Two-component adhesive composition

By developing a two-component adhesive composition containing delayed curing catalysts and heat-sensitive catalysts, the problems of strength and opening time requirements of existing adhesives in lithium-ion battery packaging are solved, and the effects of rapid curing and strength establishment are achieved.

CN118995115APending Publication Date: 2024-11-22PPG COATINGS TIANJIN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411189480.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing adhesives are difficult to meet high strength and good elongation requirements in areas such as lithium-ion battery packaging, while quickly establishing strength and having appropriate opening time.

Method used

Develop a two-component adhesive composition, including components A and components B, which contain delayed curing catalysts and thermally sensitive catalysts, and component B contains hydrophobic modified aluminum hydroxide, through specific component ratios and treatments Method to achieve rapid curing and strength establishment while having appropriate opening time.

Benefits of technology

It realizes the mechanical performance requirements in the fields of lithium-ion battery packaging, has the characteristics of rapid curing and strength establishment, and has the appropriate opening time to meet the needs of adhesives in these applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a two-component adhesive composition which comprises a component A and a component B. The component A comprises a first catalyst, a second catalyst and a first filler composition, the component B comprises a second filler composition, the first catalyst is a delayed curing catalyst, the second catalyst is a heat sensitive catalyst, and the first filler composition and the second filler composition are combined to form the two-component adhesive composition. Each of the first and second filler compositions includes a hydrophobically modified aluminum hydroxide. The invention further discloses a base material coated with the two-component adhesive composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of adhesives, and in particular to a two-component adhesive composition. Background Art

[0002] Adhesive technology is a preferred assembly method. Compared with mechanical fixation, adhesive fixation does not damage the physical structure of the substrate. At present, adhesive technology is widely used in various fields, for example, the packaging of lithium-ion batteries. In order to meet the application, the adhesive not only needs to have high strength and good elongation, but also is expected to have fast strength and suitable open time. Summary of the invention

[0003] The present inventors have conducted extensive research and developed a two-component adhesive composition that meets the mechanical property requirements of fields such as lithium-ion battery packaging, while quickly building strength and having a suitable open time, thereby providing a solution to the concerns in the adhesive field.

[0004] The invention discloses a two-component adhesive composition, comprising component A and component B, wherein component A comprises a first catalyst, a second catalyst and a first filler composition, and component B comprises a second filler composition, wherein the first catalyst is a delayed curing catalyst, the second catalyst is a heat-sensitive catalyst, and each of the first and second filler compositions comprises hydrophobically modified aluminum hydroxide.

[0005] The invention further discloses a coated substrate, comprising a substrate and the two-component adhesive composition coated on at least a portion of the substrate.

[0006] The features and advantages of the present invention will be specifically presented in the following detailed description of the embodiments. DETAILED DESCRIPTION

[0007] In this application, unless expressly stated otherwise, the use of the singular includes the plural and the plural includes the singular. For example, although "a" polymer is mentioned herein, one or more of the material may be used.

[0008] In the present application, the terms "include", "comprises", "contains", etc. are not intended to limit the present invention to exclude any variation or addition. In addition, although the present invention has described the adhesive composition, preparation method, etc. with terms such as "includes", the adhesive composition, preparation method, etc. described in detail herein may also be described as "essentially consisting of" or "consisting of". In this case, "essentially consisting of" means that any additional ingredients will not have a substantial effect on the properties of the adhesive layer formed by the adhesive composition.

[0009] In this application, unless otherwise expressly stated, the use of "or" means "and / or", even though "and / or" may be expressly used in certain circumstances. In addition, it should be understood that any numerical range listed herein is intended to include all subranges contained therein. For example, a range of "1 to 10" is intended to include all subranges between the listed minimum value of 1 and the listed maximum value of 10 (including the end values), that is, all subranges having a minimum value equal to or greater than 1 and a maximum value equal to or less than 10.

[0010] Except in the examples or otherwise explicitly stated, all numerical values ​​used in the specification and claims representing the quantity of ingredients, etc., should be considered to be subject to variation according to the term "about" in all cases. Therefore, unless otherwise stated, the numerical parameters listed in the following specification and claims are approximate values ​​and may vary according to the performance desired to be obtained by the present invention. At the very least, it is not intended to limit the application of the doctrine of equivalents to the scope of the claims. Each numerical parameter should at least be interpreted in terms of significant figures and ordinary rounding should be applied.

[0011] Although the numerical ranges and parameters setting forth the broad scope of the invention are approximate, the numerical values ​​set forth in the specific embodiments are recorded as accurately as possible. However, any numerical value inherently has certain errors, which are the inevitable result of the standard deviation obtained in its corresponding measurement method.

