Mud-resistant wet-mixed mortar plasticity retaining agent and preparation method thereof
By combining specific raw materials to form a colloidal water storage system and a colloidal system, the problem of hydration and expansion of clay minerals in manufactured sand is solved, improving the plasticity and construction quality of wet-mixed mortar and enhancing its anti-mud properties.
Patent Information
- Application Number
- CN202411121764.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
Weathered shale clay minerals in manufactured sand are prone to hydration and expansion when in contact with water, which leads to an increase in the water consumption of wet-mixed mortar, adsorption of admixtures, reduced plasticity and workability, and affects construction quality.
A stable colloidal water storage system is formed using raw materials such as water-based acrylic emulsion, polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate, and alkylphenol polyoxyethylene ether to prevent clay minerals from contacting water. Combined with polyvinyl alcohol and nano silica, a stable colloidal system is formed, which improves bonding strength and durability.
It significantly reduces hydration expansion, prolongs the plasticity retention time, maintains the plasticity and workability of wet-mixed mortar, and improves bonding strength and construction quality.
Smart Images

Figure BDA0004995299420000081 
Figure BDA0004995299420000082 
Figure BDA0004995299420000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of building material additives, in particular to an anti-mud type wet-mix mortar plasticizer and a preparation method thereof. Background Art
[0002] As an important building material, wet-mixed mortar has been widely used in modern construction, and its performance directly affects the quality and safety of construction projects. Nowadays, the wet-mixed mortar used in the construction process is generally premixed mortar. After the wet-mixed mortar is prepared at the mixing station, it often has to go through long-distance transportation and long-term storage before it is finally used in construction. At present, it is generally chosen to add a certain amount of admixtures during the preparation of wet-mixed mortar to reduce the impact of long-distance transportation and long-term storage on the performance of wet-mixed mortar.
[0003] As people's environmental awareness increases, many mixing stations have begun to use machine-made sand instead of river sand as the raw material for wet-mixed mortar. However, in the actual application of machine-made sand, mixing stations have found that when machine-made sand is used as the raw material for wet-mixed mortar, since machine-made sand is made by removing soil from rocks, mine tailings and other sand-making materials, and then undergoing mechanical crushing and screening, some machine-made sand may contain more weathered shale clay minerals. These clay minerals are very likely to hydrate and expand when in contact with water, significantly increasing the water consumption of wet-mixed mortar, and are very likely to absorb admixtures in wet-mixed mortar, resulting in a decrease in the plasticity and working performance of wet-mixed mortar, and even causing problems such as stratification and water seepage of wet-mixed mortar, which seriously affects the construction quality and use effect of wet-mixed mortar. Therefore, it is of great practical significance and application value to develop an anti-mud wet-mixed mortar plasticizer that can resist the hydration and expansion of clay minerals in machine-made sand and maintain the plasticity and working performance of wet-mixed mortar. Summary of the invention
[0004] In order to reduce the negative impact of weathered shale clay minerals on maintaining the plasticity and working performance of wet-mixed mortar, the present application provides an anti-mud wet-mixed mortar plasticizer and a preparation method thereof. The present application found in the study that by mixing water-based acrylic emulsion, polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate, and alkylphenol polyoxyethylene ether in a certain proportion and adding an appropriate amount of polyvinyl alcohol and nano-silica, the plasticity and anti-mud performance of wet-mixed mortar can be effectively improved.
[0005] In the first aspect, the present application provides an anti-mud wet-mix mortar plasticizer that adopts the following technical solution: A mud-resistant wet-mix mortar plasticizer comprises the following raw materials in parts by weight: 15-20 parts of water-based acrylic emulsion, 5-10 parts of polyglycerol ricinoleate, 5-8 parts of propylene glycol alginate, 3-5 parts of sodium n-octane sulfonate, and 0.5-1.5 parts of alkylphenol polyoxyethylene ether.
