 2-enamido-2-methylpropanesulfonic acid, 15 g of N,N-dimethylacrylamide, and 3 g of itaconic acid were dissolved in 25 g of deionized water, and 4.4 g of NaOH was added to adjust the pH value to 7 to prepare a mixture M2;

[0111] S3. Preparation of polymer materials

[0112] The mixture M1 prepared by S1 was transferred to a three-necked flask, placed in a 50°C water bath for heating, and stirred with a magnetic stirrer at a stirring speed of 100 rpm; then, a metering pump was used to simultaneously drip the mixture M2 and the aqueous solution of the initiator into the three-necked flask containing the mixture M1, and the dripping time was controlled to be 3 hours. After the dripping was completed, the temperature was raised to 55°C for reaction for 5 hours. The polymer material SSL6 was obtained;

[0113] The aqueous solution of the initiator refers to 0.12 g of ammonium persulfate and 0.07 g of sodium bisulfite dissolved in 10 g of deionized water.

[0114] Example 7

[0115] The polymer material of this embodiment includes the following components by weight: 20 g of 2-enamide-2-methylpropanesulfonic acid, 15 g of N,N-dimethylacrylamide, 4 g of maleic acid, 1.2 g of an amphiphilic unsaturated cationic monomer (wherein, in the structure of the amphiphilic unsaturated cationic monomer, R is a methyl group and n is 17), 0.12 g of ammonium persulfate (oxidation initiator), and 0.07 g of sodium bisulfite (reduction initiator);

[0116] The polymer material of this embodiment is prepared by the following steps:

[0117] S1. Preparation of mixture M1

[0118] Dissolve 1.2 g of an amphiphilic unsaturated cationic monomer in 140 g of deionized water to prepare a mixture M1;

[0119] S2. Preparation of mixture M2

[0120] 20 g of 2-enamido-2-methylpropanesulfonic acid, 15 g of N,N-dimethylacrylamide, and 4 g of maleic acid were dissolved in 25 g of deionized water, and 4.4 g of NaOH was added to adjust the pH value to 7 to prepare a mixture M2;

[0121] S3. Preparation of polymer materials

[0122] The mixture M1 prepared by S1 was transferred to a three-necked flask, placed in a 50°C water bath for heating, and stirred with a magnetic stirrer at a stirring speed of 100 rpm; then, a metering pump was used to simultaneously drip the mixture M2 and the aqueous solution of the initiator into the three-necked flask containing the mixture M1, and the dripping time was controlled to be 3 hours. After the dripping was completed, the temperature was raised to 55°C for reaction for 5 hours. The polymer material SSL7 was obtained;

[0123] The aqueous solution of the initiator refers to 0.12 g of ammonium persulfate and 0.07 g of sodium bisulfite dissolved in 10 g of deionized water.

[0124] Example 8

[0125] The polymer material of this embodiment includes the following components by weight: 20 g of 2-enamide-2-methylpropanesulfonic acid, 15 g of N,N-dimethylacrylamide, 4 g of maleic acid, 1.2 g of an amphiphilic unsaturated cationic monomer (wherein, in the structure of the amphiphilic unsaturated cationic monomer, R is a methyl group and n is 17), 0.12 g of potassium persulfate (oxidation initiator), and 0.07 g of sodium hydroxide (reduction initiator);

[0126] The polymer material of this embodiment is prepared by the following steps:

[0127] S1. Preparation of mixture M1

[0128] Dissolve 1.2 g of an amphiphilic unsaturated cationic monomer in 140 g of deionized water to prepare a mixture M1;

[0129] S2. Preparation of mixture M2

[0130] 20 g of 2-enamido-2-methylpropanesulfonic acid, 15 g of N,N-dimethylacrylamide, and 4 g of maleic acid were dissolved in 25 g of deionized water, and 4.4 g of NaOH was added to adjust the pH value to 7 to prepare a mixture M2;

[0131] S3. Preparation of polymer materials

[0132] The mixture M1 prepared by S1 was transferred to a three-necked flask, placed in a 40°C water bath for heating, and stirred with a magnetic stirrer at a stirring speed of 100 rpm; then, a metering pump was used to simultaneously drip the mixture M2 and the aqueous solution of the initiator into the three-necked flask containing the mixture M1, and the dripping time was controlled to be 3 hours. After the dripping was completed, the temperature was raised to 50°C for reaction for 5 hours. The polymer material SSL8 was obtained;

[0133] The aqueous solution of the initiator refers to 0.12 g of potassium persulfate and 0.07 g of sodium hydroxide dissolved in 10 g of deionized water.