[0012] As described above, the present invention relates to a two-component adhesive composition, comprising component A and component B, wherein component A comprises a first catalyst, a second catalyst and a first filler composition, and component B comprises a second filler composition, wherein the first catalyst is a delayed curing catalyst, the second catalyst is a thermosensitive catalyst, and each of the first and second filler compositions comprises hydrophobically modified aluminum hydroxide.

[0013] As used herein, the term "two-component", or "2K", means that the components of the adhesive composition are separated into two components and packaged separately, and the two packages are mixed in an accurate ratio before use.

[0014] As used herein, the "delayed curing catalyst" refers to a catalyst that has low or even no catalytic activity at the beginning of the reaction, but whose catalytic activity increases as the reaction progresses. In some cases, the delayed curing catalyst may contain a structure that inhibits the catalytic effect, and when the structure is consumed, the delayed curing catalyst begins to work.

[0015] As used herein, the "thermosensitive catalyst" refers to a catalyst whose catalytic activity changes with temperature, for example, the catalytic activity is low at room temperature / low temperature, but the catalytic activity increases at elevated temperature.

[0016] The delayed curing catalyst suitable for the present invention can include a tin mercapto catalyst. The tin mercapto catalyst includes a compound containing a sulfhydryl group and a carbon-tin linking group, which can catalyze the reaction of active hydrogen and isocyanate groups. Suitably, the tin mercapto catalyst can include: dibutyl tin bisthiol, dibutyl tin dimercaptoacetate, bis (dodecyl sulfide) dimethyl tin, dimethyl tin mercaptides, dioctyl tin dithioacetate, dimethyl tin dithioacetate or any combination thereof. Suitably, the tin mercapto catalyst can include dimethyl tin dithioacetate.

[0017] Based on the total weight of component A, the content of the delayed curing catalyst can be 0.005 wt% or more, 0.01 wt% or more, or 0.02 wt% or more, and / or 0.1 wt% or less, 0.09 wt% or less, 0.08 wt% or less, 0.07 wt% or less, 0.06 wt% or less, 0.05 wt% or less, 0.04 wt% or less, or 0.03 wt% or less. Based on the total weight of component A, the content of the delayed curing catalyst can be 0.005-0.1 wt%, 0.01-0.04 wt%, 0.01-0.03 wt%, or within a range with any of the above values ​​as endpoints.

[0018] The heat-sensitive catalyst suitable for the present invention may include an amine catalyst and an optional catalyst promoter. The amine catalyst may catalyze the reaction of active hydrogen and isocyanate groups. The promoter may improve the efficiency of the catalyst and / or change the working temperature of the catalyst. Suitably, the amine catalyst includes: 1,8-diazabicyclo[5.4.0]undec-7-ene, 1-dimethylaminoethyl-4-methylpiperazine, bismorpholinyl diethyl ether, or any combination thereof. Suitably, the catalyst promoter may include: formic acid, isooctanoic acid, phenol, or any combination thereof. For example, the heat-sensitive catalyst may include 1,8-diazabicyclo[5.4.0]undec-7-ene and formic acid. For example, the heat-sensitive catalyst may include 1,8-diazabicyclo[5.4.0]undec-7-ene and isooctanoic acid. For example, the heat-sensitive catalyst may include 1,8-diazabicyclo[5.4.0]undec-7-ene and phenol.

[0019] Based on the total weight of component A, the content of the thermosensitive catalyst can be 0.05 wt% or more, 0.1 wt% or more, 0.2 wt% or more, or 0.3 wt% or more, and / or 1 wt% or less, 0.9 wt% or less, 0.8 wt% or less, 0.7 wt% or less, 0.6 wt% or less, 0.5 wt% or less, or 0.4 wt% or less. Based on the total weight of component A, the content of the thermosensitive catalyst can be 0.05-1 wt%, 0.3-0.4 wt%, or in a range with any of the above values ​​as endpoints.

[0020] In the adhesive composition according to the present invention, the A component further comprises a first filler composition. The first filler composition comprises hydrophobically modified aluminum hydroxide. Suitably, the hydrophobically modified aluminum hydroxide may comprise silane-modified aluminum hydroxide. As used herein, the "modification" refers to treatment by chemical and / or physical means, such as chemical grafting, physical coating, etc.

[0021] Suitably, the silane-modified aluminum hydroxide may include: aminosilane-modified aluminum hydroxide, vinylsilane-modified aluminum hydroxide, epoxysilane-modified aluminum hydroxide, mercaptosilane-modified aluminum hydroxide, alkylsilane-modified aluminum hydroxide, titanatesilane-modified aluminum hydroxide, aluminatesilane-modified aluminum hydroxide, or any combination thereof. Suitably, the silane-modified aluminum hydroxide may include: epoxysilane-modified aluminum hydroxide, alkylsilane-modified aluminum hydroxide, or any combination thereof.

