Preparation and application of copper porphyrin metal organic framework encapsulated with ferromolybdenum polyacid
By encapsulating the PMo11Fe polyacid in NU-902 (Cu), the problems of easy soluble polyacid in solution and low electron transfer rate are solved, the performance of electrocatalytic nitrate reduction and synthesis of ammonia is improved, and efficient ammonia production is achieved.
Patent Information
- Application Number
- CN202411123699.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-15
AI Technical Summary
The existing polyacid and metal-organic frameworks are easy to dissolve in solution and have low electron transfer rates, limiting their application in electrocatalytic nitrate synthesis of ammonia.
The transition metal iron-substituted phosphomolybdenum polyacid PMo11Fe is encapsulated in the zirconium-based porphyrin metal organic frame NU-902 (Cu), and the PMo11Fe@NU-902 (Cu) composite electrocatalyst is prepared by solvothermal reaction, which overcomes the polyacid Problems of soluble and low electron transfer rate.
The catalyst's electrocatalytic nitrate reduction and synthesis performance of ammonia is improved, the electron transfer rate and active sites are enhanced, and the Faraday efficiency of 89.44% and the ammonia production of 19.38 mg h–1 mgcat.–1 is better than traditional MOF catalysts.
Smart Images

Figure HDA0004995768750000011 
Figure HDA0004995768750000012 
Figure HDA0004995768750000021
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrocatalytic materials, and in particular to a PMo 11 Preparation and application of Fe@NU-902(Cu) composite electrocatalyst. Background Art
[0002] Ammonia (NH3) is one of the world's most produced chemicals and is widely used in various fields such as dye, medicine and fertilizer production. At the same time, NH3 is also a renewable carbon-free energy carrier with high energy density and hydrogen content. At present, the large-scale synthesis of ammonia has been dominated by the energy-intensive and environmentally harmful Haber-Bosch process, which consumes 2% of the world's energy and accounts for 1.4% of global carbon dioxide emissions. Compared with the traditional Haber-Bosch method, the electrocatalytic method can convert renewable energy into ammonia with high energy density and easy storage and transportation. It can react at room temperature and pressure, reducing equipment costs and energy consumption costs, avoiding CO2 emissions, and meeting the requirements of a green and low-carbon economy. Among them, electrocatalytic nitrate synthesis of ammonia (NO3RR) can not only remove the pollutant nitrate in water bodies, but also produce high-quality and high-value zero-carbon hydrogen-rich fuel ammonia, which improves environmental pollution while alleviating the energy crisis. The rational design of highly active and highly selective electrocatalysts is the key to achieving efficient NO3RR.
[0003] Metal-organic frameworks (MOFs) are porous materials with high specific surface areas, but the poor chemical stability and poor electrical conductivity of most MOFs in water limit their applications. The zirconium-based porphyrin metal-organic framework NU-902 (Cu) has excellent chemical stability in aqueous media. In addition, the introduction of transition metal copper increases the catalytic active sites. Polyoxometalates (POMs), also known as polyoxometalates, are a type of d 0 Metal oxygen cluster compounds formed by the combination of pre-transition metals and oxygen. Transition metal-substituted polyacids are widely used in the field of electrocatalysis due to their reversible redox activity and electron-rich properties. Transition metal-substituted polyacids can adjust the composition, charge and structure by changing the type and number of transition metal atoms. However, polyacids also have the key problem of being easy to agglomerate and soluble in water.
[0004] In order to overcome these shortcomings and obtain an electrocatalyst with high catalytic performance, the present invention replaces the transition metal iron with phosphomolybdic acid H6PMo 11 FeO 40 ·xH2O (PMo 11 Fe) is encapsulated in the zirconium-based porphyrin MOF NU-902(Cu) to form PMo with excellent functions. 11 Fe@NU-902(Cu) composite electrocatalyst. Summary of the invention
[0005] The purpose of the present invention is to solve the problems of easy solubility in solution and low electron transfer rate of polyacids and metal-organic frameworks as electrode materials for electrocatalytic synthesis of ammonia. In order to improve the electrocatalytic nitrate reduction performance of the catalyst for synthesizing ammonia, the present invention provides a preparation and application of a copper porphyrin metal-organic framework encapsulating iron-molybdenum polyacid.
