Method and system for mining rare earth ore by changing direct-current electric field
Through the intelligent power control system, the electrode position and potential gradient are monitored and adjusted in real time, the problem of difficult control of electrode position and potential gradient in the weathered shell-type rare earth mine is solved, the rare earth mining efficiency and leaching rate are improved, and the power consumption cost is reduced .
Patent Information
- Application Number
- CN202411083988.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-08
AI Technical Summary
In the existing methods of power-on mining weathered shell-type rare earth ore, the electrode position and potential gradient are difficult to control, resulting in low mining efficiency, high power consumption, and uneven distribution of rare earths, which can easily lead to rare earth precipitation and hinder continuous migration.
Adopt intelligent power control system to monitor the pH value and current near the electrode in real time, adjust the electrode position and potential gradient according to the parameter standard database, realize intelligent transformation of electrode position, ensure that the current is within the range of 10-60A, and avoid the pH value exceeding the precipitation threshold. Dynamically adjust the power-on parameters.
The mining cycle is shortened, the power consumption is reduced, the effective mobility of rare earths is improved, the electrolysis near the electrode is reduced, soil pollution is prevented, and the rare earth leaching rate is improved.
Smart Images

Figure CN118997758A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of weathering crust type rare earth mining, and in particular to a method and system for mining rare earth ores by using a converted direct current electric field. Background Art
[0002] Weathering crust rare earth ore has a complete distribution of rare earth elements and is rich in medium and heavy rare earth elements. It is the main source of heavy rare earth elements and provides more than 90% of medium and heavy rare earths for the world. However, the existing ammonium salt in-situ leaching process seriously pollutes surface water, groundwater and farmland, and may also face sudden events such as landslides. There are problems such as "slow leaching", "leakage" and "many blind spots" in the leaching process. The ammonium salt in-situ leaching process seriously restricts the exploitation and utilization of weathering crust rare earth resources in my country.
[0003] CN109402417A proposes to adopt electrical mining, which mainly includes inserting an anode injection pipe and a cathode collection pipe into the rare earth mine body, and the insertion position of the cathode collection pipe is lower than the insertion position of the anode injection pipe; passing direct current between the anode injection pipe and the cathode collection pipe; so as to improve the rare earth extraction rate and shorten the mining time.
[0004] However, the actual mines are large in scale, and multiple groups of electrodes need to be powered on at the same time. There are big problems with the electrode arrangement and power-on scheme. The position of the positive and negative electrodes, the potential gradient and the duration of power-on are difficult to control, which seriously restricts the mining efficiency. During the power-on mining of weathering crust-type rare earths, the physical parameters of the weathering crust, such as conductivity, porosity and permeability, will change, and the position of the positive and negative electrodes needs to be changed in time. It is not only difficult to change the position of the positive and negative electrodes in time manually, but also difficult to redetermine the position of the positive and negative electrodes and the duration of power-on. Not only is the rare earth distribution of the weathering crust-type rare earth ore itself uneven, but the mining process will also cause uneven distribution of rare earths, and different voltages need to be applied. During the power-on mining process, the size of the applied potential gradient and the time to change the potential gradient are difficult to determine.
[0005] The application number is 202311194756.X, and the invention name is a method and system for mining rare earth ores using direct current, which proposes a scheme of rotating power supply. At least 3 rows and at least 1 column of injection holes are arranged in the mining area; electrodes are arranged in the injection holes, and each row of electrodes is connected in parallel to the power supply control system; leaching agents are added to the injection holes; the mining area is divided into M equal parts (M is a positive integer), and the electrodes are energized by a periodic rotating power supply method from 1 to M. Compared with energizing all mining areas at the same time, this method reduces the power demand of the mining process and reduces the construction cost of transformers.
[0006] However, during the power-on process, the electrolysis near the electrode continues to increase, which not only increases the electricity consumption cost, but also causes the ions in the mining area to continuously migrate, causing the conductivity of the mining area to change. After the conductivity changes, the power-on parameters need to be changed to continuously and efficiently mine rare earths. Otherwise, the effective mobility of rare earths will be reduced and the mining cycle will be extended.
[0007] On the other hand, as the power continues to be supplied, the hydrolysis near the electrode will continue to increase, and the pH near the cathode will continue to rise. When the pH value reaches the rare earth precipitation threshold, it will cause rare earth precipitation and hinder the continuous migration of rare earths. Summary of the invention
[0008] The purpose of the present invention is to solve the defects of the above-mentioned prior art and provide a method and system for mining rare earth ores by using a converted DC electric field, which aims to improve the problem that the power supply scheme is difficult to determine in the existing power supply mining method for rare earth ores.
