Silicon nitride film deposition method
Through the silicon nitride film process of multiple deposition and etching, the problems of high stress and unstable composition of the silicon nitride film in the prior art are solved, and the stability and thickness uniformity of the film are achieved, and the deterioration of the film particle index is avoided.
Patent Information
- Application Number
- CN202310600116.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-26
AI Technical Summary
In the existing silicon nitride thin film deposition process, in order to suppress unnecessary silicon component reactions, excessive ammonia is needed, which leads to high stress and easy peeling of the film. Reducing the ammonia ratio will lead to unstable film components and slow reaction rate, which will not be possible. Meet the production needs of thick silicon nitride films.
Using multiple deposition and etching methods, first deposit the first silicon nitride film on the surface of the base layer, and then pause after reaching a certain thickness. Then use etching gas to remove the unstable film. This process is repeated until the target thickness is reached to ensure the stability of the film.
Through multiple deposition and etching methods, the stability of the silicon nitride film is improved, and the film particle index deterioration caused by excessive thickness of a single deposition is prevented, and the demand for thickness uniformity is met.
Smart Images

Figure CN119020749A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of integrated circuit manufacturing process, and in particular to a silicon nitride film deposition method. Background Art
[0002] In the current manufacturing process, the process of making silicon nitride thin film generally uses film-forming gas DCS + NH3 as silicon nitride film-forming gas, which mainly includes the chemical reactions of the following two reaction equations. Reaction 1 is 3SiH 2 Cl 2 +10NH 3 ->Si 3 N 4 +6NH 4 Cl+6H 2 ; Reaction 2 is SiH 2 Cl 2 ->Si+2HCl.
[0003] Reaction 1 is the main reaction of silicon nitride film formation. In order to inhibit the progress of reaction 2, an excess of NH 3 Make NH 3 :SiH 2 Cl 2 The gas ratio is greater than 10:3, and its advantage is that the film composition is stable as Si 3 N 4 , the deposition speed is fast and the uniformity of thin film deposition is good. The disadvantage is that the residual stress is large, and a single deposition thickness that is too thick is prone to film peeling, causing the particle level to deteriorate during the film preparation process.
[0004] At present, the conventional method to reduce the stress of silicon nitride film and improve the peeling of the film is generally to reduce the proportion of NH3 in the reaction gas and increase the reaction temperature. 3 However, the effect of reducing NH 3 The disadvantage is that it will cause the film composition to be unstable, forming a silicon-rich silicon nitride film, and reduce the NH 3 The proportion of NH in the reaction gas will also lead to a slow reaction rate and cannot meet the production requirements of thick silicon nitride films. It can be seen that reducing the NH 3 The proportion of and increasing the reaction temperature will have a negative impact on the thickness uniformity of silicon nitride films.
[0005] Therefore, it is necessary to provide a novel silicon nitride thin film deposition method to solve the above problems existing in the prior art. Summary of the invention
[0006] The object of the present invention is to provide a silicon nitride film deposition method, which can ensure the deposition effect and prevent the problem of deterioration of film particle indicators caused by excessive deposition thickness.
[0007] To achieve the above object, the silicon nitride thin film deposition method of the present invention comprises:
[0008] Depositing a first layer of silicon nitride film on the surface of the substrate using a target reaction gas, and suspending the deposition after reaching a first thickness;
[0009] Using etching gas to remove the unstable film on the surface of the first silicon nitride film;
[0010] The above process is repeated to continue depositing a layer of silicon nitride film on the surface of the top silicon nitride film remaining after etching and performing surface etching until the thickness of the formed silicon nitride film reaches the target thickness, thereby completing the deposition process of the silicon nitride film.
[0011] The beneficial effect of the silicon nitride film deposition method described in the present invention is that the silicon nitride film is deposited by multiple depositions, and the unstable film formed on the surface is removed after each deposition and the deposition is continued, thereby improving the stability of the formed silicon nitride film and preventing the problem of deterioration of the film particle index when the single deposition thickness exceeds a certain level.
