Photovoltaic module and preparation method thereof
By applying a translucent hydrofluoric acid-resistant film or coating on the cover plate and frame surface of the photovoltaic module, using fluorocarbon resin materials and UV photocuring glue, the photovoltaic module cannot withstand hydrofluoric acid corrosion in fluorochemical plants. The problem is to achieve long-term stability of components and efficient power generation.
Patent Information
- Application Number
- CN202310579108.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-22
AI Technical Summary
Existing photovoltaic modules cannot withstand hydrofluoric acid corrosion in fluorochemical plants, affecting their long-term application and reliability.
Designed with photovoltaic modules including cover plates, frames and back plates, where the surface coating of the cover plates and frames is a translucent hydrofluoric acid film or coating, and a fluorocarbon resin material is used to fix hydrogen resistance through UV light curing glue. Fluoric acid film and spray the hydrofluoric acid-resistant coating on the surface of the frame to isolate the hydrofluoric acid.
Effectively isolate hydrofluoric acid, preventing the cover, frame and back plate from being corroded, while not affecting the photovoltaic module's absorption of sunlight, improving the durability and conversion efficiency of the module.
Smart Images

Figure CN119008710A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of photovoltaic technology, and in particular to a photovoltaic component and a preparation method thereof. Background Art
[0002] With the development of photovoltaic technology, photovoltaic modules have been widely used. When a fluorine chemical plant needs to install photovoltaic modules, the exhaust gas contains hydrogen fluoride during the production of fluorine products in the fluorine chemical plant. Conventional photovoltaic modules have poor acid corrosion resistance and cannot meet the requirements of long-term use in the fluorine chemical plant. The materials in contact with the air of conventional photovoltaic modules include cover plates, back plates, and frames. The material used for the cover plate is generally glass, and the main component of glass is silicon dioxide. Silicon dioxide and hydrogen fluoride will react to generate fluorosilicic acid and water, causing the glass to be corroded. The specific chemical reaction formula of the reaction is: SiO2+4HF=SiF4↑+2H2O. The frame is generally made of 6005-T6 aluminum alloy, and a dense aluminum oxide layer is electroplated on the surface in contact with the air to protect the frame and improve the corrosion resistance, hardness, wear resistance, insulation, heat resistance and other properties of the frame. However, the dense aluminum oxide layer will also react with hydrogen fluoride, causing the frame to be corroded. The specific chemical reaction formula is: Al2O3+6HF=2AlF3+3H2O. Conventional photovoltaic modules will be corroded by hydrofluoric acid because the cover and frame will be corroded by hydrofluoric acid. In the process of long-term emission of trace hydrogen fluoride by fluorination plants, photovoltaic modules will be corroded, affecting the power generation and reliability of photovoltaic modules in long-term applications.
[0003] In the prior art, for the corrosion resistance of photovoltaic modules, there are studies on resistance to seaside salt spray. Seaside salt spray is mainly sodium chloride. When the material used for the cover plate is glass, glass does not react with sodium chloride. Glass itself has the advantage of being resistant to sodium chloride corrosion. The hydrofluoric acid resistance of the cover plate has not been improved, and the frame achieves corrosion resistance by increasing the thickness of the dense aluminum oxide layer on the surface in contact with the air. The thickness of the dense aluminum oxide layer on the surface of the frame of the photovoltaic module in the conventional scenario is 10μm (micrometer) to 15μm, and the thickness of the dense aluminum oxide layer on the surface of the frame of the photovoltaic module resistant to seaside salt spray is 25μm to 35μm. By increasing the thickness of the dense aluminum oxide layer on the surface of the frame, the performance of the photovoltaic module resistant to seaside salt spray can be improved. However, when facing a hydrofluoric acid environment, the cover plate that has not been improved in hydrofluoric acid resistance and the frame after increasing the thickness of the dense aluminum oxide layer on the surface of the frame will be corroded by hydrofluoric acid, so that the photovoltaic module is still not resistant to hydrofluoric acid corrosion. Summary of the invention
[0004] The present invention provides a photovoltaic module and a preparation method thereof, aiming to solve the problem in the prior art that the photovoltaic module cannot resist hydrofluoric acid corrosion.
[0005] A first aspect of the present invention provides a photovoltaic module, comprising: a cover plate, a frame, a back plate, a first hydrofluoric acid resistant structure, and a second hydrofluoric acid resistant structure;
[0006] The first hydrofluoric acid resistant structure is located on a side of the cover plate in contact with air;
[0007] The second hydrofluoric acid resistant structure is located on the surface of the frame in contact with air;
[0008] The surface of the back plate in contact with air is a hydrofluoric acid resistant surface;
[0009] The first hydrofluoric acid-resistant structure is light-transmissive.
[0010] In the present invention, the photovoltaic module includes: a cover plate, a frame, a back plate, a first hydrofluoric acid resistant structure, and a second hydrofluoric acid resistant structure; the first hydrofluoric acid resistant structure is located on the side of the cover plate in contact with the air; the second hydrofluoric acid resistant structure is located on the surface of the frame in contact with the air. The first hydrofluoric acid resistant structure and the second hydrofluoric acid resistant structure isolate the cover plate and the frame from the hydrofluoric acid in the air, so that the cover plate and the frame will not be corroded by the hydrofluoric acid. At the same time, the surface of the back plate in contact with the air is a hydrofluoric acid resistant surface, and the back plate will not be corroded by the hydrofluoric acid. In addition, the first hydrofluoric acid resistant structure is light-transmitting, will not affect the photovoltaic module to absorb sunlight, and will not affect the conversion efficiency of the photovoltaic module.
[0011] Optionally, the material of the first hydrofluoric acid resistant structure and the material of the second hydrofluoric acid resistant structure include fluorocarbon resin.
[0012] Optionally, the first hydrofluoric acid resistant structure is a hydrofluoric acid resistant film, or a hydrofluoric acid resistant coating.
[0013] Optionally, when the first hydrofluoric acid resistant structure is a hydrofluoric acid resistant film, the fluorocarbon resin includes at least one of ethylene-tetrafluoroethylene copolymer, ethylene-chlorotrifluoroethylene polymer, polyvinyl fluoride, and polyvinylidene fluoride;
[0014] When the first hydrofluoric acid resistant structure is a hydrofluoric acid resistant coating, the fluorocarbon resin includes at least one of fluoroethylene and vinyl ether copolymer, polyvinylidene fluoride, ethylene-tetrafluoroethylene copolymer, ethylene-chlorotrifluoroethylene polymer, and polyvinyl fluoride.
[0015] Optionally, the number of layers of the hydrofluoric acid resistant film is greater than or equal to 3.