[0006] In the above technical scheme, this application adopts water-based acrylic emulsion, polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate, and alkylphenol polyoxyethylene ether, which are five specific raw materials, and are mixed in a certain proportion to prepare an anti-mud wet-mixed mortar plasticizer. The water-based acrylic emulsion can effectively adhere to the surface of the wet-mixed mortar, enhance the adhesion between the raw materials, adjust the fluidity and water retention of the mortar, and improve the bonding strength and durability; polyglycerol ricinoleate has good dispersibility and adhesion, increases the consistency and viscosity in the wet-mixed mortar, and reduces water bleeding and stratification; propylene glycol alginate has water retention and thickening properties, effectively improves the viscosity and plasticity of the wet-mixed mortar, and enhances the anti-mud performance; sodium n-octane sulfonate and alkylphenol polyoxyethylene ether are surfactants, which can reduce the surface tension between the raw materials, improve wettability and dispersibility, control the internal bubble generation, maintain a stable internal air content, and improve the plastic performance.
[0007] The present application compounded the above five raw materials. Firstly, the five materials can form a stable colloidal water storage system in the wet-mixed mortar, form a protective film in the wet-mixed mortar, and effectively prevent the clay minerals in the machine-mixed sand from direct contact with water, thereby significantly reducing the occurrence of hydration expansion, significantly prolonging the plastic preservation time of the mortar, and maintaining the plasticity and working performance of the wet-mixed mortar for a long time; then the synergistic effect of the five materials promotes the uniform dispersion of the components in the mortar. This uniform dispersion also makes the distribution of the clay minerals in the machine-mixed sand in the mortar more uniform, further reducing its influence on the mortar performance, and avoiding the stratification and water seepage of the mortar; thirdly, the colloidal water storage system can effectively fill the gaps in the mortar, reduce the surface tension of the mortar, and improve the bonding strength and durability of the wet-mixed mortar.
[0008] Preferably, the preparation method of the aqueous acrylic emulsion comprises the following steps: S1: Take 60-70 parts of water, 10-20 parts of acrylate, 5-10 parts of butyl methacrylate, 5-10 parts of styrene, 5-10 parts of maleic acid, 1-2 parts of silane coupling agent, 1-2 parts of emulsifier, and 1-2 parts of initiator; S2: premix 50%-60% by mass of water and 40%-50% by mass of emulsifier, then add acrylate, butyl methacrylate, styrene, maleic acid, and silane coupling agent, mix well, and stir until milky white; S3: In a nitrogen atmosphere, the temperature is raised to 70-80° C., an initiator, the remaining water and the remaining emulsifier are added, and the mixture is stirred for 3-4 hours to obtain a water-based acrylic emulsion.
[0009] Preferably, the emulsifier is sodium dodecyl sulfate, and the initiator is ammonium persulfate.
[0010] In the above technical scheme, the present application forms a high molecular weight water-based acrylic emulsion by selecting specific raw materials, thereby further improving the stability and performance of the water-based acrylic emulsion, thereby further improving the plasticity and mud resistance of the wet-mixed mortar.
[0011] Preferably, the anti-mud wet-mix mortar plasticizer also includes 5-10 parts of polyvinyl alcohol.
[0012] In the above technical solution, by further adding polyvinyl alcohol, polyvinyl alcohol can effectively improve the adhesion and bonding force of wet-mixed mortar, and further improve the anti-mud performance of wet-mixed mortar. Polyvinyl alcohol has good water solubility, and can form a stable colloid system in wet-mixed mortar with other components in wet-mixed mortar plasticizer, thereby enhancing the adhesion and bonding force of wet-mixed mortar. At the same time, polyvinyl alcohol can also form chemical bonds with cement particles in wet-mixed mortar, further increasing the bonding strength and durability of wet-mixed mortar.
[0013] Preferably, the anti-mud wet-mix mortar plasticizer also includes 2-5 parts of nano-silicon dioxide.
