Window and display device including same

By adopting a multi-layer structure in the window of the display device, using the combination of silica and alumina and fluorine-containing polymers, the mechanical strength of the flexible display device is improved and the reflectivity is reduced, and the easy damage to the window of the flexible display device is solved. The problem of high reflectivity improves the durability and display efficiency of the equipment.

CN119028223APending Publication Date: 2024-11-26SAMSUNG DISPLAY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410573177.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-25
Filing Date
2024-05-10
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The windows of the flexible display device are easily damaged by external impact during folding or bending operations, and have a high reflectivity, which affects the display efficiency.

Method used

A window design with a multi-layer structure, in which the second layer contains silica and alumina, the weight ratio is in the range of 25:75 to 35:65, and the third layer contains fluoropolymer, the first and third layers. The refractive index is in the range of 1.3 to 1.5 and 1.2 to 1.5, respectively, and the reflectivity of the third layer is less than 6%, to increase the mechanical strength and reduce the reflectivity.

Benefits of technology

It realizes the improvement of the mechanical strength of the display device and the reduction of reflectivity, which enhances the durability and display efficiency of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028223A_ABST
    Figure CN119028223A_ABST
Patent Text Reader

Abstract

The invention relates to a window and a display device. The window includes a base layer. The first layer is disposed on the base layer. The second layer is disposed on the first layer. The third layer is disposed on the second layer. The second layer includes silicon dioxide (SiO2) and aluminum oxide (Al2O3). A weight ratio of silica to alumina in the second layer ranges from about 25: 75 to about 35: 65.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the priority of Korean Patent Application No. 10-2023-0067837 filed on May 25, 2023 in the Korean Intellectual Property Office, the disclosure of which is incorporated herein by reference in its entirety. Technical Field

[0003] Herein, the present disclosure relates to a window and a display device including the same, and more particularly, to a window having enhanced mechanical properties and low reflectivity and a display device including the same. Background Art

[0004] Display devices are used in an increasing number of multimedia devices, such as televisions, mobile phones, tablet computers, and game consoles, to provide image information to users. Recently, various flexible display devices that are foldable or bendable have been developed to provide increased user convenience and portability. Flexible display devices can be deformed in various ways, such as folded, curled, or bent.

[0005] A flexible display device may include a foldable or bendable display panel and a window. However, the window of the flexible display device, which is deformed due to a folding or bending operation, may be easily damaged by an external impact. Summary of the invention

[0006] The present disclosure provides a window with low reflectivity and increased mechanical strength.

[0007] The present disclosure provides a display device having improved display efficiency while maintaining low reflectivity.

[0008] According to an embodiment of the present disclosure, the window includes a base layer. A first layer is disposed on the base layer. A second layer is disposed on the first layer. A third layer is disposed on the second layer. The second layer includes silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ). The weight ratio of silicon dioxide to aluminum oxide in the second layer is in the range of about 25:75 to about 35:65.

[0009] In an embodiment, the second layer may be disposed directly on the first layer, and the third layer may be disposed directly on the second layer.

[0010] In an embodiment, the second layer may have a thickness in a range of about 10 nm to about 20 nm.

[0011] In an embodiment, the second layer may have a refractive index in a range of about 1.43 to about 1.50 at a wavelength of about 550 nm.

[0012] In an embodiment, the first layer may have a refractive index in the range of about 1.3 to about 1.5 at a wavelength of about 550 nm, and the third layer may have a refractive index in the range of about 1.2 to about 1.5 at a wavelength of about 550 nm.

[0013] In an embodiment, the refractive index of the first layer may be smaller than that of the base layer, and the refractive index of the second layer may be greater than that of the first layer.

[0014] In an embodiment, the second layer may include a solid solution in which silicon dioxide and aluminum oxide are mixed.

[0015] In an embodiment, reflectivity on the upper surface of the third layer may be about 6.0% or less at a wavelength of about 550 nm.

[0016] In an embodiment, the third layer may include a fluoropolymer.

[0017] In an embodiment, the base layer may include a glass substrate or a polymer film.

[0018] In an implementation, the first layer may have a thickness in a range of about 60 nm to about 80 nm, and the third layer may have a thickness in a range of about 5 nm to about 40 nm.

[0019] In an embodiment, the window may further include a fourth layer disposed between the base layer and the first layer and including magnesium oxide.

[0020] In an embodiment, the window may further include a fifth layer disposed between the base layer and the first layer. The fifth layer has a refractive index in a range of about 1.7 to about 3.0 at a wavelength of about 550 nm.

[0021] In an embodiment, the fifth layer may include a material selected from zinc oxide (ZnO 2 ), hafnium oxide (HfO 2 ), Tantalum Oxide (Ta 2 O 5 ), niobium oxide (Nb 2 O 5 ), titanium oxide (TiO 2 ), Ytterbium oxide (Y 2 O 3 ), silicon nitride (Si 3 N 4 ), SrTiO 3 ), tungsten oxide (WO 3 ) and at least one compound selected from the group consisting of aluminum nitride (AlN).

[0022] In an embodiment, the window may further include a sixth layer disposed below the base layer. The sixth layer has a refractive index in a range of about 1.3 to about 1.5 at a wavelength of about 550 nm.

[0023] In an embodiment, the sixth layer may include at least one compound selected from the group consisting of magnesium oxide, magnesium fluoride, and yttrium oxyfluoride.

[0024] According to an embodiment of the present disclosure, a display device includes a display module and a window disposed on the display module. The window includes a base layer, a first layer disposed on the base layer, a second layer disposed on the first layer, and a third layer disposed on the second layer. The second layer includes silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ). The weight ratio of silicon dioxide to aluminum oxide in the second layer is in the range of about 25:75 to about 35:65.

