Material testing-oriented low-foam-rate epoxy resin curing sample preparation method
By using the combination of heating, centrifugation, vacuuming and bubble picking steps in the curing and sample preparation process of epoxy resin adhesive, the problem of bubble-influencing the experimental results is solved, and bubble-free sample molding and more accurate material parameter testing are achieved. .
Patent Information
- Application Number
- CN202410846995.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-11-26
AI Technical Summary
Bubbles often occur in existing epoxy resin adhesive curing sample preparation methods, which affects the accuracy of the experimental results of the sample and affects the accuracy of material parameter testing.
Using a combination of heating, centrifugation, vacuuming and bubble picking steps, including heating epoxy resin adhesive in an oven to improve fluidity, removing air bubbles from the colloid using a centrifuge and vacuum machine, and cooling naturally at high temperatures to complete curing Make samples.
Through this method, the surface and inside of the epoxy resin cured the sample without bubbles, which improves the accuracy of material experiments, ensures the molding quality of the sample and the reliability of the experimental results.
Smart Images

Figure CN119023385A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material testing pre-treatment, and in particular relates to an epoxy resin adhesive curing sample preparation method. Background Art
[0002] Epoxy resin adhesives have a wide range of applications from cutting-edge technology to home use due to their excellent bonding properties and various outstanding physical and chemical properties. They are currently widely used in various fields such as machinery, civil engineering, aerospace, shipbuilding, and automotive industries. Compared with other adhesives, epoxy resin adhesives have many advantages, such as excellent mechanical properties, thermal stability, chemical resistance, corrosion resistance, good processability, and high adhesion. In addition, it has a wide operating temperature, low shrinkage, and can be used in combination with a variety of modifiers, so it is widely used in various fields such as fiber-reinforced materials, general-purpose adhesives, and high-performance coatings.
[0003] The material parameters of epoxy resin adhesives are important factors affecting their application conditions, so it is very important to study the material properties of epoxy resin adhesives. To study the material parameters of epoxy resin adhesives, it is necessary to cure the epoxy resin adhesives and prepare samples. The existing sample preparation method will produce bubbles in the sample during the curing and sample preparation process of the epoxy resin adhesive. The bubbles produced will have a huge impact on the experimental results of the sample, seriously affecting the accuracy of the epoxy resin adhesive material parameter test. Summary of the invention
[0004] The present application provides a method for preparing samples by curing an epoxy resin adhesive to improve the accuracy of material testing.
[0005] The embodiment of the present application provides a method for preparing a sample by curing an epoxy resin adhesive, and the method for preparing a sample by curing an epoxy resin adhesive comprises the following steps:
[0006] Step 1: performing a heating step, heating the epoxy resin adhesive in an oven;
[0007] Step 2: performing a centrifugation step, pouring the heated epoxy resin adhesive into a centrifuge tube, balancing the centrifuge tube and placing it in a centrifuge, and centrifuging the epoxy resin adhesive using the centrifuge;
[0008] Step 3: Perform a vacuuming step, pour the centrifuged epoxy resin adhesive into a bowl-shaped plastic container, place it in a vacuum machine for vacuuming, and then pour the epoxy resin adhesive into the mold. After the pouring is completed, place the poured mold into the vacuum machine for further vacuuming;
[0009] Step 4: performing a bubble picking step, placing the vacuumed epoxy resin adhesive into an oven, taking it out after heating, and using a toothpick to pick out the bubbles floating on the surface;
[0010] Step 5: high temperature curing step, placing the epoxy resin adhesive after bubble picking into an oven for heating and then naturally cooling to complete the epoxy resin adhesive curing sample preparation.
[0011] In one embodiment of the present application, the heating step requires heating to a temperature lower than the curing reaction temperature to increase the fluidity of the epoxy resin adhesive, since the epoxy resin adhesive has a high viscosity at room temperature, so as to facilitate subsequent processing;
[0012] The temperature below the curing reaction temperature is set to 80°C because the curing temperature of the epoxy resin adhesive is 100°C. By heating the epoxy resin adhesive to this temperature in an oven, the fluidity of the epoxy resin adhesive can be greatly improved.
[0013] In one embodiment of the present application, the centrifugation step is performed by centrifuging the epoxy resin adhesive to remove the air in the dissolved colloid from the colloid because the air is dissolved in the colloid. The centrifugation step is performed using a centrifuge for 10 minutes.