[0006] In order to solve the above technical problems, the present invention is achieved through the following technical solutions:
[0007] 1. PMo 11 Preparation of Fe: Na2HPO4·2H2O and FeCl3 were dissolved in hot water, and then acidified with 1 mL of concentrated sulfuric acid after cooling. Then, an aqueous solution of Na2MoO4·2H2O was added to the above solution, and a large amount of flocculent precipitates appeared. Concentrated sulfuric acid was slowly added until the solution was transparent. After cooling, the heteropoly acid was extracted with ether, and the extracted heteropoly acid was redissolved in water, concentrated and crystallized, and dried to obtain iron-substituted phosphomolybdic acid H6PMo 11 FeO 40 ·xH2O (PMo 11 Fe);
[0008] 2. Preparation of composite materials: Zirconium oxychloride (ZrOCl2·8H2O) and benzoic acid were added to N,N-dimethylformamide (DMF), ultrasonically dispersed to dissolve, and then copper-substituted tetrakis (4-carboxyphenyl) porphyrin (Cu-TCPP) and PMo were added. 11 Fe was ultrasonically treated to form a clear solution, which was then placed in a 50 mL polytetrafluoroethylene-lined reactor and heated in an oven for a period of time. After the reaction, it was cooled, centrifuged, washed, and dried to obtain PMo. 11 Fe@NU-902(Cu) composites;
[0009] The mass of Na2HPO4·2H2O described in step 1 is 3.4 to 3.8 g, and the mass of FeCl3 is 1.4 to 1.8 g;
[0010] The hot water in step 1 is 20 mL of deionized water with a temperature range of 80° C. to 100° C.;
[0011] The Na2MoO4·2H2O solution described in step 1 is a solution formed by dissolving 25-27 grams of Na2MoO4·2H2O in 40 mL of deionized water;
[0012] The masses of zirconium oxychloride and benzoic acid described in step 2 are 20-25 mg and 1.4-1.6 g respectively; the amount of DMF used is 15-25 mL;
[0013] The mass of the Cu-TCPP described in step 2 is 45-55 mg; PMo 11 The mass of Fe is 80-120 mg;
[0014] The heating in step 2 is performed at a temperature of 80 to 100° C. and a heating time of 10 to 12 hours;
[0015] The centrifugation and washing in step 2 are washing with DMF and acetone for 3 to 5 times respectively;
[0016] The drying in step 2 is vacuum drying at 50-60° C. for 30-60 minutes.
[0017] Compared with the prior art, the present invention has the following characteristics:
[0018] The present invention firstly combines PMo 11 The Fe polyacid was successfully loaded into the copper porphyrin metal organic framework NU-902(Cu) with periodic pores via a one-step solvothermal reaction, overcoming the PMo 11 Fe is easy to agglomerate and dissolve in water. 11 The introduction of Fe increases the electron transfer rate of the material, and the metallic copper in the porphyrin structural unit is more likely to adsorb nitrate to synthesize ammonia, which can inhibit hydrogen production to a certain extent, improve electron utilization, and improve the performance of electrocatalytic nitrate reduction to synthesize ammonia. 11 Fe@NU-902(Cu) achieves the best Faradaic efficiency of 89.44% at a potential of -1.0 V vs. RHE, corresponding to an ammonia production of 19.38 mg h –1 mg cat. –1 , which is superior to most reported MOF catalysts. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 NU-902(Cu) and PMo 11 Powder X-ray diffraction (XRD) pattern of Fe@NU-902(Cu) composite material.
[0020] Figure 2 This is a scanning electron microscope (SEM) image of NU-902 (Cu) material.
[0021] Figure 3 For PMo 11 Scanning electron microscopy (SEM) image of Fe@NU-902(Cu) composite material.
[0022] Figure 4 NU-902(Cu) and PMo 11Comparison of infrared spectra (FT-IR) of Fe@NU-902(Cu) composite materials.
[0023] Figure 5 For PMo 11 Linear sweep voltammetry (LSV) curves of Fe@NU-902(Cu) composite materials in 0.1M Na2SO4 solution, 0.1MNaNO3 and 0.1MNa2SO4 solution respectively.
[0024] Figure 6 For PMo 11 The Fe@NU-902(Cu) composite material was used for ammonia synthesis reaction in 0.1M Na2SO4 and 0.1M NaNO3 solutions, and the time-current (it) diagram of the catalyst under different voltages.
[0025] Figure 7 For PMo 11 Fe@NU-902(Cu) composite material was subjected to ammonia synthesis reaction in 0.1M NaNO3 and 0.1M Na2SO4 solutions, and UV-visible absorption spectra (UV) at different voltages.
[0026] Figure 8 For PMo 11 Fe@NU-902(Cu) composite material was used for ammonia synthesis reaction in 0.1M NaNO3 and 0.1M Na2SO4 solutions, and the ammonia yield and Faraday efficiency at different voltages were plotted. DETAILED DESCRIPTION
[0027] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.