[0025] In an embodiment, the display module may include a base substrate. A circuit layer is disposed on the base substrate. A light-emitting element layer is disposed on the circuit layer. The light-emitting element layer includes a plurality of light-emitting elements. An encapsulation layer is disposed on the light-emitting element layer. An anti-reflection layer is disposed on the encapsulation layer. The anti-reflection layer may include a partitioning layer having a plurality of partitioning openings respectively overlapping the plurality of light-emitting elements. A plurality of color filters are respectively disposed to correspond to the plurality of partitioning openings.

[0026] In an embodiment, the first layer may be spaced apart from the display module with the base layer interposed between the first layer and the display module.

[0027] In an embodiment, the upper surface of the third layer may define an outermost surface of the window. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The accompanying drawings are included to provide a further understanding of the embodiments of the present disclosure and are incorporated into and constitute a part of this specification. The accompanying drawings illustrate non-limiting embodiments of the present disclosure and together with the description serve to explain the principles of the present disclosure. In the drawings:

[0029] Figure 1A is an assembled perspective view of a display device according to an embodiment of the present disclosure;

[0030] Figure 1B is an exploded perspective view of a display device according to an embodiment of the present disclosure;

[0031] Figure 2 is a cross-sectional view of a display device according to an embodiment of the present disclosure;

[0032] Figure 3 is a cross-sectional view showing a portion of a display module according to an embodiment of the present disclosure; and

[0033] FIG. 4A to FIG. 4D is a cross-sectional view of a window according to an embodiment of the present disclosure. DETAILED DESCRIPTION

[0034] In this specification, when an element (or region, layer, part, etc.) is referred to as being "on", "connected to" or "coupled to" another element, it means that the element can be directly set on / directly connected to / directly coupled to another element, or a third element can be set between them.

[0035] The same reference numerals always represent the same components. In addition, in the drawings, the thickness, proportion and size of the components may be exaggerated for ease of description. The term "and / or" includes all of one or more combinations that can be defined by the relevant items.

[0036] It will be understood that although the terms "first", "second", etc. may be used herein to describe various components, these components should not be limited by these terms. These terms are only used to distinguish one component from another component. For example, without departing from the scope of the embodiments of the present disclosure, a first component may be referred to as a second component, and similarly, a second component may be referred to as a first component. Terms in the singular may include plural forms unless the context clearly indicates otherwise.

[0037] In addition, terms such as "below", "under", "on", and "over" may be used to describe the relationship between components shown in the drawings. However, these terms are used as relative concepts and are described with reference to the directions shown in the drawings.

[0038] It should be understood that the terms “including” or “having” are intended to specify the presence of the features, integers, steps, operations, components, parts or combinations thereof stated in the specification, but do not exclude the presence or addition of one or more other features, integers, steps, operations, components, parts or combinations thereof.

[0039] In this document, "directly disposed on..." means that there is no intervening layer, film, region, plate, etc. between a part such as a layer, film, region, and plate and another part. For example, "directly disposed on..." may mean that two layers or two components are disposed without using another component, such as an adhesive component, therebetween.

[0040] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those commonly understood by those skilled in the art to which the present disclosure belongs. In addition, it will be understood that terms (such as those defined in commonly used dictionaries) should be interpreted as having a meaning consistent with their meaning in the context of the relevant art, and will not be interpreted in an idealized or overly formal sense unless explicitly defined as such herein.

[0041] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings.

[0042] Figure 1A is an assembled perspective view of a display device according to an embodiment of the present disclosure. Figure 1B is an exploded perspective view of a display device according to an embodiment of the present disclosure.

[0043] refer to Figure 1A , the display device DD may be a device activated according to an electrical signal. For example, in an embodiment, the display device DD may display an image IM and sense an external input. The display device DD may include various embodiments. For example, the display device DD may be applied to a variety of different electronic devices. In an embodiment, the display device DD may include a computer (e.g., a tablet, a laptop computer), a smart TV, etc. However, the embodiments of the present disclosure are not necessarily limited thereto. Figure 1A In the embodiment shown in FIG. 2 , for convenience of explanation, a smart phone is shown as the display device DD.

[0044] In an embodiment, the display device DD may display an image IM toward a third direction DR3 on a display surface FS parallel to each of the first direction DR1 and the second direction DR2. The display surface FS on which the image IM is displayed may correspond to each of the front surface of the display device DD and the front surface FS of the window WM. Hereinafter, the same reference numerals will be given to the display surface and the front surface of the display device DD and the front surface of the window WM. The image IM may include at least one still image and / or at least one dynamic image. Figure 1A In the embodiment of the present invention, the image IM is a software application icon and a clock, temperature and calendar window. However, the embodiment of the inventive concept is not necessarily limited thereto, and the image IM may be a variety of different themes.

[0045] In the present embodiment, the front surface (e.g., the upper surface in the third direction DR3) and the rear surface (e.g., the lower surface in the third direction DR3) of each component are defined relative to the direction of displaying the image IM. The front surface and the rear surface may be opposite to each other in the third direction DR3. The normal direction of each of the front surface and the rear surface may be parallel to the third direction DR3. The spacing distance in the third direction DR3 between the front surface and the rear surface of each component may correspond to the thickness in the third direction DR3 of each component. However, the directions indicated by the first direction DR1, the second direction DR2, and the third direction DR3 are relative concepts and can be converted into different directions in which the first direction DR1, the second direction DR2, and the third direction DR3 intersect with each other. In the following, the first direction to the third direction refer to the same reference numerals as the directions indicated by the first direction DR1, the second direction DR2, and the third direction DR3, respectively. In addition, in the present specification, "on a plane" may be defined as observed from the third direction DR3.

