Aerogel preparation method based on hydrothermal solvent replacement

By using organic solvents such as acid solution and n-butanol under hydrothermal conditions to replace and dry the inorganic oxide hydrogel, the problems of long time and high energy consumption in the prior art are solved, and low cost and high efficiency are achieved Prepare aerogels and reduce gel shrinkage, suitable for industrial production.

CN119018899APending Publication Date: 2024-11-26卢序
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310580489.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art uses organic solvents to replace water in hydrogels under normal temperature conditions for a long time and high energy consumption, and is not suitable for industrial production. The use of non-water-soluble organic solvents such as n-butanol leads to coagulation during the replacement process. The glue shrinks irreversibly.

Method used

Soak and heat the inorganic oxide hydrogel in acid solution, use the critical co-soluble temperature of organic solvents such as n-butanol to alcohol to replace solvents under hydrothermal conditions, reduce the gel water content through co-distillation and insulation treatment, and finally dry it to obtain Aerogel.

Benefits of technology

The preparation of high-quality aerogels at low cost is achieved, reducing gel shrinkage, improving preparation efficiency and energy efficiency, and adjusting the specific surface area and mechanical properties of the gel according to the pH value of the acid solution.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an aerogel preparation method based on hydrothermal solvent replacement. The method comprises the step of soaking inorganic oxide hydrogel with low salt content in acid liquor. And then replacing water in the hydrogel with an organic solvent under a hydrothermal condition. And finally, drying to obtain the aerogel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for preparing aerogel based on hydrothermal solvent replacement, and in particular to a method for obtaining aerogel by performing solvent replacement on water in inorganic oxide hydrogel under hydrothermal conditions and finally drying the aerogel. Background Art

[0002] Aerogel was invented by Kistler, who first synthesized silica hydrogel, then replaced the water in the silica hydrogel with an organic solvent that is miscible with water, and finally obtained silica aerogel by supercritical drying.

[0003] However, the use of water-miscible organic solvents to replace water in hydrogels at room temperature requires the consumption of a large amount of organic solvents, such as ethanol, and is extremely time-consuming. In addition, the energy consumption of ethanol dehydration and reuse is quite huge, and the drying must be done by supercritical method to obtain aerogels that are almost non-shrinking. Therefore, the current industrial preparation of aerogels almost does not directly use Kistler's initial method to prepare organic solvent gels.

[0004] The reason why Kistler did not use an organic solvent that is immiscible with water (such as n-butanol) to replace water is that the interfacial tension between the aqueous phase and the organic phase of the organic solvent will still cause the gel to shrink due to capillary forces during the solvent replacement process. Even though the interfacial tension between the aqueous phase and the organic phase of n-butanol can be lower than 1.5mN / m at normal pressure, which is much lower than water (about 72mN / m) and even much lower than ethanol (about 22mN / m), its interfacial tension will still cause the gel to shrink significantly during the replacement process, and this shrinkage is irreversible. In fact, in order to make the gel almost non-shrunk during the replacement process, the interfacial tension needs to be lower than 0.1mN / m. However, n-butanol is not immiscible with water under all temperature conditions. When it is higher than the critical solubility temperature of about 125°C, n-butanol can be soluble in water.

[0005] The present invention hopes to utilize the critical solution temperature of alcohol to propose a new method for preparing aerogel with relatively low cost and stable quality. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing aerogel based on hydrothermal solvent replacement, which has low raw material cost and simple preparation process.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is:

[0008] In the first step, the low-salt inorganic oxide hydrogel is first soaked in an acid solution.

[0009] According to the present invention, the inorganic oxide is amorphous silicon dioxide, aluminum oxide, titanium dioxide, zirconium dioxide, hafnium dioxide, and a combination of the above substances. The above inorganic oxide hydrogel can be obtained by hydrolysis of alcohol salts of corresponding elements, or by neutralization of inorganic salt solutions of corresponding elements to obtain the corresponding hydrogel. Whether the hydrogel is formed by hydrolysis of alcohol salts or neutralization of inorganic salts, a low-salt hydrogel can be obtained by washing with deionized water. Inorganic salts that account for less than 0.2% of the total hydrogel mass can be regarded as a low-salt hydrogel.

[0010] According to the present invention, the hydrogel may contain silicon dioxide, titanium dioxide, silicon carbide, zirconium dioxide, aluminum oxide, graphite, carbon black, iron oxide powder; and aluminum silicate fiber, glass fiber, pre-oxidized fiber, high silica glass fiber, polycrystalline mullite fiber, zirconium oxide fiber, aluminum oxide fiber, polyimide fiber, polyamide fiber, cellulose fiber, melamine foam. The composite hydrogel can be obtained by uniformly dispersing the above-mentioned powder and fiber materials in the sol stage, or injecting the above-mentioned fiber and foam materials as a substrate into the sol, and waiting for gelation. The size of the powder is preferably 0.5-8μm, and the fiber diameter is preferably 2-15μm.