[0014] In the above technical solution, nano-silicon dioxide is further added. Nano-silicon dioxide has a large specific surface area and excellent dispersibility, and can form a tiny network structure in the wet-mixed mortar, thereby further improving the strength and durability of the wet-mixed mortar. At the same time, nano-silicon dioxide can also effectively absorb moisture in the wet-mixed mortar, reduce the migration and evaporation of moisture, and thus enhance the water retention of the wet-mixed mortar.
[0015] Preferably, the anti-mud wet-mix mortar plasticizer also includes 5-10 parts of polyvinyl alcohol and 2-5 parts of nano-silicon dioxide.
[0016] In the above technical solution, the present application can further optimize the performance of wet-mixed mortar by simultaneously adding polyvinyl alcohol and nano-silicon dioxide to the anti-mud wet-mixed mortar plasticizer. The synergistic effect of nano-silicon dioxide and polyvinyl alcohol can cooperate with other raw materials in the plasticizer to form a more stable colloidal system in the wet-mixed mortar. This system can not only better prevent the direct contact between clay minerals in machine-made sand and water, and reduce the occurrence of hydration expansion, but also make the wet-mixed mortar easier to operate and control during construction, further improving the construction quality and use effect of the wet-mixed mortar.
[0017] In the second aspect, the present application provides a method for preparing a mud-resistant wet-mix mortar plasticizer using the following technical solution: A method for preparing a mud-resistant wet-mix mortar plasticizer comprises: taking an aqueous acrylic emulsion, sequentially adding polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate, and alkylphenol polyoxyethylene ether, and stirring and mixing them evenly to obtain the mud-resistant wet-mix mortar plasticizer.
[0018] Preferably, the method comprises: pre-mixing water-based acrylic emulsion and polyvinyl alcohol, and then sequentially adding polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate, and alkylphenol polyoxyethylene ether, and stirring and mixing evenly to obtain a mud-resistant wet-mix mortar plasticizer.
[0019] Preferably, the method comprises: pre-mixing water-based acrylic emulsion and nano-silica, ultrasonically treating for 10-20 minutes, and then sequentially adding polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate, and alkylphenol polyoxyethylene ether, and stirring and mixing evenly to obtain a mud-resistant wet-mix mortar plasticizer.
[0020] Preferably, the method comprises: pre-mixing water-based acrylic emulsion, polyvinyl alcohol and nano-silica, ultrasonically treating for 10-20 minutes, and then sequentially adding polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate and alkylphenol polyoxyethylene ether, and stirring and mixing evenly to obtain a mud-resistant wet-mix mortar plasticizer.
[0021] In the above technical scheme, the present application provides a flexible and changeable method for preparing an anti-mud type wet-mix mortar plasticizer. The present application can flexibly adjust the raw material ratio and preparation process of the plasticizer according to different engineering requirements and usage environment, thereby preparing an anti-mud type wet-mix mortar plasticizer with different usage effects.
[0022] In summary, this application includes the following beneficial technical effects: 1. The anti-mud wet-mix mortar plasticizer provided in the present application successfully solves the problem of the influence of weathered shale clay minerals on the performance of wet-mix mortar through the combination of water-based acrylic emulsion, polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate, and alkylphenol polyoxyethylene ether. The plasticizer not only has good plasticity and anti-mud properties, but also can significantly improve the strength and durability of wet-mix mortar, providing a more reliable material guarantee for construction projects.
[0023] 2. The anti-mud wet-mix mortar plasticizer provided in the present application can further be added with polyvinyl alcohol and nano-silicon dioxide, which can further enhance the stability of the colloid system formed by the plasticizer, thereby making the wet-mix mortar easier to operate and control during construction, further improving the construction quality and use effect of the wet-mix mortar, and making the anti-mud wet-mix mortar plasticizer provided in the present application applicable to more construction requirements. DETAILED DESCRIPTION
[0024] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0025] Example 1 A mud-resistant wet-mix mortar plasticizer comprises 15kg of water-based acrylic emulsion, 10kg of polyglycerol ricinoleate, 5kg of propylene glycol alginate, 3kg of sodium n-octane sulfonate and 0.5kg of alkylphenol polyoxyethylene ether.