[0012] Optionally, the step of depositing a first layer of silicon nitride film on the surface of the substrate using the target reaction gas and suspending the deposition after reaching a first thickness includes:
[0013] DCS and NH 3 The target reaction gas is continuously delivered to the surface of the substrate to deposit the first layer of the silicon nitride film on the surface of the substrate until the thickness of the first layer of the silicon oxide film reaches the first thickness, and then the delivery of the target reaction gas is stopped.
[0014] Optionally, the removing the unstable film on the surface of the first silicon nitride film layer by using etching gas includes:
[0015] Continuously introducing the etching gas into the first layer of the silicon nitride film, and maintaining the temperature and pressure conditions required for etching to etch the silicon nitride film until the thickness of the silicon nitride film is reduced by etching to reach the preset etching thickness;
[0016] Wherein, the preset etching thickness is greater than or equal to the thickness of the unstable film and less than the first thickness.
[0017] Optionally, in the process of repeating the above process to continue depositing a next layer of silicon nitride film on the surface of the retained top silicon nitride film, the thickness of the remaining silicon nitride film after each new deposition and etching is not completely the same.
[0018] Optionally, the target thickness is at least greater than 2000 angstroms.
[0019] Optionally, the base layer includes SiO 2 . BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is a flow chart of the silicon nitride thin film deposition method of the present invention;
[0021] Figure 2 It is a schematic diagram of the structure of a silicon nitride film deposited by the silicon nitride film deposition method of the present invention. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be understood by people with general skills in the field to which the present invention belongs. "Including" and similar words used in this article mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects.
[0023] In view of the problems existing in the prior art, an embodiment of the present invention provides a method for depositing a silicon nitride thin film. Figure 1 , including the following steps:
[0024] S101, using a target reaction gas to deposit a first layer of silicon nitride film on a surface of a base layer, and suspending the deposition after reaching a first thickness.
[0025] In some embodiments, the step of depositing a first layer of silicon nitride film on the surface of the substrate using the target reaction gas and suspending the deposition after reaching a first thickness includes:
[0026] DCS and NH 3 The target reaction gas is continuously delivered to the surface of the substrate to deposit the first layer of the silicon nitride film on the surface of the substrate until the thickness of the first layer of the silicon oxide film reaches the first thickness, and then the delivery of the target reaction gas is stopped.
[0027] In this embodiment, the thickness of the silicon oxide film deposited for the first time should not be too large or too small, and is generally selected to be at least greater than half of the total thickness required for deposition.
[0028] S102, using etching gas to remove the unstable film on the surface of the first silicon nitride film.
[0029] In this embodiment, after the first layer of silicon oxide film is deposited, since there is a portion of unstable film on the surface of the silicon oxide film, in order to prevent the unstable film from affecting the deposition quality, the unstable film is removed by etching to facilitate the subsequent re-deposition of a new silicon oxide film, thereby improving the stability of the silicon oxide film.
[0030] In some embodiments, the step of removing the unstable film on the surface of the first silicon nitride film by using etching gas includes:
[0031] Continuously introducing the etching gas into the first layer of the silicon nitride film, and maintaining the temperature and pressure conditions required for etching to etch the silicon nitride film until the thickness of the silicon nitride film is reduced by etching to reach the preset etching thickness;
[0032] Wherein, the preset etching thickness is greater than or equal to the thickness of the unstable film and less than the first thickness.
[0033] It should be noted that the preset etching thickness is selected according to the deposition conditions of the silicon nitride film and the type and concentration of the etching gas, and this solution does not specifically limit this.
[0034] Specifically, how to determine the unstable film thickness and then determine the appropriate preset etching thickness is generally done by an experimental method, such as presetting a series of different etching thicknesses, and performing particle measurement after etching to find and determine the preset etching thickness corresponding to the particle level that meets the process requirements. Depending on different process requirements, the specific measurement content and specification settings will be different, which will not be repeated here.
[0035] For example, after the first layer of silicon nitride film is deposited, the particle index of the silicon nitride film will deteriorate after exceeding a certain thickness during the deposition process, affecting the deposition quality. Therefore, the unstable film on the first layer of silicon nitride film is removed by etching until the thickness of the silicon nitride film is reduced to the preset etching thickness by etching, indicating that the unstable film has been completely removed, which is convenient for the subsequent new deposition process.