[0046] The display device DD according to an embodiment of the present disclosure may detect an input from a user applied from the outside. In an embodiment, the user input may include various types of external inputs, such as a part of the user's body, light, heat, or pressure. In some embodiments, the user input may be provided in various types, and the display device DD may sense the user's input applied to the side surface or rear surface of the display device DD according to the structure of the display device DD. However, embodiments of the present disclosure are not necessarily limited to this.

[0047] like Figure 1A and Figure 1B As shown in , the display device DD includes a window WM, a display module DM and a housing HU. In an embodiment, the window WM and the housing HU are connected to define the appearance (e.g., external appearance) of the display device DD. In an embodiment, the housing HU, the display module DM and the window WM can be stacked sequentially in the third direction DR3.

[0048] In an embodiment, the window WM may include an optically transparent material. The window WM may include an insulating panel. For example, in some embodiments, the window WM may be made of glass, plastic, or a combination thereof.

[0049] As described above, the front surface FS of the window WM defines the front surface of the display device DD. The transmission area TA may be an optically transparent area. For example, in an embodiment, the transmission area TA may be a region having a visible light transmittance of about 90% or more.

[0050] The bezel area BZA may have a relatively lower transmittance than the transmission area TA. In an embodiment, the bezel area BZA may at least partially surround the transmission area TA (eg, in the first direction DR1 and / or the second direction DR2) to define a shape of the transmission area TA. The bezel area BZA may be adjacent to the transmission area TA.

[0051] In an embodiment, the border area BZA may have a specific color. The border area BZA may cover the peripheral area NAA of the display module DM to prevent the peripheral area NAA from being observed from the outside. However, this is shown only as an example, and embodiments of the present disclosure are not necessarily limited to this. For example, according to some embodiments, the border area BZA may be omitted in the window WM.

[0052] The display module DM may display an image IM and sense an external input. The image IM may be displayed on the front surface IS of the display module DM. The front surface IS of the display module DM includes an active area AA and a peripheral area NAA. The active area AA may be an area activated according to an electrical signal.

[0053] In an embodiment, the active area AA may be an area where the image IM is displayed, and may also be an area where an external input is sensed. The transmissive area TA (e.g., in the third direction DR3) at least overlaps with the active area AA. For example, the transmissive area TA may overlap with the entire surface or at least a portion of the active area AA. Therefore, the user may view the image IM or provide an external input through the transmissive area TA. However, the embodiments of the present disclosure are not necessarily limited thereto. For example, in some embodiments, the area on which the image IM is displayed in the active area AA and the area on which the external input is sensed in the active area AA may be separated from each other.

[0054] The peripheral area NAA may be an area covered by the border area BZA. The peripheral area NAA is adjacent to the active area AA (e.g., in the first direction DR1 and / or the second direction DR2). In an embodiment, the peripheral area NAA may at least partially surround the active area AA. A driving circuit or driving wiring for driving the active area AA may be provided in the peripheral area NAA.

[0055] In an embodiment, the display module DM may include a display panel and a sensor layer. The image IM may be substantially displayed in the display panel, and the external input may be substantially sensed in the sensor layer. The display module DM may include a display panel and a sensor layer, and thus may sense the external input while displaying the image IM. This will be described in detail later.

[0056] The display device DD according to the embodiment may further include a driving circuit. In the embodiment, the driving circuit may include a flexible circuit board and a main circuit board. The flexible circuit board may be electrically connected to the display module DM. The flexible circuit board may connect the display module DM to the main circuit board. However, the embodiments of the present disclosure are not necessarily limited thereto. For example, the flexible circuit board according to the embodiment of the present disclosure may not be connected to the main circuit board, and the flexible circuit board may be a rigid board.

[0057] In an embodiment, the flexible circuit board may be connected to the pads of the display module DM disposed in the peripheral area NAA. The flexible circuit board may provide the display module DM with an electrical signal for driving the display module DM. The electrical signal may be generated in the flexible circuit board or the main circuit board. In an embodiment, the main circuit board may include various driving circuits for driving the display module DM, a connector for providing power, etc. The main circuit board may be connected to the display module DM through the flexible circuit board.

[0058] although Figure 1B A state in which the display module DM is unfolded is shown, but at least a portion of the display module DM may be bent. For example, in an embodiment, a portion of the display module DM may be bent toward the rear surface of the display module DM, and the portion of the display module DM bent toward the rear surface may be a portion to which the main circuit board is connected. Therefore, the main circuit board may be assembled in a state overlapping with the rear surface of the display module DM (for example, in the third direction DR3).

[0059] The housing HU is coupled to the window WM to define an appearance (eg, external appearance) of the display device DD. The housing HU provides a predetermined internal space. The display module DM may be accommodated in the internal space.

[0060] In an embodiment, the housing HU may include a material having relatively high rigidity. For example, in an embodiment, the housing HU may have a plurality of frames and / or plates including glass, plastic, or metal, or a combination thereof. The housing HU may stably protect the components of the display device DD housed in the internal space from external impacts.

[0061] Figure 2 is a cross-sectional view of a display device according to an embodiment of the present disclosure.

[0062] refer to Figure 2 , the display device DD may include a display module DM and a window WM. In an embodiment, the display module DM and the window WM may be coupled together by an adhesive layer AD. In the display device DD of an embodiment, the display module DM may include a display panel 100, a sensor layer 200, and an anti-reflection layer 300. In an embodiment, the anti-reflection layer 300 among the multiple layers in the display module DM may be coupled to the window WM via an adhesive layer AD.

