Method for preparing regenerated polyester from waste polyester
Through the depolymerization and polycondensation reaction between the depolymerization precursor and the waste polyester, combined with the twin screw reaction extruder and the melt filter, the molecular weight uneven and hydrolysis problems in polyester recycling are solved, and efficient polyester regeneration is achieved and improved Spinning performance and product quality.
Patent Information
- Application Number
- CN202411208308.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-26
AI Technical Summary
In the existing polyester recycling technology, it is difficult to achieve homogeneous mixing of polyester with different molecular weights in physical mixing methods. The chemical process is long, complex and costly. The waste polyester raw materials have many types and different properties, making it difficult to meet the spinning molding requirements. .
Depolymerization reaction is carried out by using the depolymerization precursor and waste polyester. After obtaining the intermediate, polycondensation is condensed under vacuum, molecular weight distribution is controlled, hydrolysis and thermal degradation are inhibited, and the use of linear diol and branched alcohol is combined with the use of linear diol and branched alcohols, and the reaction is carried out through a twin screw Extruders and melt filters improve reaction uniformity and product quality.
It realizes low molecular weight homogeneous mixing of polyesters of different molecular weights, improves spinning performance, improves thermal stability and spinningability of regenerated polyesters, reduces production costs, and is suitable for spinning and film fields.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waste polyester recycling, and in particular to a method for preparing recycled polyester by utilizing waste polyester. Background Art
[0002] The recycling and reuse of polymers can realize the reuse of resources on the one hand, and meet the requirements of green and low-carbon development on the other. Polyester is an important variety of synthetic polymers, and polyester fiber is the basic raw material for textiles. In 2022, China's total PET production exceeded 50 million tons, which plays a pivotal role. How to reuse waste PET resources is an important direction related to the sustainable development of the industry.
[0003] Chinese invention patent CN102605456B discloses a method for preparing polyester filaments using waste polyester raw materials, wherein the waste polyester bottle flakes are sorted, cleaned, crushed and dried, and then conveyed to a reactive exhaust screw extruder after drying, phenyldioxazoline and N,N'-carbonyl dicaprolactam polyester chain extender are added at 0.5-3% of the mass of the polyester bottle flakes, the polyester bottle flakes and the polyester chain extender are conveyed to the reactive exhaust screw extruder together, and after melting and mixing, the melt is metered and conveyed to a spinning unit to prepare polyester filaments; Chinese invention patent CN109134244A discloses a method for degrading waste polyester, After the polyester is preliminarily alcoholized with diol, the preliminarily alcoholysis product is deeply alcoholized and transesterified with a mixture of diol and methanol to obtain dimethyl terephthalate. The depolymerization rate of the polyester after the preliminarily alcoholysis is 20-60%, the depolymerization rate of the polyester after the deep alcoholysis is 90-100%, the mass content of diol terephthalate in the preliminarily alcoholysis product is 30-60%, the purity of the obtained dimethyl terephthalate is 98-99.8%, and the yield is 85-96%. Chinese invention patent CN114031756B discloses a closed-loop method for recycling waste polyester to prepare recycled polyester with typical green and low-carbon characteristics. The method comprises the following steps: selecting a specific depolymerization catalyst to depolymerize waste polyester under microwave conditions; removing the polyol solvent from the depolymerization product, purifying and removing the by-products to obtain a depolymerized monomer; mixing the depolymerized monomer with a dibasic acid, a polyol, a polymerization catalyst and a chain extender to carry out an esterification reaction, and then adding a stabilizer and a catalyst to carry out polycondensation to obtain a regenerated polyester; Chinese invention patent CN109467743A discloses a method for producing regenerated colored polyester staple fibers from waste polyester foam by a chemical method, comprising collecting waste polyester products, The waste polyester products are washed and dried, crushed in a crusher, and then vacuum dried, part of the new polyester is mixed into the waste polyester products, the mixed waste polyester products are depolymerized, and the waste polyester depolymerization liquid is filtered to obtain the waste polyester depolymerization liquid, the waste polyester depolymerization liquid is subjected to esterification reaction, the system after the esterification reaction is subjected to polycondensation reaction, and then the recycled polyester masterbatch is prepared through extrusion granulation equipment, the recycled polyester masterbatch mixed with the color masterbatch is put into a screw extruder and melt-extruded, and the extruded melt is introduced into a spinning box to prepare recycled colored polyester staple fibers.
[0004] Judging from the above disclosed technologies, there are currently two main methods for recycling polyester: physical mixing method and chemical method.