[0036] S103, repeating the above process to continue depositing a layer of silicon nitride film on the surface of the top silicon nitride film remaining after etching and performing surface etching until the thickness of the formed silicon nitride film reaches the target thickness, thereby completing the deposition process of the silicon nitride film.
[0037] In this embodiment, after the deposition and etching of the first silicon nitride film are completed, a new silicon nitride film is continuously deposited on the surface of the remaining silicon nitride film until the thickness of the formed silicon nitride film reaches the target thickness, and the deposition of the silicon nitride film is completed. The formed silicon nitride film is not prone to instability or deterioration of particle indicators.
[0038] In some embodiments, in the process of repeating the above process to continue depositing the next layer of silicon nitride film on the surface of the retained top layer of the silicon nitride film, the thickness of the remaining silicon nitride film after each new deposition and etching is not exactly the same, and this solution does not specifically limit this.
[0039] In some other embodiments, the target thickness is at least greater than 2000 Å, and the base layer is SiO 2 .
[0040] Exemplary, reference Figure 2 , SiO 2 The base layer 200 is disposed on the Si substrate 100. Taking the deposition of three silicon nitride films as an example, first, a layer of silicon nitride is deposited on the SiO 2 A first layer of silicon nitride film is deposited on the base layer, and then an etching process is used to remove the unstable portion to retain the remaining first layer of silicon nitride film 201. Then, in the same manner, a subsequent second layer of silicon nitride film is deposited on the remaining first layer of silicon nitride film 201 and the unstable portion is etched to obtain the remaining second layer of silicon nitride film 202. Then, a third layer of silicon nitride film is deposited on the remaining second layer of silicon nitride film 202 and the unstable portion is etched to obtain the remaining third layer of silicon nitride film 203, so as to obtain a silicon nitride film of a thickness that meets the requirements.
[0041] The silicon nitride film deposition method of the present invention forms a silicon nitride film by depositing it multiple times, removing the unstable film formed on the surface after each deposition and continuing the deposition, thereby improving the stability of the formed silicon nitride film and preventing the problem of deterioration of film particle indicators when the single deposition thickness exceeds a certain level.
[0042] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.
Claims
1. A method for depositing a silicon nitride thin film, It is characterized in that include: Depositing a first layer of silicon nitride film on the surface of the substrate using a target reaction gas, and suspending the deposition after reaching a first thickness; Using etching gas to remove the unstable film on the surface of the first silicon nitride film; The above process is repeated to continue depositing a layer of silicon nitride film on the surface of the top silicon nitride film remaining after etching and performing surface etching until the thickness of the formed silicon nitride film reaches the target thickness, thereby completing the deposition process of the silicon nitride film.
2. The method for depositing a silicon nitride thin film according to claim 1, It is characterized in that The method of depositing a first layer of silicon nitride film on the surface of the substrate using the target reaction gas and suspending the deposition after reaching a first thickness comprises: DCS and NH 3 The target reaction gas is continuously delivered to the surface of the substrate to deposit the first layer of the silicon nitride film on the surface of the substrate until the thickness of the first layer of the silicon oxide film reaches the first thickness, and then the delivery of the target reaction gas is stopped.
3. The method for depositing a silicon nitride thin film according to claim 1, It is characterized in that The step of removing the unstable film on the surface of the first silicon nitride film layer by using etching gas comprises: Continuously introducing the etching gas into the first layer of the silicon nitride film, and maintaining the temperature and pressure conditions required for etching to etch the silicon nitride film until the thickness of the silicon nitride film is reduced by etching to reach the preset etching thickness; Wherein, the preset etching thickness is greater than or equal to the thickness of the unstable film and less than the first thickness.
4. The method for depositing a silicon nitride thin film according to claim 3, It is characterized in that In the process of repeatedly adopting the above process to continue to deposit a next layer of silicon nitride film on the surface of the retained top silicon nitride film, the thickness of the remaining silicon nitride film after each new deposition and etching is not completely the same.
5. The method for depositing a silicon nitride thin film according to claim 1, It is characterized in that The target thickness is at least greater than 2000 angstroms.
6. The method for depositing a silicon nitride thin film according to any one of claims 1 to 5, It is characterized in that The base layer includes SiO 2 .