[0063] The display panel 100 may be a device that substantially generates an image (such as Figure 1A IM) components shown in the image IM). In an embodiment, the display panel 100 may be an emissive display panel. For example, in an embodiment, the display panel 100 may be an organic light-emitting display panel, an inorganic light-emitting display panel, a micro-LED display panel, or a nano-LED display panel. However, the embodiments of the present disclosure are not necessarily limited thereto. The display panel 100 may be referred to as a display layer.

[0064] In an implementation, the display panel 100 may include a base substrate 110 , a circuit layer 120 , a light emitting element layer 130 , and an encapsulation layer 140 .

[0065] The base substrate 110 may be a member that provides a base surface on which the circuit layer 120 is disposed. The base substrate 110 may be a rigid substrate or a flexible substrate that is bendable, foldable, rollable, etc. For example, in an embodiment, the base substrate 110 may be a glass substrate, a metal substrate, a polymer substrate, etc. However, the embodiments of the present disclosure are not necessarily limited thereto. For example, in some embodiments, the base substrate 110 may be an inorganic layer, an organic layer, or a composite material layer.

[0066] In an embodiment, the base substrate 110 may have a multi-layer structure. For example, the base substrate 110 may include a first synthetic resin layer, a multi-layer or single-layer inorganic layer, and a second synthetic resin layer disposed on the multi-layer or single-layer inorganic layer. Each of the first synthetic resin layer and the second synthetic resin layer may include a polyimide-based resin. However, embodiments of the present disclosure are not necessarily limited thereto.

[0067] The circuit layer 120 may be disposed on the base substrate 110 (eg, directly on the base substrate 110 in the third direction DR3 ). In an implementation, the circuit layer 120 may include an insulating layer, a semiconductor pattern, a conductive pattern, and a signal line.

[0068] The light emitting element layer 130 may be disposed on the circuit layer 120 (e.g., directly disposed on the circuit layer 120 in the third direction DR3). The light emitting element layer 130 may include a plurality of light emitting elements. For example, in an embodiment, the light emitting element may include an organic light emitting material, an inorganic light emitting material, an organic-inorganic light emitting material, a quantum dot, a quantum rod, a micro LED, or a nano LED. However, embodiments of the present disclosure are not necessarily limited thereto.

[0069] The encapsulation layer 140 may be disposed on the light emitting element layer 130 (e.g., directly disposed on the light emitting element layer 130). The encapsulation layer 140 may protect the light emitting element layer 130 from foreign matter such as moisture, oxygen, and dust particles. The encapsulation layer 140 may include at least one inorganic layer. For example, in an embodiment, the encapsulation layer 140 may include a stacked structure of an inorganic layer / organic layer / inorganic layer. However, embodiments of the present disclosure are not necessarily limited thereto. For example, in some embodiments, the encapsulation layer 140 may include at least one organic layer and at least one inorganic layer.

[0070] The sensor layer 200 may be disposed on the display panel 100. The sensor layer 200 may sense an external input applied from the outside. For example, the external input may be a user input. In an embodiment, the user input may include various types of external inputs such as a part of the user's body, light, heat, a pen, or pressure.

[0071] In an embodiment, the sensor layer 200 may be disposed on the display panel 100 through a continuous process. In this case, the sensor layer 200 may be directly disposed on the display panel 100 (for example, in the third direction DR3). Here, "directly disposed on" may mean that a third component is not disposed between the sensor layer 200 and the display panel 100. For example, a separate adhesive member may not be disposed between the sensor layer 200 and the display panel 100.

[0072] In an embodiment, the anti-reflection layer 300 may be directly disposed on the sensor layer 200 (e.g., in the third direction DR3). The anti-reflection layer 300 may reduce the reflectivity of external light incident from the outside of the display device DD. The anti-reflection layer 300 may be disposed on the sensor layer 200 by a continuous process. In an embodiment, the anti-reflection layer 300 may include a color filter. The color filter may have a predetermined arrangement. For example, in an embodiment, the color filter may be arranged in consideration of the emission color of the pixels included in the display panel 100. In addition, the anti-reflection layer 300 may further include a black matrix adjacent to the color filter. A detailed description of the anti-reflection layer 300 will be given later.

[0073] In an embodiment of the present disclosure, the sensor layer 200 may be omitted. In this embodiment, the anti-reflection layer 300 may be directly disposed on the display panel 100 (eg, in the third direction DR3). In an embodiment of the present disclosure, the positions of the sensor layer 200 and the anti-reflection layer 300 may be swapped.

[0074] In an embodiment of the present disclosure, the display device DD may further include an optical layer disposed on the anti-reflection layer 300 (e.g., disposed above the anti-reflection layer 300). For example, in an embodiment, the optical layer may be disposed on the anti-reflection layer 300 by a continuous process. The optical layer may control the direction of light incident from the display panel 100 to increase the front brightness of the display device DD. For example, in an embodiment, the optical layer may include an organic insulating layer and a high refractive layer, in which openings are defined to correspond to light emitting areas of pixels included in the display panel 100, respectively, and the high refractive layer covers the organic insulating layer and fills the openings. The refractive index of the high refractive layer may be higher than the refractive index of the organic insulating layer.

[0075] The window WM may provide a front surface of the display device DD. In an embodiment, the window WM may include a glass film or a synthetic resin film as a base film. In an embodiment, the window WM may also include a functional layer such as an anti-reflection layer and an anti-fingerprint layer. FIG. 4A to FIG. 4D The functional layers included in the window WM are described in more detail in the description of FIG. In an embodiment, the window WM may further include a frame pattern overlapping with the frame area BZA in the third direction DR3 (see FIG. Figure 1B ).

[0076] Figure 3 is a cross-sectional view showing a portion of a display module according to an embodiment of the present disclosure. Figure 3 A partial cross-sectional view of a single light emitting element LD and a single pixel circuit PC included in the display module DM is shown.