[0005] (1) The physical mixing method is to melt the waste polyester, filter it, and then extrude it into a shape. It can be used as plastic or fiber. When used as fiber, short fibers are mainly used due to the decrease in molecular weight after regeneration. The screw's mixing shearing cannot achieve the effect of homogeneous mixing of polyester raw materials with different characteristics, and there is a significant decrease in the characteristic viscosity after melt blending. The molecular weight of polyester is increased by introducing a chain extender during the melting process, but the molecular weight distribution coefficient of the viscosity-enhancing polyester prepared by the chain extension reaction will become wider, resulting in a decrease in spinnability.
[0006] (2) Chemical recycling is to deeply depolymerize waste polyester into monomers or other types of small molecular substances in a small molecule depolymerizer, and then re-esterify and polycondense them after purification. However, the process is long and the technology is complicated. The actual operating cost is high, making it difficult to promote.
[0007] There are many types of waste polyester raw materials in actual production, and their properties vary greatly, mainly reflected in the differences in the intrinsic viscosity and the third component. Simple physical blending cannot achieve homogeneous mixing of polyesters of different molecular weights, which is very unfavorable for recycling spinning. Although chemical methods can achieve deep depolymerization of polyesters with uneven molecular weights into monomers or small molecules, the process is long, the process is complicated, and the cost is high. Summary of the invention
[0008] In order to solve the technical problems existing in the above-mentioned background technology, one of the purposes of the present invention is to provide a method for preparing recycled polyester using waste polyester, comprising the following steps:
[0009] S0, preparing waste polyester raw materials, drying them for later use;
[0010] S1, adding a depolymerization precursor to carry out a depolymerization reaction, wherein the mass ratio of the depolymerization precursor to the waste polyester raw material is 1:(80-120), and a depolymerization intermediate is obtained, and the number average molecular weight of the depolymerization intermediate is 8000-25000 g / mol;
[0011] S2, the depolymerized intermediate undergoes polycondensation reaction under vacuum conditions to obtain a regenerated polyester having a number average molecular weight of 20,000-35,000 g / mol.
[0012] In reality, recycled polyester is not of the same type. The raw materials are relatively complex, which is mainly reflected in the differences in molecular weight and color of polyester. How to achieve uniform quality of polyesters of different molecular weights under certain process conditions has a significant impact on improving spinning performance. In particular, the raw materials of polyester bottles have a large molecular weight. It is difficult to achieve homogeneous mixing of different types of high molecular weight polyesters. Reducing the molecular weight is helpful to achieve mixing between materials.
[0013] The recycled polyester usually has a high moisture content. If it is not treated, it will cause severe hydrolysis under high temperature conditions. Although the molecular weight can be reduced, which helps different types of polyesters to be better mixed at low molecular weight, the hydrolysis process is that the ester bond combines with water molecules under high temperature conditions and breaks to form hydroxyl and carboxyl groups. Once the carboxyl groups are formed, the thermal stability of the hydrolysis product is poor, which can easily lead to deterioration of the phase, and the indexes and spinning conditions of the repolymerized product are reduced. The present invention first vacuum dries the recycled raw materials, strictly controls its moisture content, and inhibits the molecular weight reduction caused by hydrolysis. By introducing a depolymerization precursor to depolymerize waste polyesters of different molecular weights into polyesters of "intermediate" molecular weight, homogeneous mixing of polyesters of different molecular weights at low molecular weight can be achieved. While the molecular weight of the product after depolymerization decreases, the molecular weight distribution is more concentrated, and the depolymerization product is a hydroxyl-terminated structure, which has good thermal stability at high temperature, and significantly inhibits a series of problems such as molecular weight reduction and color deterioration caused by thermal degradation. In addition, the inventors have found through experiments that the molecular weight of the depolymerized intermediate is too large or too small, which mainly affects the quality of the recycled polyester obtained in the polycondensation process. Before the polycondensation process, it is necessary to first undergo the melting process of the depolymerization intermediate. If the molecular weight is too large and the time to reach a uniform melt is too long, the depolymerization intermediate will be thermally degraded, affecting the quality of the recycled polyester; if the molecular weight is too small, the time to reach the target molecular weight through polycondensation is too long, which is prone to thermal degradation and reduces the quality of the recycled polyester. In addition, if the molecular weight is too low, it is easy to cause low molecular weight substances to boil and splash during vacuum polycondensation, and be vacuum-extracted from the polymerization system, causing material loss and vacuum system blockage; splashing and adhering to the inner wall of the polymerization kettle, and separating from stirring, thermal degradation or even carbonization will occur, affecting the quality of the recycled polyester. The regenerated polyester prepared by this technical solution can be used in the field of spinning, specifically, it can be prepared into spinning slices or its melt directly spun, and can also be used in the fields of preparing films. Compared with the application in other fields, the regenerated polyester prepared by the present invention has the advantage of being used in the field of spinning. Under the same processing conditions during the processing, the viscosity drop will become lower, the melt strength will be higher, and the mechanical strength of the spun fiber is high; at the same time, the spun fiber contains a certain proportion of branched structure components, and the toughness is improved. The coloring performance (dyeing rate) of the fiber will increase under the same process during post-processing dyeing, and the dyeing effect will be brighter.
