Method for centrifugally inducing fiber orientation

The method of inducing fiber orientation through centrifugation has solved the problem of the complexity and inappropriate large-scale preparation of collagen biostents in the prior art, and achieved simplified operation and large-scale production, which is suitable for the production of biostents.

CN118994634AInactive Publication Date: 2024-11-22STAR SPORTS MEDICINE CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411479167.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing methods for building orientation structures are complex and not suitable for large-scale preparation, requiring additional experimental steps and specialized equipment, making it difficult to effectively apply in the production of biological scaffolds.

Method used

The fiber orientation is induced by centrifugation. By dissolving collagen in acidic aqueous solution, shear dispersion and alkaline aqueous solution are mixed, the pH is adjusted, and the fiber is centrifuged by a high-speed low-temperature centrifuge to achieve the macro orientation of the fiber.

Benefits of technology

The operation steps are simplified, the equipment needs are reduced, the large-scale production of collagen biostents is realized, and the fiber orientation is completed during the product centrifugal concentration process, without the need for additional separation steps, and is suitable for subsequent production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994634A_ABST
    Figure CN118994634A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of regenerative medicine, and particularly relates to a method for centrifugally inducing fiber orientation. The method comprises the following steps: swelling collagen in an acidic aqueous solution to obtain raw material slurry; shearing and dispersing the raw material slurry to obtain dispersed slurry; mixing an alkaline aqueous solution with the dispersed slurry, and adjusting the pH value to obtain a fiber suspension; and centrifuging the fiber suspension. According to the method, fiber induced orientation is achieved through a centrifugal machine, specifically, during centrifugal operation, the combination of an ultra-speed centrifugal machine and a flat-angle rotor should be selected, in this way, it can be guaranteed that a centrifugal tube is unfolded in the horizontal direction when the centrifugal operation is conducted, and vertical orientation of fibers in the tube can be achieved under the induction of centrifugal force. According to the method, induced orientation is carried out in the centrifugal concentration process of the product, and additional production steps do not need to be added; the product obtained by the technology can be directly applied to subsequent production steps without additional separation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of regenerative medicine, and in particular relates to a method for centrifugation-induced fiber orientation. Background Art

[0002] As a common biomaterial, collagen often exists in an anisotropic structure in the tissues of organisms, that is, these collagen fibers show a certain orientation in the tissues. For example, the necessary mechanical strength of load-bearing tissues (tendons, ligaments and muscles) can only be provided by regular oriented structures. The orientation of collagen fibers also has a significant effect on the tensile strength and bending strength of bones. More and more evidence shows that biological scaffolds for tissue engineering need to have a structure similar to the original tissue in the body. Therefore, biological scaffolds with oriented structures are the next key research direction.

[0003] There are many existing methods for constructing oriented structures, such as: (i) Magnetic field method (Chen S, Hirota N, Okuda M, et al. Microstructures andrheological properties of tilapia fish-scale collagen hydrogels with aligned fibrils fabricated under magnetic fields [J]. Acta Biomaterialia, 2011, 7(2):644-652); (ii) Electric field method (Cheng (iii) Shear deposition method (Saeidi N, Sander EA, Ruberti J W. Dynamic shear-influenced collagen self-assembly[J]. Biomaterials, 2009, 30(34): 6581-6592); (iv) Microfluidic method (Lee P, Lin R, Moon J, et al. Microfluidic alignment ofcollagen fibers for in vitro cell culture[J]. Biomedical microdevices, 2006,8: 35-41); (v) Spin coating method (Saeidi N, Sander EA, Zareian R, et al. Production of highly aligned collagen lamellae by combining shear force and thin filmconfinement[J]. Acta biomaterialia, 2011, 7(6): 2437-2447) and so on.

[0004] However, these methods always require complicated processes, additional experimental steps and specialized techniques and instruments, and are only applicable to small-scale preparation of collagen with oriented structures.

[0005] Therefore, based on this, the technical solution of the present invention is proposed. Summary of the invention

[0006] In order to solve the problems existing in the prior art in the process of preparing collagen bioscaffolds, the present invention provides a method for inducing fiber orientation by centrifugation, which can macroscopically prepare highly oriented collagen and combine the orientation process with normal operations in production, thereby reducing the operating steps, avoiding the purchase of additional production equipment, and realizing large-scale production of products. The method comprises the following steps: (1) Swelling collagen in an acidic aqueous solution to obtain a raw material slurry; (2) shearing and dispersing the raw material slurry to obtain a dispersed slurry; (3) mixing the dispersed slurry with an alkaline aqueous solution and adjusting the pH to obtain a fiber suspension; (4) The fiber suspension is centrifuged to complete the fiber orientation.