[0134] Example 9

[0135] The polymer material of this embodiment includes the following components by weight: 20 g of 2-enamide-2-methylpropanesulfonic acid, 15 g of N,N-dimethylacrylamide, 4 g of acrylic acid, 1.2 g of an amphiphilic unsaturated cationic monomer (wherein, in the structure of the amphiphilic unsaturated cationic monomer, R is a methyl group and n is 19), 0.12 g of ammonium persulfate (oxidation initiator), and 0.07 g of sodium bisulfite (reduction initiator);

[0136] The polymer material of this embodiment is prepared by the following steps:

[0137] S1. Preparation of mixture M1

[0138] Dissolve 1.2 g of an amphiphilic unsaturated cationic monomer in 140 g of deionized water to prepare a mixture M1;

[0139] S2. Preparation of mixture M2

[0140] 20 g of 2-enamido-2-methylpropanesulfonic acid, 15 g of N,N-dimethylacrylamide, and 4 g of maleic acid were dissolved in 25 g of deionized water, and 4.4 g of NaOH was added to adjust the pH value to 7 to prepare a mixture M2;

[0141] S3. Preparation of polymer materials

[0142] The mixture M1 prepared by S1 was transferred to a three-necked flask, placed in a 50°C water bath for heating, and stirred with a magnetic stirrer at a stirring speed of 100 rpm; then, a metering pump was used to simultaneously drip the mixture M2 and the aqueous solution of the initiator into the three-necked flask containing the mixture M1, and the dripping time was controlled to be 3 hours. After the dripping was completed, the temperature was raised to 50°C for reaction for 5 hours. The polymer material SSL9 was obtained;

[0143] The aqueous solution of the initiator refers to 0.12 g of ammonium persulfate and 0.07 g of sodium bisulfite dissolved in 10 g of deionized water.

[0144] Comparative Example 1

[0145] The intelligent polymer leak-proof material for cementing pre-fluid of Comparative Example 1 is different from that of Example 1 in that no amphiphilic unsaturated cationic monomer is added, and the obtained leak-proof material is DBL1.

[0146] Comparative Example 2

[0147] The intelligent polymer leak-proof material for cementing pre-fluid of Comparative Example 2 is different from that of Example 1 in that the amount of the amphiphilic unsaturated cationic monomer added is 2 g, and the obtained leak-proof material is DBL2.

[0148] Comparative Example 3

[0149] The intelligent polymer leak-proof material for cementing pre-fluid of Comparative Example 3 is different from that of Example 1 in that itaconic acid is not added, and the obtained leak-proof material is DBL3.

[0150] Comparative Example 4

[0151] The intelligent polymer leak-proof material for cementing pre-fluid of Comparative Example 4 is different from that of Example 1 in that the amount of itaconic acid added is 5 g, and the obtained leak-proof material is DBL4.

[0152] Comparative Example 5

[0153] The intelligent polymer leak-proof material for cementing pre-fluid of this comparative example 5 is different from that of example 1 in that its preparation method is as follows:

[0154] The amphiphilic unsaturated cationic monomer was dissolved in 180g of deionized water to prepare a mixture M1; propane-amido-2-methylpropanesulfonic acid, N,N-dimethylacrylamide and itaconic acid were dissolved in 40g of deionized water, and 4.5g of NaOH was added to adjust the pH value to 6.5 to prepare a mixture M2; the initiator was added to 10g of deionized water to prepare an initiator solution M3; M1 was transferred to a three-necked flask, and then placed in a 50°C water bath, and M1 was stirred with a magnetic stirrer; the solution M2 and the solution M3 were directly added to the three-necked flask containing M1 at the same time, rather than being added slowly and quantitatively by a metering pump, and then the temperature was raised to 55°C for reaction, and the reaction time was 5h. , and a polymer solution was obtained, which was the leakproof material DBL5.

[0155] The following leak-proof performance tests were performed on the polymer materials prepared in the above Examples 1 to 9 and Comparative Examples 1 to 5, mainly including:

[0156] 1. Contracting effect

[0157] Association refers to the behavior of polymer molecular chains entangled with each other to form a spatial structure. Strong association is conducive to the formation of a dense cementing structure in the process of leak prevention and plugging. The association can be characterized by fluorescence spectrum testing of polymer aqueous solution. The fluorescence spectrum of pyrene in water has 5 peaks, which are near 373, 379, 384, 394, and 480 nm. When the hydrophobic associating structure in the polymer solution increases, pyrene can be more solubilized in the hydrophobic structure. At the same time, the fluorescence intensity ratio I1 / I3 of peak 1 at 374 nm and peak 3 at 385 nm of the pyrene fluorescence spectrum will decrease accordingly. Therefore, the I1 / I3 value can be used to characterize the amount of hydrophobic associating structure. The lower the I1 / I3 value, the more hydrophobic associating structures there are. In the test, the emission spectrum of pyrene in the polymer solution was measured by a fluorescence spectrophotometer. The concentration of pyrene in the solution was 5×10 -6 mol·L -1 , the excitation wavelength was 335 nm, the excitation and emission slit widths were 5 nm and 2.5 nm, respectively, and the scanning rate was 350-450 nm.