[0016] Optionally, the hydrofluoric acid resistant film comprises: a bottom layer, a middle layer, and a top layer stacked in sequence from close to the cover plate to far away from the cover plate;
[0017] The material of the bottom layer is polyvinylidene fluoride;
[0018] The material of the middle layer is polyvinylidene fluoride;
[0019] The material of the top layer is ethylene-tetrafluoroethylene copolymer.
[0020] Optionally, the second hydrofluoric acid resistant structure is a hydrofluoric acid resistant coating.
[0021] A second aspect of the present invention provides a method for preparing a photovoltaic module, which is used to prepare the above-mentioned photovoltaic module, and the preparation method comprises:
[0022] preparing a cover plate;
[0023] Prepare the border;
[0024] preparing a back plate;
[0025] preparing a first hydrofluoric acid resistant structure, wherein the first hydrofluoric acid resistant structure is located on a side of the cover plate in contact with air;
[0026] preparing a second hydrofluoric acid resistant structure, wherein the second hydrofluoric acid resistant structure is located on a surface of the frame in contact with air;
[0027] The surface of the back plate in contact with air is a hydrofluoric acid resistant surface;
[0028] The first hydrofluoric acid-resistant structure is light-transmissive.
[0029] Optionally, in the case where the first hydrofluoric acid resistant structure is a hydrofluoric acid resistant film, preparing the first hydrofluoric acid resistant structure includes:
[0030] The hydrofluoric acid resistant film and the cover plate are fixed by using UV light curing glue;
[0031] The UV light-curing glue includes a light-converting agent.
[0032] Optionally, the light conversion agent is 4,8-dimethyl-7-carboxycoumarin. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments of the present invention will be briefly introduced below. Obviously, the accompanying drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.
[0034] Figure 1 A schematic diagram of fixing a hydrofluoric acid resistant film and a cover plate in an embodiment of the present invention is shown;
[0035] Figure 2 A schematic structural diagram of a photovoltaic module in an embodiment of the present invention is shown;
[0036] Figure 3 A cross-sectional schematic diagram of a frame in the prior art is shown;
[0037] Figure 4 A schematic structural diagram of another photovoltaic assembly in an embodiment of the present invention is shown;
[0038] Figure 5 A schematic diagram of the light-facing surface of a photovoltaic module in the prior art is shown.
[0039] Description of reference numerals:
[0040] 11-frame groove, 12-battery cell, 13-frame. DETAILED DESCRIPTION
[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] A photovoltaic module in an embodiment of the present invention includes: a cover plate, a frame 13, a back plate, a first hydrofluoric acid resistant structure, and a second hydrofluoric acid resistant structure; the first hydrofluoric acid resistant structure is located on the side of the cover plate in contact with the air; the second hydrofluoric acid resistant structure is located on the surface of the frame 13 in contact with the air; the surface of the back plate in contact with the air is a hydrofluoric acid resistant surface; the first hydrofluoric acid resistant structure is light-transmissive.
[0043] In the photovoltaic module, the cover plate is located on the light-facing side of the photovoltaic module, the back plate is located on the backlight side of the photovoltaic module, and the frame 13 is located around the photovoltaic module; the first hydrofluoric acid-resistant structure is located on the side of the cover plate in contact with the air, for example, the first hydrofluoric acid-resistant structure can be located on the light-facing side of the cover plate; the second hydrofluoric acid-resistant structure is located on the surface of the frame 13 in contact with the air, for example, the second hydrofluoric acid-resistant structure can be located on the outer surface of the frame 13; the surface of the back plate in contact with the air is a hydrofluoric acid-resistant surface, for example, the backlight side of the back plate is a hydrofluoric acid-resistant surface; the first hydrofluoric acid-resistant structure is located on the side of the cover plate in contact with the air, and the cover plate is located on the light-facing side of the photovoltaic module, that is, the first hydrofluoric acid-resistant structure is located on the light-facing side of the photovoltaic module, and the first hydrofluoric acid-resistant structure is light-transmitting, especially light within the wavelength range of sunlight, so as not to affect the photovoltaic module's absorption of sunlight.
[0044] The inventors have discovered that in the prior art, conventional photovoltaic modules will be corroded by hydrofluoric acid because of the cover plate and the frame 13. During the long-term emission of trace amounts of hydrogen fluoride from the fluorine chemical plant, the photovoltaic modules will be corroded, affecting the power generation and reliability of the photovoltaic modules in long-term applications. In addition, in the photovoltaic modules developed for seaside salt spray resistance, the cover plate that has not been improved in hydrofluoric acid resistance and the frame 13 with increased thickness of the dense aluminum oxide layer on the surface of the frame 13 will be corroded by hydrofluoric acid, so that the photovoltaic modules are still not resistant to hydrofluoric acid corrosion. In an embodiment of the present invention, a photovoltaic module includes: a cover plate, a frame 13, a back plate, a first hydrofluoric acid-resistant structure, and a second hydrofluoric acid-resistant structure; the first hydrofluoric acid-resistant structure is located on the side of the cover plate in contact with the air; the second hydrofluoric acid-resistant structure is located on the surface of the frame 13 in contact with the air. The first hydrofluoric acid-resistant structure and the second hydrofluoric acid-resistant structure isolate the cover plate and the frame 13 from the hydrofluoric acid in the air, so that the cover plate and the frame 13 will not be corroded by the hydrofluoric acid. At the same time, the surface of the back plate in contact with the air is a hydrofluoric acid-resistant surface, and the back plate will not be corroded by the hydrofluoric acid. In addition, the first hydrofluoric acid-resistant structure is light-transmitting, will not affect the photovoltaic module's absorption of sunlight, and will not affect the conversion efficiency of the photovoltaic module.
[0045] Optionally, the material of the first hydrofluoric acid resistant structure and the material of the second hydrofluoric acid resistant structure include fluorocarbon resin. Fluorocarbon resin is a chemical substance, and fluorocarbon resin has good hydrofluoric acid resistance, and the fluorocarbon resin material itself is transparent, so that the first hydrofluoric acid resistant structure can be light-transmissive. In addition, fluorocarbon resin has a strong carbon-fluorine bond (CF) as a skeleton and has good chemical resistance, high temperature resistance, oxidation resistance, weather resistance, and radiation resistance.
[0046] Optionally, the first hydrofluoric acid-resistant structure is a hydrofluoric acid-resistant film, or a hydrofluoric acid-resistant coating. The first hydrofluoric acid-resistant structure is a hydrofluoric acid-resistant film, the film layer has a high degree of density, the hydrofluoric acid-resistant film has good hydrofluoric acid resistance, and has the advantage of high light transmittance. Compared with other transparent materials, the hydrofluoric acid-resistant film has good hydrofluoric acid resistance, and compared with other hydrofluoric acid-resistant materials, the hydrofluoric acid-resistant film has better light transmittance and is suitable for use in a hydrofluoric acid environment; the first hydrofluoric acid-resistant structure is a hydrofluoric acid-resistant coating, and the coating can be formed by spraying the surface of the cover plate, which does not require an additional adhesive layer to be fixed to the surface of the cover plate, and the structure is relatively simple.