[0026] Among them, polyglycerol ricinoleate was purchased from Guangdong Mingtong Biotechnology Co., Ltd.
[0027] Among them, propylene glycol alginate was purchased from Hebei Hongtao Bioengineering Co., Ltd.
[0028] Among them, sodium n-octane sulfonate was purchased from Wuhan Shuer Biotechnology Co., Ltd., product number: HH8250BEY6W1.
[0029] Among them, alkylphenol polyoxyethylene ether was purchased from Foshan Keerle Building Materials Co., Ltd., model: NP-9.
[0030] The method for preparing the anti-mud wet-mix mortar plasticizer comprises the following steps: Step 1: Place the water-based acrylic emulsion in a stirring container, add polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate and alkylphenol polyoxyethylene ether into the stirring container in sequence, and turn on the stirrer to stir thoroughly until the mixture presents a stable milky white color without stratification.
[0031] Step 2: Filter the mixture to remove undissolved large particles and impurities to obtain a liquid anti-mud wet-mix mortar plasticizer.
[0032] Wherein, the preparation method of water-based acrylic emulsion comprises the following steps: Step S1: Take 60 kg of water, 10 kg of acrylate, 5 kg of butyl methacrylate, 10 kg of styrene, 5 kg of maleic acid, 1 kg of silane coupling agent, 1 kg of sodium dodecyl sulfonate, and 1 kg of ammonium persulfate.
[0033] Step S2: premix 50% by mass of water and 40% by mass of an emulsifier, then add acrylate, butyl methacrylate, styrene, maleic acid, and a silane coupling agent, mix well, and stir until milky white.
[0034] Step S3: In a nitrogen atmosphere, the temperature is raised to 70° C., an initiator, the remaining water and the remaining emulsifier are added, and the mixture is stirred for 4 hours to obtain a water-based acrylic emulsion.
[0035] Example 2 A mud-resistant wet-mix mortar plasticizer, which is different from Example 1 in that it includes 20kg of water-based acrylic emulsion, 5kg of polyglycerol ricinoleate, 8kg of propylene glycol alginate, 5kg of sodium n-octane sulfonate, and 1.5kg of alkylphenol polyoxyethylene ether.
[0036] The method for preparing the anti-mud wet-mix mortar plasticizer comprises the following steps: Step 1: Place the water-based acrylic emulsion in a stirring container, add polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate and alkylphenol polyoxyethylene ether into the stirring container in sequence, and turn on the stirrer to stir thoroughly until the mixture presents a stable milky white color without stratification.
[0037] Step 2: Filter the mixture to remove undissolved large particles and impurities to obtain a liquid anti-mud wet-mix mortar plasticizer.
[0038] Wherein, the preparation method of water-based acrylic emulsion comprises the following steps: Step S1: Take 70 kg of water, 20 kg of acrylate, 10 kg of butyl methacrylate, 5 kg of styrene, 10 kg of maleic acid, 2 kg of silane coupling agent, 2 kg of sodium dodecyl sulfonate, and 2 kg of ammonium persulfate.
[0039] Step S2: premix 60% by mass of water and 50% by mass of an emulsifier, then add acrylate, butyl methacrylate, styrene, maleic acid, and a silane coupling agent, mix well, and stir until milky white.
[0040] Step S3: In a nitrogen atmosphere, the temperature is raised to 80° C., an initiator, the remaining water and the remaining emulsifier are added, and the mixture is stirred for 3 hours to obtain a water-based acrylic emulsion.
[0041] Example 3 A mud-resistant wet-mix mortar plasticizer, which is different from Example 1 in that it includes 18kg of water-based acrylic emulsion, 7kg of polyglycerol ricinoleate, 6kg of propylene glycol alginate, 4kg of sodium n-octane sulfonate, and 1kg of alkylphenol polyoxyethylene ether.