[0009] The present invention adopts the following technical solution:
[0010] A system for mining rare earth ores using a converted direct current electric field, comprising: arranging at least 3 rows and at least 1 column of injection holes in a mining area, arranging electrodes in the injection holes, arranging a pH meter and an intelligent power supply control system near the electrodes in the mining area, wherein the intelligent power supply control system is equipped with a current and voltage detector, a conductivity detector, an integrated mother power supply, a module controller, and a parameter standard database; (the function of the integrated mother power supply is to provide voltage to the module, and the function of the module controller is to adjust the positive and negative poles).
[0011] Each row of electrodes is connected in parallel to the intelligent power control system. The intelligent power control system gives the distance between the anode electrode and the cathode electrode and the potential gradient of the initial power supply according to the resistivity of the mine and the parameter standard database data, and then makes corresponding adjustments according to the uploaded pH value or current changes and the current size;
[0012] Specifically, the pH meter uploads the measured information to the intelligent power control system in real time, and the intelligent power control system controller calls the information in the parameter standard database to obtain the pH value near the electrode, and compares the pH value near the electrode with the precipitation threshold value to control the positive and negative electrodes to move forward;
[0013] pH value near the electrode Once the precipitation threshold is exceeded Then stop the power first and move the positive and negative electrodes forward.
[0014] When the intelligent power control system detects that the current magnitude remains unchanged when the current and voltage detectors upload to the parameter standard database or when the current between the electrodes is not within 10-60A, the intelligent power control system will advance the positive and negative electrodes through the module controller or change the potential gradient through the integrated mother power supply.
[0015] Note: The forward movement of positive and negative electrodes means that after multiple rows and columns of electrodes are arranged in the mining area, each row of electrodes is connected in parallel to the intelligent power supply control system. For example, the 13th row of electrodes is positively charged and becomes the anode, and the 15th row is negatively charged and becomes the cathode. The 13th and 15th rows are a power-on loop. When the pH value near the electrode is compared with the precipitation threshold and the electrode position needs to be adjusted, the 13th and 15th rows of electrodes lose power at the same time, and the 14th row of electrodes is positively charged and becomes the positive electrode, and the 16th row of electrodes is negatively charged and becomes the cathode. In this way, relative to the original 13th and 15th rows, the energized electrodes move in the direction of the column.
[0016] Since multiple rows and columns of electrodes are arranged in the mining area, there is a situation where the 1st, 4th, 6th, 7th, 9th and 11th rows are energized at the same time. When it is necessary to move forward, the original 9th row with positive power may become negatively powered, and the original 11th row with negative power may become positively powered. Therefore, in this process, the same electrode will change from being used as the positive pole of the power supply to being used as the negative pole of the power supply, or from being used as the negative pole of the power supply to being used as the positive pole of the power supply.
[0017] The detection point of the current and voltage detector is in the current loop and is installed in the integrated mother power supply.
[0018] The current and voltage detector is used to detect the potential gradient and current of the mine in real time, and upload the data to the parameter standard database. The conductivity detector is used to check whether the current and voltage detector is abnormal.
[0019] In some examples, the original data recorded in the parameter standard database of the intelligent power control system of the weathering crust rare earth mining area: the initial current threshold between the electrodes is 10-60A, the precipitation threshold The data that need to be converted or calculated in the parameter standard database include: pH value near the electrode (1cm-100cm) and current between electrodes.
[0020] In some instances, the spacing between the positive and negative electrodes and the potential gradient of the originally arranged electrodes are determined by the integrated circuit mother power supply and parameter standard database: before formal mining, the intelligent power supply control system will automatically check the resistivity of the mine RΩ·m, the spacing between the positive and negative electrodes ≥1 / R m (and greater than a unit electrode spacing, a unit electrode spacing is the distance between the electrodes in each column. Depending on the on-site conditions, the spacing between the electrodes in each column is different. Therefore, based on the on-site conditions, the unit electrode spacing is optional), and the potential gradient is 10R V / m.