[0014] The preferred technical solution of the present invention is that in S0, the waste polyester raw material includes waste polyester bottle flakes and polyester waste silk friction material, and the mass ratio of the two is 1: (0.18-5.6).
[0015] At the same time, in addition to white bottle flakes, there are often blue bottle flakes in the discarded polyester bottle flakes. On the one hand, the sorting technology is continuously improved to reduce the proportion of blue bottle flakes. On the other hand, from the perspective of resource recycling, how to use the blue bottle flakes within a certain range is also an important direction to further expand the adaptability of raw materials and improve the utilization ratio of discarded polyester resources. In addition, there is always a certain proportion of waste silk in spinning production. The existing use of waste silk is to make it into friction material, and then use it. It is mainly used to spin short fibers. In a sense, it is to reduce the quality requirements for application. The main reason is that the molecular weight of the waste silk itself decreases after thermal degradation, and the yellowing problem is prone to occur at high temperature. The present invention fully studies and analyzes the characteristics of different discarded polyester raw materials, focuses on comparing the essential characteristics of polyester bottle flakes of different grades and waste silk friction materials, mixes different grades of polyester bottle flakes with waste silk friction materials according to proportion for reuse, and uses the low yellowing of blue bottle flakes and the high yellowing characteristics of waste silk friction materials at high temperatures to compensate for the effective control of product yellowing, thereby meeting the application requirements on the fiber.
[0016] The preferred technical solution of the present invention is that in S1, the depolymerization precursor includes linear diols and branched alcohols, and the mass fraction ratio of the two is (9-99):1, the linear diols are oligomers with a degree of polymerization of 2-5 formed by aromatic dibasic acids and aliphatic diols; the aromatic dibasic acids are one or more of terephthalic acid and isophthalic acid; the aliphatic diols are one or more of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol; the branched alcohols are one or more of pentaerythritol and sorbitol.
[0017] The introduction of linear diols contained in the depolymerization precursor realizes the "tailoring" of high molecular weight polyester, reduces its molecular weight, and facilitates the homogeneous mixing of components at low viscosity. Although the content of branched alcohol, another component in the depolymerization precursor, is extremely low, it can react with the carboxyl group in the depolymerization product, further suppressing the content of carboxyl groups. At the same time, branched alcohol plays a positive role in the spinnability of the melt, and the spinnability of the fiber is improved. The spinnability here refers to the ability of the polyester melt to withstand irreversible deformation when subjected to uniaxial stretching after being extruded from the spinneret hole in the spinning formation of polyester fibers. The spinnability of recycled polyester can only be qualitatively characterized by spinning experiments, but it can be empirically judged from the molecular weight and its distribution (number average molecular weight is 22000-30000g / mol, molecular weight distribution coefficient is 2.0-2.5) and melt index (melt index is 30-45g / 10min when the weight is 2.16kg and the temperature is 270-300℃).
[0018] The preferred technical solution of the present invention is that the linear diol is an oligomer with a polymerization degree of 2 formed by terephthalic acid and ethylene glycol, and the branched alcohol is sorbitol.
[0019] The preferred technical solution of the present invention is that, in S0, the moisture content of the waste polyester raw material after drying is less than 100 ppm.
[0020] The preferred technical solution of the present invention is that, in S1, the depolymerization reaction is carried out in a twin-screw reaction extruder with a suction device, the suction pressure is 500-1000Pa, and the reaction temperature is 255-275°C. Compared with the conventional device for polycondensation reaction, the twin-screw reaction extruder used in the present invention can provide strong shear force and mixing effect, which is conducive to the full contact and reaction between the waste polyester raw material and the depolymerization precursor, thereby improving the depolymerization efficiency and reaction uniformity. At the same time, the introduction of the suction device enables the low molecular weight volatiles generated during the reaction process to be removed in time, effectively avoiding the adverse effects of these volatiles on the depolymerization reaction, and further improving the reaction efficiency and product quality. Secondly, the depolymerization reaction is carried out at a specific suction pressure and reaction temperature, which is the key control parameter of the present technical solution. The suction pressure is set to 500-1000Pa, which not only ensures the effective extraction of volatiles, but also avoids the damage of the reaction system by excessive suction pressure. The reaction temperature is controlled between 255-275°C. This temperature range can ensure the smooth progress of the depolymerization reaction while avoiding side reactions and product degradation caused by excessively high temperature.