[0047] Optionally, when the first hydrofluoric acid-resistant structure is a hydrofluoric acid-resistant film, the fluorocarbon resin includes at least one of ethylene-tetrafluoroethylene copolymer (ETFE), ethylene-chlorotrifluoroethylene polymer (ECTFE), polyvinyl fluoride (PVF), and polyvinylidene fluoride (PVDF). These fluorocarbon resins can be made into films, so that hydrofluoric acid-resistant films can be prepared, and the wear resistance and UV resistance are good, which can improve the durability of the hydrofluoric acid-resistant film; when the first hydrofluoric acid-resistant structure is a hydrofluoric acid-resistant coating, the fluorocarbon resin includes at least one of fluoroethylene and vinyl ether copolymer (FEVE), polyvinylidene fluoride, ethylene-tetrafluoroethylene copolymer, ethylene-chlorotrifluoroethylene polymer, and polyvinyl fluoride. These fluorocarbon resin materials are easy to obtain and can be made into coatings to prepare hydrofluoric acid-resistant coatings. ETFE is a chemical substance. ETFE is the toughest fluoroplastic. While maintaining the good heat resistance, chemical resistance and electrical insulation properties of PTFE (polytetrafluoroethylene), it has greatly improved radiation resistance and mechanical properties, and the tensile strength can reach 50MPa (megapascals), which is nearly twice that of polytetrafluoroethylene. ETFE film is an economical and practical roofing material with good performance in transparent building structures. The film is made of artificial high-strength fluoropolymer ETFE. Its unique anti-adhesive surface makes it highly resistant to stains and easy to clean. It is also widely used in photovoltaic modules.
[0048] Optionally, the number of layers of the hydrofluoric acid resistant film is greater than or equal to 3. For example, the number of layers of the hydrofluoric acid resistant film can be 3, or 4, or 5, or 6, or 7, or 8. If the number of layers of the hydrofluoric acid resistant film is greater than or equal to 3, different materials can be selected according to the positions of different layers and their main functions, and the performance combination can be optimized to make the performance of the hydrofluoric acid resistant film better. In the hydrofluoric acid resistant film, the material of each layer can be selected from any one of ETFE, ECTFE, PVF, and PVDF, and the materials of different layers can be the same or different.
[0049] Optionally, the hydrofluoric acid resistant film includes: a bottom layer, a middle layer, and a top layer stacked in sequence from close to the cover plate to far away from the cover plate; the material of the bottom layer is polyvinylidene fluoride; the material of the middle layer is polyvinylidene fluoride; and the material of the top layer is ethylene-tetrafluoroethylene copolymer.
[0050] The bottom layer is closest to the cover plate, and the bottom layer and the cover plate need to be pasted and fixed. The bottom layer mainly plays the role of pasting with the adhesive layer such as the glue layer. The bottom layer needs to be corona treated before pasting. The higher the corona value of the bottom layer, the higher the surface energy of the hydrofluoric acid resistant film and the better the pasting effect. The corona value of the bottom layer when different materials are selected: PVDF>PVF>ECTFE>ETFE. When PVDF is selected, it is easy to corona. The material of the bottom layer is PVDF, which makes the surface energy of the hydrofluoric acid resistant film higher and the pasting effect is better; the middle layer mainly plays the role of mechanical support, so that when the hydrofluoric acid resistant film is pasted with the cover plate, the hydrofluoric acid resistant film has a certain mechanical strength. The mechanical strength of the middle layer when different materials are selected: PVDF<ECTFE<ETFE<PVF, all meet the requirements of mechanical strength during processing and pasting, but the processing performance of the middle layer when different materials are selected: PVDF>ECTFE>ET FE>PVF, the processing temperatures of ECTFE, ETFE, and PVF are all over 300℃ (degrees Celsius), and the requirements for the heat resistance of equipment and additives are higher. The processing temperature of PVDF is the lowest, and the material of the middle layer is PVDF, so that when the hydrofluoric acid resistant film and the cover are pasted, the hydrofluoric acid resistant film has a certain mechanical strength and is easy to process; the top layer is farthest from the cover, that is, the sunlight enters the top layer first, and the top layer mainly plays the role of wear resistance, hydrofluoric acid resistance, and high light transmittance. When different materials are used for the top layer, the wear resistance and UV resistance performance are: ETFE>ECTFE>PVF>PVDF, the wear resistance and UV resistance performance are better when ETFE is selected, and the material of the top layer is ETFE, which can increase the service life of the hydrofluoric acid resistant film; through the selection of materials for the bottom layer, the middle layer, and the top layer, the performance combination is optimized, so that the performance of the hydrofluoric acid resistant film is better. The hydrofluoric acid resistant film can be composed of a co-extruded bottom layer, a middle layer, and a top layer. Optionally, the thickness of the middle layer is greater than that of the bottom layer and the top layer, so that when the hydrofluoric acid resistant film and the cover plate are pasted together, the hydrofluoric acid resistant film has a certain mechanical strength.
[0051] Optionally, the thickness of the hydrofluoric acid resistant film is 10μm to 30μm. For example, the thickness of the hydrofluoric acid resistant film is 10μm, or 15μm, or 18μm, or 20μm, or 25μm, or 30μm. The thickness of the hydrofluoric acid resistant film is relatively high, so that the hydrofluoric acid resistant film has a better density and a better barrier ability to hydrofluoric acid, thereby having better hydrofluoric acid resistance, and has a certain strength, which is convenient for pasting with the cover plate, and at the same time, it is easier to meet the assembly line operation. Optionally, the hydrofluoric acid resistant film includes: in the case of a bottom layer, an intermediate layer, and a top layer stacked in sequence from close to the cover plate to away from the cover plate, the thickness of the top layer can account for 30% of the total thickness of the hydrofluoric acid resistant film, the thickness of the intermediate layer can account for 50% of the total thickness of the hydrofluoric acid resistant film, and the thickness of the bottom layer can account for 20% of the total thickness of the hydrofluoric acid resistant film. For example, the thickness of the hydrofluoric acid resistant film is 30 μm, the thickness of the top layer is 9 μm, the thickness of the middle layer is 15 μm, and the thickness of the bottom layer is 6 μm. For another example, the thickness of the hydrofluoric acid resistant film is 10 μm, the thickness of the top layer is 3 μm, the thickness of the middle layer is 5 μm, and the thickness of the bottom layer is 2 μm.