[0021] On the other hand, a method for mining rare earth ores by using a converted direct current electric field is also provided, comprising: arranging at least 3 rows and at least 1 column of injection holes in the mining area, and arranging electrodes in the injection holes, each row of electrodes being connected in parallel to an intelligent power supply control system, the intelligent power supply control system will determine the original power supply parameters (positive and negative electrode positions and potential gradient) of the weathering crust type rare earth ore mining area by automatic inspection, and then call the parameter matching in the parameter standard database according to the collected pH changes and / or current size and current changes, so as to adjust the electrode positions and power supply voltages;
[0022] When the pH value near the electrode is greater than the precipitation threshold, the power is stopped first, and the positive and negative electrodes move forward;
[0023] When the current tends to be stable or the current size is not between 10-60A, the positive and negative electrodes move forward or change the potential gradient.
[0024] Furthermore, the intelligent power supply control system will determine the power supply parameters of the weathering crust rare earth mining area through automatic inspection:
[0025] Determine the resistivity of the weathering crust rare earth mining area, then call the parameter standard database to match the appropriate power supply method (positive and negative electrode positions and potential gradient).
[0026] Before formal mining, the intelligent power supply control system will automatically check the resistivity of the mine.
[0027] Specifically: if the resistivity of the weathering crust type rare earth ore is RΩ·m, the distance between the positive and negative electrodes is ≥1 / Rm (and greater than a unit electrode distance), and the potential gradient is ≥10R V / m.
[0028] At the same time, the distance between the positive and negative electrodes and the potential gradient are affected by the current between the electrodes, and the current between the electrodes should be between 10-60A.
[0029] The duration of power supply to the positive and negative electrodes is affected by the pH value near the electrodes. The pH value near the electrodes affects the occurrence state of rare earths. The pH value at which hydrated rare earth ions begin to precipitate is obtained by the mass average precipitation value of 15 kinds of rare earth ions. pH value near the electrode Once the precipitation threshold is exceeded Then stop the power supply first, and then power on again after the positive and negative electrodes are pushed forward.
[0030] At the same time, the intelligent power control system will monitor the conductivity changes in the mining area in real time, and adjust the power supply parameters of the electrode as the pH and conductivity change.
[0031] In one embodiment, the data recorded in the parameter standard database includes: pH, current and voltage.
[0032] In one embodiment, the number of rows of electrodes is determined according to the area of the mining region, and the spacing between each row of electrodes is 0.5-5 meters.
[0033] Optionally, the spacing between each row of electrodes is 1 meter.
[0034] In one embodiment, the number of rows of electrodes is determined according to the area of the mining region, and the spacing between each row of electrodes is 0.5-5 meters.
[0035] Optionally, the spacing between each column of electrodes is 1 meter.
[0036] In one embodiment, the depth of the injection hole is determined according to the thickness of the weathering crust.
[0037] Optionally, the depth of the injection hole is 5-30 meters.
[0038] In one embodiment, a voltage is applied between the positive and negative electrodes so that the potential gradient in the ore body is 10-100 V / m.
[0039] Beneficial effects of the present invention:
[0040] Compared with the continuous power supply of fixed positive and negative electrodes, the DC electric field power supply method of the present invention shortens the mining cycle, reduces power consumption, and improves the effective mobility of rare earth. In the process of intelligently transforming the DC electric field power supply, the power supply method (positive and negative electrode positions and potential gradient) can be changed in time according to the change of conductivity of the weathered crust type rare earth ore, and the positive and negative electrode intelligent transformation phenomenon occurs.
[0041] The intelligent transformation of positive and negative electrodes in the present invention can, on the one hand, formulate an appropriate power-on method (positive and negative electrode positions and potential gradient) in real time according to the changes in pH and conductivity, and rare earth ions can migrate quickly. On the other hand, it weakens the electrolysis near the electrodes to prevent soil pollution. At the same time, in the process of changing the power-on of the positive and negative electrodes, the rare earth ions in the leaching agent and the soil in the non-powered area can be fully exchanged, thereby improving the rare earth leaching rate. Through the online monitoring of the monitor and the automatic control of the control system, the key parameters such as the power-on voltage are automatically adjusted, and automatic mining of the mine is realized. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is a schematic diagram of the intelligent conversion DC electric field power-on adopted in Example 1;
[0043] Figure 2 A comparison chart of rare earth extraction rates between Example 1 and Comparative Example 1;
[0044] Figure 3 This is a comparison chart of power consumption between Example 1 and Comparative Example 1;
[0045] Figure 4 This is a schematic diagram of the intelligent conversion DC electric field power-on adopted in Example 2;
[0046] Figure 5 A comparison chart of rare earth extraction rates between Example 2 and Comparative Example 2;
[0047] Figure 6 This is a comparison chart of power consumption between Example 2 and Comparative Example 2;
[0048] Figure 7 It is a working schematic diagram of the intelligent power supply control system of the present invention.
