Fly ash surface thin coating self-degradation material as well as preparation method and application thereof
By coating the surface of fly ash grouting material with polycaprolactone generated by esterification of caprolactam and ethylene glycol, the clogging problem during the transportation of fly ash grouting material is solved, achieving efficient transportation and performance maintenance during the grouting process.
Patent Information
- Application Number
- CN202410990019.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-26
AI Technical Summary
Existing fly ash grouting materials are prone to segregation and sedimentation during transportation due to changes in temperature and humidity, which can cause blockages in transportation pipelines and affect the grouting effect.
A self-degradable material is applied to the surface of fly ash. Caprolactone is generated through the esterification reaction of caprolactam and ethylene glycol, which is then polymerized into polycaprolactone. This polycaprolactone is then applied to the surface of the fly ash grouting material to form a hydrophobic layer, reducing adhesion to the wall and self-degrading under alkaline conditions.
It effectively prevents grouting materials from sticking to the walls of transport pipelines, ensuring grouting efficiency. At the same time, it self-degrades after grouting is completed, without affecting the performance of fly ash grouting materials.
Smart Images

Figure CN119019652A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of grouting materials, and in particular relates to a self-degradable material thinly coated on the surface of fly ash, a preparation method and application thereof. Background Art
[0002] Coal mining is an important way to obtain coal resources. However, during the coal mining process, due to the influence of geological structure, mine deformation and mining technology, surface water enters the mining area through cracks and pores, causing groundwater surges, which can corrode equipment at the least and cause casualties at the worst.
[0003] Using grouting technology to inject grouting materials into underground aquifers is one of the most effective methods for treating aquifers above coal seams. Fly ash geopolymer grouting material is a commonly used green solid waste grouting material at this stage. Its advantages are good gelling properties, water resistance, low cost, and abundant sources. At present, in order to ensure the smooth transportation of fly ash grouting liquid and minimize the wall adhesion phenomenon, most projects use a water-cement ratio of about 1.0-1.2. The large water-cement ratio grouting liquid can reduce the wall adhesion of the grouting material macroscopically, but its material performance is weaker than that of the low water-cement ratio. However, the fly ash geopolymer grouting material with a low water-cement ratio of about 0.6-0.8 may experience changes in temperature and humidity during pipeline transportation, coupled with long-term transportation, which may lead to the segregation and sedimentation of fly ash or geopolymer, and adhere to the inner wall of the grouting pipeline, causing the transportation pipeline to be blocked, affecting the grouting effect. Therefore, it is necessary to treat the surface of the fly ash grouting material to improve the accumulation of the grouting material on the inner wall of the pipe.
[0004] Therefore, it is necessary to provide an improved technical solution to address the above-mentioned deficiencies in the prior art. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a self-degradable material thinly coated on the surface of fly ash, which can be added to fly ash geopolymer grouting material, reduce the viscosity of the fly ash geopolymer grouting material with the inside of the transportation pipeline during transportation, improve the slurry transportation efficiency, and thus solve the pipe blockage problem during the transportation of the grouting material; at the same time, after a period of time, the self-degradable material thinly coated on the surface of fly ash can degrade itself and will not affect the various properties of the fly ash geopolymer grouting material.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A self-degradable material thinly coated on the surface of fly ash comprises 1 to 5 mole parts of caprolactone, 2 to 6 mole parts of ethylene glycol, 10 to 60 mole parts of solvent and 0.05 to 0.5 mole parts of catalyst.
[0008] Furthermore, the molar ratio of caprolactone to ethylene glycol is 1:(1-2); the molar ratio of the total amount of caprolactone and ethylene glycol to the solvent is 1:(10-30); and the molar ratio of the total amount of caprolactone and ethylene glycol to the catalyst is 10:(1-3).
[0009] Furthermore, the molar ratio of caprolactone and ethylene glycol is 1:1; the molar ratio of the total amount of caprolactone and ethylene glycol to the solvent is 1:10; and the molar ratio of the total amount of caprolactone and ethylene glycol to the catalyst is 10:2.