[0028] Implementation Case 1
[0029] This example is a preparation case of ellipsoidal NU-902(Cu), which is prepared according to the following method:
[0030] 22 mg of zirconium oxychloride (ZrOCl2·8H2O) and 1.5 g of benzoic acid were added to 20 mL of N,N-dimethylformamide (DMF for short), and ultrasonically dispersed to dissolve them. Then, 50 mg of copper-substituted tetrakis(4-carboxyphenyl)porphyrin (Cu-TCPP for short) was added, and a clear solution was formed by ultrasonication. The solution was loaded into a 50 mL polytetrafluoroethylene-lined reactor and heated at 90°C in an oven for 48 h. After heating, the solution was cooled and washed by centrifugation with DMF and acetone for 4 times respectively, and dried in a vacuum drying oven at 60°C for 1 h to obtain NU-902(Cu).
[0031] Implementation Case 2
[0032] This implementation case provides a PMo 11 Fe@NU-902(Cu) composite catalyst, which is prepared according to the following method:
[0033] (1)PMo 11 Preparation of Fe: 3.6 g Na2HPO4·2H2O and 1.6 g FeCl3 were dissolved in 20 mL deionized water at 90°C, and then acidified with 1 mL concentrated sulfuric acid. Then, a solution formed by dissolving 26 g Na2MoO4·2H2O in 40 mL water was added to the above solution. A large amount of flocculent precipitate appeared, and concentrated sulfuric acid was slowly added until the solution was transparent. After cooling, the heteropoly acid was extracted with ether, and the extracted heteropoly acid was redissolved in water, concentrated and crystallized, and dried to obtain iron-substituted phosphomolybdic acid H6PMo 11 FeO 40 ·xH2O (PMo 11 Fe);
[0034] (2) Preparation of composite materials: 22 mg of zirconium oxychloride (ZrOCl2·8H2O) and 1.5 g of benzoic acid were added to 20 mL of N,N-dimethylformamide (DMF) and dissolved by ultrasonic dispersion. Then, 50 mg of copper-substituted tetrakis(4-carboxyphenyl)porphyrin (Cu-TCPP) and 100 mg of PMo were added. 11 Fe was subjected to ultrasound to form a clear solution, which was loaded into a 50 mL polytetrafluoroethylene-lined reactor and heated in an oven at 90 °C for 48 h. After the heating was completed, it was cooled and washed by centrifugation with DMF and acetone for 4 times, respectively, and dried in a vacuum drying oven at 60 °C for 1 h to obtain PMo 11 Fe@NU-902(Cu) composite materials.
[0035] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:
[0036] Figure 1 NU-902(Cu) and PMo are shown 11 The powder X-ray diffraction (XRD) pattern of the Fe@NU-902(Cu) composite material, compared with the simulated pattern obtained by the model structure, proves the successful synthesis of NU-902(Cu), PMo 11 The characteristic peaks of Fe@NU-902(Cu) composite materials at 2θ=18°, 29° and 32° are PMo 11 The characteristic peaks of Fe prove that PMo 11 Synthesis of Fe@NU-902(Cu) composites.
[0037] Figure 2The figure shows a scanning electron microscope (SEM) image of the NU-902 (Cu) monomer material. It is observed that the NU-902 (Cu) monomer material is micrometer-sized and presents an ellipsoid-like shape.
[0038] Figure 3 PMo shown 11 Scanning electron microscopy (SEM) image of Fe@NU-902(Cu) composite material, showing that 11 Fe-synthesized PMo 11 The Fe@NU-902(Cu) composite material also exhibits a micrometer-sized ellipsoidal morphology, proving that the addition of polyacids does not destroy the structure of the original MOF.
[0039] Figure 4 NU-902(Cu) and PMo are shown 11 Infrared spectrum (FT-IR) comparison of Fe@NU-902(Cu) composite materials. As shown in the figure, the composite materials have both NU-902(Cu), PMo 11 The characteristic peaks of Fe monomer materials are only 11 The peak intensity of Fe is reduced, which may be due to encapsulation in the pores of NU-902 (Cu).
[0040] Figure 5 PMo shown 11 The linear sweep voltammetry (LSV) curves of Fe@NU-902(Cu) composite materials in 0.1M Na2SO4 solution, 0.1M NaNO3 and 0.1M Na2SO4 solution are shown in the figure. In the same voltage range, the PMo 11 The reduction current density of Fe@NU-902(Cu) is significantly higher than that of the electrolyte without nitrate, indicating that PMo 11 Fe@NU-902(Cu) catalyst has a certain ability of electrocatalytic nitrate reduction.
[0041] Figure 6 PMo shown 11 Fe@NU-902(Cu) composite material was used for ammonia synthesis in 0.1M Na2SO4 and 0.1M NaNO3 solution. The time-current (it) diagram of the composite material at different voltages. 11 Fe@NU-902(Cu) was subjected to a 1-hour electrocatalytic nitrate reduction experiment to synthesize ammonia. The time-current curves (it) at different potentials showed that the current density remained stable, indicating that the catalyst has good electrochemical stability.