[0049] Note: Because each electrode will be fixed in the soil, the distance between electrodes is fixed. A unit electrode spacing is the smallest distance between two electrodes. The distance between electrodes can only be an integer multiple of the unit electrode spacing. DETAILED DESCRIPTION
[0050] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0051] like Figure 7 As shown, a method for mining rare earth ores by using a converted DC electric field of the present invention comprises: arranging at least 3 rows and at least 1 column of injection holes in the mining area, and arranging electrodes in the injection holes, each row of electrodes being connected in parallel to an intelligent power supply control system, and the intelligent power supply control system will determine the power-on parameters (positive and negative electrode positions and potential gradient) of the weathering crust type rare earth ore mining area by automatic inspection, and then call the parameter matching in the parameter standard database according to the collected pH changes and / or current size and current changes, so as to adjust the electrode positions and power-on voltages;
[0052] When the pH value near the electrode is greater than the precipitation threshold, the power is stopped first, and the positive and negative electrodes move forward;
[0053] When the current tends to be stable or the current size is not between 10-60A, the positive and negative electrodes move forward or change the potential gradient.
[0054] As an example, when the resistivity of weathered crust-type rare earth ore is 1.5Ω·m, the intelligent power supply control system gives the power-on method based on the parameter standard database, with the positive and negative pole spacing being 1.8m and the potential gradient being 50V / m; when the resistivity changes to 0.5Ω·m during the power-on process, the potential gradient in the mining area will promptly change to 20V / m.
[0055] For example, when the pH near the electrodes during the power-on process is greater than the rare earth precipitation threshold, the positive and negative electrodes move forward, and the positive and negative poles in the mining area move forward; when the current in the power-on process stabilizes to 20A, the positive and negative poles in the mining area will move forward.
[0056] At least 3 rows of electrodes are arranged in the mining area, for example, the electrodes can be 3 rows, 4 rows, 5 rows, 10 rows, 20 rows, 100 rows, etc. The number of rows of electrodes is determined according to the area of the mining area, and the spacing between each row of electrodes is 0.5-3 meters, for example, it can be 0.5 meters, 1 meter, 2 meters or 3 meters.
[0057] At least one row of electrodes is arranged in the mining area. For example, the number of electrodes can be 1 row, 2 rows, 3 rows, 20 rows, 50 rows, 100 rows, etc. The number of rows of electrodes is determined according to the area of the mining area. The spacing between each row of electrodes is 1.8-5 meters (i.e., 1 unit pole distance), for example, it can be 1.8 meters, 2.5 meters or 5 meters.
[0058] The method of the present invention does not limit the positive and negative poles of each electrode. When the intelligent power control system realizes the intelligent switching of the positive and negative poles, the same electrode will change from being used as the positive pole of the power supply to being used as the negative pole of the power supply. Or from being used as the negative pole of the power supply to being used as the positive pole of the power supply. This reduces the number of sub-power supplies required for the intelligent power control system. For example, in the original power-on process, 10 rows of electrodes require 9 independent power supplies to realize the power-on control of 12, 23, 34, ... 910 rows. However, in this intelligent power control system, since the positive and negative poles can be switched, only 5 module controllers are needed to provide 10 rows of wiring.
[0059] At the same time, the intelligent power supply control system can timely change the position of the positive and negative electrodes according to the actual mining needs. For example, the distance between the positive and negative electrodes can be 1.8 meters, 2 meters, 3 meters, 3.2 meters, 4 meters or 10 meters.
[0060] In the actual mining process, due to the large scale of the mine, multiple groups of electrodes need to be powered on at the same time. In the traditional electrified mining process, the electrodes are powered on for a long time, which will enhance the electrolysis on the electrode surface, not only increasing power consumption, but also hindering the electrification of rare earth mining. On the other hand, with the continuous electrification process, the conductivity of the weathering crust type rare earth mining area will change. It is difficult to formulate reasonable electrification parameters in time according to the changes in pH and conductivity, which reduces the effective mining rate of rare earths and increases the mining cycle. In addition, weathering crust rare earth ores belong to a complex system with uneven conductivity in various parts. It is difficult for traditional power supplies to output appropriate electrification parameters in time according to changes in pH and conductivity. Mining rare earths with fixed electrification parameters will increase power consumption costs.