[0042] The method for preparing the anti-mud wet-mix mortar plasticizer comprises the following steps: Step 1: Place the water-based acrylic emulsion in a stirring container, add polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate and alkylphenol polyoxyethylene ether into the stirring container in sequence, and turn on the stirrer to stir thoroughly until the mixture presents a stable milky white color without stratification.
[0043] Step 2: Filter the mixture to remove undissolved large particles and impurities to obtain a liquid anti-mud wet-mix mortar plasticizer.
[0044] Wherein, the preparation method of water-based acrylic emulsion comprises the following steps: Step S1: Take 65 kg of water, 15 kg of acrylate, 8 kg of butyl methacrylate, 8 kg of styrene, 8 kg of maleic acid, 1.5 kg of silane coupling agent, 1.5 kg of sodium dodecyl sulfonate, and 1.5 kg of ammonium persulfate.
[0045] Step S2: premix 55% by mass of water and 45% by mass of an emulsifier, then add acrylate, butyl methacrylate, styrene, maleic acid, and a silane coupling agent, mix well, and stir until milky white.
[0046] Step S3: Under a nitrogen atmosphere, the temperature was raised to 75° C., an initiator, the remaining water and the remaining emulsifier were added, and the mixture was stirred for 3.5 hours to obtain a water-based acrylic emulsion.
[0047] Example 4 A mud-resistant wet-mix mortar plasticizer, which is different from Example 1 in that it also includes 5kg of polyvinyl alcohol.
[0048] The method for preparing the anti-mud wet-mix mortar plasticizer comprises the following steps: Step 1: Place water-based acrylic emulsion and polyvinyl alcohol in a stirring container, stir evenly, then add polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate and alkylphenol polyoxyethylene ether into the stirring container in sequence, and turn on the stirrer to stir thoroughly until the mixture presents a stable milky white color without stratification.
[0049] Step 2: Filter the mixture to remove undissolved large particles and impurities to obtain a liquid anti-mud wet-mix mortar plasticizer.
[0050] Example 5 A mud-resistant wet-mix mortar plasticizer, which is different from Example 1 in that it also includes 10 kg of polyvinyl alcohol.
[0051] The method for preparing the anti-mud wet-mix mortar plasticizer comprises the following steps: Step 1: Place water-based acrylic emulsion and polyvinyl alcohol in a stirring container, stir evenly, then add polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate and alkylphenol polyoxyethylene ether into the stirring container in sequence, and turn on the stirrer to stir thoroughly until the mixture presents a stable milky white color without stratification.
[0052] Step 2: Filter the mixture to remove undissolved large particles and impurities to obtain a liquid anti-mud wet-mix mortar plasticizer.
[0053] Example 6 A mud-resistant wet-mix mortar plasticizer, which is different from Example 1 in that it also includes 2kg of nano silicon dioxide.
[0054] The method for preparing the anti-mud wet-mix mortar plasticizer comprises the following steps: Step 1: Place the aqueous acrylic emulsion and nano-silica in a stirring container, stir and then perform ultrasonic treatment at 20 kHz for 20 minutes, then add polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate and alkylphenol polyoxyethylene ether into the stirring container in sequence, and turn on the stirrer to stir thoroughly until the mixture presents a stable milky white color without stratification.
[0055] Step 2: Filter the mixture to remove undissolved large particles and impurities to obtain a liquid anti-mud wet-mix mortar plasticizer.
[0056] Example 7 A mud-resistant wet-mix mortar plasticizer, which is different from Example 1 in that it also includes 5kg of nano silicon dioxide.
