Production method of ultralow-manganese ultralow-phosphorus steel
Through the converter + LF duplex smelting technology, combined with low alkaline slag production, slag pouring and high oxygen potential processes, the problem of manganese and phosphorus content control in converter operation is solved, and the production of ultra-low manganese and ultra-low phosphorus steel is achieved, which has improved the Steel properties.
Patent Information
- Application Number
- CN202411006093.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-22
AI Technical Summary
There is no clear research literature in the prior art on the method of producing ultra-low manganese and ultra-low phosphorus steel by converter-LF refining furnaces, and it is impossible to effectively control the content of manganese and phosphorus in the steel, especially in converter operations.
The converter + LF duplex smelting technology is adopted. The converter has low alkalinity slag and pours slag in the early stage. The end point is low-temperature and high alkalinity and high oxygen potential to produce steel. The slag material is added during the converter steel discharge process, and the bottom of the ladle is opened when adding the material. Blow argon to stir, add slag material after the steel water enters the LF refining furnace, and controls the finished manganese ≤0.02% and phosphorus ≤0.003%.
Through this method, the effective reduction of the content of manganese and phosphorus in the steel is achieved, ensuring that the finished manganese is ≤0.02% and the phosphorus is ≤0.003%, and the performance of the steel is improved, especially in electrical steel and rare earth permanent magnet materials.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy and relates to a production method of ultra-low manganese and ultra-low phosphorus steel. Background Art
[0002] Phosphorus is a harmful element in steel. It can increase the strength of steel in small amounts, but greatly reduce the plasticity and toughness of steel and increase the sensitivity of weld cracks. At the same time, phosphorus is easy to segregate, thereby aggravating the banded structure of steel and having a great impact on the performance of steel. Therefore, in the smelting process of most steels, it is hoped that the phosphorus content will be controlled as low as possible. Manganese has long been added to steel as a beneficial alloying element, but in some of the latest developed steels, manganese is no longer a beneficial alloying element, but it is hoped that the manganese content in steel is as low as possible, for example, electrical steel, industrial pure iron, etc. Electrical steel (also known as silicon steel) is mainly used for various motors and transformer cores, ballasts in fluorescent lamps, magnetic switches, etc. If the manganese content in the molten steel is too high, it will cause incomplete solid solution of manganese sulfide, resulting in reduced magnetic properties of the finished steel; for industrial pure iron products used for rare earth permanent magnet materials, manganese salt inclusions will also reduce the "remanent magnetism" of the magnetic material and affect the magnetic properties.
[0003] The Chinese patent with publication number CN108929933A discloses a method for smelting low-manganese and low-phosphorus steel, which uses an electric furnace + refining smelting method, uses an electric furnace for secondary slag making, and uses a refining slag packing method to control the manganese and phosphorus content of scrap steel and pig iron with a manganese content of no more than 0.5% and a phosphorus content of no more than 0.04% to less than 0.05% and 0.004% respectively in the finished product. However, the environment of the electric furnace and the converter is quite different, and the process of the electric furnace cannot be applied to the converter operation.
[0004] The Chinese patent with publication number CN114807507A discloses a method for producing ultra-low manganese steel, which adopts BOF+LF composite smelting technology, uses the early slag pouring process in the converter to remove manganese, and further removes manganese by using the final large slag volume and high oxygen potential process and LF refining oxidizing slag demanganization process, and develops a finished steel grade with Mn≤0.025%. However, the invention only describes the key technical requirements for demanganization under the same process conditions, and does not take into account the dephosphorization function.
[0005] There is no clear research literature on the method of producing ultra-low manganese and ultra-low phosphorus steel by converter-LF refining furnace. Summary of the invention
[0006] In order to overcome the deficiencies of the prior art, the present invention provides a method for producing ultra-low manganese and ultra-low phosphorus steel, which can control the finished manganese content in molten steel to below 0.02% and the phosphorus content to below 0.003%.