[0158] According to the above operation, the I1 / I3 values ​​of polymer materials with different concentrations at room temperature were tested, and the test results were recorded in Table 2 below; at the same time, the I1 / I3 values ​​of polymer materials with a concentration of 0.5% at different temperatures were tested, and the test results were recorded in Table 3 below.

[0159] 2. Adsorption of solid particles

[0160] The total organic carbon method can be used to analyze the adsorption of polymers on the surface of solid particles. Add 2g of polymer to 98g of water and fully dissolve it. Then add 4g of the solid-phase auxiliary filling material combination to the aqueous solution and stir evenly. Perform adsorption experiments under different conditions. After the adsorption is completed, centrifuge the mixed solution and then dilute the filtrate 20 times for TOC testing. The adsorption of polymers on the surface of solid particles can be obtained by analyzing the difference in total organic carbon in the filtrate before and after the addition of the solid-phase auxiliary filling material combination. The calculation method is as follows:

[0161]

[0162] In the formula, q t : adsorption amount during the test time (mg / g); C0: initial concentration of polymer solution (mg / L);

[0163] C t : Concentration of polymer solution at time t (mg / L); V: volume of polymer solution (L); m: mass of cement (g).

[0164] According to the above calculation formula, the adsorption amount of polymer material on the surface of solid particles at different temperatures is determined.

[0165] Table 2 shows the I1 / I3 values ​​of polymer materials with different concentrations at room temperature

[0166]

[0167]

[0168] It can be seen from Table 2 that at room temperature, the I1 / I3 values ​​of the polymer material SSL1 to SSL9 solutions prepared in the embodiments of the present invention are all less than the value of pure water (1.8), indicating that there are hydrophobic micro-regions in the system. As the concentration of the polymer material increases, the polarity of the polymer solution decreases, indicating that the hydrophobic association is enhanced. In the concentration range of 0.3% to 0.7%, the micro-polarity decreases rapidly, indicating that as the concentration of the polymer increases, the association between its molecules is enhanced, and there is a critical association concentration in this range, and a large amount of hydrophobic association is generated in the solution after exceeding this concentration.

[0169] In addition, from the test results in Table 2, it can be found that compared with Example 1, no amphiphilic cationic monomer was added in Comparative Example 1, so DBL1 had no obvious hydrophobic association. In Comparative Example 5, since the polymer was prepared by directly mixing multiple monomers, the prepared DBL5 did not have the designed molecular structure, so its hydrophobic association was weak.

[0170] Table 3 shows the I1 / I3 values ​​of polymer materials with a concentration of 0.5% at different temperatures

[0171]

[0172]

[0173] It can be found from the experimental test results in Table 3 that when the temperature rises to 50°C, the I1 / I3 value of the polymer materials prepared in Examples 1 to 9 decreases, indicating that more hydrophobic microdomains formed by the association of hydrophobic groups appear in the polymer solution. At 90°C, the I1 / I3 value decreases significantly, and the hydrophobicity of the solution is greatly enhanced, indicating that a large number of hydrophobic microdomains are formed. This is because as the temperature rises, the hydrophobic groups become more hydrophobic, so they tend to associate with each other to form a denser network. This hydrophobic association can provide support for polymer leakage prevention.

[0174] Table 4 shows the adsorption amount of 2% polymer material on the surface of solid particles at different temperatures, and the adsorption time is 1h

[0175]

[0176] Combined with the test results in Table 4, it can be seen that SSL1~SSL9 have a higher adsorption capacity, and as the temperature rises to 90°C, the adsorption capacity first decreases and then increases. Comparing the adsorption capacity at 70~90°C, it can be seen that as the adsorption temperature increases, the equilibrium adsorption capacity increases. This is because as the temperature rises, the polymer molecular chains are in an extended state, and the groups in contact with cement particles increase, making it easier to be adsorbed on the adsorption sites on the surface of the hydration product. In addition, no unsaturated carboxylic acid monomer was added in Comparative Example 3, so DBL3 has few adsorption sites and an extremely small adsorption capacity. In Comparative Example 5, since the polymer was prepared by directly mixing multiple monomers, the prepared DBL5 does not have the designed molecular structure, so its adsorption capacity is relatively low. In Comparative Examples 2 to 4, the polymer structure is inconsistent with the design, and its adsorption capacity is also much smaller than that of the embodiment.