[0077] The display panel 100 included in the display module DM of the embodiment may include a base substrate 110. The base substrate 110 may be a member that provides a base surface on which the circuit layer 120 is disposed. In an embodiment, the base substrate 110 may be a glass substrate, a metal substrate, a plastic substrate, a silicone substrate, etc. However, the embodiments of the present disclosure are not necessarily limited thereto, and in some embodiments, the base substrate 110 may be an inorganic layer, an organic layer, or a composite material layer.

[0078] The buffer layer 10br may be disposed on the base substrate 110 (e.g., directly on the base substrate 110 in the third direction DR3). In an embodiment, the buffer layer 10br may prevent metal atoms or impurities from diffusing from the base substrate 110 to the first semiconductor pattern SP1 thereover. The first semiconductor pattern SP1 includes a channel region AC1 of a silicon transistor S-TFT. The buffer layer 10br may adjust a heat supply speed during a crystallization process for forming the first semiconductor pattern SP1, thereby uniformly forming the first semiconductor pattern SP1.

[0079] The first semiconductor pattern SP1 may be disposed on the buffer layer 10br (e.g., directly disposed on the buffer layer 10br in the third direction DR3). In an embodiment, the first semiconductor pattern SP1 may include a silicon semiconductor. For example, in an embodiment, the silicon semiconductor may include amorphous silicon, polycrystalline silicon, or single crystal silicon. For example, the first semiconductor pattern SP1 may include low temperature polycrystalline silicon. However, embodiments of the present disclosure are not necessarily limited thereto.

[0080] Figure 3 Only a portion of the first semiconductor pattern SP1 disposed on the buffer layer 10br is shown, and the first semiconductor pattern SP1 may be further disposed in other regions. The first semiconductor pattern SP1 may be arranged throughout the pixel in a specific rule. Depending on whether the first semiconductor pattern SP1 is doped, the electrical properties of the first semiconductor pattern SP1 may be different. For example, in an embodiment, the first semiconductor pattern SP1 may include a first region having high conductivity and a second region having low conductivity. The first region may be doped with an N-type dopant or a P-type dopant. A P-type transistor may include a doped region doped with a P-type dopant, and an N-type transistor may include a doped region doped with an N-type dopant. The second region may be a non-doped region, or may be a region doped with a concentration less than that of the first region.

[0081] The first region may have a greater conductivity than the second region and may be substantially used as an electrode or a signal line. The second region may substantially correspond to an active region (e.g., a channel) of a transistor. For example, a portion of the first semiconductor pattern SP1 may be an active region of a transistor, another portion may be a source or drain of the transistor, and another portion may be a connecting electrode or a connecting signal line.

[0082] A source region SE1 (eg, source), a channel region AC1 (eg, channel), and a drain region DE1 (eg, drain) of the silicon transistor S-TFT may be formed from the first semiconductor pattern SP1. The source region SE1 and the drain region DE1 may extend in opposite directions from the channel region AC1 in cross section.

[0083] In an embodiment, the rear metal layer may be disposed under each of the silicon transistor S-TFT and the oxide transistor O-TFT. The rear metal layer may be disposed to overlap with the pixel circuit PC (e.g., in the third direction DR3), and may block external light from reaching the pixel circuit PC. The rear metal layer may be disposed between the base substrate 110 and the buffer layer 10br (e.g., in the third direction DR3). However, the embodiments of the present disclosure are not necessarily limited thereto. For example, in an embodiment, the rear metal layer may be disposed between the second insulating layer 20 and the third insulating layer 30 (e.g., in the third direction DR3). The rear metal layer may include a reflective metal. For example, in an embodiment, the rear metal layer may include silver (Ag), an alloy containing silver (Ag), molybdenum (Mo), an alloy containing molybdenum, aluminum (Al), an alloy containing aluminum, aluminum nitride (AlN), tungsten (W), tungsten nitride (WN), copper (Cu), P+ doped amorphous silicon, etc. The rear metal layer may be connected to an electrode or wiring, and may receive a constant voltage or signal therefrom. According to an embodiment of the present disclosure, the rear metal layer may be a floating electrode isolated from another electrode or wiring. In an embodiment of the present disclosure, an inorganic barrier layer may be further disposed between the base substrate 110 and the buffer layer 10br (eg, in the third direction DR3).

[0084] The first insulating layer 10 may be disposed on the buffer layer 10br (e.g., directly disposed on the buffer layer 10br in the third direction DR3). The first insulating layer 10 overlaps with a plurality of pixels in common and may cover the first semiconductor pattern SP1. The first insulating layer 10 may be an inorganic layer and / or an organic layer and have a single-layer or multi-layer structure. For example, in an embodiment, the first insulating layer 10 may include at least one of aluminum oxide, titanium oxide, silicon oxide, silicon nitride, silicon oxynitride, zirconium oxide, and hafnium oxide. In this embodiment, the first insulating layer 10 may include a single-layer silicon oxide layer. The insulating layer of the circuit layer 120 to be described later except the first insulating layer 10 may be an inorganic layer and / or an organic layer and may have a single-layer or multi-layer structure. The inorganic layer may include at least one of the above materials. However, embodiments of the present disclosure are not necessarily limited thereto.

[0085] The gate GT1 of the silicon transistor S-TFT is disposed on the first insulating layer 10 (for example, directly disposed on the first insulating layer 10 in the third direction DR3). The gate GT1 may be a part of the metal pattern. The gate GT1 (for example, in the third direction DR3) overlaps with the channel region AC1. In a process in which the first semiconductor pattern SP1 is doped, the gate GT1 may be used as a mask. In an embodiment, the gate GT1 may include titanium (Ti), silver (Ag), an alloy containing silver, molybdenum (Mo), an alloy containing molybdenum, aluminum (Al), an alloy containing aluminum, aluminum nitride (AlN), tungsten (W), tungsten nitride (WN), copper (Cu), indium tin oxide (ITO), indium zinc oxide (IZO), etc. However, embodiments of the present disclosure are not necessarily limited thereto.