[0010] Furthermore, in terms of molar ratio, the molar ratio of capric acid, ethylene glycol, solvent and catalyst in the self-degradable material thinly coated on the fly ash surface is 3:4:16:0.45.
[0011] Furthermore, the catalyst is one or more of diethyl dibutyrate, dimethyl phosphate, and toluic acid.
[0012] Furthermore, the solvent is one or more of toluene solution, xylene, methanol, and dioxane.
[0013] The present invention also proposes a method for preparing the fly ash surface thin coating self-degradable material, comprising the following steps:
[0014] Step 1, weigh caprolactone and ethylene glycol in a container, stir and mix, heat in a water bath to 50°C to 70°C after stirring, dropwise add a catalyst into the container and mix evenly to obtain a solution A;
[0015] Step 2: adding a solvent dropwise to solution A at 110° C. to 130° C. while stirring to obtain solution B; the reaction time after the addition is 75 min to 120 min, and stirring is maintained during the reaction;
[0016] Step 3: After the reaction is completed, solution B is cooled to room temperature, filtered, and the precipitate is dried to obtain a self-degradable material thinly coated on the surface of fly ash.
[0017] Furthermore, in step 2, the catalyst is added at a rate of 110 to 130 drops / minute; and in step 3, the solvent is added at a rate of 30 to 50 drops / minute.
[0018] The present invention also proposes an application of a self-degradable material thinly coated on the surface of fly ash in a grouting project. Before the fly ash-based grouting material is used, the aforementioned self-degradable material on the surface of the fly ash is mixed with the fly ash-based grouting material and ball-milled so that the self-degradable material on the surface of the fly ash-based grouting material is attached to the surface of the fly ash-based grouting material to obtain a mixed grouting material.
[0019] Furthermore, the usage of the fly ash surface self-degradable material is 1.5wt.% of the fly ash-based grouting material; the fly ash surface self-degradable material and the fly ash-based grouting material need to be grouted and used within 0 to 60 minutes after mixing.
[0020] The beneficial effects of the present invention are:
[0021] (1) The fly ash surface thinly coated with the self-degradable material prepared by the present invention can prevent the fly ash-based grouting material from sticking to the wall during the grouting process, and the self-degradable material can achieve self-degradation under alkaline conditions, so that the slurry does not block the pipe during the grouting process, and after the slurry reaches the formation, the subsequent performance of the fly ash-based grouting material is not affected;
[0022] (2) The present invention prepares the self-degradable material by esterification and polymerization of the two substances, which has a simple preparation process, good stability and convenient application;
[0023] (3) The self-degradable material prepared by the present invention reduces the adhesion between the fly ash-based grouting material and the grouting pipe, thereby eliminating the pipe blockage during the grouting process, ensuring the efficiency of the grouting project, and maintaining the subsequent performance stability of the grouting material, thereby better meeting the actual needs of the project. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. Among them:
[0025] Figure 1 It is a schematic diagram of the setting of the grouting pipe in the performance test of the embodiment of the present invention. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.
[0027] The present invention will be described in detail below in conjunction with embodiments. It should be noted that the embodiments and features in the embodiments of the present invention can be combined with each other without conflict.
[0028] Aiming at the problem that fly ash-based grouting materials are easily attached to and accumulated on the inner wall of a grouting pipe during operation, thus causing pipe blockage, the present invention provides a self-degradable material for a thin coating on the surface of fly ash. By esterifying and copolymerizing two substances (capric acid and ethylene glycol), the material has good hydrophobicity and self-degradation properties, so that the fly ash grouting material does not block the pipe during transportation in the grouting pipe, and can also maintain various subsequent properties of the fly ash grouting material, thereby achieving the purpose of not blocking the pipe and maintaining various properties of the material.