[0052] Optionally, when the first hydrofluoric acid-resistant structure is a hydrofluoric acid-resistant coating, the thickness of the hydrofluoric acid-resistant coating is 10 μm to 30 μm. For example, the thickness of the hydrofluoric acid-resistant coating may be 10 μm, or 15 μm, or 18 μm, or 20 μm, or 25 μm, or 30 μm. The thickness of the hydrofluoric acid-resistant coating is 10 μm to 30 μm, which can avoid affecting the transmittance of the photovoltaic module to the light surface when the thickness of the hydrofluoric acid-resistant coating is too large, thereby affecting the power generation efficiency of the photovoltaic module.
[0053] Optionally, the hydrofluoric acid resistant coating for preparing the hydrofluoric acid resistant coating is composed of an adhesive, a fluorocarbon resin, a solvent, and a leveling agent. The adhesive plays a role of sticking to the frame 13, the fluorocarbon resin plays a role of protecting the frame 13, optimizing the hydrofluoric acid resistance and aging resistance of the frame 13, the solvent is mainly used as a coating solvent, and will volatilize in the subsequent drying process, and the leveling agent promotes the coating to form a flat, smooth, and uniform coating film during the drying and film forming process. Optionally, the adhesive can be one or two of the following: acrylic resin, epoxy resin, and the ratio of the adhesive can be 10 to 25 parts. For example, the ratio of the adhesive can be 10 parts, or 13 parts, or 15 parts, or 20 parts, or 23 parts, or 25 parts. The fluorocarbon resin can be one or more of the following: FEVE, PVDF, ETFE, ECTFE, PVF, and the ratio can be 20 to 45 parts. For example, the ratio of the fluorocarbon resin can be 20 parts, or 25 parts, or 30 parts, or 35 parts, or 40 parts, or 45 parts. Optionally, the solvent can be one or two of the following: propylene glycol methyl ether acetate, butyl acetate, and the ratio can be 15 to 45 parts. For example, the ratio of the solvent can be 15 parts, or 20 parts, or 25 parts, or 30 parts, or 35 parts, or 45 parts. Optionally, the ratio of the leveling agent can be 0.5 to 1.5 parts. For example, the ratio of the leveling agent can be 0.5 parts, or 0.8 parts, or 1.0 parts, or 1.1 parts, or 1.3 parts, or 1.5 parts. In the embodiment of the present invention, the ratio of the hydrofluoric acid resistant coating is calculated according to the mass fraction.
[0054] Optionally, the second hydrofluoric acid resistant structure is a hydrofluoric acid resistant coating. The second hydrofluoric acid resistant structure is a hydrofluoric acid resistant coating, and the coating can be formed by spraying the surface of the frame 13, which does not require an additional adhesive layer to be fixed to the surface of the frame 13, and the structure is relatively simple. When the first hydrofluoric acid resistant structure and the second hydrofluoric acid resistant structure are both hydrofluoric acid resistant coatings, the thickness of the hydrofluoric acid resistant coatings of the two structures can be the same or different, and the composition of the hydrofluoric acid resistant coatings used to prepare the hydrofluoric acid resistant coatings of the two structures can be the same or different.
[0055] Optionally, the second hydrofluoric acid resistant structure is a hydrofluoric acid resistant film. When both the first hydrofluoric acid resistant structure and the second hydrofluoric acid resistant structure are hydrofluoric acid resistant films, the thickness of the hydrofluoric acid resistant films can be the same or different, and the materials used to prepare the hydrofluoric acid resistant films can be the same or different.
[0056] A method for preparing a photovoltaic module in an embodiment of the present invention is applied to preparing the above-mentioned photovoltaic module, and the preparation method includes: preparing a cover plate; preparing a frame 13; preparing a back plate; preparing a first hydrofluoric acid-resistant structure, the first hydrofluoric acid-resistant structure is located on the side of the cover plate in contact with the air; preparing a second hydrofluoric acid-resistant structure, the second hydrofluoric acid-resistant structure is located on the surface of the frame 13 in contact with the air; the surface of the back plate in contact with the air is a hydrofluoric acid-resistant surface; the first hydrofluoric acid-resistant structure is light-transmissive.
[0057] Prepare a cover plate; prepare a frame 13; prepare a back plate; prepare a first hydrofluoric acid resistant structure, the first hydrofluoric acid resistant structure is located on the side of the cover plate in contact with the air; prepare a second hydrofluoric acid resistant structure, the second hydrofluoric acid resistant structure is located on the surface of the frame 13 in contact with the air; the first hydrofluoric acid resistant structure and the second hydrofluoric acid resistant structure isolate the cover plate and the frame 13 from the hydrofluoric acid in the air, so that the cover plate and the frame 13 will not be corroded by the hydrofluoric acid, and at the same time, the surface of the back plate in contact with the air is a hydrofluoric acid resistant surface, and the back plate will not be corroded by the hydrofluoric acid. In addition, the first hydrofluoric acid resistant structure is light-transmitting and will not affect the photovoltaic module's absorption of sunlight, and will not affect the conversion efficiency of the photovoltaic module.
[0058] The inventors have found that in the prior art, after the frame 13 is extruded and formed, an oxide film is electroplated, and then it is cut to make corner brackets, punching holes, etc. After the oxide film is electroplated, the cutting actions such as corner brackets and punching holes are performed, and the newly added cutting surface is not protected by the oxide film. The cutting surface is particularly susceptible to corrosion during subsequent long-term use. In an embodiment of the present invention, the method for preparing the frame 13 is: extrusion molding of the frame 13; electroplating of an oxide film; cutting processing. After the cutting processing of the frame 13 is completed, a hydrofluoric acid-resistant coating is sprayed on the surface of the frame 13 in contact with the air to prepare a hydrofluoric acid-resistant coating to ensure that the cutting surface is also covered with the hydrofluoric acid-resistant coating.
[0059] Optionally, when the first hydrofluoric acid resistant structure is a hydrofluoric acid resistant film, preparing the first hydrofluoric acid resistant structure includes: fixing the hydrofluoric acid resistant film and the cover plate with UV (Ultraviolet) light-curing glue; the UV light-curing glue includes a light-converting agent.