[0061] The position of the positive and negative electrodes directly affects the effective mobility of rare earth ions. The rare earth content of weathering crust-type rare earth ores is uneven, and the mineral composition and structure are specifically layered, resulting in great differences in the conductivity of different parts of weathering crust-type rare earth ores. The potential gradient applied between the electrodes will affect the electrolytic strength and rare earth migration rate on the electrode surface. As the rare earth migrates out of the weathering crust-type rare earth mining area, the migration rate of the rare earth will decrease, and a higher voltage will be required to drive the rare earth migration. The length of time the positive and negative electrodes are energized will affect the precipitation of rare earth ions on the electrode surface. The continuous energization process will cause the pH near the electrodes to increase, thereby causing the precipitation of rare earth ions, and the position of the positive and negative electrodes needs to be changed. The intelligent conversion DC electric field can change the position of the positive and negative electrodes, the applied potential gradient, and the length of time the positive and negative electrodes are energized according to the pH and current size of the weathering crust-type rare earth ore.
[0062] Compared with the continuous power supply of fixed positive and negative electrodes, the intelligent power control system can change the power supply parameters (positive and negative electrode positions and potential gradient) in real time by changing the DC electric field power supply method, simplifying the complex requirements of electrode arrangement (need to find the anode electrode position and cathode electrode position according to actual survey, but now no such design is required) and the length of wires and cables (the original electrodes were fixed with the anode distributed on the top of the mountain and the cathode distributed on the hillside, but now all of them are distributed on the top of the mountain, and the length of wires and cables can be reduced), improving the mining efficiency of the power supply process, shortening the mining cycle, reducing the power consumption required for mining, and improving the effective mobility of rare earth ions in weathered crust-type rare earth ores. At the same time, in the process of changing the positive and negative electrodes, the rare earth ions in the leaching agent and soil in the non-powered area can be fully exchanged, thereby improving the rare earth leaching rate.
[0063] Furthermore, the data recorded in the parameter standard database of the intelligent power supply control system of the weathering crust type rare earth mining area are: the current between the electrodes is 10-60A threshold, the precipitation threshold
[0064]
[0065] The distance between the positive and negative electrodes and the potential gradient of the original electrode are determined by the intelligent power controller and the parameter adjustment database; the pH value near the electrode Once the precipitation threshold is exceeded Then stop the power first and move the positive and negative electrodes forward.
[0066] In this energizing method, the energizing method (positive and negative electrode positions and potential gradient) can be changed in time according to the change of conductivity of weathering crust type rare earth ore, and the phenomenon of intelligent transformation of positive and negative electrodes occurs. On the one hand, an appropriate energizing method can be formulated in real time according to the change of pH and conductivity, and rare earth ions can migrate quickly. On the other hand, the electrolysis near the electrode is weakened to prevent soil pollution. It is worth noting that the intelligent transformation of positive and negative electrodes in the energizing method of the present invention is not the electrode exchange between two sets of fixed electrodes in the traditional sense, but the intelligent transformation of positive and negative electrodes is carried out according to the change of pH value and conductivity during the mining process.
[0067] The intelligent conversion of positive and negative electrodes in the energizing method of the present invention can improve the effective migration rate of rare earths. The migration direction of rare earth ions is always consistent between any electrodes, and there will be no reversal of current direction and reverse migration of rare earth ions.
[0068] At the same time, compared with the continuous power supply of fixed positive and negative poles, not only the mining cycle is shortened, but also the rare earth mining efficiency is improved. In the embodiment of the intelligent conversion DC field power supply method, 3 / 4 of the power consumption is saved.
[0069] The depth of the injection hole is determined by the range of the rich ore layer, and its depth range is from the surface to above the semi-weathered layer, which can be 5 meters, 10 meters, 20 meters or 30 meters.
[0070] When voltage is applied between the two electrodes, rare earth ions in the soil migrate in a directional manner under the action of the electric field. Based on experimental results, when the potential gradient in the ore body is 10-800V / m, it is conducive to the flow of rare earth ions to the cathode. The potential gradient in the ore body can be 10V / m, 20V / m, 30V / m, 40V / m, 50V / m, 60V / m or 80V / m, etc.