[0029] A self-degradable material thinly coated on the surface of fly ash, the components of which, by molar fraction, include: 1-5 parts of caprolactone (for example, 1 part, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts or 5 parts), 2-6 parts of ethylene glycol (for example, 2 parts, 3 parts, 4 parts, 5 parts or 6 parts), 10-60 parts of solvent (for example, 10 parts, 20 parts, 30 parts, 40 parts, 50 parts or 60 parts), 0.05-0.5 parts of catalyst (for example, 0.05 parts, 0.15 parts, 0.2 parts, 0.25 parts, 0.3 parts, 0.35 parts, 0.4 parts or 0.5 parts).
[0030] The catalyst is one or more of diethyl dibutyrate, dimethyl phosphate, and toluic acid; the solvent is one or more of toluene solution, methanol, and dioxane.
[0031] In the present invention, caprolactone is generated by esterification reaction of caprolactone with ethylene glycol, and caprolactone is polymerized in toluene solvent to generate polycaprolactone (PCL). PCL has the advantages of high dispersibility, complete degradability, and good adhesion of the polymer. It can be covered on the surface of fly ash grouting material to form a hydrophobic layer, so that the surface viscosity of fly ash grouting material is reduced and it is not easy to stick to the pipe wall; at the same time, polycaprolactone can be degraded by water, and the slurry properties of fly ash grouting material itself can be restored after the slurry reaches the grouting formation. Polycaprolactone is a chemically synthesized biodegradable polymer material. In nature, the ester structure is easily decomposed by microorganisms or enzymes, and the final products are carbon dioxide and water. In the present invention, polycaprolactone is accelerated to degrade in an alkaline environment, and the degradation process is mainly divided into four parts: (1) Water and action, PCL absorbs water from the slurry and begins to degrade after 45 minutes. The degradation rate of PCL depends on the performance of the material itself and the specific surface area in contact with water; (2) Structural changes: PCL degradation in water is due to the breakage of the PCL main chain, which leads to a decrease in the molecular weight of PCL and a decrease in mechanical properties; (3) Decomposition: After the PCL main chain breaks, low molecular weight polymers are formed, and the oligomers continue to hydrolyze into CO2 and H2O. Since the amount added during use is small, the amount of decomposed products has a negligible effect on the performance of the grouting material. The present invention prepares PCL by adjusting the raw material ratio, and provides a fly ash surface thin coating self-degradable material with different degradation rates and degradation times. It can be adjusted according to the needs of the working conditions to obtain a fly ash surface thin coating self-degradable material suitable for the current situation, so as to prevent the grouting material from clogging the grouting pipe.
[0032] In a preferred embodiment, the molar ratio of caprolactone to ethylene glycol is 1:(1-2) (e.g., 1:1, 1:2 or 1:1.5); the molar ratio of the total amount of caprolactone and ethylene glycol to the solvent is 1:(10-30) (e.g., 1:10, 1:15, 1:20, 1:25, 1:30); the molar ratio of the total amount of caprolactone and ethylene glycol to the catalyst is 10:(1-3) (e.g., 10:1, 10:2, 10:3).
[0033] In a preferred embodiment, the molar ratio of caprolactone to ethylene glycol is 1:1; the molar ratio of the total amount of caprolactone and ethylene glycol to the solvent is 1:10; and the molar ratio of the total amount of caprolactone and ethylene glycol to the catalyst is 10:2.
[0034] In the present invention, by limiting the ratio of caprolactone and ethylene glycol, the ratio of the total amount of caprolactone and ethylene glycol to the solvent, and the ratio of the total amount of caprolactone and ethylene glycol to the catalyst, PCL can have a higher yield and better adhesion. The time required for PCL degradation is controlled by controlling the molecular weight of PCL, and then the debonding time of the grouting material and the pipeline is controlled by controlling the proportion of PCL in the fly ash grouting material. The experimental results show that when the molar ratio of caprolactone and ethylene glycol is 1:1, the esterification reaction yield of the two is the highest, and more caprolactone monomers are produced; when the molar ratio of the solution to the total amount of caprolactone and ethylene glycol is 10:1, the concentration of caprolactone monomers in the fixed solvent is high, and it is easy to induce a polymerization reaction; when the molar ratio of the catalyst to the total amount of caprolactone and ethylene glycol is 2:10, the initiation efficiency is high and the molecular weight of PCL is appropriate.