[0007] In order to achieve the above-mentioned object of the invention, the technical solution of the present invention is: A method for producing ultra-low manganese and ultra-low phosphorus steel comprises the following steps: (1) Early stage of slag discharge and slag pouring in converter: target C content in molten steel 3.5wt%, target basicity 1.5-1.7, target temperature 1320-1370℃, target slag pouring volume 50%; (2) Converter end stage: The converter end oxygen level is 550-750 ppm, the end basicity is 4.0-5.0, and the end temperature is controlled at 1610-1630°C. When 1 / 4 of the steel is tapped, slag-making agent is added, but no deoxidizer is added. When adding material, argon blowing from the bottom of the ladle is turned on for stirring. (3) LF refining stage: After the molten steel enters the station, slag-forming agent is added, but no deoxidizing alloy material is added.
[0008] Furthermore, the composition of the molten iron raw material used is calculated by mass percentage as follows: C: 4.1-4.8%, Mn: 0.10-0.17%, Si: 0.20-0.50%, P: 0.080-0.110%, S: 0.001-0.003%, and the rest is Fe and unavoidable impurities.
[0009] Furthermore, a slide plate is used to block slag during the converter tapping process, and 2.8-3.2 kg / t of lime and 0.4-0.6 kg / t of fluorite as slag-forming agents are added when 1 / 4 of the steel is tapped. When adding materials, argon blowing from the bottom of the ladle is turned on for stirring.
[0010] Furthermore, after the molten steel enters the LF refining stage, 3-3.5 kg / t of refining slag and 1.5-2 kg / t of lime are added, the argon flow rate is controlled at 400-600 NL / min, the temperature is controlled at 1570-1610°C during the treatment, and the treatment cycle is 35-43 min.
[0011] Furthermore, the composition of the molten steel before LF refining is calculated by mass percentage as follows: C: 0.025-0.04%, Mn≤0.026%, S≤0.003%, P≤0.004%, Si≤0.01%, Als≤0.01%, and the rest is Fe and unavoidable impurities.
[0012] Furthermore, the composition of the molten steel after LF refining treatment is calculated by mass percentage as follows: C: 0.03-0.05%, Mn≤0.02%, S≤0.005%, P≤0.003%, Si≤0.01%, Als≤0.01%, and the rest is Fe and unavoidable impurities.
[0013] Furthermore, the main components of the high-oxidizing slag after LF refining and slagging are calculated in percentage by mass: FeO: 25-32%, CaO: 40-55%, MgO: 1.5-7%, SiO2: 3-8%, and Al2O3: 10-20%.
[0014] The beneficial effects of the technical solution are as follows: the present invention reduces the content of Mn and P in steel through the converter + LF dual-process smelting technology, adopts low-basicity slag making and slag dumping in the early stage of the converter, and taps steel at the end with low temperature, high basicity and high oxygen potential, adds slag making material but no deoxidizer during the converter tapping process, opens argon blowing at the bottom of the ladle for stirring when adding materials, and adds slag making material after the molten steel enters the LF refining furnace. The present invention achieves the control requirements of Mn≤0.02% and P≤0.003% in the finished steel. DETAILED DESCRIPTION
[0015] Embodiment 1: The production method of ultra-low manganese and ultra-low phosphorus steel in this embodiment comprises the following steps: (1) Composition of molten iron raw materials: by mass percentage, C: 4.42%, Mn: 0.11%, Si: 0.29%, P: 0.090%, S: 0.002%, and the rest is Fe and unavoidable impurities; (2) In the early stage of converter slag discharge and slag pouring: the C content of semi-steel is 3.51%, the actual basicity is 1.56, the actual temperature is 1340℃, and the slag pouring amount is 6.7t; (3) Final stage of converter: Final oxygen level 554ppm, final basicity 4.4, final temperature 1617℃, slide plate used to block slag during steel tapping, slag-forming agent lime 3.02kg / t and fluorite 0.4kg / t were added at 1 / 4 of the steel tapping process, no deoxidizer was added, and argon blowing from the bottom of the ladle was turned on for stirring during charging; (4) Composition of molten steel before LF refining: by mass percentage: C: 0.033%, Mn: 0.023%, Si: 0.0016%, P: 0.0038%, S: 0.0021%, Als: 0.0011%, and the rest is Fe and unavoidable impurities; (5) After the LF refining station is entered, 3.0 kg / t of refining slag and 1.53 kg / t of lime are added, the argon flow rate is controlled at 400-600 NL / min, the LF cycle is 38 min, and the temperature is controlled at 1585-1603 °C during the treatment; (6) Composition of molten steel after LF refining: by mass percentage: C: 0.038%, Mn: 0.018%, Si: 0.0019%, P: 0.0022%, S: 0.0025%, Als: 0.0014%, and the rest is Fe and unavoidable impurities; (7) The main components of the highly oxidizing slag after LF refining are as follows in terms of mass percentage: FeO: 28.4%, CaO: 49.01%, MgO: 1.76%, SiO2: 4.92%, and Al2O3: 13.98%.