[0022] Based on the total weight of the first filler composition, the content of the hydrophobically modified aluminum hydroxide can be 50 wt% or more, 55 wt% or more, or 60 wt% or more, and / or 75 wt% or less, 70 wt% or less, or 65 wt% or less. Based on the total weight of the first filler composition, the content of the hydrophobically modified aluminum hydroxide can be 50-75 wt%, 55-70 wt%, 60-65 wt%, or within a range with any of the above values ​​as endpoints.

[0023] In addition to the hydrophobically modified aluminum hydroxide, the first filler composition may also include other fillers. Suitably, the other fillers may include fumed silica, hydrophobically modified fumed silica, aluminum hydroxide, silicon dioxide, calcium carbonate, aluminum hypophosphite, diethyl aluminum hypophosphite, or any combination thereof. As used herein, the "modification" refers to treatment by chemical and / or physical means, such as chemical grafting, physical coating, etc. Suitably, the first filler composition may also include fumed silica, diethyl aluminum hypophosphite, or any combination thereof.

[0024] Suitably, the first filler composition may include hydrophobically modified aluminum hydroxide, fumed silica and diethyl aluminum hypophosphite. Suitably, in the first filler composition, the weight ratio of hydrophobically modified aluminum hydroxide, fumed silica and diethyl aluminum hypophosphite may be (5-15): (0-1): (1-15). Suitably, the content of diethyl aluminum hypophosphite may be 15 to 25 wt%, such as 18-22 wt%, of the total weight of the A component.

[0025] In the adhesive composition according to the present invention, the component B further comprises a second filler composition. The second filler composition may be the same as or different from the first filler composition.

[0026] The second filler composition includes hydrophobically modified aluminum hydroxide. Suitably, the hydrophobically modified aluminum hydroxide may include silane-modified aluminum hydroxide. As used herein, the "modification" refers to treatment by chemical and / or physical means, such as chemical grafting, physical coating, etc.

[0027] Suitably, the silane-modified aluminum hydroxide may include: aminosilane-modified aluminum hydroxide, vinylsilane-modified aluminum hydroxide, epoxysilane-modified aluminum hydroxide, mercaptosilane-modified aluminum hydroxide, alkylsilane-modified aluminum hydroxide, titanatesilane-modified aluminum hydroxide, aluminatesilane-modified aluminum hydroxide, or any combination thereof. Suitably, the silane-modified aluminum hydroxide may include: epoxysilane-modified aluminum hydroxide, alkylsilane-modified aluminum hydroxide, or any combination thereof.

[0028] Based on the total weight of the second filler composition, the content of the hydrophobically modified aluminum hydroxide can be 40 wt% or more, 45 wt% or more, or 50 wt% or more, and / or 65 wt% or less, 60 wt% or less, or 55 wt% or less. Based on the total weight of the second filler composition, the content of the hydrophobically modified aluminum hydroxide can be 40-65 wt%, 45-60 wt%, 50-55 wt%, or in a range with any of the above values ​​as endpoints.

[0029] In addition to the hydrophobically modified aluminum hydroxide, the second filler composition may also include other fillers. Suitably, the other fillers may include fumed silica, hydrophobically modified fumed silica, aluminum hydroxide, silicon dioxide, calcium carbonate, aluminum hypophosphite, diethyl aluminum hypophosphite, or any combination thereof. As used herein, the "modification" refers to treatment by chemical and / or physical means, such as chemical grafting, physical coating, etc. Suitably, the second filler composition may also include fumed silica, diethyl aluminum hypophosphite, or any combination thereof.

[0030] Suitably, the second filler composition may include hydrophobically modified aluminum hydroxide, fumed silica and diethyl aluminum hypophosphite. Suitably, in the second filler composition, the weight ratio of hydrophobically modified aluminum hydroxide, fumed silica and diethyl aluminum hypophosphite may be (5-15): (0-1): (1-15). Suitably, the content of diethyl aluminum hypophosphite may be 15 to 25 wt%, such as 18-22 wt%, of the total weight of the B component.

[0031] In the adhesive composition according to the present invention, the A component may also include a polyol. As used herein, the "polyol" refers to a compound containing at least two hydroxyl groups in each molecule. The polyol may include a simple polyol, a polyether polyol, a polyester polyol, a polycarbonate polyol, a polybutadiene polyol, or any combination thereof. The polyol may include a modified polyol and / or an unmodified polyol. As used herein, the "simple polyol" refers to a polyol that does not contain a polymerized organic unit. As used herein, the "modification" refers to the access of a functional group through a chemical bond to change properties such as hydrophobicity / hydrophilicity.