[0035] In an optional embodiment, the self-degradable material thinly coated on the fly ash surface includes 3 molar parts of caprolactone, 4 molar parts of ethylene glycol, 16 molar parts of solvent and 0.45 molar parts of catalyst.
[0036] The present invention also proposes a method for preparing a fly ash surface thin coating self-degradable material, comprising the following steps:
[0037] Step 1, weigh caprolactone and ethylene glycol in a container, stir and heat in a water bath to 50°C to 70°C (e.g., 55°C, 60°C, 65°C, 70°C), dropwise add a catalyst into the container and mix well to obtain a solution A;
[0038] Step 2, at 110° C. to 130° C. (e.g., 110° C., 120° C., 130° C.), adding a solvent dropwise to solution A while stirring to obtain solution B, the reaction time after the dropwise addition is 75 min to 120 min (e.g., 70 min, 80 min, 90 min, 100 min, 110 min, 120 min), and stirring is maintained during the reaction;
[0039] Step 3: After the reaction is completed, solution B is cooled to room temperature, filtered with filter paper, and the precipitate is dried to obtain a self-degradable material thinly coated on the surface of fly ash.
[0040] Furthermore, in step 2, the dropping speed of the catalyst is 110 to 130 drops / minute; in step 3, the dropping speed of solvent A is 30 to 50 drops / minute; preferably, in step 2, the dropping speed of the catalyst is 120 drops / minute; in step 3, the dropping speed of the solvent is 45 drops / minute.
[0041] The preparation process of the present invention has a great influence on the performance of the synthesized polymer. If the addition or dripping rate is too fast, the polymerization reaction may be too violent, resulting in an undesirable chain structure and molecular weight distribution. On the contrary, if the addition or dripping rate is too slow, the polymer molecular chain may be too long to form a cross-linked polymer. Therefore, in step 2 and step 3, controlling the catalyst addition rate and the slow dripping rate of the solvent can obtain better polymer performance and avoid the appearance of other white floccules.
[0042] The fly ash surface thin coating self-degradable material prepared by the above method can be wrapped on the fly ash surface, making it insoluble in water in the grouting pipe and not sticking to the wall, thereby achieving the purpose of improving the problem of fly ash-based grouting materials clogging the grouting pipe; and under alkaline conditions (the fly ash geopolymer grouting material used by the fly ash surface thin coating self-degradable material is itself alkaline), it begins to degrade after 45 minutes, and will not affect the performance of the grouting material after solidification.
[0043] The present invention also proposes an application of a self-degradable material thinly coated on the surface of fly ash in a grouting project: before the fly ash-based grouting material is used, the aforementioned self-degradable material on the surface of the fly ash is mixed with the fly ash-based grouting material and ball-milled to make the self-degradable material on the surface of the fly ash-based grouting material adhere to the surface of the fly ash-based grouting material to obtain a mixed grouting material, and then the mixed grouting material is transported through a grouting pipeline. After the grouting of the fly ash-based grouting material is completed, the phenomenon of material sticking to the wall of the grouting pipeline is significantly reduced.
[0044] The usage amount of the fly ash surface self-degradable material is 1.5wt.% of the fly ash-based grouting material; the fly ash surface self-degradable material and the fly ash-based grouting material need to be grouted and used within 0 to 60 minutes after mixing.
[0045] Next, specific examples and comparative examples are given for illustration.
[0046] Example 1
[0047] The invention provides a self-degradable material for thin coating on the surface of fly ash, which comprises the following raw materials, measured by molar fractions: 3 parts of caprolactone, 3 parts of ethylene glycol, 30 parts of toluene solution, and 0.25 parts of diethyl dibutyrate; that is, the molar ratio of caprolactone to ethylene glycol is 1:1, the molar ratio of the solvent to the total amount of caprolactone and ethylene glycol is 10:1, and the molar ratio of the catalyst to the total amount of caprolactone and ethylene glycol is 2:10.