[0086] The second insulating layer 20 may be disposed on the first insulating layer 10 (for example, in the third direction DR3) to cover the gate GT1. The third insulating layer 30 may be disposed on the second insulating layer 20 (for example, in the third direction DR3). The second electrode CE20 of the storage capacitor Cst may be disposed between the second insulating layer 20 and the third insulating layer 30. In addition, the first electrode CE10 of the storage capacitor Cst may be disposed between the first insulating layer 10 and the second insulating layer 20.

[0087] The second semiconductor pattern SP2 may be disposed on the third insulating layer 30 (e.g., directly on the third insulating layer 30 in the third direction DR3). The second semiconductor pattern SP2 may include a channel region AC2 of an oxide transistor O-TFT to be described later. The second semiconductor pattern SP2 may include an oxide semiconductor. In an embodiment, the second semiconductor pattern SP2 may include a transparent conductive oxide (TCO) such as indium tin oxide (ITO), indium zinc oxide (IZO), indium gallium zinc oxide (IGZO), zinc oxide (ZnO), or indium oxide (In 2 O 3 ). However, the embodiments of the present disclosure are not necessarily limited thereto.

[0088] The oxide semiconductor may include a plurality of regions divided according to whether the transparent conductive oxide is reduced or not. The region where the transparent conductive oxide is reduced (hereinafter referred to as the reduction region) has a greater conductivity than the region where the transparent conductive oxide is not reduced (hereinafter referred to as the non-reduction region). The reduction region substantially serves as a source / drain or a signal line of a transistor. The non-reduction region substantially corresponds to a semiconductor region (e.g., an active region or a channel) of a transistor. For example, a portion of the second semiconductor pattern SP2 may be a semiconductor region of a transistor, another portion of the region may be a source region / drain region of a transistor, and another portion of the region may be a signal transmission region.

[0089] A source region SE2 (eg, source), a channel region AC2 (eg, channel), and a drain region DE2 (eg, drain) of the oxide transistor O-TFT may be formed from the second semiconductor pattern SP2. The source region SE2 and the drain region DE2 may extend in opposite directions from the channel region AC2 in a cross section.

[0090] The fourth insulating layer 40 may be disposed on the third insulating layer 30 (e.g., in the third direction DR3). The fourth insulating layer 40 overlaps the plurality of pixels in common and may cover the second semiconductor pattern SP2. In an embodiment, the fourth insulating layer 40 may be disposed in the form of an insulating pattern that overlaps the gate electrode GT2 of the oxide transistor O-TFT and exposes the source region SE2 and the drain region DE2 of the oxide transistor O-TFT.

[0091] The gate GT2 of the oxide transistor O-TFT is disposed on the fourth insulating layer 40. The gate GT2 of the oxide transistor O-TFT may be a part of the metal pattern. The gate GT2 of the oxide transistor O-TFT overlaps the channel region AC2 (eg, in the third direction DR3).

[0092] The fifth insulating layer 50 may be disposed on the fourth insulating layer 40 (e.g., in the third direction DR3) and may cover the gate GT2. The first connection electrode CNE1 may be disposed on the fifth insulating layer 50 (e.g., directly on the fifth insulating layer 50 in the third direction DR3). In an embodiment, the first connection electrode CNE1 may be connected to the drain region DE1 of the silicon transistor S-TFT through a contact hole passing through the first insulating layer 10, the second insulating layer 20, the third insulating layer 30, the fourth insulating layer 40, and the fifth insulating layer 50.

[0093] The sixth insulating layer 60 may be disposed on the fifth insulating layer 50 (e.g., directly disposed on the fifth insulating layer 50 in the third direction DR3). The second connection electrode CNE2 may be disposed on the sixth insulating layer 60 (e.g., directly disposed on the sixth insulating layer 60 in the third direction DR3). In an embodiment, the second connection electrode CNE2 may be connected to the first connection electrode CNE1 through a contact hole passing through the sixth insulating layer 60. The seventh insulating layer 70 may be disposed on the sixth insulating layer 60 (e.g., directly disposed on the seventh insulating layer 70 in the third direction DR3) to cover the second connection electrode CNE2. The eighth insulating layer 80 may be disposed on the seventh insulating layer 70 (e.g., directly disposed on the seventh insulating layer 70 in the third direction DR3).

[0094] In an embodiment, each of the sixth insulating layer 60, the seventh insulating layer 70, and the eighth insulating layer 80 may be an organic layer. For example, in an embodiment, each of the sixth insulating layer 60, the seventh insulating layer 70, and the eighth insulating layer 80 may include a general polymer such as benzocyclobutene (BCB), polyimide, hexamethyldisiloxane (HMDSO), polymethylmethacrylate (PMMA), or polystyrene (PS), a polymer derivative having a phenol group, an acrylic polymer, an imide polymer, an aryl ether-based polymer, an amide-based polymer, a fluorine-based polymer, a p-xylene-based polymer, a vinyl alcohol-based polymer, a blend thereof, and the like.

[0095] The light emitting element LD may include a first electrode AE ​​(eg, a pixel electrode), an emission layer EML, and a second electrode CE (eg, a common electrode). Each of the emission layer EML and the second electrode CE may be commonly provided in a plurality of pixels.