[0014] The centrifuge needs to fill the adhesive into the centrifuge tube, perform a balancing step, and then put the tube into the centrifuge for centrifugation. The balancing step is performed by an electronic scale.
[0015] In one embodiment of the present application, the vacuuming step is required to remove bubbles in the colloid because the centrifugation step cannot completely eliminate the air dissolved in the epoxy resin adhesive, and the vacuuming step is completed using a vacuum machine;
[0016] The vacuum machine performs the vacuuming step by removing the air in the vacuum machine. During the use of the vacuum machine, the epoxy resin adhesive after the centrifugal step needs to be poured into a bowl-shaped plastic container, and the plastic container is placed in the vacuum machine for vacuuming. The vacuuming is repeated for 30 seconds or more for more than 5 times until the resin adhesive in the plastic container reaches a boiling state with bubbles constantly gushing out and bursting. The vacuuming is stopped and the adhesive in the bowl-shaped plastic container is poured into the mold. After the pouring is completed, the container is put into the vacuum machine for vacuuming. The vacuuming is repeated for 10 seconds or more for more than 3 times until the resin adhesive in the mold reaches a boiling state with bubbles constantly gushing out and bursting. The vacuuming step is terminated.
[0017] The bowl-shaped plastic container has a capacity of 500 ml. When pouring the epoxy resin adhesive, it is necessary to ensure that the poured adhesive is less than 100 ml to avoid overflow during vacuuming;
[0018] The mold can be made of different shapes and materials according to the sample requirements. In this embodiment, a mold made of silicone material is selected because this material is easy to demould.
[0019] In one embodiment of the present application, the bubble picking step requires that the mold filled with the epoxy resin adhesive be placed in an oven, heated to 90°C for 0.5h, then taken out wearing heat-insulating gloves, and the bubbles floating on the surface of the adhesive be picked with a toothpick. The bubbles mostly float at the edges, and stirring is performed when bubbles are inconvenient to pick.
[0020] In one embodiment of the present application, the high-temperature curing step requires placing the mold filled with the epoxy resin adhesive after the bubble picking is completed into an oven, heating it to 100°C for 0.5h, keeping it at 100°C for 3h, and then naturally cooling it for 3h to complete the epoxy resin adhesive curing and sample preparation.
[0021] By applying the epoxy resin adhesive curing sample preparation method involved in the technical solution provided in this embodiment, the epoxy resin cured samples produced have good molding quality and are free of bubbles inside and on the surface of the samples. Compared with samples with bubbles on the surface produced by other curing sample preparation methods, the samples produced by the epoxy resin adhesive curing sample preparation method provided by this technical solution can obtain more accurate experimental results in material experiments, which is conducive to improving the accuracy of research on epoxy resin material properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The accompanying drawings are incorporated into and constitute a part of this specification.
[0023] Figure 1 A schematic flow chart of the epoxy resin adhesive curing sample preparation method provided in this embodiment. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0025] See also Figure 1 , Figure 1 A schematic flow chart of a method for preparing a sample by curing an epoxy resin adhesive provided in this embodiment is provided. The method is applied to preparing a sample by curing an epoxy resin adhesive in a material pre-experiment treatment.
[0026] The equipment used in the epoxy resin adhesive curing sample preparation method includes: oven, centrifuge, electronic scale, and vacuum machine.
[0027] The following describes in detail Figure 1 The epoxy resin adhesive curing sample preparation method shown in the figure specifically comprises the following steps:
[0028] Step 1, placing the epoxy resin adhesive in a bowl-shaped plastic container, placing the container in an oven and heating it to a temperature lower than the curing reaction temperature of the epoxy resin adhesive. Since the curing temperature of the epoxy resin adhesive is 100° C., the temperature lower than the curing reaction temperature is set to 80° C., and the epoxy resin adhesive is heated to this temperature by the oven.
[0029] In this embodiment, the container used is a bowl-shaped plastic container, which can be replaced by a container of other materials and shapes that do not react with the adhesive according to actual conditions. The use of the plastic bowl-shaped container here is mainly due to cost considerations. The use of the bowl-shaped plastic container is low in cost and easy to use.
[0030] In this embodiment, the epoxy resin adhesive is heated to a temperature lower than the curing reaction temperature using an oven, which can greatly improve the fluidity of the epoxy resin adhesive, and is beneficial to improving the bubble elimination efficiency during the subsequent centrifugation step and vacuum step.