[0016] Embodiment 2: The method for producing ultra-low manganese and ultra-low phosphorus steel in this embodiment comprises the following steps: (1) Composition of molten iron raw materials: by mass percentage, C: 4.31%, Mn: 0.12%, Si: 0.36%, P: 0.099%, S: 0.003%, and the rest is Fe and unavoidable impurities; (2) In the early stage of converter slag discharge and slag pouring: the C content of semi-steel is 3.38%, the actual basicity is 1.65, the actual temperature is 1321℃, and the slag pouring volume is 5.7t; (3) Final stage of converter: Final oxygen level 585ppm, final basicity 4.31, final temperature 1620℃, slide plate used to block slag during steel tapping, slag-forming agent lime 3.1kg / t and fluorite 0.43kg / t were added at 1 / 4 of the steel tapping process, no deoxidizer was added, and argon blowing from the bottom of the ladle was turned on for stirring during charging; (4) Composition of molten steel before LF refining: by mass percentage: C: 0.032%, Mn: 0.024%, Si: 0.0009%, P: 0.0037%, S: 0.002%, Als: 0.0010%, and the rest is Fe and unavoidable impurities; (5) After the LF refining station, 3.14 kg / t of refining slag and 1.52 kg / t of lime were added, the argon flow rate was controlled at 400-600 NL / min, the LF cycle was 41 min, and the temperature was controlled at 1588-1608 °C during the treatment; (6) Composition of molten steel after LF refining: by mass percentage: C: 0.04%, Mn: 0.017%, Si: 0.0012%, P: 0.0024%, S: 0.0024%, Als: 0.0017%, and the rest is Fe and unavoidable impurities; (7) The main components of the highly oxidizing slag after LF refining are as follows in terms of mass percentage: FeO: 31.03%, CaO: 47.07%, MgO: 1.51%, SiO2: 3.56%, and A12O3: 14.79%.
[0017] Embodiment 3: The production method of ultra-low manganese and ultra-low phosphorus steel in this embodiment comprises the following steps: (1) Composition of molten iron raw materials: by mass percentage, C: 4.53%, Mn: 0.14%, Si: 0.31%, P: 0.104%, S: 0.002%, and the rest is Fe and unavoidable impurities; (2) In the early stage of converter slag discharge and slag pouring: the C content of semi-steel is 3.41%, the actual basicity is 1.69, the actual temperature is 1347℃, and the slag pouring volume is 5.9t; (3) Final stage of converter: Final oxygen level 625ppm, final basicity 4.43, final temperature 1630℃, slide plate used to block slag during steel tapping, slag-forming agent lime 3.07kg / t and fluorite 0.4kg / t were added at 1 / 4 of the steel tapping process, no deoxidizer was added, and argon blowing from the bottom of the ladle was turned on for stirring during charging; (4) Composition of molten steel before LF refining: by mass percentage: C: 0.034%, Mn: 0.026%, Si: 0.001%, P: 0.0042%, S: 0.0021%, Als: 0.0021%, and the rest is Fe and unavoidable impurities; (5) After the LF refining station is entered, 3.17 kg / t of refined slag and 1.55 kg / t of lime are added, the argon flow rate is controlled at 400-600 NL / min, the LF cycle is 39 min, and the temperature is controlled at 1590-1609 °C during the treatment; (6) Composition of molten steel after LF refining: by mass percentage: C: 0.038%, Mn: 0.019%, Si: 0.0013%, P: 0.0028%, S: 0.0028%, Als: 0.0029%, and the rest is Fe and unavoidable impurities; (7) The main components of the highly oxidizing slag after LF refining are as follows in terms of mass percentage: FeO: 28.2%, CaO: 47.23%, MgO: 3.39%, SiO2: 3.77%, and A12O3: 15.10%.