[0096] The first electrode AE ​​of the light emitting element LD may be disposed on the eighth insulating layer 80 (for example, directly disposed on the eighth insulating layer 80 in the third direction DR3). The first electrode AE ​​of the light emitting element LD may be a transmissive electrode, a semi-transmissive and semi-reflective electrode, or a reflective electrode. According to an embodiment of the present disclosure, the first electrode AE ​​of the light emitting element LD may include a reflective layer formed of Ag, Mg, Al, Pt, Pd, Au, Ni, Nd, Ir, Cr, or a compound thereof, and a transparent or semi-transparent electrode layer formed on the reflective layer. In an embodiment, the transparent or semi-transparent electrode layer may include an electrode selected from indium tin oxide (ITO), indium zinc oxide (IZO), indium gallium zinc oxide (IGZO), zinc oxide (ZnO), indium oxide (In 2 O 3 ) and aluminum-doped zinc oxide (AZO). For example, the first electrode AE ​​of the light emitting element LD may include a stacked structure of ITO / Ag / ITO.

[0097] The pixel defining film PDL may be disposed on the eighth insulating layer 80 (e.g., directly disposed on the eighth insulating layer 80 in the third direction DR3). In an embodiment, the pixel defining film PDL may include the same material and may be formed by the same process. The pixel defining film PDL may have a property of absorbing light, and for example, the pixel defining film PDL may have a black color. For example, the pixel defining film PDL may include a black colorant. The black colorant may include a black dye and a black pigment. In an embodiment, the black colorant may include carbon black, a metal such as chromium, or an oxide thereof. The pixel defining film PDL may correspond to a shading pattern having a shading property.

[0098] The pixel definition film PDL may cover a portion of the first electrode AE ​​of the light emitting element LD. For example, an opening PDL-OP for exposing a portion of the first electrode AE ​​of the light emitting element LD may be defined in the pixel definition film PDL. Figure 3 As shown in, in an embodiment, the pixel defining film PDL may cover the side ends of the first electrode AE, and the opening PDL-OP may expose the central portion of the first electrode AE. However, the embodiments of the present disclosure are not necessarily limited thereto. The pixel defining film PDL may increase the distance between the edge of the first electrode AE ​​and the second electrode CE of the light emitting element LD. Therefore, arcing, etc. may be prevented from being generated at the edge of the first electrode AE ​​by the pixel defining film PDL.

[0099] In an embodiment, the hole control layer may be disposed between the first electrode AE ​​and the emission layer EML (for example, in the third direction DR3). In an embodiment, the hole control layer may include a hole transport layer and may further include a hole injection layer. The electron control layer may be disposed between the emission layer EML and the second electrode CE (for example, in the third direction DR3). In an embodiment, the electron control layer may include an electron transport layer and may further include an electron injection layer. The hole control layer and the electron control layer may be formed in a plurality of pixels by using an open mask.

[0100] The encapsulation layer 140 may be disposed (for example, in the third direction DR3) on the light emitting element layer 130. In an embodiment, the encapsulation layer 140 may include (for example, in the third direction DR3) an inorganic layer 141, an organic layer 142, and an inorganic layer 143 sequentially stacked, but the layers constituting the encapsulation layer 140 are not necessarily limited thereto.

[0101] The inorganic layers 141 and 143 may protect the light emitting element layer 130 from moisture and oxygen, and the organic layer 142 may protect the light emitting element layer 130 from foreign matter such as dust particles. In an embodiment, the inorganic layers 141 and 143 may include a silicon nitride layer, a silicon oxynitride layer, a silicon oxide layer, a titanium oxide layer, an aluminum oxide layer, etc. The organic layer 142 may include an acrylic-based organic layer. However, embodiments of the present disclosure are not necessarily limited thereto.

[0102] In an embodiment, the sensor layer 200 may be disposed on the display panel 100 (for example, in the third direction DR3). The sensor layer 200 may be referred to as a sensor, an input sensing layer, or an input sensing panel. In an embodiment, the sensor layer 200 may include a sensor base layer 210, a first conductive layer 220, a sensing insulating layer 230, and a second conductive layer 240.

[0103] In an embodiment, the sensor base layer 210 may be directly disposed on the display panel 100 (for example, in the third direction DR3). In an embodiment, the sensor base layer 210 may be an inorganic layer including at least one of silicon nitride, silicon oxynitride, and silicon oxide. Alternatively, the sensor base layer 210 may be an organic layer including epoxy resin, acrylic resin, or imide-based resin. The sensor base layer 210 may have a single-layer structure or a multi-layer structure stacked in the third direction DR3.

[0104] Each of the first conductive layer 220 and the second conductive layer 240 may have a single layer structure or a multilayer structure stacked in the third direction DR3. The first conductive layer 220 and the second conductive layer 240 may include conductive lines defining sensing electrodes in a mesh shape. The conductive lines may not overlap with the opening PDL-OP (for example, in the third direction DR3), but may overlap with the pixel definition film PDL (for example, in the third direction DR3).

[0105] In an embodiment, the single-layer conductive layer may include a metal layer or a transparent conductive layer. The metal layer may include molybdenum, silver, titanium, copper, aluminum or an alloy thereof. The transparent conductive layer may include a transparent conductive oxide such as indium tin oxide (ITO), indium zinc oxide (IZO), zinc oxide (ZnO), indium zinc tin oxide (IZTO), etc. In addition, the transparent conductive layer may include a conductive polymer such as PEDOT, a metal nanowire, graphene, etc. However, the embodiments of the present disclosure are not necessarily limited thereto.

[0106] The conductive layer having a multi-layer structure may include a metal layer. In an embodiment, the metal layer may have a three-layer structure of titanium / aluminum / titanium. The conductive layer having a multi-layer structure may include at least one metal layer and at least one transparent conductive layer.