[0057] The method for preparing the anti-mud wet-mix mortar plasticizer comprises the following steps: Step 1: Place the aqueous acrylic emulsion and nano-silica in a stirring container, stir and then perform ultrasonic treatment at 25 kHz for 10 minutes, then add polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate and alkylphenol polyoxyethylene ether into the stirring container in sequence, and turn on the stirrer to stir thoroughly until the mixture presents a stable milky white color without stratification.
[0058] Step 2: Filter the mixture to remove undissolved large particles and impurities to obtain a liquid anti-mud wet-mix mortar plasticizer.
[0059] Example 8 A mud-resistant wet-mix mortar plasticizer, which is different from Example 1 in that it also includes 5kg of polyvinyl alcohol and 5kg of nano silicon dioxide.
[0060] The method for preparing the anti-mud wet-mix mortar plasticizer comprises the following steps: Step 1: Place water-based acrylic emulsion, polyvinyl alcohol and nano-silica in a stirring container, stir and then perform ultrasonic treatment at 25 kHz for 10 minutes, then add polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate and alkylphenol polyoxyethylene ether into the stirring container in sequence, and turn on the stirrer to stir thoroughly until the mixture presents a stable milky white color without stratification.
[0061] Step 2: Filter the mixture to remove undissolved large particles and impurities to obtain a liquid anti-mud wet-mix mortar plasticizer.
[0062] Comparative Example 1 A mud-resistant wet-mix mortar plasticizer is different from Example 1 in that an equal amount of water-based acrylic emulsion is replaced by a commercially available water-based epoxy resin emulsion, which is a water-dispersible emulsion with a solid content of 52%.
[0063] Comparative Example 2 A mud-resistant wet-mix mortar plasticizer, which is different from Example 1 in that an equal amount of polyglycerol ricinoleate is replaced by hydroxypropyl cellulose.
[0064] Comparative Example 3 A mud-resistant wet-mix mortar plasticizer, which is different from Example 1 in that propylene glycol alginate is replaced by polyethylene glycol distearate in an equal amount.
[0065] Comparative Example 4 A mud-resistant wet-mix mortar plasticizer, which is different from Example 1 in that an equal amount of sodium n-octane sulfonate is replaced by sodium dodecylbenzene sulfonate.
[0066] Comparative Example 5 A mud-resistant wet-mix mortar plasticizer, which is different from Example 1 in that an equal amount of alkylphenol polyoxyethylene ether is replaced by fatty alcohol polyoxyethylene ether.
[0067] Detection The anti-mud wet-mixed mortar plasticizer prepared in the above embodiments and comparative examples was mixed with wet-mixed mortar, and the consistency, bulk density, water retention rate and open time of the wet-mixed mortar were tested with reference to relevant standards such as JGJ / T70-2009 "Standard for Test Methods of Basic Properties of Building Mortar", JG / T426-2013 "Plastering Mortar Plasticizer" and JG / T164-2004 "Masonry Mortar Plasticizer".
[0068] Among them, the basic mix ratio of wet mixed mortar is shown in Table 1.
[0069] Table 1: The above test results are shown in Table 2. The amount added in Table 2 refers to the amount of plasticizer added per cubic meter.
[0070] Table 2: Combined with the analysis of Examples 1-8 and Comparative Examples 1-5, it is not difficult to see that the anti-mud wet-mix mortar plasticizer of the present invention effectively and significantly improves the plasticity and working performance of the wet-mix mortar through a specific raw material combination and preparation process.
[0071] Specifically combined with the analysis of Example 1 and Comparative Examples 1-5, Comparative Examples 1-5 use water-based epoxy resin emulsion, hydroxypropyl cellulose, polyethylene glycol distearate, sodium dodecylbenzene sulfonate or fatty alcohol polyoxyethylene ether as substitutes compared to Example 1, and Example 1 has better plasticity and working performance. It can be seen that the present application selects five specific raw materials, namely water-based acrylic emulsion, polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate, and alkylphenol polyoxyethylene ether, to add to the anti-mud wet-mixed mortar plasticizer. The synergistic effect between the five plays a key role in the plasticity and working performance of the wet-mixed mortar, can significantly improve the influence of weathered shale clay minerals on the performance of wet-mixed mortar, can significantly improve the plasticity and working performance of the wet-mixed mortar, make it more convenient and quick in the construction process, and has excellent water retention and mud resistance, which can meet various construction needs.
