Treatment method of aluminum electrolysis waste cathode carbon block based on magnesium cementing material
Through the treatment method of magnesium gelling material, the problem of high-temperature fluorine-containing gas and fluorine-containing wastewater treatment in aluminum electrolytic waste cathode carbon blocks is solved, and harmless treatment and resource reuse is achieved, the process is simplified and the reagent consumption is reduced. , suitable for the preparation of building materials.
Patent Information
- Application Number
- CN202411133203.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art produces high-temperature fluorine-containing gas and fluorine-containing wastewater when dealing with aluminum electrolytic waste cathode carbon blocks. The process is complex and the amount of reagents is large, making it difficult to effectively reuse resources.
Using the treatment method based on magnesium gelling materials, fine particles and coarse particles are obtained through crushing and sieving, and acidification and halogenation are carried out to form magnesium gelling materials to avoid the generation of high-temperature fluorine-containing flue gas and fluorine-containing wastewater. The toxic elements are sealed for the preparation of building materials.
The harmless treatment of aluminum electrolytic waste cathode carbon block is realized, and the generation of high-temperature flue-containing flue gas and fluorine-containing wastewater is avoided. The process is simple, the reagent is used in small amounts, and harmful elements can be directly sealed and waste is used as building materials to achieve Reuse of resources.
Smart Images

Figure CN119019101A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of harmless treatment and recycling of waste cathode carbon blocks from aluminum electrolysis, and in particular relates to a treatment method for waste cathode carbon blocks from aluminum electrolysis based on a magnesium gelling material. Background Art
[0002] The cathode of aluminum electrolysis is deformed, bulged, and broken due to the erosion, scouring, and thermal stress of molten salt and aluminum liquid, thus producing waste cathode carbon blocks. Under normal circumstances, about 10kg of waste cathode carbon blocks are produced for every ton of electrolytic aluminum produced. Because it is immersed in a large amount of electrolyte during use, has a high fluorine content, and contains trace amounts of cyanide, it is listed in the national hazardous waste list and is a hazardous waste. At present, the domestic disposal methods for waste cathode carbon blocks from aluminum electrolysis are mainly stockpiling and incineration. The stockpiling method occupies land resources and poses safety hazards to the environment; the incineration disposal cost is high and cannot be comprehensively utilized, resulting in a waste of resources.
[0003] Aluminum electrolysis waste cathode carbon blocks contain carbon, aluminum fluoride, sodium fluoride, calcium fluoride, cryolite, alumina, nepheline and cyanide, etc. The carbon content accounts for 50-70%, and is highly graphitized. The remaining fluoride is an important component of the electrolyte and is a renewable resource. Therefore, the separation and recycling of waste cathode carbon blocks is not only conducive to the sustainable development of the electrolytic aluminum industry, but also can achieve good economic benefits.
[0004] At present, the recycling and treatment of waste cathode carbon blocks can be roughly divided into two technical routes: wet method and pyrotechnic method. The wet method can be further divided into flotation method, chemical method, flotation-chemical combined method, etc.; the pyrotechnic method includes high-temperature volatilization of fluorides and preparation of carbon materials, coordinated treatment and utilization of steel, cement clinker, thermal power generation, etc., rotary kiln calcination to produce cement raw materials, etc. Although there have been many studies on cathode disposal technology and industrialization, due to the influence of environmental protection policies or technical maturity, not many industrial operations have been achieved. In addition, due to the high chemical activity of fluorides and the fine embedded particle size, it is difficult to completely dissolve fluorides by wet method, and the pyrotechnic method is also prone to produce fluorine-containing solid waste, and there are problems such as the generation of a large amount of wastewater in secondary treatment and high equipment performance requirements for treatment at high temperature.