[0031] Step 2, after the heating step in step 1 is completed, a centrifugation step is performed. First, step 201 is performed to pour the epoxy resin adhesive after heating into the centrifuge tube. The volume of the adhesive in the single centrifuge tube after pouring cannot exceed two-thirds of the volume of the centrifuge tube. This treatment is conducive to improving the bubble elimination efficiency of the centrifugation step.
[0032] Step 202, an electronic scale is used to balance the centrifuge tube filled with the epoxy resin adhesive. In this embodiment, the accuracy of the electronic scale used is 0.01 grams, and the electronic scale is used to weigh the centrifuge tube filled with the epoxy resin adhesive.
[0033] In this embodiment, water is used for balancing and water is poured into an empty centrifuge tube. Since the density of the epoxy resin adhesive is 1.05 g / ml and the density of water is 1.00 g / ml, the volume of the water poured is first controlled to be close to the epoxy resin adhesive poured, and then a rubber-tipped dropper is used to specifically control the volume of the water poured. The electronic scale is used to repeatedly weigh the centrifuge tube poured with water until the weight difference between the centrifuge tube poured with water and the centrifuge tube poured with epoxy resin adhesive is less than 0.1 gram.
[0034] Step 203, put all the centrifuge tubes filled with water and the centrifuge tubes filled with epoxy resin adhesive after balancing into a centrifuge. In this embodiment, the centrifuge can accommodate six centrifuge tubes. After placement, there are three groups of centrifuge tubes filled with water and three groups of centrifuge tubes filled with epoxy resin adhesive in the centrifuge. Turn on the centrifuge to centrifuge the epoxy resin adhesive for 10 minutes.
[0035] Step 3, perform a vacuuming step, first perform step 301, take out all six centrifuge tubes from the centrifuge, pour the epoxy resin adhesive in the centrifuge tubes into the bowl-shaped plastic container, place the bowl-shaped plastic container in a vacuum machine, and repeatedly perform vacuuming for 30 seconds for more than 5 times until the resin adhesive in the bowl-shaped plastic container reaches a boiling state with bubbles constantly gushing out and bursting, and then stop vacuuming.
[0036] In this embodiment, the volume of the bowl-shaped plastic container is 500 ml. To ensure the expected vacuum effect of eliminating bubbles, the volume of the epoxy resin adhesive poured into the bowl-shaped plastic container shall not exceed one fifth of the volume of the bowl-shaped plastic container. In practical applications, containers of different volumes can be used to hold the epoxy resin adhesive, but the volume of the epoxy resin adhesive poured into the container shall not exceed one fifth of the volume of the container used.
[0037] In this embodiment, due to the volume of the bowl-shaped plastic container, the bubble elimination effect can be achieved by vacuuming for 30 seconds. In other embodiments, the vacuuming time of the vacuum machine should be controlled according to the bubble bursting situation, so that the bubbles of the epoxy resin adhesive will not overflow the container when they burst.
[0038] Step 302, pour the epoxy resin adhesive in the bowl-shaped plastic container into the mold, put the mold into the vacuum machine, and repeatedly perform vacuuming for 10 seconds for more than 3 times until the resin adhesive in the mold reaches a boiling state with bubbles constantly gushing out and bursting, and then end the vacuuming.
[0039] In this embodiment, the mold is a silicone mold. In other embodiments, the mold can also be made of other materials for easy demolding. The silicone mold is selected here because the silicone mold has good sample molding quality and is easy to demold.
[0040] In this embodiment, the mold is a standard stretching sample mold. In other embodiments, molds for making different samples can be selected according to the requirements of the material experiments. During the vacuuming process, the vacuuming time of the vacuum machine should be controlled according to the bubble bursting situation to ensure that the epoxy resin adhesive does not overflow the mold and bubble bursting occurs.
[0041] Step 4, put the mold filled with the epoxy resin adhesive into an oven, set it to heat to 90°C for 0.5h, then take it out wearing heat-insulating gloves, and use a toothpick to prick the bubbles floating on the surface of the adhesive until no bubbles floating on the surface of the epoxy resin adhesive can be seen.
[0042] In this embodiment, the bubbles in the mold mostly float at the edge, and sometimes it is difficult to burst the bubbles. In this case, a toothpick needs to be used to stir the bubbles to eliminate them.