[0032] Based on the total weight of component A, the content of the polyol can be 35 wt% or more, 40 wt% or more, or 45 wt% or more, and / or 65 wt% or less, 60 wt% or less, or 55 wt% or less. Based on the total weight of component A, the content of the polyol can be 35-65 wt%, 40-60 wt%, 45-55 wt%, or within the range of any of the above values ​​as endpoints.

[0033] In the adhesive composition according to the present invention, the component B may further include an isocyanate prepolymer. As used herein, the "isocyanate prepolymer" refers to a compound prepared by reacting a polyol with an isocyanate compound and having an isocyanate terminal group.

[0034] The content of the isocyanate prepolymer may be 30 wt % or more, 40 wt % or more, or 50 wt % or more, and / or 80 wt % or less, 70 wt % or less, or 60 wt % or less, based on the total weight of component B. The content of the isocyanate prepolymer may be 30-80 wt %, 40-70 wt %, 50-60 wt %, or within a range with any of the above values ​​as endpoints, based on the total weight of component B.

[0035] In the adhesive composition according to the present invention, the polyol in the component A and the isocyanate prepolymer in the component B undergo a cross-linking reaction to form an adhesive film.

[0036] The adhesive composition according to the present invention may further include a dehumidifier. Suitably, the dehumidifier may include 1,3-oxazapentane, p-toluenesulfonyl isocyanate, triethyl orthoformate, a molecular sieve activator, or any combination thereof.

[0037] The dewatering agent may be present in the component A and / or the component B. The dewatering agent present in the component A may be the same as or different from the dewatering agent present in the component B. For example, the dewatering agent in the component A may include: molecular sieve activation powder, 1,3-oxazapentane, triethyl orthoformate, or any combination thereof. For example, the dewatering agent in the component B may include: 1,3-oxazapentane, p-toluenesulfonyl isocyanate, triethyl orthoformate, or any combination thereof. The content of the dewatering agent may be 0-15 wt%, such as 1-15 wt%, such as 5-10 wt% in the component A. The content of the dewatering agent may be 0-1 wt%, such as 0.01-1 wt%, such as 0.3-0.5 wt% in the component B.

[0038] The adhesive composition according to the present invention may further include a silane coupling agent. Suitably, the silane coupling agent may include: γ-glycidyloxypropyltrimethoxysilane, isocyanatepropyltrimethoxysilane, 3-(2,3-epoxypropyloxy)propyltrimethoxysilane, or any combination thereof.

[0039] The silane coupling agent may be present in the component A and / or the component B. The silane coupling agent present in the component A may be the same as or different from the silane coupling agent present in the component B. The silane coupling agent may be present in the component A in an amount of 0-5 wt%, such as 1-5 wt%, such as 2-5 wt%. The silane coupling agent may be present in the component B in an amount of 0-5 wt%, such as 1-5 wt%, such as 2-5 wt%.

[0040] The adhesive composition according to the present invention may further include one or more other additives. The other additives may be present in the component A and / or the component B, and the amount thereof is determined by those skilled in the art according to the desired performance.

[0041] Suitably, the adhesive composition according to the present invention may include component A and component B, wherein:

[0042] The A component may include, based on the total weight of the A component:

[0043] 35-65 wt% polyol,

[0044] 0.005-0.1 wt% delayed curing catalyst,

[0045] 0.05-1 wt% heat-sensitive curing agent,

[0046] 5-15 wt% of a water scavenger, and

[0047] 20-59 wt% filler;

[0048] The B component may include, based on the total weight of the B component:

[0049] 40-80 wt% of isocyanate prepolymer,

[0050] 1-5 wt% of silane coupling agent,

[0051] 0-1 wt% of water scavenger, and

[0052] 15-58 wt% filler.

[0053] Suitably, the adhesive composition according to the present invention may include component A and component B, wherein:

[0054] The A component may include, based on the total weight of the A component:

[0055] 45-50 wt% polyol,

[0056] 0.005-0.05 wt% delayed curing catalyst,

[0057] 0.3-0.5 wt% heat-sensitive curing agent,

[0058] 5-10 wt% of dehumidifier, and

[0059] 40-50 wt% filler;

[0060] The B component may include, based on the total weight of the B component:

[0061] 50-60 wt% of isocyanate prepolymer,

[0062] 2-5 wt% of silane coupling agent,

[0063] 0.3-0.5 wt% of water scavenger, and

[0064] 35-46 wt% filler.

[0065] In the adhesive composition according to the present invention, the A component and the B component have appropriate viscosities. Suitably, the A component has a viscosity of 50,000-70,000 cps at room temperature. Suitably, the B component has a viscosity of 50,000-70,000 cps at room temperature. In this article, the room temperature refers to 15-30° C., such as 23° C. The viscosity can be measured using a commercially available Brookfield viscometer using a #7 rotor.