[0177] Taking the polymer materials prepared in Examples 1 to 3 and Example 8 as examples, they are applied to the cementing intelligent leakproof pre-fluid system, and the following performance evaluation test is carried out. The specific operation is: fix the artificial cores or fracture simulation molds with different simulated fracture widths with a clamp, and then put the clamp into the high-temperature and high-pressure fracture plugging simulation device; pour the cementing intelligent leakproof pre-fluid into the kettle, turn on the heating switch, heat the slurry to the preset temperature, and stir the pre-fluid with a stirrer; connect the kettle containing the pre-fluid to the air source, slowly pressurize it, pause for 15 minutes after reaching 1MPa, and then repeat this step, with the pressure increasing by 1MPa each time, until a pressure breakthrough occurs; then cool the kettle to room temperature, release the pressure and clean the kettle. The cementing intelligent leakproof pre-fluid is evaluated with breakthrough pressure and cumulative leakage as indicators.

[0178] Application Example 1

[0179] The formula of cementing intelligent leak-proof pre-fluid is as follows: 100 parts by weight of tap water, 2 parts of polymer material SSL1, 2 parts of solid phase auxiliary filling material combination, 1.5 parts of solid phase supporting material, 2 parts of suspension stabilizer, and 0.3 parts of antifoaming agent. After mixing evenly, the cementing intelligent leak-proof pre-fluid SP1 is prepared.

[0180] Application Example 2

[0181] The formula of cementing intelligent leak-proof pre-fluid: 100 parts by weight of tap water, 1 part of polymer material SSL1, 1 part of solid phase auxiliary filling material combination, 1 part of solid phase support material, 1.5 parts of suspension stabilizer, and 0.3 parts of antifoaming agent. After mixing evenly, the cementing intelligent leak-proof pre-fluid SP2 is prepared.

[0182] Application Example 3

[0183] The formula of cementing intelligent leak-proof pre-fluid: 100 parts by weight of tap water, 3 parts of polymer material SSL1, 4 parts of solid phase auxiliary filling material combination, 2 parts of solid phase support material, 3 parts of suspension stabilizer, and 0.3 parts of antifoaming agent. After mixing evenly, the cementing intelligent leak-proof pre-fluid SP3 is prepared.

[0184] Application Example 4

[0185] The formula of cementing intelligent leak-proof pre-fluid: 100 parts by weight of tap water, 2 parts of polymer material SSL2, 2 parts of solid phase auxiliary filling material combination, 1.5 parts of solid phase support material, 2 parts of suspension stabilizer, and 0.3 parts of antifoaming agent. After mixing evenly, the cementing intelligent leak-proof pre-fluid SP4 is prepared.

[0186] Application Example 5

[0187] The formula of cementing intelligent leak-proof pre-fluid: 100 parts by weight of tap water, 2 parts of polymer material SSL3, 2 parts of solid phase auxiliary filling material combination, 1.5 parts of solid phase support material, 2 parts of suspension stabilizer, and 0.3 parts of antifoaming agent. After mixing evenly, the cementing intelligent leak-proof pre-fluid SP5 is prepared.

[0188] Application Example 6

[0189] The formula of cementing intelligent leak-proof pre-fluid: 100 parts by weight of tap water, 2 parts of polymer material SSL8, 2 parts of solid phase auxiliary filling material combination, 1.5 parts of solid phase support material, 2 parts of suspension stabilizer, and 0.3 parts of antifoaming agent. After mixing evenly, the cementing intelligent leak-proof pre-fluid SP6 is prepared.

[0190] Application Comparative Example 1

[0191] The difference from Application Example 1 is that the smart polymer leak-proof material 1 for cementing pre-fluid is not used.

[0192] Application Comparative Example 2

[0193] The difference from Application Example 1 is that no solid-phase auxiliary filling material combination is used.

[0194] Application Comparative Example 3

[0195] The difference from Application Example 1 is that no solid phase support material is used.

[0196] Application Comparative Example 4

[0197] The difference from Application Example 1 is that the leakage-proof material DBL1 prepared in Comparative Example 1 is used to replace the intelligent polymer leakage-proof material 1 for cementing pre-fluid.

[0198] Application Comparative Example 5

[0199] The difference from Application Example 1 is that the leakage-proof material DBL3 prepared in Comparative Example 3 is used to replace the intelligent polymer leakage-proof material 1 for cementing pre-fluid.