[0048] The method for preparing the fly ash surface thin coating self-degradable material comprises the following steps:
[0049] Step 1, caprolactone (commercially available caprolactone), catalyst (diethyl dibutyrate), solvent (toluene solution, mass concentration 20%), ethylene glycol (ethylene glycol solution, mass concentration 10%) are separately placed in a separatory funnel for use;
[0050] Install a separatory funnel containing caprolactone and ethylene glycol on a three-necked round-bottom flask, add caprolactone and ethylene glycol to the three-necked round-bottom flask; then add a catalyst at a rate of 120 drops / minute, and keep stirring during the dropwise addition process (use a stirring paddle to stir the solution); fully mix the caprolactone and ethylene glycol; heat in a water bath during the reaction, and the water bath temperature is 60°C;
[0051] Step 2: Raise the temperature to 110°C, install a separatory funnel containing toluene solution on a three-necked round-bottom flask, and drop the toluene solution at a rate of 45 drops / minute. Stir the mixture during the dropwise addition process. The reaction time after the dropwise addition is 80 minutes. Stir the mixture during the reaction process.
[0052] During the process of adding and mixing in step 1 and step 2, a condenser is used to condense the generated steam to cool and condense it, so as to avoid the temperature inside the reaction container from rising too fast and to prevent the danger of explosion;
[0053] Step 3: After the reaction is completed, solution B is cooled to room temperature, filtered with filter paper, and the precipitate is dried to obtain a self-degradable material thinly coated on the surface of fly ash.
[0054] The application of the fly ash surface thin coating self-degradable material in grouting engineering: the prepared self-degradable material is mixed with the prepared fly ash-based grouting material by a ball mill. The heat generated by the ball mill during the mixing process can wrap the prepared polycaprolactone on the surface of the fly ash material. The amount of the self-degradable material is 1.5wt.% of the fly ash-based grouting material. The fly ash-based grouting liquid is immediately injected into the transportation pipeline by a 6Mpa grouting pump. The fly ash-based grouting liquid is obtained by uniformly stirring 10Kg of fly ash-based grouting material and 8Kg of water.
[0055] Example 2
[0056] This embodiment provides a fly ash surface thin coating self-degradable material, the raw material composition and preparation method of the fly ash surface self-degradable material are the same as those of Example 1. The application of the fly ash surface self-degradable material in grouting pipes is different from that of Example 1.
[0057] In this Example 2, the application of fly ash surface self-degradable material in grouting engineering: the prepared self-degradable material is mixed with the prepared fly ash-based grouting material by a ball mill. The heat generated by the ball mill during the mixing process can wrap the prepared polycaprolactone on the surface of the fly ash material. The amount of the self-degradable material is 1.5wt.% of the fly ash-based grouting material. After 30 minutes, the fly ash-based grouting liquid is injected into the transportation pipeline by a 6Mpa grouting pump. The fly ash-based grouting liquid is obtained by uniformly stirring 10Kg of fly ash-based grouting material and 8Kg of water.
[0058] Example 3
[0059] This embodiment provides a fly ash surface thin coating self-degradable material, the raw material composition and preparation method of the fly ash surface self-degradable material are the same as those of Example 1. The application of the fly ash surface self-degradable material in grouting pipes is different from that of Example 1.
[0060] In this embodiment 3, the fly ash surface self-degradable material is used in the grouting project: the prepared self-degradable material is mixed with the prepared fly ash-based grouting material by a ball mill. The heat generated by the ball mill during the mixing process can wrap the prepared polycaprolactone on the surface of the fly ash material. The amount of the self-degradable material is 1.5wt.% of the fly ash-based grouting material. After 60 minutes, the fly ash-based grouting liquid is injected into the transportation pipeline by a 6Mpa grouting pump. The fly ash-based grouting liquid is obtained by uniformly stirring 10Kg of fly ash-based grouting material and 8Kg of water.
[0061] Example 4
[0062] The present embodiment provides a self-degradable material for thin coating on the surface of fly ash, which comprises the following raw materials, measured by molar fractions: 3 parts of capric acid, 6 parts of ethylene glycol, 30 parts of solvent, and 0.25 parts of catalyst.