[0011] According to the present invention, the acid solution is hydrochloric acid, hydrobromic acid, hydroiodic acid, or sulfuric acid solution. The increase in hydrogen ion concentration can significantly inhibit the decrease in the specific surface area of ​​the gel under hydrothermal conditions. The room temperature pH of the acid solution is directly related to the specific surface area of ​​the aerogel that is ultimately desired. If a gel with a high specific surface area is desired, for example, a gel with a specific surface area greater than 600 m 2 / g silica aerogel, the pH value of the acid solution at room temperature needs to be lower than 0. If aerogel with a high specific surface area is not required, for example, a specific surface area greater than 400m 2 / g silica aerogel, the pH value of the acid solution at room temperature is less than 2. If the specific surface area is only required to be greater than 200m 2 / g of silica aerogel, and keep the pH less than 7 at room temperature.

[0012] The second step is to heat the acid hydrogel after being soaked in acid solution.

[0013] Heating can further age the gel and increase the mechanical properties of the gel. It also prepares for the subsequent reduction of the interfacial tension between the organic solvent and water. The shorter the heating time, the better, in order to reduce the decrease in the specific surface area of ​​the gel.

[0014] In the third step, the acid gel is replaced by a hot solution.

[0015] According to the present invention, the solution comprises one or more combinations of n-butanol, isobutanol, sec-butanol, n-pentanol and pentanol isomers, and water. The above organic solvents are not miscible with water at room temperature, and have low solubility in water, generally less than 20g / 100g. The critical solubility temperature of the above organic solvent and water is less than 185°C.

[0016] According to the present invention, the temperature for heating the acid gel and the temperature of the solution for replacement are both not less than 10°C of the critical eutectic temperature of the organic solvent and water.

[0017] Because the solubility of organic solvent and water is much higher than that at room temperature, they are even miscible. Therefore, it is entirely possible to replace the gel at high temperature with the upper organic phase solution, which is layered at room temperature. Then, the replaced solution is cooled to room temperature, and the water is removed by draining the lower aqueous phase liquid.

[0018] In the fourth step, the water in the gel is removed by co-distillation.

[0019] The main purpose of removing water from the gel by azeotropic distillation is to promote the esterification reaction of alcohol on the surface of the inorganic oxide, thereby achieving hydrophobic modification of the surface, forming, for example, n-butoxy groups, and reducing surface hydroxyl groups. The water content of the liquid in the gel is preferably less than 1wt%.

[0020] The fifth step is to keep the low water content solvent containing the gel warm.

[0021] According to the present invention, the temperature is kept at 110-220° C. The main purpose is to increase the degree of gel surface modification, that is, to further promote the esterification reaction on the gel surface and reduce the number of surface hydroxyl groups.

[0022] The sixth step is to dry the gel to obtain aerogel.

[0023] According to the present invention, the drying method includes atmospheric pressure hot air drying, vacuum drying, subcritical drying, supercritical drying, and closed cycle spray drying.

[0024] In the seventh step, water vapor is passed through the dried aerogel or the aerogel is heated and dried to obtain a hydrophilic aerogel.

[0025] According to the present invention, the water vapor is unsaturated vapor at 100-200° C. The aerogel surface obtained after the sixth step has a large number of organic groups. Different from the traditional organic silicon surface modification, these organic groups can react with water vapor to generate alcohol and surface hydroxyl groups, thereby restoring the hydrophilicity of the aerogel.

[0026] According to the present invention, the heating and drying temperature is 250-600° C. If a higher ratio of organic groups needs to be removed, high temperature baking is a more effective method than steam treatment. DETAILED DESCRIPTION

[0027] The diluted sodium water glass (modulus 3.3) is neutralized with dilute sulfuric acid to obtain silica sol, and then the silica sol is diluted with water to a silica content of about 60 g / L. The silica sol is allowed to stand for gelation and aging. The gel is then washed with deionized water until the conductivity of the washed water is less than 200 μS / cm, and a 6wt% silica hydrogel is obtained.

[0028] Example 1

[0029] Silica hydrogel particles (3-5 mm) containing 6 wt% were immersed in 1 mol / L hydrochloric acid at room temperature for 24 hours. The acidic silica hydrogel was then placed in a sealed container and heated to 130°C. Then, a 130°C n-butanol solution with a water content of 20 wt% was poured into the sealed container. The n-butanol solution was drained after 12 hours. The n-butanol solution discharged this time was stratified after it cooled to room temperature.

[0030] Then, 130°C n-butanol with a water content of 1 wt% was poured into the sealed container and kept at 130°C for 12 hours. Then, the pressure in the sealed container was slowly reduced to normal pressure by discharging the mixed steam of n-butanol and water. After the pressure was reduced to normal pressure, the sealed container was closed again, and the temperature was raised to 215°C and kept at this temperature for 1 hour.

[0031] In the drying stage, the pressure of 1.4 MPa is maintained to discharge most of the liquid in the sealed container for subcritical drying. Then the pressure is slowly reduced to normal pressure, and finally the aerogel in the sealed container is vacuum dried.

[0032] The obtained aerogel has super hydrophobicity. If the obtained aerogel is placed in boiling water for 30 minutes, the aerogel will sink into the water; if the obtained aerogel is baked at 500°C for 1 hour, the aerogel has good water absorption.