[0021] The preferred technical solution of the present invention is that in S1, the number average molecular weight of the depolymerized intermediate is 10000-18000 g / mol, the molecular weight distribution coefficient PDI is 1.2-1.8, and the b value is -1.5-2. Too wide a molecular weight distribution of the depolymerized intermediate will cause difficulty in its forming, and in the subsequent polycondensation process, the molecular weight distribution of the recycled polyester will be too wide, resulting in the appearance of droplets during the spinning process and even difficulty in forming. The b value mainly affects the appearance quality. PDI is mainly affected by the twin-screw processing parameters and the composition and addition amount of the depolymerized precursor, and the b value is mainly affected by the composition and water content of the waste polyester.
[0022] The preferred technical solution of the present invention is that in S2, the depolymerized intermediate is filtered through a melt filter before undergoing a polycondensation reaction, and the filter mesh number of the melt filter is 100-500 meshes. This technical solution can effectively remove impurities and unmelted particles in the melt. According to the inventor's test, this has a significant effect on improving spinning performance and ensuring spinning quality. Before the depolymerized intermediate enters the polycondensation reaction, filtering through a melt filter can significantly reduce the impurity content entering the subsequent reaction system, thereby improving the purity and performance stability of the final product.
[0023] The preferred technical solution of the present invention is that in S2, the reaction temperature of the polycondensation reaction is 260-280°C, the reaction pressure is ≤50Pa, and the reaction time is 0.5-2.5h. Within the temperature range of 260-280°C, the polyester molecular chain can effectively undergo polycondensation to form high molecular weight polyester. This temperature range not only ensures the smooth progress of the reaction, but also avoids the polyester degradation and side reactions that may be caused by excessively high temperatures, thereby ensuring the quality and performance of the product. Controlling the reaction pressure within a low pressure range of ≤50Pa helps to reduce the oxygen and water vapor content in the reaction system and reduce the risk of oxidative degradation of the polyester molecular chain during the polycondensation process. At the same time, the low pressure environment is also conducive to the timely discharge of small molecular by-products, promotes the forward progress of the polycondensation reaction, and increases the degree of polymerization of the polyester. The reaction time range of 0.5-2.5h ensures the full progress of the polycondensation reaction and avoids excessive cross-linking and molecular chain breakage of the polyester that may be caused by too long a reaction time. Within this time range, the polyester molecular chain can reach an ideal degree of polymerization while maintaining good processing properties.
[0024] The preferred technical solution of the present invention is that, in S2, the number average molecular weight of the recycled polyester is 22000-30000g / mol, the molecular weight distribution coefficient is 2.0-2.5, and the b value is 3-8. Within the range of 22000-30000g / mol, the recycled polyester has a moderate molecular weight, which not only ensures sufficient chain length to form a stable fiber structure, but also avoids the processing difficulties caused by excessive molecular weight. Such a molecular weight range helps to obtain good fiber properties and processing stability in the subsequent spinning process. The molecular weight distribution coefficient of 2.0-2.5 means that the molecular weight distribution of the recycled polyester is relatively concentrated, which helps to reduce the uneven phenomenon in the spinning process and improve the uniformity and quality of the fiber. The narrower molecular weight distribution is also conducive to improving the mechanical properties of the fiber, such as tensile strength and elongation at break. In the melt processing, especially the spinning process, the polyester will undergo a filtering component before the melt enters the spinning plate to remove impurities and condensed ions that may exist in the melt, so as to ensure the service life and spinning stability of the spinning component. If the melt filter pressure difference is too large, it means there are too many impurities and condensed ions, which will cause frequent replacement of filter components during processing, increasing processing time and economic costs. When the molecular weight distribution coefficient is 2.0-2.5, the melt filter pressure difference can be effectively reduced to less than 0.45MPa. After experiments, it is easier to process within this range.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) The present invention introduces a depolymerization precursor to achieve efficient homogeneous mixing and high-quality reuse of different types of complex mixed polyesters, thereby increasing the utilization ratio of waste raw materials and being more in line with the development direction of regeneration. The method can achieve homogeneous mixing of polyesters of different molecular weights at low molecular weight. The molecular weight of the depolymerized product decreases while the molecular weight distribution is more concentrated. The depolymerized product is a hydroxyl-terminated structure with good thermal stability at high temperatures, which significantly inhibits a series of problems such as molecular weight decrease and color deterioration caused by thermal degradation;