[0007] Preferably, in step (1), the collagen is insoluble type I collagen.

[0008] Preferably, in step (1), the acidic aqueous solution includes but is not limited to acetic acid aqueous solution, lactic acid aqueous solution, and hydrochloric acid aqueous solution.

[0009] Preferably, in step (2), the shear dispersion rate is 5000-20000 r / min, the time is 60-240 min, and the temperature is 0°C.

[0010] Preferably, in step (3), the alkaline aqueous solution includes but is not limited to aqueous ammonia, aqueous sodium bicarbonate solution, and aqueous sodium hydroxide solution.

[0011] Preferably, in step (3), the pH of the fiber suspension is 4.0-5.5.

[0012] Preferably, in step (4), the number of centrifugation is 5 to 10 times, the centrifugal speed is 8000 to 50000 r / min, and the centrifugal temperature is 0 to 8°C.

[0013] The obtained fiber suspension is concentrated using a high-speed low-temperature centrifuge, preferably a Beckman XP-100 centrifuge, which can provide a rotation speed of up to 100,000 rpm and can be replaced by a rotor to facilitate the use of various types of centrifuge tubes. The rotor used for centrifugation is selected according to the centrifugation parameters, preferably a SW32Ti flat-angle rotor, and the centrifuge tube is preferably a Beckman 38.5 mL Ultra-clear centrifuge tube.

[0014] The beneficial effects of the present invention are: The method of the present invention uses a centrifuge to achieve fiber induced orientation. Specifically, during the centrifugal operation, a combination of an ultracentrifuge and a flat-angle rotor should be selected to ensure that the centrifuge tube is unfolded in the horizontal direction during the centrifugal operation, and the fibers in the tube can be induced to achieve vertical orientation under the induction of centrifugal force. The present invention induces orientation during the centrifugal concentration process of the product without adding additional production steps; the product obtained by applying this technology can be directly used in subsequent production steps without additional separation. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0016] Figure 1 This is the electron microscope image of the first orientation result.

[0017] Figure 2 This is the electron microscope image of the second orientation result.

[0018] Figure 3 This is the electron microscope image of the third orientation result.

[0019] Figure 4 This is the electron microscope image of the fourth orientation result. DETAILED DESCRIPTION

[0020] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0021] Example 1 This embodiment provides a method for centrifugation-induced fiber orientation, the method comprising the following steps: (1) 5 g of insoluble type I collagen was dispersed in 1000 mL of acetic acid aqueous solution to obtain a raw material slurry with a solid content of 0.5% and a pH of 3.2; (2) at 0° C., using a high-speed shearing machine to shear and disperse the raw material slurry at a speed of 12,000 r / min for 180 min to obtain a dispersed slurry; (3) at 0° C., mixing a sodium bicarbonate aqueous solution with a pH of 10 with the dispersed slurry and adjusting the pH to 4.7 to obtain a fiber suspension; (4) Centrifuge at 6°C and 12,000 r / min for 10 min in a low-temperature high-speed centrifuge (Beckman XP-100 centrifuge) and discard the supernatant in the centrifuge tube (Beckman 38.5 mL Ultra-clear centrifuge tube). Then, add the fiber suspension and place the centrifuge tube into a rotor (SW32Ti flat-angle rotor). Repeat the centrifugation at 6°C and 12,000 r / min for 7 times to achieve centrifugal induced orientation of the collagen fibers.

[0022] Example 2 This embodiment provides a method for centrifugation-induced fiber orientation, the method comprising the following steps: (1) 7.5 g of insoluble type I collagen was dispersed in 1000 mL of acetic acid aqueous solution to obtain a raw material slurry with a solid content of 0.75% and a pH of 2.6; (2) at 0° C., using a high-speed shearing machine to shear and disperse the raw material slurry at a speed of 8000 r / min for 60 min to obtain a dispersed slurry; (3) at 0° C., mixing the dispersed slurry with dilute ammonia water having a pH of 11 and adjusting the pH to 5.0 to obtain a fiber suspension; (4) Centrifuge at 10,000 r / min for 15 min at 4°C in a low-temperature high-speed centrifuge (Beckman XP-100 centrifuge), discard the supernatant in the centrifuge tube (Beckman 38.5 mL Ultra-clear centrifuge tube), add the fiber suspension, place the centrifuge tube in a rotor (SW32Ti flat-angle rotor), and repeat the centrifugation at 4°C and 10,000 r / min for 10 times to achieve centrifugal induced orientation of the collagen fibers.