[0005] In response to the above problems, the prior art has proposed a series of waste cathode carbon block treatment processes based on sulfuric acid roasting. For example, patent CN201910373382.5 discloses a method for recycling waste cathode carbon blocks from aluminum electrolytic cells. The waste cathode carbon block raw materials of aluminum electrolytic cells are crushed, pulverized, and ball-milled to form powders, and then hydrogen peroxide is added to remove cyanide; concentrated sulfuric acid is then added to react to generate hydrogen fluoride gas, and 25-40% hydrofluoric acid products are obtained after cyclic absorption; carbon powder is made and can be recycled as a raw material for processing new cathodes; a large amount of sodium sulfate in the filtrate is concentrated to obtain sodium sulfate crystals. However, the process of treating waste cathode carbon blocks in this patent is complicated, and concentrated sulfuric acid equivalent to 5-7 times the mass of the waste cathode carbon blocks needs to be added to treat fluorine-containing substances.
[0006] Therefore, there is an urgent need for a method for treating spent cathode carbon blocks from aluminum electrolysis that does not produce high-temperature fluorine-containing gas and fluorine-containing wastewater during the treatment process and has a simple process and a small amount of reagents to solve the above problems. Summary of the invention
[0007] In order to solve the above technical problems, the present invention proposes a method for treating aluminum electrolysis waste cathode carbon blocks based on magnesium gelling material.
[0008] To achieve the above object, the present invention provides the following technical solutions:
[0009] The present invention provides a method for treating aluminum electrolysis waste cathode carbon blocks based on magnesium gel material, comprising the following steps:
[0010] (1) crushing and screening the waste cathode carbon blocks from aluminum electrolysis to obtain fine particles and coarse particles;
[0011] (2) acidifying the fine particles obtained in step (1) to obtain an acid slurry; halogenating part of the coarse particles, and then mixing them with active MgO to obtain a halogen slurry;
[0012] (3) The acid slurry, brine slurry, and remaining coarse particles obtained in step (2) are mixed with dead-burned MgO to obtain a magnesia cementitious material; the remaining coarse particles can be added in the form of slurry or particles.
[0013] The term "dead burned MgO" is formed by calcining ordinary magnesium oxide at high temperature, usually at a temperature of 1500-2000°C. The term "active MgO" refers to magnesium oxide with higher chemical activity after special treatment (such as calcination, fine grinding, etc.), which usually has high purity and fine particle size.
[0014] Preferably, in step (1), the particle size of the fine particles is less than 5 mm.
[0015] Preferably, in step (2), the particle size of the coarse particles is 5 to 10 mm.
[0016] Preferably, in step (2), the acidulant comprises a phosphoric acid solution, the acidulant temperature is 30° C., and the acidulant time is more than 2 hours; and the volume mass ratio of the acidulant to the fine particles is (0.3-1):(0.6-2).
[0017] Preferably, in step (2), the halogenating agent comprises one or more of old brine and bittern, and the halogenating time is more than 1 day; the volume mass ratio of the halogenating agent to some coarse particles is (1-5):(5-10).
[0018] Preferably, in step (2), the mass ratio of the part of coarse particles to the active MgO is 1:0.5.
[0019] Preferably, in step (3), the particle size of the remaining coarse particles is 10 to 50 mm.
[0020] Preferably, in step (3), the mass ratio of the acid slurry, the brine slurry, the remaining coarse particles and the dead-burned MgO is 1:(1-2):(3-5):(0.5-0.7).
[0021] The present invention provides a magnesium gelling material obtained by the method for treating aluminum electrolysis waste cathode carbon blocks based on magnesium gelling material as described in the above technical solution.
[0022] The present invention also provides the application of the magnesium cementitious material described in the above technical solution in the field of construction.
[0023] Compared with the prior art, the present invention has the following advantages and technical effects:
[0024] The present invention performs particle size classification screening on waste cathode carbon blocks, acidifies particles with fine particle sizes, and halogenates part or all of coarse particles. The surfaces and pores of the coarse particles are enriched with halogenating agents through halogenation, and then react with active MgO to form a magnesium cement filling layer and a coating layer to prevent the leakage of toxic elements in the coarse particles. Finally, the acidified fine particles, the halogenated coarse particles and the dead-burned MgO are mixed and reacted to form magnesium cement. The formed magnesium cement can coat the unhalogenated coarse particles to prevent the leakage of toxic elements therein, thereby realizing the direct sealing of harmful elements in the waste cathode carbon blocks of aluminum electrolysis, without generating high-temperature fluorine-containing flue gas and fluorine-containing wastewater, and the process is simple and the amount of reagents used is small.