[0027] (2) The technical solution of the present invention is based on the characteristics of the raw materials and the evolution mechanism during the regeneration process. It can mix different grades of polyester bottle flakes and waste silk friction materials in proportion for reuse. The low yellowing characteristics of blue bottle flakes and the high yellowing characteristics of waste silk friction materials at high temperatures are used to compensate for each other to achieve effective control of product yellowing, thereby meeting the application requirements on fibers;
[0028] (3) Through the technical solution of the present invention, recycled polyester can be prepared into spinning chips or melt direct spinning, and the fiber quality is significantly improved, making full use of the advantages of the waste raw materials themselves and avoiding low-value recycling. The technical solution for producing fibers has the advantages of high intrinsic viscosity, good spinnability, simple process and short flow, strong operability, relatively low cost, and is easy to promote. DETAILED DESCRIPTION
[0029] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0030] Example 1
[0031] A method for preparing recycled polyester using waste polyester in this embodiment comprises the following steps:
[0032] Step S0: Collect discarded polyester bottle flakes and polyester waste silk friction materials as raw materials. Waste polyester bottle flakes refer to polyester white bottle flakes containing 5-20% mass fraction of polyester blue bottle flakes. The characteristic viscosity of polyester white bottle flakes is 0.70-0.80dl / g, and the characteristic viscosity of polyester blue bottle flakes is 0.75-0.85dl / g. Polyester waste silk friction material is obtained after processing of oil-free waste silk produced in polyester fiber spinning, and its characteristic viscosity is 0.55-0.60dl / g. The classified polyester raw materials are cleaned to remove dirt, oil stains, dust and other impurities on the surface. The cleaning can be carried out by water washing, solvent washing and the like. For larger polyester waste, it is necessary to crush it into smaller fragments or particles first, which is conducive to the uniformity and efficiency of subsequent processing. The discarded polyester bottle flakes and polyester waste silk friction materials are mixed in a mass ratio of 1:0.2 and vacuum dried to ensure that the moisture content is less than 100ppm. The final moisture content is 94ppm;
[0033] Step S1: Add a depolymerization precursor (the mass fraction ratio of linear diol to branched alcohol is 90:10) to carry out a depolymerization reaction. The mass ratio of the depolymerization precursor to the waste polyester raw material is 1:100. The depolymerization reaction is carried out in a twin-screw reaction extruder with a suction device. The suction pressure is 700Pa and the reaction temperature is 255-275°C to obtain a depolymerized intermediate. Its number average molecular weight is 8000g / mol, the molecular weight distribution coefficient PDI is 1.2, and the b value is -1. Among them, the linear diol terephthalic acid and 1,3-propylene glycol form an oligomer with a degree of polymerization of 2, and the branched alcohol is pentaerythritol;
[0034] Step S2: The depolymerized intermediate is filtered and then subjected to polycondensation reaction in a horizontal viscosity-increasing reactor under vacuum conditions to obtain recycled polyester. The polycondensation reaction temperature is 260-280° C., the reaction pressure is 50 Pa, and the reaction time is 1 hour.
[0035] Example 2
[0036] The method for preparing recycled polyester from waste polyester in this embodiment is different from that in Embodiment 1 in that, in step S0, waste polyester bottle flakes and polyester waste silk friction material are mixed in a mass ratio of 1:0.5.
[0037] Example 3
[0038] The method for preparing recycled polyester from waste polyester in this embodiment is different from that in Embodiment 1 in that, in step S0, waste polyester bottle flakes and polyester waste silk friction material are mixed in a mass ratio of 1:5.5.
[0039] Example 4
[0040] The method for preparing recycled polyester from waste polyester in this embodiment is different from that in embodiment 1 in that in step S1, the mass fraction ratio of linear diol to branched alcohol in the depolymerization precursor is 90:10, wherein the linear diol is an oligomer with a degree of polymerization of 2 formed by terephthalic acid and ethylene glycol, and the branched alcohol is sorbitol. In step S2, the reaction time of the polycondensation reaction is shortened to 45 min.