[0018] Embodiment 4: The production method of ultra-low manganese and ultra-low phosphorus steel in this embodiment comprises the following steps: (1) Composition of molten iron raw materials: by mass percentage, C: 4.11%, Mn: 0.17%, Si: 0.32%, P: 0.109%, S: 0.001%, and the rest is Fe and unavoidable impurities; (2) In the early stage of converter slag discharge and slag pouring: the C content of semi-steel is 3.52%, the actual basicity is 1.6, the actual temperature is 1359℃, and the slag pouring amount is 6.1t; (3) Final stage of converter: Final oxygen level 745ppm, final basicity 4.8, final temperature 1622℃, slide plate used to block slag during steel tapping, slag-forming agent lime 3.08kg / t and fluorite 0.51kg / t were added at 1 / 4 of the steel tapping process, no deoxidizer was added, and argon blowing from the bottom of the ladle was turned on for stirring during charging; (4) Composition of molten steel before LF refining: by mass percentage: C: 0.029%, Mn: 0.021%, Si: 0.001%, P: 0.0025%, S: 0.0019%, Als: 0.0015%, and the rest is Fe and unavoidable impurities; (5) After the LF refining station is entered, 3.42 kg / t of refined slag and 1.65 kg / t of lime are added, the argon flow rate is controlled at 400-600 NL / min, the LF cycle is 38 min, and the temperature is controlled at 1582-1605 °C during the treatment; (6) Composition of molten steel after LF refining: by mass percentage: C: 0.034%, Mn: 0.015%, Si: 0.0014%, P: 0.0019%, S: 0.0025%, Als: 0.0020%, and the rest is Fe and unavoidable impurities; (7) The components of the highly oxidizing slag after LF refining are as follows by mass percentage: FeO: 29.6%, CaO: 45.3%, MgO: 3.21%, SiO2: 3.22%, Al2O3: 16.44%.
[0019] Embodiment 5: The production method of ultra-low manganese and ultra-low phosphorus steel in this embodiment comprises the following steps: (1) Composition of molten iron raw materials: by mass percentage, C: 4.49%, Mn: 0.14%, Si: 0.31%, P: 0.110%, S: 0.001%, and the rest is Fe and unavoidable impurities; (2) In the early stage of converter slag discharge and slag pouring: the C content of semi-steel is 3.61%, the actual basicity is 1.52, the actual temperature is 1361℃, and the slag pouring volume is 5.9t; (3) Final stage of converter: Final oxygen level 555ppm, final basicity 4.7, final temperature 1621℃, slide plate used to block slag during steel tapping, slag-forming agent lime 2.83kg / t and fluorite 0.42kg / t were added at 1 / 4 of the steel tapping process, no deoxidizer was added, and argon blowing from the bottom of the ladle was turned on for stirring during charging; (4) Composition of molten steel before LF refining: by mass percentage: C: 0.033%, Mn: 0.026%, Si: 0.0013%, P: 0.0037%, S: 0.0022%, Als: 0.0025%, and the rest is Fe and unavoidable impurities; (5) After the LF refining station, 3.04 kg / t of refining slag and 1.53 kg / t of lime were added, the argon flow rate was controlled at 400-600 NL / min, the LF cycle was 41 min, and the temperature was controlled at 1575-1604 °C during the treatment; (6) Composition of molten steel after LF refining: by mass percentage: C: 0.037%, Mn: 0.020%, Si: 0.0013%, P: 0.0029%, S: 0.0027%, Als: 0.0031%, and the rest is Fe and unavoidable impurities; (7) The components of the highly oxidizing slag after LF refining and slagging are as follows by mass percentage: FeO: 26.8%, CaO: 44.35%, MgO: 3.98%, SiO2: 4.33%, Al2O3: 15.51%.