[0025] The present invention does not generate high-temperature fluorine-containing flue gas and fluorine-containing waste water during the process of treating spent cathode carbon blocks from aluminum electrolysis. The harmful elements in the spent cathode carbon blocks from aluminum electrolysis are directly sealed and used for preparing building materials. While ensuring that the harmful elements are not leaked, the light weight and carbon activity of the spent cathode carbon blocks from aluminum electrolysis are utilized as beneficial components of building materials, thereby realizing the solid waste utilization of spent cathode carbon blocks from aluminum electrolysis. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0027] Figure 1 This is a process flow chart of the method for treating aluminum electrolysis waste cathode carbon blocks based on magnesium gelling material in Example 2. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0030] The embodiment of the present invention provides a method for treating aluminum electrolysis waste cathode carbon blocks based on magnesium gelling material, comprising the following steps:
[0031] (1) crushing and screening the waste cathode carbon blocks from aluminum electrolysis to obtain fine particles and coarse particles;
[0032] (2) acidifying the fine particles obtained in step (1) to obtain an acid slurry; halogenating part of the coarse particles, and then mixing them with active MgO to obtain a halogen slurry;
[0033] (3) The acid slurry, brine slurry, and remaining coarse particles obtained in step (2) are mixed with dead-burned MgO to obtain a magnesia cementitious material; the remaining coarse particles can be added in the form of slurry or particles.
[0034] In a preferred embodiment, in step (1), the crushing is: crushing the aluminum electrolysis waste cathode carbon blocks to less than 5 cm. The present invention separates the crushed aluminum electrolysis waste cathode carbon blocks into fine particles with a particle size of less than 5 mm and coarse particles with a particle size of 5 to 10 mm and 10 to 50 mm by screening. The present invention obtains particles of different particle sizes by crushing and screening the aluminum electrolysis waste cathode carbon blocks. The fine particles can be used as a modifier for magnesium cementitious materials, and the coarse particles can be used as aggregates to prepare magnesium cementitious materials.
[0035] In a preferred embodiment, in step (1), the particle size of the fine particles is less than 5 mm.
[0036] In a preferred embodiment, in step (2), the acidifying agent comprises a phosphoric acid solution, the acidifying temperature is 30°C, the acidifying time is more than 2 hours, preferably 12 to 24 hours; the volume mass ratio of the acidifying agent to the fine particles is (0.3-1):(0.6-2), preferably 0.4:0.8. The fine particles in the present invention account for a relatively small proportion, and most of the fluorine-containing substances in the fine particles can be dissolved in the solution through acidification, while only a trace amount of fluorine-containing substances (very small amount) is discharged. At the same time, the fine particles as the raw material of the gelling material can fix a large amount of fluorine-containing substances in the coarse particles, thereby realizing the reuse of the waste cathode material.
[0037] In a preferred embodiment, in step (2), the particle size of the coarse particles is 5 to 10 mm.
[0038] In a preferred embodiment, in step (2), the halogenating agent comprises one or more of old brine and bittern, and the old brine comprises the magnesium-containing solution remaining after seawater, salt lake or underground brine is extracted (extracting potassium, lithium, sodium and other salts); the halogenation time is more than 1 day, preferably 4 to 7 days; the volume mass ratio of the halogenating agent to part of the coarse particles is (1-5): (5-10), preferably 3: 6. The present invention enriches the surface and pores of the coarse particles with the halogenating agent through halogenation, so that it can react with active MgO to form a magnesium cement filling layer and a coating layer, thereby preventing the leakage of toxic elements in the coarse particles.
[0039] In a preferred embodiment, in step (2), the mass ratio of the part of coarse particles to the active MgO is 1:0.5. The present invention prevents the leakage of toxic elements in the part of coarse particles by mixing the part of halogenated coarse particles with the active MgO to form a magnesium cement filling layer and a coating layer.