[0200] Performance Testing

[0201] 1. Test 1

[0202] The above Application Examples 1 to 6 and Application Comparative Examples 1 to 5 were placed under 90° C. to test the leak-proof and plugging performance of 1 mm cracks. The test results are recorded in Table 5 below.

[0203] Table 5 Leakage-proofing and plugging performance of different leak-proof pre-filling fluids on 1 mm cracks at 90°C

[0204] Leak-proof pre-fill fluid Temperature / ℃ Pressure bearing capacity / MPa Pressure bearing time / min Leakage volume / mL SP1 90 9 >10 9 SP2 90 9 >10 14.2 SP3 90 9 >10 12.5 SP4 90 9 >10 14.5 SP5 90 8 >10 13 SP6 90 8 >10 10 SPD1 90 - - Full leak SPD2 90 - - Full leak SPD3 90 2 5 26 SPD4 90 2 4 22 SPD5 90 3 6 23

[0205] It can be seen from the data results in Table 5 that the intelligent anti-leakage pre-fluid of cementing in Application Examples 1 to 5 can effectively prevent and plug 1mm cracks at 90°C, and its pressure bearing capacity is >8MPa, and the cumulative leakage is less than 15mL. In Application Comparative Example 1, no intelligent polymer anti-leakage material for cementing pre-fluid is added, so it is impossible to form a polymer-solid phase particle composite structure, and it is impossible to further form a "rigid material bridging + flexible material filling" structure in the cracks. The pre-fluid is completely unable to play the role of anti-leakage and plugging, and a full leakage occurs; in Application Comparative Example 2, no solid phase auxiliary filling material combination is added, and a polymer-solid phase particle composite structure cannot be formed, and a full leakage occurs; in Application Comparative Example 3, no solid phase support material is added, and it is impossible to play a good auxiliary support role, so the anti-leakage ability is poor. It can be seen from the above three comparative examples that the lack of any component cannot play a role in preventing and plugging. From the comparison between SP1 and SPD4, it can be seen that the polymer without the addition of amphiphilic unsaturated cationic monomers cannot effectively associate, and therefore has poor leakage prevention and plugging capabilities. From the comparison between SP1 and SPD5, it can be seen that the polymer without the addition of unsaturated carboxylic acid monomers has poor adsorption capacity for the solid phase, and therefore has poor ability to form a polymer-solid phase particle composite structure.

[0206] 2. Test 2

[0207] The above Application Example 1 was placed under different temperature conditions to test the leak-proof and plugging performance of a 1 mm crack, and the test results are recorded in the following Table 6.

[0208] Table 6 Leakage-proofing and plugging performance of leak-proof pre-fluid SP1 on 1 mm cracks at different temperatures

[0209] Leak-proof pre-fill fluid Temperature / ℃ Pressure bearing capacity / MPa Pressure bearing time / min Leakage volume / mL SP1 50 6 >10 11.2 SP1 60 6 >10 11 SP1 70 7 >10 10.5 SP1 80 8 >10 10.7 SP1 90 9 >10 9 SP1 100 9 >10 9 SP1 110 10 >10 8.5 SP1 120 10 >10 8.2 SP1 130 10 >10 8.5 SP1 140 9 >10 9 SP1 150 7 >10 10

[0210] By comparing the plugging effects at different temperatures, it can be seen that as the temperature rises from 50°C to 120°C, the plugging ability of the cementing intelligent anti-leakage pre-fluid gradually increases, and the pressure bearing capacity increases. After further increasing the temperature, the plugging ability tends to be stable, but the pressure bearing capacity decreases slightly at 150°C. This is because the association effect of the intelligent polymer anti-leakage material used in the cementing pre-fluid is the main characteristic to exert its anti-leakage ability, and the degree of association gradually increases with the increase of temperature. As the temperature rises from 50°C to 120°C, the pressure bearing capacity of the cementing intelligent anti-leakage pre-fluid increases. When the temperature rises to 150°C, the water solubility of the polymer decreases, and the intermolecular association network effect decreases, and the plugging ability decreases at this time.

[0211] 3. Test 3

[0212] The leak-proofing and plugging performance of the cementing intelligent leak-proof pre-fluids prepared in Examples 1 to 6 on 3 mm cracks was tested at different temperatures. The results are shown in Table 7.