[0033] Comparative Example 1

[0034] A 6 wt% silica hydrogel disc (10 mm thick, 75 mm in diameter) was immersed in a large amount of anhydrous n-butanol at room temperature. After 7 days, the gel broke into particles less than 10 mm, with a linear shrinkage of about 20%.

[0035] Example 2

[0036] Silica hydrogel particles (3-5 mm) containing 6 wt% are immersed in 1 mol / L hydrochloric acid at room temperature for 24 hours. The acidic silica hydrogel is then placed in a closed container and heated to 130°C. Then, a 130°C 1 wt% n-butanol solution is continuously injected into the bottom of the closed container, and mixed steam of n-butanol and water is discharged at the same time. When the absolute pressure in the closed container is less than 1.5 atmospheres, the mixed steam is stopped from being discharged, and the temperature is kept for 1 hour, and finally cooled to room temperature.

[0037] The obtained gel is dried by hot air at 250°C under normal pressure, and the gel has no obvious shrinkage during the drying process. The obtained aerogel has good water absorption.

[0038] Comparative Example 2

[0039] A 6wt% silica hydrogel disc (thickness 10mm, diameter 75mm) was heated to 93°C, and then immersed in a 20wt% n-butanol solution at 93°C, and water was removed by azeotropic distillation at normal pressure. Heating was stopped when the distilled gas reached 118°C. The gel was broken into particles less than 10mm, and the linear shrinkage was about 30%.

[0040] The obtained gel is dried by hot air at 250°C under normal pressure, and the gel particles do not shrink significantly during the drying process. The obtained aerogel has good water absorption.

[0041] Comparative Example 3

[0042] The pH value of the gel was 6, and the silica hydrogel particles (3-5 mm) containing 6 wt% were immersed in water with a pH value of 6, sealed in a hydrothermal reactor, heated to 130°C, and kept warm for 8 hours. After cooling to room temperature, the reactor was opened, and it was found that the original 3-5 mm particles were broken into particles less than 0.5 mm, and the appearance was a paste-like object.

[0043] Example 4

[0044] Pour the silica sol containing 6wt% of silicon dioxide into a 1cm thick glass fiber mat, and then let it stand to wait for gelation and aging. After the composite gel is soaked in 1mol / L hydrochloric acid for 24 hours, put the composite gel into a closed container and heat it to 130℃. Then, continuously inject a 130℃ 1wt% water content n-butanol solution into the bottom of the closed container, and discharge the mixed steam of n-butanol and water at the same time. When the absolute pressure in the closed container is less than 1.5 atmospheres, stop discharging the mixed steam, keep it warm for 1 hour, and finally continue to discharge the mixed steam until the pressure in the closed container drops to normal pressure.

[0045] After the pressure drops to normal pressure, 200°C unsaturated water vapor is introduced into the sealed container while the mixed gas is exhausted for 30 minutes. Finally, the composite material is taken out and hot air dried at 350°C under normal pressure to obtain a hydrophilic aerogel composite material.

[0046] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing aerogel based on hydrothermal modification, the method comprising the following steps: (a) firstly immersing a low-salt content inorganic oxide hydrogel in an acid solution; (b) heating the acidic hydrogel after being soaked in the acid solution; (c) replacing the acid gel with a hot solution; (d) removing water from the gel by azeotropic distillation; (e) keeping the low water content solvent containing the gel warm; (f) drying the gel to obtain an aerogel; (g) passing water vapor through the dried aerogel or heating and drying the aerogel to obtain a hydrophilic aerogel.

2. The method according to claim 1, wherein the inorganic oxide is amorphous silicon dioxide, aluminum oxide, titanium dioxide, zirconium dioxide, hafnium dioxide, and a combination of a plurality of the above substances.

3. The method according to claim 1, wherein the hydrogel may comprise silicon dioxide, titanium dioxide, silicon carbide, zirconium dioxide, aluminum oxide, graphite, carbon black, ferric oxide powder; and aluminum silicate fiber, glass fiber, pre-oxidized fiber, high silica glass fiber, polycrystalline mullite fiber, zirconium oxide fiber, aluminum oxide fiber, polyimide fiber, polyamide fiber, cellulose fiber, melamine foam.

4. The method according to claim 1, wherein the acid solution is hydrochloric acid, hydrobromic acid, hydroiodic acid or sulfuric acid solution.

5. The method according to claim 1, wherein the solution comprises a combination of one or more of n-butanol, isobutanol, sec-butanol, n-pentanol and pentanol isomers, and water.

6. The method according to claim 1, wherein the temperature of heating the acid gel and the temperature of the solution used for replacement are not less than 10°C of the critical solution temperature of the organic solvent and water.

7. The method according to claim 1, wherein the temperature is kept at 110-220°C.

8. The method according to claim 1, wherein the drying method comprises atmospheric hot air drying, vacuum drying, subcritical drying, supercritical drying, and closed cycle spray drying.

9. The method according to claim 1, wherein the water vapor is unsaturated steam at 100-200°C.

10. The method according to claim 1, wherein the heating and drying temperature is 250-600°C.