[0040] In a preferred embodiment, in step (2), the mixing time is 5 min to 4 h.
[0041] In a preferred embodiment, in step (3), the particle size of the remaining coarse particles is 10 to 50 mm.
[0042] In a preferred embodiment, in step (3), the mass ratio of the acid slurry, the brine slurry, the remaining coarse particles and the dead-burned MgO is 1:(1-2):(3-5):(0.5-0.7); the remaining coarse particles are added in the form of slurry or granules. In the present invention, when the remaining coarse particles are added in the form of slurry, the preparation method is the same as the process of making part of the coarse particles into brine slurry; when the remaining coarse particles are added in the form of granules, the dead-burned MgO can react with the phosphoric acid in the acid slurry to form magnesia cement, thereby forming a coating for the remaining coarse particles, preventing the leakage of toxic elements in the remaining coarse particles.
[0043] In a preferred embodiment, in step (3), the mixing time is 5 min to 4 h.
[0044] The present invention provides a magnesium gelling material obtained by the method for treating aluminum electrolysis waste cathode carbon blocks based on magnesium gelling material as described in the above technical solution.
[0045] The present invention also provides the application of the magnesium cementitious material described in the above technical solution in the field of construction.
[0046] In a preferred embodiment, the magnesium cementitious material is used to prepare enclosure structures or curbstones.
[0047] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources.
[0048] Example 1
[0049] A method for treating aluminum electrolysis waste cathode carbon blocks based on magnesium gel material, the specific steps are as follows:
[0050] (1) crushing the waste cathode carbon blocks from aluminum electrolysis to less than 5 cm, and then sieving them to obtain fine particles with a particle size of less than 5 mm, some coarse particles with a particle size of 5 to 10 mm, and the remaining coarse particles with a particle size of 10 to 50 mm;
[0051] (2) mixing the fine particles obtained in step (1) with a phosphoric acid solution in a dosage ratio of 0.8 kg:0.4 L, and acidifying at 30° C. for 12 h to obtain an acid slurry;
[0052] (3) soaking part of the coarse particles with a particle size of 5 to 10 mm obtained in step (1) in old brine for 4 days, and then mixing and reacting with active MgO for 2 hours to obtain brine slurry; wherein the dosage ratio of part of the coarse particles to old brine is 6 kg:3 L, the mass ratio of active MgO to part of the coarse particles is 0.5:1, and the old brine is the magnesium-containing solution remaining after ore extraction from seawater;
[0053] (4) The acid slurry obtained in step (2), the brine slurry obtained in step (3), the remaining coarse particles with a particle size of 10 to 50 mm obtained in step (1), and dead-burned MgO are mixed in a mass ratio of 1:1:5:0.5 for 2 hours to obtain a magnesia cementitious material.
[0054] Example 2
[0055] A method for treating aluminum electrolysis waste cathode carbon blocks based on magnesium gel material, the process flow is shown in Figure 1 , the specific steps are as follows:
[0056] (1) crushing the waste cathode carbon blocks from aluminum electrolysis to less than 5 cm, and then sieving them to obtain fine particles with a particle size of less than 5 mm, some coarse particles with a particle size of 5 to 10 mm, and the remaining coarse particles with a particle size of 10 to 50 mm;
[0057] (2) mixing the fine particles obtained in step (1) with a phosphoric acid solution in a dosage ratio of 0.6 kg:0.3 mL, and acidifying at 30° C. for 12 h to obtain an acid slurry;
[0058] (3) soaking part of the coarse particles with a particle size of 5 to 10 mm obtained in step (1) in old brine for 4 days, and then mixing and reacting with active MgO for 4 hours to obtain a brine slurry of part of the coarse particles; wherein the dosage ratio of the part of the coarse particles to the old brine is 10 kg:5 L, the mass ratio of the active MgO to the part of the coarse particles is 0.5:1, and the old brine is the magnesium-containing solution remaining after the seawater is extracted;
[0059] (4) soaking the remaining coarse particles with a particle size of 10 to 50 mm obtained in step (1) in old brine for 4 days, and then mixing and reacting with active MgO for 2 hours to obtain a brine slurry of the remaining coarse particles; wherein the dosage ratio of the remaining coarse particles to the old brine is 10 kg:5 L, the mass ratio of the active MgO to the remaining coarse particles is 0.5:1, and the old brine is the magnesium-containing solution remaining after ore extraction from seawater;
[0060] (5) The acid slurry obtained in step (2), the partial coarse-grained brine slurry obtained in step (3), the remaining coarse-grained brine slurry obtained in step (4), and dead-burned MgO are mixed in a mass ratio of 1:2:3:0.7 for 0.5 h to obtain a magnesia cementitious material.