[0072] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A mud-resistant wet-mix mortar plasticizer, characterized in that: The invention comprises the following raw materials in parts by weight: 15-20 parts of water-based acrylic emulsion, 5-10 parts of polyglycerol ricinoleate, 5-8 parts of propylene glycol alginate, 3-5 parts of sodium n-octane sulfonate and 0.5-1.5 parts of alkylphenol polyoxyethylene ether.
2. The anti-mud wet-mix mortar plasticizer according to claim 1, characterized in that: The preparation method of the aqueous acrylic emulsion comprises the following steps: S1: Take 60-70 parts of water, 10-20 parts of acrylate, 5-10 parts of butyl methacrylate, 5-10 parts of styrene, 5-10 parts of maleic acid, 1-2 parts of silane coupling agent, 1-2 parts of emulsifier, and 1-2 parts of initiator; S2: premix 50%-60% by mass of water and 40%-50% by mass of emulsifier, then add acrylate, butyl methacrylate, styrene, maleic acid, and silane coupling agent, mix well, and stir until milky white; S3: In a nitrogen atmosphere, the temperature is raised to 70-80° C., an initiator, the remaining water and the remaining emulsifier are added, and the mixture is stirred for 3-4 hours to obtain a water-based acrylic emulsion.
3. The anti-mud wet-mix mortar plasticizer according to claim 2, characterized in that: The emulsifier is sodium dodecyl sulfate, and the initiator is ammonium persulfate.
4. The anti-mud wet-mix mortar plasticizer according to claim 1, characterized in that: The anti-mud wet-mix mortar plasticizer also includes 5-10 parts of polyvinyl alcohol.
5. The anti-mud wet-mix mortar plasticizer according to claim 1, characterized in that: The anti-mud wet-mix mortar plasticizer also includes 2-5 parts of nano silicon dioxide.
6. The anti-mud wet-mix mortar plasticizer according to claim 1, characterized in that: The anti-mud wet-mixed mortar plasticizer also includes 5-10 parts of polyvinyl alcohol and 2-5 parts of nano silicon dioxide.
7. A method for preparing the anti-mud wet-mix mortar plasticizer according to any one of claims 1 to 6, characterized in that: include: Take water-based acrylic emulsion, add polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate, alkylphenol polyoxyethylene ether in sequence, and stir and mix evenly to obtain a mud-resistant wet-mix mortar plasticizer.
8. The method for preparing the anti-mud wet-mix mortar plasticizer according to claim 7, characterized in that: include: Premix the water-based acrylic emulsion and polyvinyl alcohol, then add polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate and alkylphenol polyoxyethylene ether in sequence, and stir and mix evenly to obtain an anti-mud wet-mix mortar plasticizer.
9. The method for preparing the anti-mud wet-mix mortar plasticizer according to claim 7, characterized in that: include: The aqueous acrylic emulsion and nano-silica are pre-mixed, ultrasonically treated for 10-20 minutes, and then polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate, and alkylphenol polyoxyethylene ether are added in sequence and stirred to mix evenly to obtain an anti-mud wet-mix mortar plasticizer.
10. The method for preparing the anti-mud wet-mix mortar plasticizer according to claim 7, characterized in that: include: Aqueous acrylic emulsion, polyvinyl alcohol and nano-silica are pre-mixed, ultrasonically treated for 10-20 minutes, and then polyglycerol ricinoleate, propylene glycol alginate, sodium n-octane sulfonate and alkylphenol polyoxyethylene ether are added in sequence and stirred to mix evenly to obtain an anti-mud wet-mix mortar plasticizer.