[0213] Table 7 Leakage prevention and plugging performance of intelligent leak-proof pre-fluid for 3mm cracks at different temperatures

[0214] Leak-proof pre-fill fluid Temperature / ℃ Pressure bearing capacity / MPa Pressure bearing time / min Leakage volume / mL SP1 50 6 >10 11.2 SP1 120 10 >10 8.2 SP1 150 7 >10 10 SP2 50 6 >10 11.5 SP2 120 10 >10 9.1 SP2 150 7 >10 10.5 SP3 50 6 >10 14.1 SP3 120 10 >10 8.5 SP3 150 8 >10 11.8 SP4 50 6 >10 13.5 SP4 120 10 >10 8.3 SP4 150 7 >10 13.7 SP5 50 6 >10 13.8 SP5 120 9 >10 9.1 SP5 150 6 >10 13.4 SP6 50 6 >10 14.1 SP6 120 9 >10 9.2 SP6 150 6 >10 13.9

[0215] From the data results in Table 7, it can be seen that the cementing intelligent leak-proof pre-fluid still has good leak-proof and plugging capabilities for 3mm cracks, and the pressure bearing capacity and cumulative filtration loss do not decrease with the increase of crack width. The pressure bearing capacity is greater than 6MPa, and the cumulative leakage is less than 15mL. By comparing the leak-proof and plugging capabilities of cementing intelligent leak-proof pre-fluids with different compositions at different temperatures, it can be seen that its leak-proof capability is significantly enhanced at 120℃, which shows that the system has certain temperature-sensitive characteristics, which is derived from the cementing intelligent leak-proof material. This is conducive to accurate leak-proofing of formations at a specific depth.

[0216] 4. Test 4

[0217] The leak-proofing and plugging performance of the cementing intelligent leak-proof pre-fluids prepared in Examples 1 to 6 on 5 mm cracks was tested at different temperatures. The results are shown in Table 8.

[0218] Table 8 Leakage-proofing and plugging performance of different leak-proof pre-filling fluids on 5 mm cracks at 90°C

[0219] Leak-proof pre-fill fluid Temperature / ℃ Pressure bearing capacity / MPa Pressure bearing time / min Leakage volume / mL SP1 50 6 >10 11.7 SP1 120 10 >10 8.7 SP1 150 7 >10 10.8 SP2 50 6 >10 12.3 SP2 120 8 >10 9.3 SP2 150 5 >10 14.8 SP3 50 6 >10 14.4 SP3 120 10 >10 9 SP3 150 8 >10 12 SP4 50 6 >10 13.7 SP4 120 9 >10 8.6 SP4 150 6 >10 14 SP5 50 6 >10 14 SP5 120 8 >10 9 SP5 150 6 >10 13.8 SP6 50 6 >10 14.7 SP6 120 8 >10 9.9 SP6 150 6 >10 14.1

[0220] Combined with the data results in Table 8, it can be seen that the cementing intelligent anti-leakage pre-fluid still has good anti-leakage and plugging capabilities for 5mm cracks, and the pressure bearing capacity and cumulative filtration loss do not decrease with the increase of crack width. The pressure bearing capacity is greater than 5MPa, and the cumulative leakage is less than 15mL. By comparing SP2 and SP3, it can be seen that when the crack width is large, the anti-leakage and plugging capabilities of the system with a low content of intelligent polymer anti-leakage materials, solid-phase auxiliary filling materials, and solid-phase support materials for cementing pre-fluids have decreased to a certain extent. This is because the 5mm crack is large and has certain requirements for the concentration of plugging pressure bearing materials. Therefore, the maximum crack width targeted by this system should not be higher than 5mm.

[0221] 5. Test 5

[0222] The leak-proofing and plugging performance of the cementing intelligent leak-proof pre-fluids prepared in Examples 1 to 6 on 0.5 mm cracks was tested at different temperatures. The results are shown in Table 9.

[0223] Table 9 Leakage-proofing and plugging performance of different leak-proof pre-fluids on 0.5 mm cracks

[0224] Leak-proof pre-fill fluid Temperature / ℃ Pressure bearing capacity / MPa Pressure bearing time / min Leakage volume / mL SP1 50 8 >10 10.2 SP1 120 12 >10 7.5 SP1 150 10 >10 8.8 SP2 50 8 >10 10 SP2 120 11 >10 7 SP2 150 8 >10 8.4 SP3 50 8 >10 8.8 SP3 120 11 >10 8.1 SP3 150 8 >10 102 SP4 50 7 >10 9.8 SP4 120 10 >10 7.4 SP4 150 8 >10 10.9 SP5 50 7 >10 10.1 SP5 120 10 >10 7.1 SP5 150 7 >10 8.7 SP6 50 7 >10 12.4 SP6 120 9 >10 7.5 SP6 150 7 >10 9.6

[0225] Combined with the data results in Table 9, it can be seen that the cementing intelligent anti-leakage pre-fluid has good anti-leakage and plugging capabilities for 0.5mm cracks, with a pressure bearing capacity greater than 9MPa and a cumulative leakage volume less than 13mL. Test examples 1 to 5 show that the cementing intelligent anti-leakage pre-fluid has good adaptability to 0.5-5mm cracks, showing the characteristics of intelligent anti-leakage.