[0066] In the adhesive composition according to the present invention, the component A and the component B are mixed before being applied to the substrate. Suitably, the weight ratio of the component A to the component B may be 1:1.1 to 1.1:1, for example 1:1.

[0067] The adhesive composition according to the present invention can be prepared by the following method:

[0068] Component A: (1) mix all liquid raw materials except the catalyst; (2) add all solid raw materials to the mixture obtained in (1), stir under vacuum at 80°C for 2 hours to remove moisture and make the mixture uniform; and (3) cool the mixture obtained in (2) to room temperature, add the catalyst, and stir under vacuum for 1 hour.

[0069] Component B: (1) adding other raw materials except the silane coupling agent, stirring under vacuum at 80° C. for 2 h to remove moisture and make the mixture uniform; and (2) cooling the mixture obtained in (1) to room temperature, adding the silane coupling agent, and stirring under vacuum for 1 hour.

[0070] The adhesive composition according to the present invention can achieve rapid curing and build strength. In this article, the rapid curing characteristics of the adhesive composition according to the present invention can be characterized by measuring the clamping strength of the adhesive film formed by the adhesive composition after curing for 5 minutes at 70°C, and the specific test method is described in detail in the Examples section below. Suitably, the clamping strength of the adhesive composition according to the present invention after curing for 5 minutes at 70°C is greater than 0.2 MPa.

[0071] The adhesive composition according to the present invention can have a suitably long open time. In this article, the term "open time" refers to the time from the adhesive composition being applied to the first substrate to the adhesive composition where the second substrate is joined to the first substrate. Suitably, the open time of the adhesive composition according to the present invention at room temperature can be at least 15 minutes. In this article, the room temperature refers to 15-30°C, such as 23°C.

[0072] The present invention further relates to a coated substrate, comprising a substrate and the above-mentioned two-component adhesive composition applied to at least part of the substrate. Suitably, the substrate may include aluminum alloy, tinplate, anodized aluminum, stainless steel, ASA plastic, ABS plastic, and / or PET plastic. Suitably, the substrate may include a coated substrate, such as a substrate coated with an epoxy coating.

[0073] The method of applying the adhesive composition to a substrate may include: applying the adhesive composition to a first substrate, and then contacting the adhesive composition on the first substrate with a second substrate. The "first substrate" and the "second substrate" may be the same material or different materials, such as aluminum alloy, tinplate, anodized aluminum, stainless steel, ASA plastic, ABS plastic, and / or PET plastic.

[0074] The coated substrate can be cured by exposure to curing conditions for a certain period of time. Suitably, the adhesive composition according to the present invention can be cured within 10 days to 2 hours at 10-100°C. For example, the adhesive composition according to the present invention can be cured within 7 days at 25°C. For example, the adhesive composition according to the present invention can be cured within 1 day at 60°C. For example, the adhesive composition according to the present invention can be cured within 4 hours at 80°C. After curing, the thickness of the adhesive layer formed by the adhesive composition according to the present invention can be 0.1-5 mm, such as 0.1-2 mm.

[0075] Example

[0076] The following examples are provided to further illustrate the present invention but should not be construed as limiting the invention to the details described in the examples. Unless otherwise indicated, all parts and percentages in the following examples are by weight.

[0077] Example 1-2 (Ex 1-2): Adhesive composition according to the present invention

[0078] The adhesive composition according to the present invention is prepared according to the ingredients and amounts listed in Table 1 below, specifically comprising:

[0079] Component A: Add modified polyol, polyether polyol and chain extender to the reaction kettle, stir at room temperature for 1 hour to mix the liquid materials evenly; add dehumidifier, fumed silica, hydrophobically modified aluminum hydroxide and diethyl aluminum hypophosphite to the above components, stir at 80°C in vacuum for 2 hours to remove moisture and mix evenly; wait for the reaction kettle to return to room temperature, add delayed curing catalyst and thermosensitive catalyst, stir under vacuum for 1 hour to mix evenly, and obtain component A; and

[0080] Component B: add isocyanate prepolymer, dehydrating agent, fumed silica, hydrophobically modified aluminum hydroxide and diethyl aluminum hypophosphite into a reactor, stir for 2 hours under vacuum at 80°C to remove moisture and mix evenly; wait for the reactor to return to room temperature, add silane coupling agent, stir for 1 hour under vacuum to mix evenly, and obtain component B.

[0081] Table 1.