[0043] Step 5: Place the mold filled with the epoxy resin adhesive after the bubble selection is completed in an oven, heat it to a set temperature of 100°C for 0.5h, keep it at 100°C for 3h, and then cool it naturally for 3h. Figure 1 The epoxy resin adhesive curing sample preparation process shown.
[0044] In this embodiment, after the sample preparation is completed according to the epoxy resin adhesive curing sample preparation process, it can be seen from human eye observation that the surface molding quality of the epoxy resin adhesive cured sample is good and there are no bubbles.
[0045] The epoxy resin adhesive curing sample preparation method of the present invention is further illustrated below by listing specific examples as comparative examples.
[0046] Comparative Example 1
[0047] A method for preparing a sample by curing an epoxy resin adhesive. Compared with the specific embodiment, the heating step is not performed, and the other steps are the same as those of the specific embodiment.
[0048] Comparative Example 2
[0049] A method for preparing samples by curing an epoxy resin adhesive. Compared with the specific embodiment, the centrifugation step is not performed, and the other steps are the same as those of the specific embodiment.
[0050] Comparative Example 3
[0051] A method for preparing a sample by curing an epoxy resin adhesive. Compared with the specific embodiment, the vacuuming step is not performed, and the other steps are the same as those of the specific embodiment.
[0052] Comparative Example 4
[0053] A method for preparing a sample by curing an epoxy resin adhesive. Compared with the specific embodiment, the bubble picking step is not performed, and the other steps are the same as those of the specific embodiment.
[0054] Compared with the specific embodiment, in the comparative example 1, the heating step was not performed during the curing sample preparation process. After the centrifugation step, the number of fine bubbles on the adhesive surface was significantly less than that on the adhesive surface after the centrifugation step in the specific embodiment. During the vacuuming step, the adhesive did not reach a boiling state where the bubbles kept gushing out and bursting. Obvious bubbles and pits appeared on the surface of the sample obtained after the curing sample preparation was completed.
[0055] Compared with the specific embodiment, in the comparative example 2, since the centrifugation step was not performed during the curing sample preparation process, the time taken for the adhesive to reach the boiling state with bubbles constantly gushing out and bursting during the vacuuming step was significantly longer than the time taken for the specific embodiment to reach the boiling state with bubbles constantly gushing out and bursting during the vacuuming step. Obvious fine bubbles and small pits were generated on the surface of the sample obtained after the curing sample preparation was completed.
[0056] Compared with the specific embodiment, in the comparative example 3, during the curing sample preparation process, since the vacuum extraction step is not performed, a large number of obvious bubbles emerge on the surface of the adhesive during the bubble picking step, and a large number of bubbles and pits are generated on the surface of the sample obtained after the curing sample preparation is completed.
[0057] Compared with the specific embodiment, in the comparative example 4, since the bubble picking step is not performed during the curing sample preparation process, bubbles and pits are generated on the surface of the sample obtained after the curing sample preparation is completed.
[0058] In order to detect the specific performance of the specific embodiments and the comparative examples in the material experiment, the tensile strength test is carried out on the samples obtained by curing the specific embodiments and the comparative examples, which specifically includes the following steps: five samples are selected from the samples obtained by curing the specific embodiments and the comparative examples and marked, and the tensile strength is tested by a tensile test according to the GB / T1040.2-2006 standard for the determination of tensile properties of plastics. The ambient temperature during the test is 20°C, and the tensile strength is taken as the average value of the test results of the five samples. The specific results are shown in Table 1.
[0059] Table 1 Tensile strength test results
[0060] Group Tensile strength / MPa Specific embodiments 19.10829 Comparative Example 1 12.99265 Comparative Example 2 15.43266 Comparative Example 3 7.08262 Comparative Example 4 16.58326
[0061] It can be seen from the data in Table 1 that the tensile strength of the sample is significantly greater than . In the adhesive material experiment, the number of bubbles generated on the surface of the sample will significantly affect the tensile strength. The more bubbles there are, the smaller the tensile strength value obtained by the tensile test of the sample. The epoxy resin adhesive curing sample preparation method proposed in this article can effectively improve the accuracy of the epoxy resin adhesive material parameter test.