[0042] Figure 7 PMo shown 11 The Fe@NU-902(Cu) composite material was subjected to ammonia synthesis reaction in 0.1M NaNO3 and 0.1M Na2SO4 solutions. The UV-visible absorption spectra (UV) at different voltages were as shown in the figure. As the voltage increased, the absorbance of the electrolyte that was color-developed after the catalytic test also gradually increased in the absorbance test.
[0043] Figure 8 PMo shown 11 The Fe@NU-902(Cu) composite material was used for ammonia synthesis in 0.1M NaNO3 and 0.1M Na2SO4 solutions. The ammonia yield and Faraday efficiency at different voltages were plotted. As shown in the figure, at a potential of -1.0V vs. RHE, the best Faraday efficiency was 89.44%, and the corresponding ammonia yield was 19.38mg h –1 mg cat. –1 , much higher than NU-902(Cu) monomer and similar materials. 11 Fe@NU-902(Cu) composite material can be used as an efficient electrocatalytic nitrate reduction catalyst for ammonia synthesis.
[0044] In summary: Example 2 is a copper porphyrin metal organic framework PMo encapsulated with iron molybdenum polyacid 11 Fe@NU-902(Cu) was successfully prepared by solvothermal synthesis and used as an electrode material for electrocatalytic nitrate reduction to synthesize ammonia. 11 The addition of Fe increases the electron transfer rate and the number of active sites in the composite material. The encapsulation of NU-902 (Cu) increases the specific surface area of the material and solves the problem of PMo 11 Fe is easy to agglomerate and dissolve in water. The material has good redox activity, excellent conductivity and stability, and has great potential in electrocatalytic nitrate reduction to synthesize ammonia.
Claims
1. A preparation process of a copper porphyrin metal organic framework encapsulating iron molybdenum polyacid, characterized in that: (1)PMo 11 Preparation of Fe: Na2HPO4·2H2O and FeCl3 were dissolved in hot water, and then acidified with 1 mL of concentrated sulfuric acid after cooling. Then, an aqueous solution of Na2MoO4·2H2O was added to the above solution, and a large amount of flocculent precipitates appeared. Concentrated sulfuric acid was slowly added until the solution was transparent. After cooling, the heteropoly acid was extracted with ether, and the extracted heteropoly acid was redissolved in water, concentrated and crystallized, and dried to obtain iron-substituted phosphomolybdic acid H6PMo 11 FeO 40 ·xH2O (PMo 11 Fe); (2) Preparation of composite materials: Zirconium oxychloride (ZrOCl2·8H2O) and benzoic acid were added to N,N-dimethylformamide (DMF), ultrasonically dispersed to dissolve them, and then copper-substituted tetrakis(4-carboxyphenyl)porphyrin (Cu-TCPP) and PMo were added. 11 Fe was ultrasonically treated to form a clear solution, which was then placed in a 50 mL polytetrafluoroethylene-lined reactor and heated in an oven for a period of time. After the reaction, it was cooled, centrifuged, washed, and dried to obtain PMo. 11 Fe@NU-902(Cu) composite materials.
2. According to step (1) of claim 1, the mass of Na2HPO4·2H2O is 3.4 to 3.8 g; the mass of FeCl3 is 1.4 to 1.8 g.
3. The hot water according to step (1) of claim 1 is 20 mL of deionized water with a temperature range of 80° C. to 100° C.
4. The Na2MoO4·2H2O solution according to step (1) of claim 1 is a solution formed by dissolving 25 to 27 grams of Na2MoO4·2H2O in 40 mL of deionized water.
5. According to step (2) of claim 1, the masses of zirconium oxychloride and benzoic acid are 20-25 mg and 1.4-1.6 g, respectively; and the amount of DMF is 15-25 mL.
6. The mass of the Cu-TCPP according to step (2) of claim 1 is 45 to 55 mg; PMo 11 The mass of Fe is 80 to 120 mg.
7. According to the heating in step (2) of claim 1, the heating temperature is 80-100° C. and the heating time is 10-12 hours.
8. According to the centrifugation and washing of step (2) of claim 1, the product is washed with DMF and acetone for 3 to 5 times respectively, and the drying is vacuum drying at 50 to 60° C. for 30 to 60 minutes.
9. PMo prepared by the method for preparing a composite material according to claims 1 to 8 11 Fe@NU-902(Cu) is used for electrocatalytic nitrate reduction to synthesize ammonia.
Citation Information
Patent Citations
Optical material and preparation method
CN108873557A
Defective polyacid-based metal organic framework catalyst as well as preparation and application thereof
CN116159599A
Novel transition metal substituted polyoxometalates and process for their preparation
US20080177118A1