[0082]

[0083] 1 1,4-Butanediol;

[0084] 2 Mercaptotin catalyst;

[0085] 3 Amine catalyst and optional catalyst co-agent;

[0086] 4 Molecular sieve activated powder;

[0087] 5 γ-Glycidyloxypropyltrimethoxysilane; and

[0088] 6 p-Toluenesulfonyl isocyanate.

[0089] Comparative Example 1-8 (CE 1-8): Containing no delayed curing catalyst and / or heat-sensitive catalyst

[0090] The adhesive composition of the comparative example was prepared according to the components and amounts listed in Table 2 below, specifically comprising:

[0091] Component A: add modified polyol, polyether polyol and chain extender to a reaction kettle, stir at room temperature for 1 hour to mix the liquid materials evenly; add dehydrating agent, fumed silica, hydrophobically modified aluminum hydroxide and diethyl aluminum hypophosphite to the above components, stir at 80°C in vacuum for 2 hours to remove moisture and mix evenly; wait for the reaction kettle to return to room temperature, add delayed curing catalyst or thermosensitive catalyst, stir at vacuum for 1 hour to mix evenly, and obtain component A; and

[0092] Component B: add isocyanate prepolymer, dehydrating agent, fumed silica, hydrophobically modified aluminum hydroxide and diethyl aluminum hypophosphite into a reactor, stir for 2 hours under vacuum at 80°C to remove moisture and mix evenly; wait for the reactor to return to room temperature, add silane coupling agent, stir for 1 hour under vacuum to mix evenly, and obtain component B.

[0093] Table 2.

[0094]

[0095] 1 1,4-Butanediol;

[0096] 2 Mercaptotin catalyst;

[0097] 3 Amine catalyst and optional catalyst co-agent;

[0098] 4 Molecular sieve activated powder;

[0099] 5 γ-Glycidyloxypropyltrimethoxysilane; and

[0100] 6 p-Toluenesulfonyl isocyanate.

[0101] Comparative Example 9-11 (CE 9-11): Replacement of Hydrophobically Modified Aluminum Hydroxide

[0102] The adhesive composition of the comparative example was prepared according to the components and amounts listed in Table 3 below, specifically comprising:

[0103] Component A: add modified polyol, polyether polyol and chain extender to a reaction kettle, stir at room temperature for 1 hour to mix the liquid materials evenly; add dehumidifier, fumed silica, silica / calcium carbonate / aluminum hydroxide and diethyl aluminum hypophosphite to the above components, stir at 80°C in vacuum for 2 hours to remove moisture and mix evenly; wait for the reaction kettle to return to room temperature, add delayed curing catalyst and thermosensitive catalyst, stir at vacuum for 1 hour to mix evenly, and obtain component A; and

[0104] Component B: add isocyanate prepolymer, dehydrating agent, fumed silica, silica / calcium carbonate / aluminum hydroxide and diethylaluminum hypophosphite into a reactor, stir for 2 hours under vacuum and 80°C to remove moisture and mix evenly; wait for the reactor to return to room temperature, add silane coupling agent, stir for 1 hour under vacuum to mix evenly, and obtain component B.

[0105] Table 3.

[0106]

[0107] 1 1,4-Butanediol;

[0108] 2 Mercaptotin catalyst;

[0109] 3 Amine catalyst and optional catalyst co-agent;

[0110] 4 Molecular sieve activated powder;

[0111] 5 γ-Glycidyloxypropyltrimethoxysilane; and

[0112] 6 p-Toluenesulfonyl isocyanate.

[0113] Comparative Example 12-15 (CE 12-15): Variation of diethylaluminum hypophosphite

[0114] The adhesive composition of the comparative example was prepared according to the components and amounts listed in Table 4 below, specifically comprising:

[0115] Component A: adding modified polyol, polyether polyol and chain extender to a reaction kettle, stirring at room temperature for 1 hour to mix the liquid materials evenly; adding dehydrating agent, fumed silica, hydrophobically modified aluminum hydroxide and optional diethyl aluminum hypophosphite to the above components, stirring at 80° C. in vacuum for 2 hours to remove moisture and mix evenly; waiting for the reaction kettle to return to room temperature, adding delayed curing catalyst and thermosensitive catalyst, stirring at vacuum for 1 hour to mix evenly, to obtain component A; and

[0116] Component B: add isocyanate prepolymer, dehydrating agent, fumed silica, hydrophobically modified aluminum hydroxide and optional diethyl aluminum hypophosphite into a reactor, stir for 2 hours under vacuum and 80°C to remove moisture and mix evenly; wait for the reactor to return to room temperature, add silane coupling agent, stir for 1 hour under vacuum to mix evenly, and obtain component B.

[0117] Table 4.