[0060] The inventors have found that in the prior art, the two-component glue used to stick the film layer requires a long drying time during sticking. Specifically, most of the sticking adopts a heating curing process, which requires a lengthy drying tunnel and a certain drying time. The drying time is usually 5 minutes to 30 minutes, which has a great impact on the production capacity of the sticking film layer. In the embodiment of the present invention, UV light-curing glue is used to stick the hydrofluoric acid-resistant film. The curing time required for the UV light-curing glue is relatively short. Specifically, the curing of the UV light-curing glue is performed by ultraviolet irradiation, and the required time is 25 seconds to 70 seconds, thereby reducing the process time for sticking the hydrofluoric acid-resistant film and the cover plate. The hydrofluoric acid-resistant film and the cover plate are fixed with UV light-curing glue, and the UV light-curing glue is located between the hydrofluoric acid-resistant film and the cover plate. That is to say, after the sunlight passes through the hydrofluoric acid-resistant film, it will irradiate the UV light-curing glue. The hydrofluoric acid-resistant film has no ability to cut off ultraviolet rays. When the photovoltaic module needs to be used outdoors for a long time (for example, 25 years), the ultraviolet rays in the sunlight pass through the hydrofluoric acid-resistant film and irradiate the UV light-curing glue. The UV light-curing The chemical glue needs to withstand long-term exposure to ultraviolet rays in sunlight. The inventors also found that in the prior art, ultraviolet additives are generally added to the materials to prevent the materials from aging after being exposed to ultraviolet rays. Some of the existing ultraviolet additives prevent the materials from aging after being exposed to ultraviolet rays by shielding, reflecting ultraviolet rays or absorbing ultraviolet rays and converting them into harmless heat energy; some can quench the excited state of molecules or groups excited by ultraviolet rays, restore them to the ground state, eliminate or slow down the possibility of photo-oxidation-reduction reactions, and prevent the materials from aging after being exposed to ultraviolet rays; some capture the free radicals generated by photo-oxidation-reduction, thereby preventing the free radical reactions that cause material aging and protecting the materials from ultraviolet damage. However, the above-mentioned ultraviolet additives will have a huge attenuation in ultraviolet cutoff ability as the ultraviolet irradiation time increases. In the embodiment of the present invention, the UV light-curing glue includes a light-converting agent, which is generally composed of a large conjugated system and some chromophores and auxochrome groups with electron-donating properties. It uses its own chromophores to absorb ultraviolet light, causing the energy level transition of π electrons in the molecule, and emitting light waves with longer wavelengths to achieve the purpose of light conversion. The light-converting agent converts ultraviolet light into light, which can prevent the UV light-curing glue from being intolerant to the ultraviolet radiation in sunlight, causing the rapid aging of the UV light-curing glue. In addition, the UV light-curing glue also includes a prepolymer, a reactive diluent, and a photoinitiator.Prepolymer refers to a class of low-polymerization intermediates that can be converted into high-molecular-weight polymers. The prepolymer can be one or more of the following: polyacrylate, epoxy acrylate, polyurethane acrylate, unsaturated polyester, polyolefin, thiol. The main function of the prepolymer is to provide the key performance of UV light-curing adhesive. The ratio is: 34 to 41 parts. For example, the ratio of the prepolymer can be: 34 parts, or 35 parts, or 37 parts, or 38 parts, or 40 parts, or 41 parts; the active diluent mainly refers to a low-molecular-weight epoxy compound containing an epoxy group. The active diluent can be one or more of the following: styrene, butyl acrylate, isooctyl acrylate, isobornyl acrylate, tripropylene glycol diacrylate, hexanediol, Alcohol diacrylate, trimethylolpropane triacrylate, the main function of the active diluent is to adjust the viscosity and participate in the polymerization reaction, the ratio is: 51 parts to 59 parts, for example, the ratio of the active diluent can be: 51 parts, or 52 parts, or 55 parts, or 56 parts, or 57 parts, or 59 parts; the photoinitiator is a class of compounds that can absorb energy of a certain wavelength in the ultraviolet light region or the visible light region to generate free radicals, cations, etc., thereby initiating monomer polymerization and cross-linking curing. The photoinitiator can be one or more of the following: dibenzoyl, benzophenone, benzoin, benzoin ether compounds (such as benzoin ethyl ether, benzoin butyl ether). The main function of the photoinitiator is to adjust the sensitivity of the UV curing system, the ratio is: 1 The ratio of the photoinitiator can be 1 part, 2 parts, 3 parts, 4 parts, 5 parts, or 6 parts; the light conversion agent can be one or more of the following: BPPO (N, N'-bis (2-phenylphenyl) oxalic acid), POPOP (1, 4-bis (5-phenyl-2-oxazolyl) benzene), fluorescein sodium, acridine yellow, fluorescent yellow YG-51, 4,8-dimethyl-7-carboxycoumarin, acridine red, lissamine rhodamine B, fluorescent red GG, DCM (4-dicyanomethylene-2-methyl-p-xylidine phenylvinyl-4H-pyran), the ratio is 0.08 parts to 0.15 parts (excluding 0.15 parts), for example, the ratio of the light conversion agent can be 0.08 Part, or 0.09 part, or 0.10 part, or 0.11 part, or 0.13 part, or 0.14 part, the UV resistance of UV light curing glue is mainly reflected by the cut-off ability of UV light curing glue to ultraviolet rays. When the ratio is less than 0.08 parts, the cut-off rate of UV light curing glue to ultraviolet rays is less than 95%, when the ratio is ≥ 0.08 parts, the cut-off rate of UV light curing glue to ultraviolet rays is ≥ 95%, when the ratio is less than 0.15 parts, the visible light transmittance of UV light curing glue is ≥ 95%, when the ratio is ≥ 0.15 parts, the visible light transmittance of UV light curing glue is less than 95%, and the ratio of the light conversion agent is: 0.08 parts to 0.15 parts, which not only ensures the UV resistance of UV light curing glue, but also ensures high light transmittance. In the embodiment of the present invention, the ratio of UV light curing glue is calculated according to the mass fraction.The material used for the cover plate can be glass, and the adhesion effect of fixing the hydrofluoric acid resistant film and the glass cover plate with UV light curing glue is better. Figure 1 , Figure 1 A schematic diagram of fixing a hydrofluoric acid resistant film and a cover plate in an embodiment of the present invention is shown.
[0061] Optionally, the light conversion agent is 4,8-dimethyl-7-carboxy coumarin. The absorption bands and emission bands of different light conversion agents are shown in Table 1. As shown in Table 1, the ultraviolet wavelength absorbed by 4,8-dimethyl-7-carboxy coumarin is the largest, which is 330 to 370 nm (nanometers). The light conversion agent is 4,8-dimethyl-7-carboxy coumarin, which can prevent more ultraviolet rays from damaging the UV light-curing glue.
[0062] Table 1 Absorption and emission bands of different light conversion agents
[0063] Name of light conversion agent Absorption band / nm Emission band / nm BPPO 330~350 390~430 POPOP 340~370 420~480 Fluorescein sodium 340~370 570 Acridine yellow 340~375 500~550 Fluorescent Yellow YG-51 350 510~560 4,8-Dimethyl-7-carboxycoumarin 330~370 455~505 Acridine Red 350 590~640 Lissamine Rhodamine B 320~355 585~640 Fluorescent red GG 350 600~640 DCM 310 630~690
[0064] The present invention is further explained below in conjunction with specific embodiments.