[0071] The present invention also provides a system for mining rare earth ores using a converted DC electric field, comprising: arranging at least 3 rows and at least 1 column of injection holes in a mining area, arranging electrodes in the injection holes, arranging a pH meter and an intelligent power control system near the electrodes in the mining area, and installing a current and voltage detector, a conductivity detector, an integrated mother power supply, a module controller, and a parameter standard database in the intelligent power control system;
[0072] Each row of electrodes is connected in parallel to the intelligent power control system. The intelligent power control system gives the distance between the anode electrode and the cathode electrode and the potential gradient of the initial power supply according to the resistivity of the mine and the parameter standard database data, and then makes corresponding adjustments according to the uploaded pH value or current changes and the current size;
[0073] Specifically, the pH meter uploads the measured information to the intelligent power control system in real time, and the intelligent power control system controller calls the information in the parameter standard database to obtain the pH value near the electrode, and compares the pH value near the electrode with the precipitation threshold value to control the positive and negative electrodes to move forward;
[0074] pH value near the electrode Once the precipitation threshold is exceeded Then stop the power first and move the positive and negative electrodes forward.
[0075] When the intelligent power control system detects that the current magnitude remains unchanged or the current between the electrodes is not within 10-60A when the current and voltage detectors upload to the parameter standard database, the intelligent power control system will advance the positive and negative electrodes or change the potential gradient through the integrated mother power supply.
[0076] Compared with the continuous power supply of fixed positive and negative electrodes, the conversion DC electric field can change the position of positive and negative electrodes in real time, improve the effective mobility of rare earths, shorten the mining cycle of weathering crust rare earth ore, and reduce power consumption costs. At the same time, in the process of switching the positive and negative electrodes, the rare earth ions in the leaching agent and soil in the non-powered area can be fully exchanged, thereby improving the rare earth leaching rate.
[0077] For example, when the pH near the electrode is greater than the rare earth precipitation threshold, the power control system will power off the electrode that is being powered on and automatically switch to the next alternating rotation state to prevent the pH from further increasing and causing rare earth precipitation.
[0078] For another example, when the current in the power-on process stabilizes to 20A, the positive and negative poles in the mining area will move forward.
[0079] In the energizing method of the present invention, each row of electrodes can be connected to the positive or negative pole of the power supply in time, and the positive and negative poles can be intelligently transformed. On the one hand, a corresponding energizing plan can be formulated in real time according to the changes in pH and conductivity, and rare earth ions can migrate quickly. On the other hand, the electrolysis near the electrode is weakened to prevent soil pollution.
[0080] However, the intelligent conversion of positive and negative electrodes in the energization method of the present invention is not the electrode exchange between two groups of fixed electrodes in the traditional sense, but the intelligent conversion of positive and negative electrodes is performed according to the changes in pH value and conductivity during the mining process.
[0081] The intelligent conversion of positive and negative electrodes in the power-on scheme of the present invention can improve the effective migration rate of rare earths. The migration direction of rare earth ions is always consistent between any electrodes, and there will be no reversal of current direction and reverse migration of rare earth ions.
[0082] At the same time, compared with continuous power supply to fixed positive and negative poles, not only the efficiency of rare earth mining has been improved, but the mining cycle has been shortened by 70-80% and power consumption has been reduced by 50%-80%.
[0083] Example 1
[0084] This embodiment provides a method for mining rare earth ore by using a DC electric field conversion, and experiments were conducted in the Renju mining area of Meizhou City, Guangdong Province. The method for mining rare earth ore by using power conversion includes:
[0085] (1) Arrangement of injection holes and electrodes: A total of 176 injection holes were evenly arranged in 16 rows and 11 columns in a test area that was 15 meters long and 10 meters wide. The vertical and horizontal spacing of the injection holes was 1 meter, and the depth of the injection holes was 24 meters. A 12-meter-long electrode was arranged in each injection hole. The electrode depth ranged from 12 meters from the bottom of the injection hole to cover the rich ore layer. A 13-meter wire was used to connect the top of the electrode. The electrodes in each row and 11 columns were connected in parallel to the intelligent power control system.
[0086] (2) Arrangement of intelligent power control system: 64 pH meters are evenly distributed in 176 injection holes and connected to the intelligent power control system.
[0087] (3) Injection of leaching agent: A 2.5% by mass ammonium sulfate solution is introduced into the injection hole, and the total amount of ammonium sulfate is 3 times the total amount of rare earth ions.