[0061] The compressive strength of the cementitious material obtained in Example 1-2 was tested, and the results are shown in Table 1.
[0062] Table 1 Properties of the gelling materials obtained in Examples 1-2
[0063]
[0064] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for treating aluminum electrolysis waste cathode carbon blocks based on magnesium gelled materials, characterized in that: The following steps are involved: (1) crushing and screening the waste cathode carbon blocks from aluminum electrolysis to obtain fine particles and coarse particles; (2) acidifying the fine particles obtained in step (1) to obtain an acid slurry; halogenating part of the coarse particles, and then mixing them with active MgO to obtain a halogen slurry; (3) The acid slurry, brine slurry, and remaining coarse particles obtained in step (2) are mixed with dead-burned MgO to obtain a magnesia cementitious material; the remaining coarse particles can be added in the form of slurry or particles.
2. The method for treating aluminum electrolysis waste cathode carbon blocks based on magnesium gelling material according to claim 1 is characterized in that: In step (1), the particle size of the fine particles is less than 5 mm.
3. The method for treating aluminum electrolysis waste cathode carbon blocks based on magnesium gelling material according to claim 1, characterized in that: In step (2), the particle size of the coarse particles is 5 to 10 mm.
4. The method for treating aluminum electrolysis waste cathode carbon blocks based on magnesium gelling material according to claim 1, characterized in that: In step (2), the acidulant for acidification includes a phosphoric acid solution, the acidification temperature is 30° C., and the acidification time is more than 2 hours; the volume mass ratio of the acidulant to the fine particles is (0.3-1):(0.6-2).
5. The method for treating aluminum electrolysis waste cathode carbon blocks based on magnesium gelling material according to claim 1, characterized in that: In step (2), the halogenating agent for halogenation includes one or more of old brine and bittern, and the halogenation time is more than 1 day; the volume mass ratio of the halogenating agent to some coarse particles is (1-5):(5-10).
6. The method for treating aluminum electrolysis waste cathode carbon blocks based on magnesium gelling material according to claim 1, characterized in that: In step (2), the mass ratio of the part of coarse particles to the active MgO is 1:0.
5.
7. The method for treating aluminum electrolysis waste cathode carbon blocks based on magnesium gelling material according to claim 1, characterized in that: In step (3), the particle size of the remaining coarse particles is 10 to 50 mm.
8. The method for treating aluminum electrolysis waste cathode carbon blocks based on magnesium gelling material according to claim 1, characterized in that: In step (3), the mass ratio of the acid slurry, the brine slurry, the remaining coarse particles and the dead-burned MgO is 1:(1-2):(3-5):(0.5-0.7).
9. The magnesium gelled material obtained by the method for treating spent cathode carbon blocks from aluminum electrolysis based on magnesium gelled material according to any one of claims 1 to 8.
10. Use of the magnesium cementitious material according to claim 9 in the field of construction.
Citation Information
Patent Citations
Recycling method for waste cathode carbon blocks of electrolytic aluminum electrolysis cell
CN110127649A
Treatment method and application of aluminum electrolysis waste cathode carbon block
CN114535260A
Method for preparing magnesium material by taking waste cathode carbon block in waste aluminum electrolysis as raw material