[0065] Example 1
[0066] Reference Figure 2 , Figure 2 A schematic diagram of the structure of a photovoltaic module in an embodiment of the present invention is shown. The photovoltaic module is a single-glass module, including a backplane, a film, a battery cell 12, a film, a cover plate, a UV light-cured glue, and a hydrofluoric acid-resistant film stacked in sequence, the hydrofluoric acid-resistant film faces the sunlight, the backplane faces away from the sunlight, and a frame 13 (not shown in the figure) is installed around the photovoltaic module. The frame 13 is an aluminum frame, and the second hydrofluoric acid-resistant structure is a hydrofluoric acid-resistant coating (not shown in the figure). The preparation method of this photovoltaic module specifically includes the following steps:
[0067] 1. Prepare the cover plate;
[0068] The cover is fully tempered photovoltaic glass with a size of 2102*1042*3.2mm. The light-facing side of the cover is flat, which is convenient for subsequent fixation with the hydrofluoric acid-resistant film. The backlight side of the cover adopts an embossed design, which is convenient for subsequent lamination with the adhesive film. The light-facing side of the fully tempered photovoltaic glass includes an anti-reflection film.
[0069] Optionally, the cover plate may be semi-tempered photovoltaic glass or fully tempered photovoltaic glass. Optionally, the thickness of the cover plate may be 1 mm to 5 mm.
[0070] 2. Preparation of border 13:
[0071] The frame 13 is extruded, electroplated with an oxide film, and cut.
[0072] 3. preparing a back plate; the surface of the back plate in contact with air is a hydrofluoric acid resistant surface;
[0073] The surface of the back plate in contact with the air is provided with a PVF film, the thickness of the PVF film is 24 μm, and the PVF film plays a role in protecting the backlight surface of the photovoltaic module from being corroded by hydrofluoric acid.
[0074] Optionally, the surface of the back plate in contact with the air has a PVF film or a PVDF film, and the thickness of the PVF film or the PVDF film is greater than or equal to 22 μm.
[0075] 4. Prepare a hydrofluoric acid resistant film, which is located on the side of the cover plate in contact with the air:
[0076] (1) Preparation of UV light-curing glue:
[0077] ① The prepolymer is polyacrylate, the ratio is 40 parts, and the active diluent is styrene, the ratio is 54 parts; the prepolymer and the active diluent are added into a stirring kettle according to the ratio, protected from light, and the first stirring is performed at a speed of 1000 rpm (Revolutions Per Minute, revolutions per minute) for 60 minutes to obtain a mixture;
[0078] ② The photoinitiator is dibenzoyl, the ratio is: 5.9 parts; the light conversion agent is 4,8-dimethyl-7-carboxycoumarin, the ratio is: 0.1 parts, the mixture obtained in step ① is mixed with the photoinitiator and the light conversion agent, protected from light, and stirred for the second time, maintaining the temperature at 30°C, the speed at 1000rpm, and the stirring time is 30min. After the stirring is completed, filter, stand and remove bubbles to obtain UV light-curing glue.
[0079] (2) Preparation of hydrofluoric acid resistant film:
[0080] The hydrofluoric acid resistant film includes: a bottom layer, a middle layer, and a top layer which are stacked in sequence from close to the cover plate to far away from the cover plate; the material of the bottom layer is PVDF; the material of the middle layer is PVDF; the material of the top layer is ETFE, and the hydrofluoric acid resistant film is composed of a co-extruded bottom layer, a middle layer, and a top layer, the thickness of the top layer is 9μm, the thickness of the middle layer is 15μm, and the thickness of the bottom layer is 6μm.
[0081] (3) Use UV light curing glue to fix the hydrofluoric acid resistant film and cover plate:
[0082] Place the cover plate on the conveyor belt of the assembly line, and the cover plate enters the machine. The machine cleans the stains on the surface of the cover plate. The cleaned cover plate enters the fan, and the water stains on the surface of the cover plate are blown dry by hot air. Apply UV light-curing glue on the side of the dried cover plate that contacts the air, and paste the hydrofluoric acid-resistant film on the surface of the UV light-curing glue that contacts the air. The film surface is flattened by a roller, and the cover plate covered with the hydrofluoric acid-resistant film is pre-cured for the first time. The time for the first pre-curing is 8s. The first pre-curing plays the role of preliminarily fixing the hydrofluoric acid-resistant film and the cover plate. After the first pre-curing, trim the edges and trim off the excess hydrofluoric acid-resistant film and UV light-curing glue. Then perform the second curing, and the time for the second curing is 40s. In the first pre-curing and the second curing, the UV wavelength is 300nm. A hydrofluoric acid-resistant film is obtained.
[0083] Optionally, in the above step ①, the rotation speed of the first stirring can be 400 rpm to 1100 rpm, and the time of the first stirring can be 30 min to 90 min. In the above step ②, the temperature of the second stirring can be 15°C to 35°C, the rotation speed of the second stirring can be 400 rpm to 1100 rpm, and the time of the second stirring can be 10 min to 60 min.
[0084] Optionally, the first pre-curing time may be 5s to 10s. Optionally, the second curing time may be 20s to 60s. Optionally, during the first pre-curing and the second curing, the UV wavelength may be 280nm to 400nm.
[0085] 5. Prepare a hydrofluoric acid resistant coating, which is located on the surface of the frame 13 in contact with air:
[0086] (1) preparing a hydrofluoric acid resistant coating, wherein the hydrofluoric acid resistant coating is used to prepare a hydrofluoric acid resistant coating;
[0087] The hydrofluoric acid resistant coating is composed of adhesive, fluorocarbon resin, solvent and leveling agent: the adhesive is acrylic resin, with a ratio of 25 parts; the fluorocarbon resin is PVDF, with a ratio of 30 parts; the solvent is propylene glycol methyl ether acetate, with a ratio of 44 parts; the leveling agent, with a ratio of 1 part;
[0088] (2) Obtain the frame 13 obtained in step 2 after the cutting process is completed, and use a high-voltage electrostatic spray gun to spray a hydrofluoric acid-resistant coating on the surface of the frame 13 that contacts the air. After spraying, the aluminum frame is baked at a temperature of 220° C. for 20 minutes to obtain a hydrofluoric acid-resistant coating.
[0089] Optionally, the baking temperature may be 200° C. to 250° C., and the baking time may be 10 min to 30 min.
[0090] 6. Lamination:
[0091] (1) preparing a battery cell 12, a film on the light-facing side of the battery cell 12, and a film on the backlight side of the battery cell 12;
[0092] The film on the light-facing side of the cell 12 is a highly transparent EVA (ethylene-vinyl acetate copolymer) with a gram weight of 380 g / m 2 (g / m2), the size is 2102*1036mm, and it is a high-transmittance type, which can ensure that more light can pass through the film to reach the battery cell 12, thereby playing a role in power efficiency.