[0041] Example 5
[0042] The method for preparing recycled polyester from waste polyester in this embodiment is different from that in Embodiment 1 in that, in step S1, the mass fraction ratio of linear diol to branched alcohol in the depolymerization precursor is 99:1, and the mass ratio of the depolymerization precursor to the waste polyester raw material is 2: 100. The linear diol is an oligomer with a degree of polymerization of 2 formed by terephthalic acid and 1,3-propylene glycol, and the branched alcohol is pentaerythritol.
[0043] Example 6
[0044] The method for preparing recycled polyester using waste polyester in this embodiment is different from that in Embodiment 1 in that, in S0, the moisture content of the waste polyester raw material after drying is 200 ppm.
[0045] Example 7
[0046] The method for preparing recycled polyester from waste polyester in this embodiment is different from that in Embodiment 1 in that, in S2, the depolymerized intermediate is passed through a melt filter and then subjected to polycondensation reaction, and the filter mesh number of the melt filter is 100-500 meshes.
[0047] Example 8
[0048] The method for preparing recycled polyester from waste polyester in this embodiment is different from that in Embodiment 1 in that, in S0, the waste polyester raw materials are all waste polyester bottle flakes.
[0049] The recycled polyester obtained in the above examples 1-8 is prepared into slices and then spun to obtain polyester fibers. The short fiber spinning process is as follows: the spinning temperature is 270-300°C, the spinning speed is 800-1500 m / min, the stretching temperature is 60-80°C, the pre-stretching ratio is 1.02-1.10, the first stretching ratio is 2.80-3.20, the second stretching ratio is 1.05-1.15, and then cut to obtain the recycled polyester short fibers. It is noted that in addition to the short fiber spinning process, the recycled polyester slices prepared by the technical solution of the present invention can be melt-spun into polyester filaments, not just short fibers.
[0050] Comparative Example 1
[0051] This embodiment provides a method for preparing regenerated polyester and polyester fiber. The specific preparation method refers to Example 1 in CN102605456B to obtain regenerated polyester and polyester fiber.
[0052] Comparative Example 2
[0053] This embodiment provides a method for preparing regenerated polyester and polyester fiber. The specific preparation method refers to Example 1 in CN109467743A to obtain regenerated polyester and polyester fiber.
[0054] Comparative Example 3
[0055] The method for preparing regenerated polyester and polyester fiber in this embodiment is different from that in Embodiment 1 in that the mass ratio of the depolymerization precursor to the waste polyester raw material is 3.2:100.
[0056] Comparative Example 4
[0057] The method for preparing regenerated polyester and polyester fiber in this embodiment is different from that in Embodiment 1 in that the mass ratio of the depolymerization precursor to the waste polyester raw material is 0.05:100.
[0058] Performance testing
[0059] 1. Number average molecular weight, PDI: The number average molecular weight and PDI of the samples were tested by GPC-50 gel permeation chromatograph produced by PL Company of Britain. The equipment was equipped with a differential refractometer and a PL gel column (5μmmixed-C). 1,1,1,3,3,3-hexafluoro-2-propanol was used as the eluent with a flow rate of 1mL / min. During the test, the sample was dried and dissolved in hexafluoroisopropanol to prepare a solution with a concentration of 1.0mg / mL. The test was carried out when the column temperature reached 40±1℃; PDI=weight average molecular weight / number average molecular weight; The weight average molecular weight was tested in the same way as the number average molecular weight.
[0060] 2. b value: Tested according to method 5.5 of GB / T 14190-2017
[0061] 3. Tensile strength: Tested according to GB / T 14344-2022
[0062] 4. Elongation at break: Tested in accordance with GB / T 14343-2008
[0063] The test results are shown in Table 1
[0064] Table 1 - Performance test results of Examples 1-8 and Comparative Examples 1-4
[0065]
[0066]
[0067] According to Table 1, the tensile strength of the polyester fiber prepared by the present invention is 5.42-6.43 cN / dtex, and the elongation at break is 23.34-28.78%. It is noted that the elongation at break is regulated according to the application field of the fiber, and the elongation at break is in the optimal range of 20-30% under the present invention. The b value of the material is relatively small, between 3-8. The inventors have found through experimental tests that controlling the intrinsic viscosity of the waste polyester raw material in the range of 0.55-0.85 dL / g is more beneficial to the subsequent reaction, processing, molecular weight and other parameter regulation.