[0088] (4) Power on: Power on by intelligently transforming the DC electric field, such as Figure 1 Table 1 shows the power-on status after automatic inspection by the intelligent power control system, and the power-on status after the pH or current in the mining area changes. Each change in the positive and negative electrode positions is controlled by the intelligent power supply, and the potential gradient is 50V / m.
[0089] Table 1
[0090]
[0091] (5) Liquid collection: A kilometer-long borehole is arranged at the bottom of the mining area to collect the rare earth mother liquor from electric mining.
[0092] The power requirement for the electrified mining process was about 4kW. 1.16 tons of rare earths were collected in one month, with a rare earth recovery rate of 95% and a total power consumption of 2129kW·h.
[0093] Comparative Example 1
[0094] This comparative example provides a method for mining rare earth ores by power supply, and experiments were carried out in the Renju mining area of Meizhou City, Guangdong Province. The difference between this method and Example 1 lies in steps (3) and (4). In this comparative example: (3) there is no intelligent monitoring system; (4) all motors are powered on continuously for 1 month in a positive-negative...positive-negative manner.
[0095] The power demand of the comparative electrified mining process was about 8 kW. 0.42 tons of rare earths were collected in 2 months, with a rare earth recovery rate of 35% and a total power consumption of 10,238 kW·h.
[0096] like Figure 2 , Figure 3 As shown, it can be seen from Comparative Example 1 and Example 1 that the method provided by Example 1 increases the rare earth recovery rate by 60%, reduces power consumption by 79%, reduces power demand by 50%, and shortens the mining cycle by 82% compared with Comparative Example 1. In Comparative Example 1, since all areas are continuously energized, the long-term energization process produces strong polarization and electrolysis, and the positive-negative-positive electrode arrangement and energization scheme require at least half of the rare earth to overcome gravity and migrate to the negative electrode in the reverse direction, reducing the rare earth extraction rate. In addition, power consumption increases and power demand increases.
[0097] Example 2
[0098] This embodiment provides a method for mining rare earth ores by using a converted DC electric field. The experiment was conducted in Renju Mining Area, Meizhou City, Guangdong Province. The difference between this method and Embodiment 1 lies in steps (1), (2), (3) and (4). In this embodiment:
[0099] (1) Arrangement of injection holes and electrodes: A total of 357 injection holes were evenly arranged in 21 rows and 17 columns in the test area with a length of 30 meters and a width of 24 meters. The vertical and horizontal spacing of the injection holes was 1.5 meters, and the depth of the injection holes was 15 meters. An 8-meter-long electrode was arranged in each injection hole. The electrode depth ranged from 8 meters from the bottom of the injection hole to cover the rich ore layer. A 7-meter wire was used to connect the electrodes above. The electrodes in each row and 17 columns were connected in parallel to the control system.
[0100] (2) Arrangement of intelligent monitoring system: 84 pH meters are evenly distributed in 357 injection holes, current and voltage detectors and module controllers are installed at the terminals of the power supply, and the parameter standard database is imported.
[0101] (3) Injection of leaching agent: an ammonium sulfate solution with a molar concentration of 0.2 M is introduced into the injection hole, and the total amount of ammonium sulfate used is 4 times the total amount of rare earth ions.
[0102] (4) Power on: Power on by intelligently transforming the DC electric field, such as Figure 4 Table 2 shows the power-on status after automatic inspection by the intelligent power control system, and the power-on status after the pH or current in the mining area changes. Each change in the positive and negative electrode positions is controlled by the intelligent power supply, and the potential gradient is 55V / m.
[0103] Table 2
[0104]
[0105] The power requirement for the electrified mining process was about 7kW. 3.13 tons of rare earths were collected in 2 months, with a rare earth recovery rate of 93% and a total power consumption of 9827kW·h.
[0106] Comparative Example 2
[0107] This comparative example provides a method for mining rare earth ores by electricity, and experiments were carried out in the Renju mining area of Meizhou City, Guangdong Province. The difference between this method and Example 2 lies in step (3). In this comparative example, (3) electricity is supplied to all electrodes in a positive-negative...positive-negative manner for 3 months.
[0108] The power requirement of the comparative electrified mining process was about 16 kW. 1.02 tons of rare earths were collected in 3 months, with a rare earth recovery rate of 30% and a total power consumption of 30,489 kW·h.