[0093] The battery cell 12 is a P-type battery cell with a size of 166*166mm.
[0094] The film on the backlight side of the cell 12 is high cut-off EVA with a gram weight of 380g / m 2 , the size is 2102*1036mm, it is a high cutoff type, which cuts off the ultraviolet rays that pass through the light side and plays a role in protecting the back panel of the backlight side.
[0095] Optionally, the size of the cell 12 can be 166*166mm, 182*182mm, 210*210mm, the type of the cell 12 can be P-type, N-type, HJT (Heterojunction with Intrinsic Thin layer), and the shape can be half-cell, whole-cell, shingled, or one-third-cell. Optionally, the adhesive film on the backlight side of the cell 12 can be white EVA or co-extruded white EVA.
[0096] (2) According to Figure 2 The structure shown is laid, and then laminated. During the lamination process, the adhesive film melts and the cell 12 is pasted together with the cover plate and the back plate. The lamination temperature is 140°C and the lamination time is 15 minutes. After lamination, the photovoltaic module is edge-cut to remove excess adhesive film and back plate. Install the junction box, and then install the frame 13. Glue is applied in the frame groove 11 of the frame 13 after the above step 5 is completed. Refer to Figure 3 , Figure 3 A cross-sectional schematic diagram of a frame 13 in the prior art is shown, in which the enclosed space is the cross-section of the frame 13, and the frame groove 11 is approximately U-shaped, which is used to fix the photovoltaic module. After the gluing is completed, the frame 13 is installed around the photovoltaic module. After the glue is cured in room temperature and humidity for 2 hours, the photovoltaic module is completed.
[0097] Optionally, the lamination temperature may be 130° C. to 145° C., and the lamination time may be 10 min to 20 min. Optionally, the glue may be cured at room temperature and moisture for 1 h to 3 h.
[0098] Example 2
[0099] Reference Figure 4 , Figure 4 A schematic diagram of the structure of another photovoltaic module in an embodiment of the present invention is shown, the photovoltaic module is a double-glass module, including a back plate, a film, a battery cell 12, a film, a cover plate, a UV light-curing glue, and a first hydrofluoric acid-resistant film stacked in sequence, the first hydrofluoric acid-resistant film faces the sunlight, the back plate includes a second hydrofluoric acid-resistant film, a UV light-curing glue, and glass stacked in sequence, the second hydrofluoric acid-resistant film faces away from the sunlight, a frame 13 (not shown in the figure) is installed around the photovoltaic module, the frame 13 is an aluminum frame, and the second hydrofluoric acid-resistant structure is a hydrofluoric acid-resistant coating (not shown in the figure), and the preparation method of the photovoltaic module specifically includes the following steps:
[0100] 1. Prepare the cover plate;
[0101] The cover is fully tempered photovoltaic glass with a size of 2102*1042*2.0mm. The light-facing side of the cover is flat, which is convenient for subsequent fixation with the hydrofluoric acid-resistant film. The backlight side of the cover adopts an embossed design, which is convenient for subsequent lamination with the adhesive film. The light-facing side of the fully tempered photovoltaic glass includes an anti-reflection film.
[0102] 2. Preparation of frame 13: Same as step 2 of embodiment 1.
[0103] 3. Prepare a backplane, the surface of the backplane in contact with air is a hydrofluoric acid resistant surface, and prepare a first hydrofluoric acid resistant film:
[0104] (1) Preparation of UV light-curing glue:
[0105] The same as step (1) in step 4 of Example 1.
[0106] (2) Preparing a first hydrofluoric acid resistant film and a second hydrofluoric acid resistant film:
[0107] The same conditions and parameters as those in step (2) of step 4 of Example 1 are used to prepare the first hydrofluoric acid resistant film and the second hydrofluoric acid resistant film, respectively.
[0108] (3) Use UV light curing glue to fix the first hydrofluoric acid resistant film and the cover plate:
[0109] The same as step (3) in step 4 of Example 1.
[0110] (4) Use UV light curing glue to fix the second hydrofluoric acid resistant film and glass:
[0111] Put the glass on the conveyor belt of the assembly line, and the glass enters the machine. The machine cleans the stains on the surface of the glass. The cleaned glass enters the fan, and the water stains on the surface of the glass are blown dry by hot air. Apply UV light-curing glue on the side of the dried glass that is in contact with the air, and paste the second hydrofluoric acid-resistant film on the surface of the UV light-curing glue that is in contact with the air. The film surface is flattened by a roller, and the glass covered with the hydrofluoric acid-resistant film is pre-cured for the first time. The time of the first pre-curing is 8s. The first pre-curing plays the role of preliminarily fixing the second hydrofluoric acid-resistant film and the glass. After the first pre-curing, trim the edges and trim off the excess second hydrofluoric acid-resistant film and UV light-curing glue. Then perform the second curing, and the time of the second curing is 40s. In the first pre-curing and the second curing, the UV wavelength is 300nm. The second hydrofluoric acid-resistant film is obtained.
[0112] 4. Prepare a hydrofluoric acid resistant coating, which is located on the surface of the frame 13 in contact with air:
[0113] Same as step 5 in Example 1.
[0114] 5. Lamination:
[0115] (1) preparing a battery cell 12, a film on the light-facing side of the battery cell 12, and a film on the backlight side of the battery cell 12;
[0116] The film on the light-facing side of the cell 12 is made of highly transparent POE (polyolefin elastomer) with a gram weight of 380g / m 2 , with a size of 2102*1036mm, and is of high-transmittance type, which can ensure that more light passes through the film to reach the battery cell 12, thereby playing a role in power efficiency.
[0117] The battery cell 12 is a P-type battery cell with a size of 166*166mm.
[0118] The film on the backlight side of the cell 12 is high cutoff POE with a gram weight of 380g / m 2 , the size is 2102*1036mm, it is a high cutoff type, which cuts off the ultraviolet rays that pass through the light surface and plays a role in protecting the back glass glaze.
[0119] Optionally, the size of the battery cell 12 can be 166*166mm, 182*182mm, 210*210mm, the type of the battery cell 12 can be P-type, N-type, HJT, and the shape can be half-cell, whole-cell, shingled, or one-third-cell.
[0120] (2) According to Figure 4The structure shown is laid and then laminated. During the lamination process, the adhesive film melts and the cell 12 is pasted together with the cover plate and the glass. The lamination temperature is 140°C and the lamination time is 15 minutes. The laminated photovoltaic module is edge-cut to remove excess adhesive film and back plate. The junction box is installed, and then the frame 13 is installed. After the step 4 is completed, glue is applied in the frame groove 11 of the frame 13. After the glue is applied, the frame 13 is installed around the photovoltaic module. After the glue is cured at room temperature and humidity for 2 hours, the photovoltaic module is completed.