[0226] 6. Test 6

[0227] The leakage prevention and plugging performance of the cementing intelligent anti-leakage pre-fluid prepared in Examples 1 to 6 was tested on loose sandstone at different temperatures. The sandstone as a whole is mainly composed of pores of 60-120 μm. The results are shown in Table 10.

[0228] Table 10 Leakage prevention and plugging performance of different leak prevention pre-fluids on loose sandstone at 90℃

[0229] Leak-proof pre-fill fluid Temperature / ℃ Pressure bearing capacity / MPa Pressure bearing time / min Leakage volume / mL SP1 50 10 >10 8.2 SP1 120 13 >10 6.5 SP1 150 12 >10 7.1 SP2 50 10 >10 8.1 SP2 120 12 >10 7.2 SP2 150 11 >10 8.1 SP3 50 11 >10 9.4 SP3 120 11 >10 9.1 SP3 150 10 >10 9.2 SP4 50 8 >10 10.4 SP4 120 11 >10 8.8 SP4 150 10 >10 8.9 SP5 50 12 >10 9.4 SP5 120 12 >10 8.3 SP5 150 11 >10 9.1 SP6 50 9 >10 9.1 SP6 120 10 >10 7.9 SP6 150 9 >10 8.6

[0230] It can be seen from the data recorded in Table 10 that the cementing intelligent anti-leakage pre-fluid has good anti-leakage and plugging capabilities for loose sandstone, among which the pressure bearing capacity is greater than 9MPa and the cumulative leakage volume is less than 10mL. Test examples 1 to 6 show that the cementing intelligent anti-leakage pre-fluid has good adaptability to cracks and gaps with different openings.

[0231] 7. Test 7: Evaluation of the compatibility between the intelligent anti-leakage pre-fluid and cement slurry

[0232] Taking application example 1 as an example, according to the national standard GB / T19139-2012 "Test Method for Oil Well Cement", the influence of cementing intelligent anti-leakage pre-fluid on cement slurry rheology, thickening time and cement stone compressive strength was tested, and the compatibility of cementing intelligent anti-leakage pre-fluid and cement slurry was analyzed. The monitoring results are recorded in Table 11 below.

[0233] Table 11 is the evaluation of the compatibility between the intelligent anti-leakage pre-fluid SP1 and cement slurry

[0234]

[0235]

[0236] Note: The cement used in the present invention is Jiahua G-grade oil well cement (high sulfur resistance, HSR). # represents the mass percentage of cement. Cement slurry formula: 600g Jiahua G-grade cement + 25% reinforcing material DRB-2S (200 mesh) + 4% toughening material DRE-3S + 1% microsilica + 1% early strength agent DRA-1S + 1% dispersant DRS-1S + 0.2% DRK-3S stabilizer + 2% fluid loss reducer DRF-3L + 1.2% anti-channeling regulator DRT-LT + 8% latex anti-channeling agent DRT-1L + 45% water + 0.5% anti-foaming agent DRX-2L (density 1.89g / cm 3 ).

[0237] According to the test results in Table 11, it can be seen that the pre-fluid has little effect on the rheological properties of cement slurry and has good rheological compatibility. At the same time, it does not cause a significant shortening of the cement slurry thickening time or a significant reduction in the compressive strength of the cement stone, which can meet the requirements of cementing construction and later cementing quality.

[0238] The above are only preferred feasible embodiments of the present invention, and the protection scope of the present invention is not limited thereto. Various modifications or applications made according to the above embodiments are within the protection scope of this technical solution.

[0239] Although the specific embodiments of the present invention have been described in detail, it will be understood by those skilled in the art. According to all the teachings disclosed, various modifications and replacements can be made to those details, and these changes are all within the protection scope of the present invention. The full scope of the present invention is given by the attached claims and any equivalents thereof.

Claims

1. A polymer material, characterized in that The polymer material refers to a polymer having anionic groups, cationic groups and hydrophobic groups on the molecular chain; the polymer is a straight-chain polymer, and the anionic groups, cationic groups and hydrophobic groups are randomly distributed on the main chain of the polymer through covalent bonds.