[0068] The technical solution in Comparative Example 1 (CN102605456B) is not to depolymerize to an intermediate and then perform a chain extension reaction. Its process is to melt the waste polyester raw material and then perform chain extension, and more importantly, to reduce the decrease in the molecular weight of the molten polyester as much as possible before the chain extension reaction. The technical solution in Comparative Example 2 (CN109467743A) clearly states that the waste polyester raw material is depolymerized into a substance that can undergo an esterification reaction. The number average molecular weight of the substance that can undergo an esterification reaction does not exceed 2000g / mol. The depolymer in Comparative Example 2 and the depolymer intermediate in the present invention are not the same concept. The biggest difference from the solution of the present invention is the number average molecular weight of the depolymer intermediate. The number average molecular weight of the depolymer intermediate of the present invention is higher, so the depolymer intermediate can directly enter the polycondensation reaction, while in Comparative Example 2, it is necessary to undergo an esterification reaction before entering the polycondensation reaction. By comparing Examples 1-8 with Comparative Examples 1-2, it can be seen that the polyester fiber prepared by the present invention has substantially better mechanical properties and appearance quality than that prepared by the existing process method. In addition, during the spinning process of Comparative Example 2, due to the relatively high PDI, melt droplets will appear in the short fiber spinning, which is not suitable for promotional production.
[0069] Comparing Example 1 with Comparative Examples 3-4, it can be seen that the number average molecular weight of the depolymer intermediate is too large or too small, which will have an adverse effect on the tensile strength and elongation at break of the polyester fiber prepared subsequently. When the number average molecular weight of the depolymer intermediate is too large, the length of the molecular chain increases, resulting in enhanced entanglement and interaction between the molecular chains. In the subsequent polycondensation and spinning process, these entangled molecular chains are difficult to effectively arrange and orient, and the fiber structure finally formed is relatively loose, thereby affecting the tensile strength of the fiber. When the number average molecular weight of the depolymer intermediate is too small, the length of the molecular chain is too short, and sufficient physical entanglement and interaction cannot be formed to maintain the structural stability of the fiber. This will cause the fiber to slip and break easily during the stretching process, significantly reducing the tensile strength of the fiber. Low molecular weight depolymer intermediates may be more likely to form defects such as gaps, cracks, etc. during the polycondensation process. These defects will become stress concentration points, and the fibers prepared subsequently will expand rapidly and break when subjected to external forces, thereby reducing the tensile strength and elongation at break of the fiber. Moreover, under the conditions of Comparative Example 3, low molecular weight substances are easily caused to boil and splash during vacuum polycondensation, and are vacuum-drawn out of the polymerization system, causing material loss and blockage of the vacuum system; the splashes adhere to the inner wall of the polymerization kettle and are separated from stirring, resulting in thermal degradation or even carbonization, which seriously affects production efficiency.
[0070] By comparing Examples 1 and 4, it can be seen that when the mass fraction ratio of linear diols to branched alcohols in the depolymerization precursor is the same, the number average molecular weight of the depolymerized intermediate generated by the composition of the depolymerization precursor of Example 4 is smaller, and the tensile strength of the obtained polyester fiber is higher. The inventor found through analysis that the reason is that the oligomer with a degree of polymerization of 2 formed by terephthalic acid and ethylene glycol is the basic molecular segment in the waste polyester, which has the best compatibility, and the low degree of polymerization makes the terminal hydroxyl group have better reactivity and high depolymerization efficiency, while sorbitol contains 6 hydroxyl groups available for reaction, and the reaction sites can better capture carboxyl groups, and its linear structure makes the steric hindrance between the hydroxyl groups small. Under the action of the above factors, the depolymerization process of the waste polyester raw material is fast. It is calculated that the polycondensation of Example 4 can be shortened by 15min relative to that of Example 1, and because the molecular weight of the depolymerization intermediate is small, the melting process time before the polycondensation is short, and it is not easy to thermally degrade and reduce the quality of the recycled polyester, so that the tensile strength, elongation at break and appearance quality are all better.
[0071] By comparing Examples 1 and 5, it can be seen that the number average molecular weight of the depolymerized intermediate generated by the composition of the depolymerization precursor in Example 5 is smaller. This is because increasing the proportion of linear diols in the depolymerization precursor and the proportion of the depolymerization precursor in the waste polyester raw material can improve the depolymerization efficiency and achieve more uniform molecular weight of the depolymerization intermediate.
[0072] From the comparison between Examples 1 and 6, it can be seen that a higher water content will make the number average molecular weight of the depolymerized intermediate relatively smaller, but because the ester bond combines with water molecules under high temperature conditions and breaks, forming hydroxyl and carboxyl groups, the thermal stability of the hydrolyzed product is poor, and the indexes of the repolymerized product and the spinning condition are reduced. Under normal circumstances, the waste polyester is dried before the reaction, and it is more appropriate to control the water content at a lower level. Under the balance between time efficiency and production quality, a water content of less than 100ppm is more appropriate.