[0121] A photovoltaic module prepared according to the above embodiment 1 and a photovoltaic module prepared according to the above embodiment 2 were subjected to a hydrofluoric acid fumigation resistance test. A hydrofluoric acid solution was added into the fluoridation tank. The concentration of the hydrofluoric acid solution was 40%. The photovoltaic module prepared in embodiment 1 was facing the light side toward the hydrofluoric acid solution. Figure 5 , Figure 5 The schematic diagram of the light-facing side of a photovoltaic module in the prior art is shown. The photovoltaic module includes a plurality of cells 12, surrounded by a frame 13 of the photovoltaic module. The backlight side of the photovoltaic module prepared in Example 2 faces the hydrofluoric acid solution. The photovoltaic module is placed on the fluoridation pool, and the photovoltaic module is tightly covered on the pool mouth of the fluoridation pool, compacted to prevent it from being blown off by the wind. After 48 hours of fumigation, the appearance corrosion of the photovoltaic module cover plate, back plate, and surrounding frames 13 is observed. The appearance of the photovoltaic module has no corrosion and blackening phenomenon. After the appearance observation is completed, a mechanical load test is performed. After the mechanical load test is completed, the output power of the photovoltaic module is tested. The output power test results are shown in Table 2.
[0122] Table 2 Output power test results
[0123]
[0124] In Table 2, the initial power is the output power of the photovoltaic module before the hydrofluoric acid fumigation resistance test, the power after fumigation + mechanical load is the output power of the photovoltaic module after the hydrofluoric acid fumigation resistance test and the mechanical load test, and the power attenuation is the attenuation percentage of the output power from before the hydrofluoric acid fumigation resistance test to the end of the mechanical load test. It can be seen from Table 2 that the power attenuation of Example 1 and Example 2 is ≤5%, indicating that the photovoltaic module in the embodiment of the present invention has good hydrofluoric acid resistance.
[0125] It should be noted that the relevant parts of the aforementioned photovoltaic module and the method for preparing the photovoltaic module can be referenced to each other and can achieve the same or similar effects.
[0126] It should be noted that, in this document, the terms "first", "second", etc. in the specification and claims are used to distinguish similar objects, rather than to describe a specific order or sequence. Moreover, the objects distinguished by "first", "second", etc. are usually of the same type, and the number of objects is not limited. For example, the second object can be one.
[0127] It should be noted that, for the method embodiments, for the sake of simplicity of description, they are all expressed as a series of action combinations, but those skilled in the art should be aware that the embodiments of the present application are not limited by the described order of actions, because according to the embodiments of the present application, certain steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also be aware that the embodiments described in the specification are all preferred embodiments, and the actions involved are not necessarily required by the embodiments of the present application.
[0128] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.
[0129] Through the description of the above implementation methods, those skilled in the art can clearly understand that the above-mentioned embodiment methods can be implemented by means of software plus a necessary general hardware platform, and of course by hardware, but in many cases the former is a better implementation method. Based on such an understanding, the technical solution of the present invention, or the part that contributes to the prior art, can be embodied in the form of a software product, which is stored in a storage medium (such as ROM / RAM, a magnetic disk, or an optical disk), and includes a number of instructions for enabling a terminal (which can be a mobile phone, a computer, a server, an air conditioner, or a network device, etc.) to execute the methods described in each embodiment of the present invention.
[0130] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation modes, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are within the protection of the present invention.
Claims
1. A photovoltaic module, characterized in that: include: Cover plate, frame, back plate, first hydrofluoric acid resistant structure, second hydrofluoric acid resistant structure; The first hydrofluoric acid resistant structure is located on a side of the cover plate in contact with air; The second hydrofluoric acid resistant structure is located on the surface of the frame in contact with air; The surface of the back plate in contact with air is a hydrofluoric acid resistant surface; The first hydrofluoric acid-resistant structure is light-transmissive.
2. The photovoltaic module according to claim 1, characterized in that: The material of the first hydrofluoric acid resistant structure and the material of the second hydrofluoric acid resistant structure include fluorocarbon resin.
3. The photovoltaic module according to claim 2, characterized in that: The first hydrofluoric acid resistant structure is a hydrofluoric acid resistant film, or a hydrofluoric acid resistant coating.
4. The photovoltaic module according to claim 3, characterized in that: In the case where the first hydrofluoric acid resistant structure is a hydrofluoric acid resistant film, the fluorocarbon resin includes at least one of ethylene-tetrafluoroethylene copolymer, ethylene-chlorotrifluoroethylene polymer, polyvinyl fluoride, and polyvinylidene fluoride; When the first hydrofluoric acid resistant structure is a hydrofluoric acid resistant coating, the fluorocarbon resin includes at least one of fluoroethylene and vinyl ether copolymer, polyvinylidene fluoride, ethylene-tetrafluoroethylene copolymer, ethylene-chlorotrifluoroethylene polymer, and polyvinyl fluoride.
5. The photovoltaic module according to claim 3, characterized in that: The number of layers of the hydrofluoric acid resistant film is greater than or equal to 3.
6. The photovoltaic module according to claim 5, characterized in that: The hydrofluoric acid resistant film comprises: a bottom layer, a middle layer, and a top layer stacked in sequence from close to the cover plate to far away from the cover plate; The material of the bottom layer is polyvinylidene fluoride; The material of the middle layer is polyvinylidene fluoride; The material of the top layer is ethylene-tetrafluoroethylene copolymer.
7. The photovoltaic module according to claim 1, characterized in that: The second hydrofluoric acid resistant structure is a hydrofluoric acid resistant coating.
8. A method for preparing a photovoltaic module, characterized in that: Applicable to preparing the photovoltaic module according to any one of claims 1 to 7, the preparation method comprising: preparing a cover plate; Prepare the border; preparing a back plate; preparing a first hydrofluoric acid resistant structure, wherein the first hydrofluoric acid resistant structure is located on a side of the cover plate in contact with air; preparing a second hydrofluoric acid resistant structure, wherein the second hydrofluoric acid resistant structure is located on a surface of the frame in contact with air; The surface of the back plate in contact with air is a hydrofluoric acid resistant surface; The first hydrofluoric acid-resistant structure is light-transmissive.
9. The preparation method according to claim 8, characterized in that: In the case where the first hydrofluoric acid resistant structure is a hydrofluoric acid resistant film, preparing the first hydrofluoric acid resistant structure includes: The hydrofluoric acid resistant film and the cover plate are fixed by using UV light curing glue; The UV light-curing glue includes a light-converting agent.
10. The preparation method according to claim 9, characterized in that: The light conversion agent is 4,8-dimethyl-7-carboxylcoumarin.