[0063] That is, the molar ratio of caprolactic acid to ethylene glycol is 1:2, the molar ratio of the solution to the total amount of caprolactic acid and ethylene glycol is 10:1, and the molar ratio of the catalyst to the total amount of caprolactic acid and ethylene glycol is 2:10.
[0064] The catalyst is diethyl dibutyrate, and the solvent is toluene solution.
[0065] The preparation method of the fly ash surface thin coating self-degradable material is the same as that of Example 1.
[0066] The application of the self-degradable material thinly coated on the surface of fly ash in grouting engineering is the same as that in Example 1.
[0067] Example 5
[0068] This embodiment provides a self-degradable material thinly coated on the surface of fly ash. The raw material composition of the self-degradable material on the surface of the self-degradable grouting material is the same as that of Example 1.
[0069] The difference between the preparation method of the self-degradable grouting material and that of Example 1 is that the reaction time after the toluene solution is added dropwise in step 2 is 100 minutes.
[0070] The application of the self-degradable material thinly coated on the surface of fly ash in grouting engineering is the same as that in Example 1.
[0071] Example 6
[0072] This embodiment provides a self-degradable material for thin coating on the surface of fly ash. The raw material composition of the self-degradable grouting material is the same as that of Example 1.
[0073] The difference between the preparation method of the self-degradable grouting material and that of Example 1 is that in step 2, the reaction time after the toluene solution is added dropwise is 120 min.
[0074] The application of the fly ash surface thin coating of self-degradable material in grouting engineering is the same as that in Example 1.
[0075] Example 7
[0076] This comparative example relates to a self-degradable material thinly coated on the surface of fly ash, which comprises the following raw materials, measured by molar fractions: 3 parts of capric acid, 3 parts of ethylene glycol, 60 parts of toluene solution, and 0.25 parts of diethyl dibutyrate.
[0077] That is, the molar ratio of caprolactic acid to ethylene glycol is 1:1, the molar ratio of the solution to the total amount of caprolactic acid and ethylene glycol is 20:1, and the molar ratio of the catalyst to the total amount of caprolactic acid and ethylene glycol is 2:10.
[0078] The preparation method of the fly ash surface thin coating self-degradable material is the same as that of Example 1.
[0079] The application of the self-degradable material thinly coated on the surface of fly ash in grouting engineering is the same as that in Example 1.
[0080] Example 8
[0081] This comparative example relates to a self-degradable material thinly coated on the surface of fly ash, which comprises the following raw materials, measured in molar parts: 3 parts of caprolactone, 3 parts of ethylene glycol, 30 parts of solvent, and 0.1 part of catalyst; that is, the molar ratio of caprolactone to ethylene glycol is 1:1, the molar ratio of the solution to the total amount of caprolactone and ethylene glycol is 10:1, and the molar ratio of the catalyst to the total amount of caprolactone and ethylene glycol is 1:10.
[0082] The preparation method of the fly ash surface thin coating self-degradable material is the same as that of Example 1.
[0083] The application of the self-degradable material thinly coated on the surface of fly ash in grouting engineering is the same as that in Example 1.
[0084] Comparative Example 1
[0085] This comparative example does not involve the preparation of a thin coating of self-degradable material on the surface of fly ash.
[0086] The fly ash-based grouting liquid is directly injected into the grouting pipe with a grouting pressure of 6 MPa. The fly ash-based single-liquid grouting liquid is obtained by uniformly mixing 10 kg of fly ash-based liquid grouting material and 8 kg of water.
[0087] Comparative Example 2
[0088] This embodiment provides a self-degradable material thinly coated on the surface of fly ash. The raw material composition of the surface of the self-degradable grouting material is the same as that of Example 1.
[0089] The method for preparing the thin coating material on the surface of the self-degradable grouting material is different from that in Example 1 in that: in step 2, the reaction time after the toluene solution is added dropwise is 60 minutes.
[0090] The application of the self-degradable material thinly coated on the surface of fly ash in grouting engineering is the same as that in Example 1.