[0062] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a sample by curing an epoxy resin adhesive, comprising the following steps: Step 1: performing a heating step, heating the epoxy resin adhesive in an oven; Step 2: performing a centrifugation step, pouring the heated epoxy resin adhesive into a centrifuge tube, balancing the centrifuge tube and placing it in a centrifuge, and centrifuging the epoxy resin adhesive using the centrifuge; Step 3: Perform a vacuuming step, pour the centrifuged epoxy resin adhesive into a bowl-shaped plastic container, place it in a vacuum machine for vacuuming, and then pour the epoxy resin adhesive into the mold. After the pouring is completed, place the poured mold into the vacuum machine for further vacuuming; Step 4: performing a bubble picking step, placing the vacuumed epoxy resin adhesive into an oven, taking it out after heating, and using a toothpick to pick out the bubbles floating on the surface; Step 5: high temperature curing step, placing the epoxy resin adhesive after bubble picking into an oven for heating and then naturally cooling to complete the epoxy resin adhesive curing sample preparation.
2. The epoxy resin adhesive according to claim 1, characterized in that: The improved one-component epoxy adhesive based on 7-2312 one-component epoxy adhesive comprises epoxy resin, curing agent and toughening agent.
3. The epoxy resin adhesive curing sample preparation method according to claim 1, characterized in that: In step 1, the heating step, since the epoxy resin adhesive has high viscosity at room temperature, it is necessary to heat it to a temperature lower than the curing reaction temperature to increase the fluidity of the epoxy resin adhesive for subsequent processing; The temperature below the curing reaction temperature is set to 80°C because the curing temperature of the epoxy resin adhesive is 100°C. By heating the epoxy resin adhesive to this temperature in an oven, the fluidity of the epoxy resin adhesive can be greatly improved.
4. The epoxy resin adhesive curing sample preparation method according to claim 1, characterized in that: In step 2, the centrifugation step, since the epoxy resin adhesive has air dissolved in the colloid, it is necessary to separate the air in the dissolved colloid from the colloid by centrifugation. The centrifugation step is completed using a centrifuge, and the centrifugation time is 10 minutes; The centrifuge needs to fill the adhesive into the centrifuge tube, perform a balancing step, and then put the tube into the centrifuge for centrifugation. The balancing step is performed by an electronic scale.
5. The epoxy resin adhesive curing sample preparation method according to claim 1 and the phenomenon of air dissolving in colloid according to claim 4, characterized in that: In step 3, the vacuuming step is performed to remove bubbles in the colloid because the centrifugation step cannot completely eliminate the air dissolved in the epoxy resin adhesive. The vacuuming step is performed using a vacuum machine. The vacuum machine performs the vacuuming step by removing the air in the vacuum machine. During the use of the vacuum machine, the epoxy resin adhesive after the centrifugal step is first poured into a bowl-shaped plastic container, and the plastic container is placed in the vacuum machine for vacuuming. The vacuuming is repeated for more than 5 times for 30 seconds until the resin adhesive in the plastic container reaches a boiling state with bubbles constantly gushing out and bursting. The vacuuming is stopped and the adhesive in the bowl-shaped plastic container is poured into the mold. After the pouring is completed, the container is put into the vacuum machine for vacuuming. The vacuuming is repeated for more than 3 times for 10 seconds until the resin adhesive in the mold reaches a boiling state with bubbles constantly gushing out and bursting. The vacuuming step is terminated. The bowl-shaped plastic container has a capacity of 500 ml. When pouring the epoxy resin adhesive, it is necessary to ensure that the poured adhesive is less than 100 ml to avoid overflow during vacuuming; The mold can be made of different shapes and materials according to the sample requirements. In this embodiment, a mold made of silicone material is selected because this material is easy to demould.
6. The epoxy resin adhesive curing sample preparation method according to claim 1, characterized in that: In step 4, the bubble picking step requires that the mold filled with the epoxy resin adhesive be placed in an oven, heated to 90°C for 0.5h, then taken out wearing heat-insulating gloves, and the bubbles floating on the surface of the adhesive are picked with a toothpick. The bubbles mostly float at the edge, and stirring is performed when bubbles are inconvenient to pick.
7. The epoxy resin adhesive curing sample preparation method according to claim 1, characterized in that: In step 5, the high-temperature curing step requires placing the mold filled with the epoxy resin adhesive after bubble picking into an oven, heating it to 100°C for 0.5h, keeping it at 100°C for 3h, and then naturally cooling it for 3h to complete the epoxy resin adhesive curing and sample preparation.
Citation Information
Cited By
Coaxial structure glue pouring and hole forming process for high-frequency signal transmission test
CN120232768A
Adhesive curing sample preparation method suitable for aerospace evaluation
CN121655962A