2. The polymer material according to claim 1, characterized in that The composition comprises the following components by weight: 15 to 22 parts of 2-enamide-2-methylpropanesulfonic acid, 0.8 to 1.8 parts of amphiphilic unsaturated cationic monomer and 2.5 to 4 parts of unsaturated carboxylic acid monomer.

3. The polymer material according to claim 2, characterized in that The composition comprises the following components by weight: 15 to 22 parts of 2-enamide-2-methylpropanesulfonic acid, 0.8 to 1.8 parts of amphiphilic unsaturated cationic monomer, 2.5 to 4 parts of unsaturated carboxylic acid monomer, and 10 to 20 parts of unsaturated amide monomer.

4. The polymer material according to claim 3, characterized in that The amphiphilic unsaturated cationic monomer is shown in formula (I): In the formula, R is H or a C1-C4 alkyl group, and n is 11, 13, 15, 17 or 19.

5. The polymer material according to claim 3, characterized in that The unsaturated carboxylic acid monomer is selected from one of maleic acid, itaconic acid or acrylic acid.

6. The polymer material according to claim 3, characterized in that The unsaturated amide monomer is selected from one of diacetone acrylamide, N,N-dimethyl acrylamide or N,N-diethyl acrylamide.

7. The polymer material according to claim 3, characterized in that The polymeric material also includes an initiator.

8. The method for preparing a polymer material according to claim 7, characterized in that: The mass of the initiator accounts for 0.15-0.5% of the total mass of the four substances of the 2-enamide-2-methylpropane sulfonic acid, the amphiphilic unsaturated cationic monomer, the unsaturated carboxylic acid monomer and the unsaturated amide monomer.

9. The polymer material according to claim 8, characterized in that The initiator adopts an oxidant-reducing agent initiation system.

10. The polymer material according to claim 9, characterized in that The oxidizing agent is selected from ammonium persulfate and / or potassium persulfate; the reducing agent is selected from sodium bisulfite and / or sodium hydroxide.

11. The polymer material according to claim 10, characterized in that The molar ratio of the oxidizing agent to the reducing agent is 1:(0.5-1).

12. A method for preparing a polymer material according to any one of claims 1 to 11, characterized in that: The method uses 2-enamide-2-methylpropanesulfonic acid, anionic groups introduced by unsaturated carboxylic acid monomers, and cationic groups and hydrophobic groups introduced by amphiphilic unsaturated cationic monomers when preparing polymer materials.

13. The method for preparing a polymer material according to claim 12, characterized in that: The following steps are involved: S1. Preparation of mixture M1 adding water to dissolve the amphiphilic unsaturated cationic monomer to prepare a mixture M1; S2. Preparation of mixture M2 Add 2-enamide-2-methylpropanesulfonic acid, unsaturated amide monomer and unsaturated carboxylic acid monomer to water in sequence, stir to dissolve, and adjust the pH value of the solution to obtain a mixture M2; S3. Preparation of polymer solution S1 is heated in a water bath to obtain a mixture M1, and the mixture M2 obtained by S2 and an aqueous solution of an initiator are simultaneously added dropwise under stirring. After the addition is completed, the temperature is raised to react to obtain a polymer solution.

14. The method for preparing a polymer material according to claim 13, characterized in that: In S2, the pH value of the solution is adjusted to 6-7.

15. The method for preparing a polymer material according to claim 13, characterized in that: In S3, the water bath temperature is set to 40-50°C.

16. The method for preparing a polymer material according to claim 13, characterized in that: In S3, the stirring speed is set to 50-150 rpm.

17. The method for preparing a polymer material according to claim 13, characterized in that: In S3, the dropping time is controlled to be 3 to 5 hours.

18. The method for preparing a polymer material according to claim 13, characterized in that: In S3, the temperature is raised to 50-55° C. for 4-6 hours.

19. A leakproof material, characterized in that: The leakage-proof material uses the polymer material according to any one of claims 1 to 18.

20. A cementing anti-leakage pre-fluid, characterized in that: The cementing leak-proof pre-fluid comprises the leak-proof material as claimed in claim 19.

21. A cementing process, characterized in that: The cementing process uses the cementing anti-leakage pre-fluid as claimed in claim 20.

Citation Information

Patent Citations

  • Acrylic amide modified graft copolymer, preparation method and application thereof

    CN101492515A

  • Plugging agent and preparation method thereof

    CN103396774A

  • Treating agent for zwitter-ion inorganic-organic monomer polymer drilling fluid and preparation method of treating agent

    CN104357026A

  • Oil well cement high temperature resistance suspending agent

    CN105199690A

  • Preparation method for hydrophobic associated polymer coating agent used for drilling fluid

    CN106221680A