[0091] Comparative Example 3
[0092] This embodiment provides a self-degradable material thinly coated on the surface of fly ash. The raw material composition of the surface of the self-degradable grouting material is the same as that of Example 1.
[0093] The method for preparing the thin coating material on the surface of the self-degradable grouting material is different from that in Example 1 in that: in step 2, the reaction time after the toluene solution is added dropwise is 130 minutes.
[0094] The application of the self-degradable material thinly coated on the surface of fly ash in grouting engineering is the same as that in Example 1.
[0095] Performance measurement:
[0096] The residual amount of the fly ash surface thin coating self-degradable material in the grouting pipe with a diameter of 0.1m and a length of 1m in the above Examples 1-8 and Comparative Examples 1-3 was tested and evaluated, and it was stipulated that the residual slurry in the pipe exceeding 3% of the total slurry was considered to be too large and unqualified. Table 1 lists the weight of the residual slurry in the pipe and the percentage of the residual slurry in the total slurry.
[0097] In order to evaluate the effect of self-degradable materials on slurry performance, the 28-day compressive strength of fly ash grouting materials without self-degradable materials and those with self-degradable materials were compared. The 28-day compressive strength of the grouting material without fly ash thinly coated with self-degradable materials was 31.2MPa. Table 1 shows the 28-day strength after degradation using the surface self-degradable materials.
[0098] The test process is: Figure 1 As shown, the grouting pipe is inclined at 45°, and the pipe is filled with fly ash grouting material after treatment. After being sealed for 60 minutes, the slurry outflow is tested; the slurry residual amount in the pipe is obtained by subtracting the slurry outflow from the known total experimental grouting amount (about 15kg).
[0099] The test method for 28d axial compressive strength refers to the test method for axial compressive strength, and refers to "T0554-2005 Test method for axial compressive strength of cement concrete cylinder". The size of the cylindrical specimen is Ф50mm×100mm.
[0100] Table 1
[0101] sample Residue in tube / KG Residual Assessment 28d strength / MPa Example 1 0.23 1.53% 29.2 Example 2 0.21 1.4% 30.4 Example 3 0.26 1.73% 28.6 Example 4 0.31 2.06% 25.8 Example 5 0.25 1.67% 28 Example 6 0.29 1.93% 27.3 Comparative Example 7 0.25 1.67% 29.2 Comparative Example 8 0.52 3% 26.1 Comparative Example 1 0.84 5.6% (unqualified) 24.1 Comparative Example 2 0.64 4.26% (unqualified) 25.4 Comparative Example 3 0.58 3.87% (unqualified) 24.6
[0102] The fly ash grouting materials and the homemade surface self-degrading materials in Examples 1 to 3 are mixed with different residence times. It can be seen from the residual amount in the pipe that the residual amount in the pipe first decreases and then increases with the extension of the residence time after the materials are mixed. This shows that the residence time of the self-degradable material and the fly ash grouting material after mixing is appropriate, which helps to cool the polycaprolactone retained on the outside of the grouting material, makes the internal bonding of the self-degradable material more firmly, and reduces the amount of fly ash grouting liquid sticking to the pipe during transportation; according to the embodiment of the present invention, the optimal residence time of the obtained self-degradable material and the fly ash grouting material after mixing is 30 minutes.
[0103] By comparing Example 4 with Example 1, the molar ratio of caprolactone to ethylene glycol was changed to 1:2, and the residual amount in the grouting pipe of Example 4 was 0.08 kg more than that of Example 1. Analysis showed that because caprolactone is a precursor of polycaprolactone, if its molar amount is insufficient, some ethylene glycol may not be able to completely react with caprolactone to form caprolactone, which will affect the quality of the final polymer. As a result, the self-degradable material cannot be fully or better mixed with the fly ash grouting material, so the residual slurry in the pipe is relatively large during the implementation process.
[0104] Comparison between Comparative Example 2, Comparative Example 3, Example 5, Example 6 and Example 1 shows that the reaction time after the addition of the toluene solution in step 2 will affect the effect of the thin coating of the self-degradable material on the surface of the fly ash; within the reaction time of 80min to 120min given in the embodiments of the present invention, the effect of the self-degradable material is relatively optimal, and the amount of the treated grouting material remaining in the grouting pipe is relatively small.