[0109] like Figure 5 , Figure 6 As shown, it can be seen from Comparative Example 2 and Example 2 that the method provided by Example 2 increases the rare earth recovery rate by 63%, reduces the power consumption by 68%, reduces the power demand by 56%, and shortens the mining cycle by 78% compared with Comparative Example 2.
[0110] From the above, it can be seen that in the method provided by the embodiment of the present invention, the use of the intelligent conversion DC electric field power-on scheme can significantly improve the rare earth recovery rate, reduce power consumption, power demand and shorten the mining cycle.
[0111] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for mining rare earth ores by using a DC electric field conversion, comprising: Arrange at least 3 rows and at least 1 column of injection holes in the mining area, and arrange electrodes in the injection holes. Each row of electrodes is connected in parallel to an intelligent power supply control system. The intelligent power supply control system will determine the original power supply parameters of the weathering crust type rare earth ore mining area by automatic inspection, and then call the parameter matching in the parameter standard database according to the collected pH change value, current size, and current change to adjust the electrode position and power supply voltage; When the pH value near the electrode is greater than the precipitation threshold, the power is stopped first, and the positive and negative electrodes move forward; When the current tends to be stable or the current size is not between 10-60A, the positive and negative electrodes move forward or change the potential gradient.
2. The method according to claim 1, characterized in that The original power-on parameters specifically include the positions of the positive and negative electrodes and the potential gradient.
3. The method according to claim 1, characterized in that Positive and negative electrodes move forward: When the positive and negative electrodes move forward by one unit electrode spacing, if the initial current between the electrodes is not between 10-60A, continue to increase the electrode spacing or change the potential gradient; Prioritize increasing the forward movement distance.
4. The method according to claim 1, characterized in that: The pH value changes collected are measured by a pH meter installed near the electrode. The precipitation threshold is calculated by Calculated.
5. The method according to claim 2, characterized in that: The original power-on parameters are determined in the following way: if the initial resistivity of the weathering crust type rare earth ore is RΩ·m, the distance between the positive and negative electrodes is ≥1 / R m, and is greater than a unit electrode distance, and the potential gradient is ≥10R V / m.
6. The method according to claim 5, characterized in that The potential gradient must also meet 10-100V / m.
7. The method according to claim 1, characterized in that The number of rows of electrodes is determined according to the area of the mining area, and the spacing between each row of electrodes is 0.5-5 meters; Optionally, the spacing between each row of electrodes is 1 meter.
8. The method according to claim 1, characterized in that The number of rows of electrodes is determined according to the area of the mining area, and the spacing between each row of electrodes is 0.5-5 meters; Optionally, the spacing between each column of electrodes is 1 meter.
9. The method according to claim 1, characterized in that: The depth of the injection hole is determined by the thickness of the weathering crust type rare earth ore; at the same time, the depth of the injection hole is 5-30 meters.
10. A system for mining rare earth ores using a converted DC electric field, characterized in that: include: Arrange at least 3 rows and at least 1 column of injection holes in the mining area, and arrange electrodes in the injection holes. Arrange pH meters and intelligent power control systems near the electrodes in the mining area. The intelligent power control system is equipped with current and voltage detectors, conductivity detectors, integrated mother power supplies, module controllers, and parameter standard databases. Each row of electrodes is connected in parallel to the intelligent power control system. The intelligent power control system gives the distance between the anode electrode and the cathode electrode and the potential gradient of the initial power supply according to the resistivity of the mine and the parameter standard database data, and then makes corresponding adjustments according to the uploaded pH value or current changes and the current size; The pH meter uploads the measured information to the intelligent power control system in real time. The controller of the intelligent power control system calls the information in the parameter standard database to obtain the pH value near the electrode, and compares the pH value near the electrode with the precipitation threshold. Once the pH value near the electrode is greater than the precipitation threshold, the power is stopped first, and the positive and negative electrodes move forward. When the intelligent power control system detects that the current magnitude remains unchanged or the current between the electrodes is not within the range of 10-60A when the current and voltage detectors are uploaded to the parameter standard database, the intelligent power control system will move the positive and negative electrodes forward or change the potential gradient through the integrated mother power supply.
Citation Information
Patent Citations
Method for electrically restoring soil and underground water
CN101698521A
Method for removing soluble heavy metal ions in situ
CN101838740A
Method and system for exploiting rare earth ore by adopting direct current
CN117167010A
Electrochemical device for treating organic and inorganic pollutants in soil and underground water
CN203754475U
Electrolysis system
JP2007100187A