[0118]

[0119] 1 1,4-Butanediol;

[0120] 2 Mercaptotin catalyst;

[0121] 3 Amine catalyst and optional catalyst co-agent;

[0122] 4 Molecular sieve activated powder;

[0123] 5 γ-Glycidyloxypropyltrimethoxysilane; and

[0124] 6 p-Toluenesulfonyl isocyanate.

[0125] Performance Testing

[0126] 1-Stability

[0127] The adhesive compositions of Examples 1-2 and Comparative Examples 1-15 obtained above were placed in a sealed environment at 25° C., and then the stability was determined by whether the viscosity of component A and component B changed significantly. The viscosity was measured by a Brookfield viscometer.

[0128] 2- Opening hours

[0129] The open time of the adhesive is determined by the wire drawing method. Specifically, the components A and B of the adhesive are mixed, and then placed in an environment of 25°C and 50% RH. The surface of the adhesive strip is lightly touched. The time when the adhesive strip no longer draws is the open time.

[0130] For the adhesive composition examples 1-2 and comparative examples 1-15 obtained as above, component A and component B were mixed respectively, and then the adhesive mixture was applied to the first 3003AL surface, and then the second 3003AL surface was pressed on the adhesive area and the thickness was controlled. The prepared samples were cured under appropriate conditions, and the cured adhesive films were tested as follows.

[0131] 3-Clamping strength

[0132] The thickness between the first and second 3003AL surfaces was controlled to be 0.2 mm, and the film was cured at 70° C. for 5 minutes. The shear strength of the film was tested according to GB / T7124-2008.

[0133] 4- Adhesion

[0134] In this context, the substrate adhesion of an adhesive composition is characterized by its failure mode.

[0135] The thickness between the first and second 3003AL surfaces was controlled to be 0.2 mm, and the film was cured at 25°C for 7 days. The shear strength of the film was tested according to GB / T7124-2008, and the failure form after the test was determined.

[0136] Observe the failure type of the adhesive layer bonding part with the naked eye: CF represents cohesive failure, which means that there are adhesive layers remaining on both sides of the bonding part; AF represents interfacial failure, which means that at least one side of the bonding part has exposed substrate.

[0137] The test results are summarized in Table 5-6 below.

[0138] Table 5.

[0139] Ex 1 Ex 2 CE 1 CE 2 CE 3 CE 4 CE 5 CE 6 CE 7 stability > 6 months > 6 months > 6 months > 6 months > 6 months > 6 months > 6 months > 6 months > 6 months Opening hours 28 minutes 15 minutes 50 minutes 50 minutes 37 minutes 18 minutes <5 minutes 50 minutes 39 minutes Clamping strength 0.22 MPa 0.34 MPa No strength No strength No strength No strength 0.28 MPa 0.08 MPa 0.14 MPa Destruction form CF CF CF CF CF CF CF CF CF

[0140] Table 6.

[0141] CE 8 CE 9 CE 10 CE 11 CE 12 CE 13 CE 14 CE 15 stability > 6 months > 6 months > 6 months 2 months > 6 months > 6 months > 6 months > 6 months Opening hours 27 minutes 25 minutes 7 minutes 11 minutes 15 minutes 15 minutes 15 minutes 15 minutes Clamping strength 0.33 MPa No strength 0.19 MPa 0.26 MPa 0.33 MPa 0.3 MPa 0.29 MPa 0.31 MPa Destruction form CF 10% CF* 10% CF* 80% CF* 80% CF* 50% CF* 50% CF* 80% CF*

[0142] *The percentage represents the damage form between CF and AF, for example, 10%CF represents 10%CF and 90%AF.

[0143] As can be seen from the above table, under the combined action of a specific delayed curing catalyst and a heat-sensitive catalyst, the adhesive composition according to the present invention can achieve a suitably long open time and quickly build strength while satisfying stability. In addition, a specific filler combination enables the adhesive composition according to the present invention to achieve improved adhesion requirements.

[0144] While particular aspects of the invention have been illustrated and described, it will be apparent to those skilled in the art that various other changes and modifications may be made without departing from the spirit and scope of the invention. It is therefore intended that the appended claims cover all such changes and modifications as fall within the scope of the invention.

Claims

1. A two-component adhesive composition, comprising component A and component B, wherein component A comprises a first catalyst, a second catalyst and a first filler composition, and component B comprises a second filler composition, wherein the first catalyst is a delayed curing catalyst, the second catalyst is a thermosensitive catalyst, and each of the first and second filler compositions comprises hydrophobically modified aluminum hydroxide.

2. The two-component adhesive composition of claim 1, wherein the delayed curing catalyst comprises a tin mercapto catalyst.