[0105] From the 28d compressive strength data of Examples 1-8, it can be seen that the use of fly ash surface self-degradable materials has a slight effect on the compressive strength of the fly ash material, but generally meets the requirement of the expected 28d compressive strength of more than 25 MPa for the grouting reinforcement project.
[0106] In summary, the present invention reduces the amount of slurry residue in the grouting pipe by thinly coating the surface of homemade fly ash with self-degradable material, thereby reducing the risk of pipe blockage during the grouting process, allowing the fly ash grouting material to reach the receiving layer more effectively during the grouting process, thereby improving the efficiency of the grouting project.
[0107] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention are within the scope of protection of the pending claims of the present invention.
Claims
1. A self-degradable material thinly coated on the surface of fly ash, characterized in that: The invention comprises 1 to 5 mole parts of caprolactone, 2 to 6 mole parts of ethylene glycol, 10 to 60 mole parts of solvent and 0.05 to 0.5 mole parts of catalyst.
2. The fly ash surface thin coating self-degradable material according to claim 1, characterized in that: The molar ratio of caprolactone and ethylene glycol is 1:(1-2); the molar ratio of the total amount of caprolactone and ethylene glycol to the solvent is 1:(10-30); and the molar ratio of the total amount of caprolactone and ethylene glycol to the catalyst is 10:(1-3).
3. The fly ash surface thin coating self-degradable material according to claim 1, characterized in that: The molar ratio of caprolactone and ethylene glycol is 1:1; the molar ratio of the total amount of caprolactone and ethylene glycol to the solvent is 1:10; and the molar ratio of the total amount of caprolactone and ethylene glycol to the catalyst is 10:
2.
4. The fly ash surface thin coating self-degradable material according to claim 1, characterized in that: In terms of molar ratio, the molar ratio of capric acid, ethylene glycol, solvent and catalyst in the self-degradable material thinly coated on the surface of fly ash is 3:4:16:0.
45.
5. The fly ash surface thin coating self-degradable material according to claim 1, characterized in that: The catalyst is one or more of diethyl dibutyrate, dimethyl phosphate and toluic acid.
6. The fly ash surface thin coating self-degradable material according to claim 1, characterized in that: The solvent is one or more of toluene solution, xylene, methanol and dioxane.
7. A method for preparing the self-degradable material thinly coated on the surface of fly ash according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1, weigh caprolactone and ethylene glycol in a container, stir and mix, heat in a water bath to 50°C to 70°C after stirring, dropwise add a catalyst into the container and mix evenly to obtain a solution A; Step 2: adding a solvent dropwise to solution A at 110° C. to 130° C. while stirring to obtain solution B; the reaction time after the addition is 75 min to 120 min, and stirring is maintained during the reaction; Step 3: After the reaction is completed, solution B is cooled to room temperature, filtered, and the precipitate is dried to obtain a self-degradable material thinly coated on the surface of fly ash.
8. The method for preparing a self-degradable material thinly coated on the surface of fly ash according to claim 7, characterized in that: In step 2, the catalyst is added at a rate of 110 to 130 drops / minute; in step 3, the solvent is added at a rate of 30 to 50 drops / minute.
9. Application of a self-degradable material thinly coated on the surface of fly ash in grouting engineering, characterized in that: Before the fly ash-based grouting material is used, the fly ash surface self-degradable material according to any one of claims 1 to 6 is mixed with the fly ash-based grouting material and ball-milled to make the fly ash surface self-degradable material adhere to the surface of the fly ash-based grouting material to obtain a mixed grouting material.
10. The use of the fly ash surface thin coating self-degradable material in grouting engineering according to claim 9, characterized in that: The usage amount of the fly ash surface self-degradable material is 1.5wt.% of the fly ash-based grouting material; the fly ash surface self-degradable material and the fly ash-based grouting material need to be grouted and used within 0 to 60 minutes after mixing.