[0020] Embodiment 6: The production method of ultra-low manganese and ultra-low phosphorus steel in this embodiment comprises the following steps: (1) Composition of molten iron raw materials: by mass percentage, C: 4.79%, Mn: 0.14%, Si: 0.21%, P: 0.104%, S: 0.0012%, and the rest is Fe and unavoidable impurities; (2) In the early stage of converter slag discharge and slag pouring: the C content of semi-steel is 3.66%, the actual basicity is 1.51, the actual temperature is 1365℃, and the slag pouring volume is 6.3t; (3) Final stage of converter: Final oxygen level 575ppm, final basicity 4.3, final temperature 1614℃, slide plate used to block slag during steel tapping, slag-forming agent lime 3.08kg / t and fluorite 0.42kg / t were added at 1 / 4 of the steel tapping process, no deoxidizer was added, and argon blowing from the bottom of the ladle was turned on for stirring during charging; (4) Composition of molten steel before LF refining: by mass percentage: C: 0.027%, Mn: 0.024%, Si: 0.0023%, P: 0.0038%, S: 0.0024%, Als: 0.0015%, and the rest is Fe and unavoidable impurities; (5) After the LF refining station is entered, 3.2 kg / t of refining slag and 1.62 kg / t of lime are added, the argon flow rate is controlled at 400-600 NL / min, the LF cycle is 39 min, and the temperature is controlled at 1581-1607 °C during the treatment; (6) Composition of molten steel after LF refining: by mass percentage: C: 0.033%, Mn: 0.017%, Si: 0.0027%, P: 0.0026%, S: 0.0034%, Als: 0.0025%, and the rest is Fe and unavoidable impurities; (7) The components of the highly oxidizing slag after LF refining and slagging are as follows by mass percentage: FeO: 30.25%, CaO: 45.32%, MgO: 3.66%, SiO2: 4.68%, Al2O3: 13.93%.
Claims
1. A method for producing ultra-low manganese and ultra-low phosphorus steel, characterized in that: It includes the following steps: (1) Early stage of slag discharge and slag pouring in converter: target C content in molten steel 3.5wt%, target basicity 1.5-1.7, target temperature 1320-1370℃, target slag pouring volume 50%; (2) Converter end stage: The converter end oxygen level is 550-750 ppm, the end basicity is 4.0-5.0, and the end temperature is controlled at 1610-1630°C. When 1 / 4 of the steel is tapped, slag-making agent is added, but no deoxidizer is added. When adding material, argon blowing from the bottom of the ladle is turned on for stirring. (3) LF refining stage: After the molten steel enters the station, slag-forming agent is added, but no deoxidizing alloy material is added.
2. The method for producing ultra-low manganese and ultra-low phosphorus steel according to claim 1, characterized in that: The components of the molten iron raw material used are calculated by mass percentage as follows: C: 4.1-4.8%, Mn: 0.10-0.17%, Si: 0.20-0.50%, P: 0.080-0.110%, S: 0.001-0.003%, and the rest are Fe and unavoidable impurities.
3. The method for producing ultra-low manganese and ultra-low phosphorus steel according to claim 2, characterized in that: During the steel-tapping process of the converter, a slide plate is used to block the slag. When 1 / 4 of the steel is tapped, 2.8-3.2 kg / t of lime and 0.4-0.6 kg / t of fluorite are added as slag-forming agents. When adding materials, argon blowing from the bottom of the ladle is turned on for stirring.
4. The method for producing ultra-low manganese and ultra-low phosphorus steel according to claim 3, characterized in that: After the molten steel enters the LF refining stage, 3-3.5kg / t of refining slag and 1.5-2kg / t of lime are added, the argon flow rate is controlled at 400-600NL / min, the temperature is controlled at 1570-1610℃ during the treatment, and the treatment cycle is 35-43min.
5. The method for producing ultra-low manganese and ultra-low phosphorus steel according to claim 4, characterized in that: The composition of molten steel before LF refining is calculated in percentage by mass: C: 0.025-0.04%, Mn≤0.026%, S≤0.003%, P≤0.004%, Si≤0.01%, Als≤0.01%, and the rest are Fe and unavoidable impurities.
6. The method for producing ultra-low manganese and ultra-low phosphorus steel according to claim 5, characterized in that: The composition of molten steel after LF refining treatment is calculated in mass percentage as follows: C: 0.03~0.05%, Mn≤0.02%, S≤0.005%, P≤0.003%, Si≤0.01%, Als≤0.01%, and the rest are Fe and unavoidable impurities.
7. The method for producing ultra-low manganese and ultra-low phosphorus steel according to any one of claims 1 to 6, characterized in that: The main components of the highly oxidizing slag after LF refining and slagging are as follows in terms of mass percentage: FeO: 25-32%, CaO: 40-55%, MgO: 1.5-7%, SiO2: 3-8%, Al2O3: 10-20%.