3. The two-component adhesive composition according to claim 2, wherein the mercaptotin catalyst comprises: Dibutyltin bisthiol, dibutyltin dimercaptoacetate, bis(dodecylthio)dimethyltin, dimethyltin mercaptan, dioctyltin dithioacetate, dimethyltin dithioacetate, or any combination thereof.

4. The two-component adhesive composition according to any one of claims 1 to 3, wherein the heat-sensitive catalyst comprises an amine catalyst.

5. The two-component adhesive composition according to claim 4, wherein the amine catalyst comprises: 1,8-diazabicyclo[5.4.0]undec-7-ene, 1-dimethylaminoethyl-4-methylpiperazine, bismorpholinyl diethyl ether, or any combination thereof.

6. The two-component adhesive composition according to any one of claims 4 to 5, wherein the heat-sensitive catalyst further comprises a catalyst aid, wherein the catalyst aid comprises: Formic acid, isooctanoic acid, phenol, or any combination thereof.

7. The two-component adhesive composition according to any one of claims 1 to 6, wherein the hydrophobically modified aluminum hydroxide comprises silane-modified aluminum hydroxide.

8. The two-component adhesive composition according to claim 7, wherein the silane-modified aluminum hydroxide comprises: Aminosilane-modified aluminum hydroxide, vinylsilane-modified aluminum hydroxide, epoxysilane-modified aluminum hydroxide, mercaptosilane-modified aluminum hydroxide, alkylsilane-modified aluminum hydroxide, titanatesilane-modified aluminum hydroxide, aluminatesilane-modified aluminum hydroxide, or any combination thereof.

9. The adhesive composition according to any one of claims 1 to 8, wherein the A component comprises 0.005-0.1 wt% of the delayed curing catalyst based on the total weight of the A component.

10. The two-component adhesive composition according to any one of claims 1 to 9, wherein the A component comprises 0.05 to 1 wt% of the heat-sensitive catalyst based on the total weight of the A component.

11. The two-component adhesive composition according to any one of claims 1 to 10, wherein the A component comprises 0.01-0.03 wt% of the delayed curing catalyst and 0.3-0.4 wt% of the heat-sensitive catalyst based on the total weight of the A component.

12. The two-component adhesive composition according to any one of claims 1 to 11, wherein the first and / or second filler composition further comprises diethyl aluminum hypophosphite.

13. The two-component adhesive composition according to any one of claims 1 to 12, wherein the first and / or second filler composition further comprises fumed silica.

14. The two-component adhesive composition of any one of claims 1 to 13, wherein the first filler composition comprises 50 wt% or more of the hydrophobically modified aluminum hydroxide based on the total weight of the first filler composition.

15. The two-component adhesive composition of any one of claims 1 to 14, wherein the second filler composition comprises 40 wt% or more of the hydrophobically modified aluminum hydroxide based on the total weight of the second filler composition.

16. The two-component adhesive composition according to any one of claims 12 to 15, wherein the A component comprises 15 to 25 wt% of diethyl aluminum hypophosphite based on the total weight of the A component.

17. The two-component adhesive composition according to any one of claims 12 to 16, wherein the B component comprises 15 to 25 wt% of diethyl aluminum hypophosphite based on the total weight of the B component.

18. The two-component adhesive composition according to any one of claims 1 to 17, wherein the component A further comprises a dehydrating agent, wherein the dehydrating agent comprises: Molecular sieve activated powder, 1,3-oxazapentane, triethyl orthoformate, or any combination thereof.

19. The two-component adhesive composition according to any one of claims 1 to 18, wherein the component B further comprises a dehydrating agent, wherein the dehydrating agent comprises: 1,3-Oxazopentane, p-toluenesulfonyl isocyanate, triethyl orthoformate, or any combination thereof.

20. The two-component adhesive composition according to any one of claims 1 to 19, wherein the component B further comprises a silane coupling agent, and the silane coupling agent comprises: γ-glycidyloxypropyltrimethoxysilane, isocyanatepropyltrimethoxysilane, 3-(2,3-epoxypropyloxy)propyltrimethoxysilane, or any combination thereof.

21. The two-component adhesive composition according to any one of claims 1 to 20, wherein the component A further comprises a polyol, and the component B further comprises an isocyanate prepolymer.

22. The two-component adhesive composition according to any one of claims 1 to 21, wherein the viscosity of each of the A component and the B component is 50,000 to 70,000 cps at room temperature.

23. A coated substrate comprising a substrate and the two-component adhesive composition according to any one of claims 1 to 22 coated on at least a portion of the substrate.

24. The coated substrate of claim 23, wherein the substrate comprises aluminum alloy, tinplate, anodized aluminum, stainless steel, ASA plastic, ABS plastic, and / or PET plastic.

25. The coated substrate of claim 23 or 24, wherein the substrate comprises an epoxy coating applied thereon.