[0073] By comparing Examples 1 and 7, it can be seen that after melt filtration, impurities and condensed ions that may exist in the melt are removed, which not only ensures the service life of the spinning assembly, but also improves the quality and stability of spinning. The tensile strength and elongation at break of the polyester fiber are significantly increased, and subsequent fiber breakage is less likely to occur. However, since the pressurization will increase the temperature of the melt to a certain extent, the appearance quality will be affected.
[0074] From the comparison between Examples 1 and 8, it can be seen that the waste polyester raw materials are all waste polyester bottle flakes. Due to their high intrinsic viscosity, the number average molecular weight of the intermediates obtained in the depolymerization process is also relatively large, which increases the degree of thermal degradation in the subsequent polycondensation process, resulting in a partial decrease in the indexes of the repolymerized product and the spinning conditions. The low yellowing of blue bottle flakes and the high yellowing of waste silk friction materials at high temperatures are used to compensate for each other to achieve effective control of product yellowing, thereby meeting the application requirements on fibers.
[0075] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing recycled polyester using waste polyester, It is characterized in that The following steps are involved: S0, preparing waste polyester raw materials, drying them for later use; S1, adding a depolymerization precursor to carry out a depolymerization reaction, wherein the mass ratio of the depolymerization precursor to the waste polyester raw material is 1:(80-120), to obtain a depolymerized intermediate, wherein the number average molecular weight of the depolymerized intermediate is 8000-25000 g / mol; S2, the depolymerized intermediate undergoes a polycondensation reaction under vacuum conditions to obtain a regenerated polyester, wherein the number average molecular weight of the regenerated polyester is 20000-35000 g / mol.
2. The method for preparing recycled polyester using waste polyester according to claim 1, Features: In S0, the waste polyester raw materials include waste polyester bottle flakes and polyester waste silk friction materials, and the mass ratio of the two is 1: (0.18-5.6).
3. The method for preparing recycled polyester using waste polyester according to claim 1, Features: In S1, the depolymerization precursor includes a linear diol and a branched alcohol, and the mass fraction ratio of the two is (9-99):
1. The linear diol is an oligomer with a degree of polymerization of 2-5 formed by an aromatic dibasic acid and an aliphatic diol. The aromatic dibasic acid is one or more of terephthalic acid and isophthalic acid, the aliphatic diol is one or more of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol, and the branched alcohol is one or more of pentaerythritol and sorbitol.
4. The method for preparing recycled polyester using waste polyester according to claim 3, Features: The linear diol is an oligomer with a polymerization degree of 2 formed by terephthalic acid and ethylene glycol, and the branched alcohol is sorbitol.
5. The method for preparing recycled polyester using waste polyester according to claim 1, Features: In S0, the moisture content of the waste polyester raw material after drying is less than 100 ppm.
6. The method for preparing recycled polyester using waste polyester according to claim 1, Features: In S1, the depolymerization reaction is carried out in a twin-screw reaction extruder with a suction device, the suction pressure is 500-1000 Pa, and the reaction temperature is 255-275°C.
7. The method for preparing recycled polyester using waste polyester according to claim 1, Features: In S1, the number average molecular weight of the depolymerized intermediate is 10000-18000 g / mol, the molecular weight distribution coefficient PDI is 1.2-1.8, and the b value is -1.5-2.
8. The method for preparing recycled polyester using waste polyester according to claim 1, Features: In S2, the depolymerized intermediate is passed through a melt filter and then subjected to polycondensation reaction, wherein the filter mesh number of the melt filter is 100-500 meshes.
9. The method for preparing recycled polyester using waste polyester according to claim 1, Features: In S2, the reaction temperature of the polycondensation reaction is 260-280°C, the reaction pressure is ≤50Pa, and the reaction time is 0.5-2.5h.
10. The method for preparing recycled polyester using waste polyester according to claim 1, Features: In S2, the number average molecular weight of the recycled polyester is 22000-30000 g / mol, the molecular weight distribution coefficient is 2.0-2.5, and the b value is 3-8.
Citation Information
Patent Citations
Method for preparing polyester filament yarns by using waste polyester raw materials
CN102605456B
Waste polyester degradation method
CN109134244A
Chemical regeneration method for waste polyester textiles, regenerated polyester and polyester thermofuse
CN109467743A
A closed-loop method for preparing recycled polyester from waste polyester with typical green and low-carbon characteristics.
CN114031756B