[0023] Example 3 This embodiment provides a method for centrifugation-induced fiber orientation, the method comprising the following steps: (1) 15 g of insoluble type I collagen was dispersed in 1000 mL of acetic acid aqueous solution to obtain a raw material slurry with a solid content of 1.5% and a pH of 2.5; (2) at 0° C., using a high-speed shearing machine to shear and disperse the raw material slurry at a speed of 20,000 r / min for 180 min to obtain a dispersed slurry; (3) at 0° C., mixing the dispersed slurry with an aqueous sodium hydroxide solution having a pH of 12 and adjusting the pH to 5.2 to obtain a fiber suspension; (4) Centrifuge at 20,000 r / min at 4°C for 20 min in a low-temperature high-speed centrifuge (Beckman XP-100 centrifuge). Discard the supernatant in the centrifuge tube (Beckman 38.5 mL Ultra-clear centrifuge tube), add the fiber suspension, place the centrifuge tube in a rotor (SW32Ti flat-angle rotor), and repeat the centrifugation at 4°C and 20,000 r / min for 5 times to achieve centrifugal induced orientation of the collagen fibers.

[0024] Test example The morphology of the collagen scaffold and the orientation of the surface collagen fibers were detected by scanning electron microscopy. The sample was pre-frozen with liquid nitrogen and quenched. After repeating the freeze-drying process, the sample was sprayed with gold and glued to the sample stage with conductive glue. The surface morphology and fiber orientation of the sample were observed using an S-4800 scanning electron microscope at a voltage of 15KV. The results are as follows. The red arrows in the scanning electron microscope image indicate the orientation direction of the fibers. Figure 1~Figure 4 As shown, Figure 1 The centrifugal result at 10000 rpm for 10 min shows that the orientation of the fibers can be vaguely observed on the surface. Figure 2 The centrifugation result of 10000 rpm and 20 min showed that obviously oriented fibers appeared on the surface of the sample, but the number was small; Figure 3 The centrifugation result of 20000 rpm and 10 min showed that a large number of fibers with oriented structures could be observed on the surface of the samples. Although the first three samples showed the phenomenon of fiber orientation, fibers that did not conform to the orientation direction could still be observed. Figure 4 In the figure, we increased the centrifugation conditions to 30,000 rpm for 10 min. We found that most of the fibers on the surface of the sample have an oriented structure toward the left side of the image. Therefore, it can be determined that the degree of oriented structure becomes more obvious as the centrifugal speed or centrifugal time increases.

[0025] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for centrifugally inducing fiber orientation, characterized in that: The method comprises the following steps: (1) Swelling collagen in an acidic aqueous solution to obtain a raw material slurry; (2) shearing and dispersing the raw material slurry to obtain a dispersed slurry; (3) mixing the dispersed slurry with an alkaline aqueous solution and adjusting the pH to obtain a fiber suspension; (4) The fiber suspension is centrifuged to complete the fiber orientation.

2. The method of centrifugally inducing fiber orientation according to claim 1, characterized in that: In step (1), the collagen is insoluble type I collagen.

3. The method of centrifugally inducing fiber orientation according to claim 1, characterized in that: In step (1), the acidic aqueous solution is an acetic acid aqueous solution, a lactic acid aqueous solution or a hydrochloric acid aqueous solution.

4. The method of centrifugally inducing fiber orientation according to claim 1, characterized in that: In step (1), the solid content of the raw material slurry is 0.5-1.5%, and the pH of the raw material slurry is 2.0-3.

5.

5. The method of centrifugally inducing fiber orientation according to claim 1, characterized in that: In step (2), the shear dispersion rate is 5000-20000 r / min, the time is 60-240 min, and the temperature is 0°C.

6. The method of centrifugally inducing fiber orientation according to claim 1, characterized in that: In step (3), the alkaline aqueous solution is aqueous ammonia, aqueous sodium bicarbonate solution or aqueous sodium hydroxide solution.

7. The method of centrifugally inducing fiber orientation according to claim 1, characterized in that: In step (3), the pH of the fiber suspension is 4.0-5.

5.

8. The method of centrifugally inducing fiber orientation according to claim 1, characterized in that: In step (4), the number of centrifugation is 5 to 10 times, the centrifugal speed is 8000 to 50000 r / min, and the centrifugal temperature is 0 to 8°C.

Citation Information

Patent Citations

  • Method for improving tensile strength of collagen fiber material

    CN104213238A

  • Modified type-I collagen, modification method, and collagen gel prepared from modified type-I collagen

    CN110343169A

  • Preparation method for and use method of collagen microfiber hemostatic material

    US20230173136A1