[0107] The sensing insulating layer 230 may be disposed between the first conductive layer 220 and the second conductive layer 240. In an embodiment, the sensing insulating layer 230 may include an inorganic film. For example, the inorganic film may include at least one of aluminum oxide, titanium oxide, silicon oxide, silicon nitride, silicon oxynitride, zirconium oxide, and hafnium oxide. However, embodiments of the present disclosure are not necessarily limited thereto.

[0108] Alternatively, the sensing insulating layer 230 may include an organic film. For example, the organic film may include at least any one of acrylic resin, methacrylic resin, polyisoprene, vinyl resin, epoxy resin, urethane resin, cellulose resin, siloxane resin, polyimide resin, polyamide resin, and perylene resin. However, embodiments of the present disclosure are not necessarily limited thereto.

[0109] In an implementation, the anti-reflection layer 300 may be disposed on the sensor layer 200 (eg, directly on the sensor layer 200 in the third direction DR3 ). In an implementation, the anti-reflection layer 300 may include a dividing layer 310 , a plurality of color filters 320 , and a planarization layer 330 .

[0110] The anti-reflection layer 300 may reduce the reflectivity of external light. The anti-reflection layer 300 may include a plurality of color filters 320, and the plurality of color filters 320 may have a predetermined arrangement. For example, the arrangement of the plurality of color filters 320 may be determined in consideration of the emission colors of the pixels included in the display panel 100. In the display module DM of the embodiment, the anti-reflection layer 300 may not include a phase retarder and a polarizer, and the reflectivity of the display module DM may be reduced by the plurality of color filters 320. In the display module DM of the embodiment, the anti-reflection layer 300 may not include a polarizing film or a polarizing layer.

[0111] The material constituting the partition layer 310 is not particularly limited as long as it is a material that absorbs light. In an embodiment, the partition layer 310 is a black layer. For example, the partition layer 310 may include a black colorant. The black colorant may include a black dye and a black pigment. For example, the black colorant may include carbon black, a metal such as chromium, or an oxide thereof.

[0112] The dividing layer 310 may cover the second conductive layer 240 of the sensor layer 200. The dividing layer 310 may prevent external light reflection of the second conductive layer 240. The dividing layer 310 may overlap a portion of the pixel defining layer PDL (eg, in the third direction DR3).

[0113] In an embodiment, at least one partition opening 310-OP2 may be defined in the partition layer 310. For example, the partition layer 310 may include a plurality of partition openings 310-OP2. Each of the plurality of partition openings 310-OP2 may overlap (for example, in the third direction DR3) with one of the plurality of light emitting elements LD (such as the first electrode AE ​​of the light emitting element LD). Any one of the plurality of color filters 320 may overlap with the first electrode AE ​​of the light emitting element LD. Any one of the plurality of color filters 320 may cover the partition opening 310-OP2. For example, the plurality of color filters 320 may be respectively arranged to correspond to the plurality of partition openings 310-OP2. Each of the plurality of color filters 320 may be in direct contact with the partition layer 310.

[0114] The planarization layer 330 may cover the partition layer 310 and the plurality of color filters 320. In an embodiment, the planarization layer 330 may include an organic material, and a flat surface may be provided in the upper surface of the planarization layer 330. However, the embodiments of the present disclosure are not necessarily limited thereto. For example, in an embodiment, the planarization layer 330 may be omitted.

[0115] FIG. 4A to FIG. 4D Each of is a cross-sectional view of a window according to an embodiment of the present disclosure.

[0116] refer to Figure 4A According to an embodiment of the present disclosure, the window WM includes a base layer BL, a first layer LRL, a second layer ML, and a third layer FL. Figure 4A In the window WM of the embodiment shown in , the base layer BL, the first layer LRL, the second layer ML, and the third layer FL may be sequentially stacked (eg, in the third direction DR3 ).

[0117] The base layer BL may include a transparent material. For example, in an embodiment, the base layer BL may include glass, tempered glass, or a polymer film. In an embodiment, the base layer BL may be a chemically strengthened glass substrate. In an embodiment in which the base layer BL is a chemically strengthened glass substrate, the base layer BL may be relatively thin and increase mechanical strength, and thus may be used as a window of a foldable display device. In an embodiment in which the base layer BL includes a polymer film, the base layer BL may include a polyimide (PI) film or a polyethylene terephthalate (PET) film.

[0118] The base layer BL of the window WM may have a multi-layer structure or a single-layer structure. For example, in an embodiment, the base layer BL may have a structure in which a plurality of polymer films are coupled to each other by an adhesive member, or may have a structure in which a glass substrate and a polymer film are coupled to each other by an adhesive. The base layer BL may be made of a flexible material.

[0119] In an embodiment, the thickness d1 of the base layer BL (eg, the length in the third direction DR3) may be, for example, in the range of about 20 μm to about 60 μm. For example, in an embodiment, the thickness d1 of the base layer BL may be in the range of about 20 μm to about 40 μm. Figure 4A and Figure 4B The base layer BL is shown to have a rectangular shape, but the base layer BL is not necessarily limited thereto. For example, in an embodiment, the base layer BL may have a shape in which a side edge portion of an upper surface of the base layer BL is rounded by curving the surface. For example, the base layer BL may have a shape in which a side edge portion of an upper surface of the base layer BL is rounded by curving the surface. Figure 1B ) The overlapping edge portions are rounded by curving the surface.

[0120] The first layer LRL is a layer having a refractive index lower than that of the base layer BL, and may be a layer for reducing the surface reflectivity of the window WM. The first layer LRL may be disposed on the base layer BL (for example, in the third direction DR3). The first layer LRL may be a layer directly disposed on the base layer BL. For example, the first layer LRL may be disposed on the upper surface of the base layer BL, and the lower surface of the base layer BL may be the same as the display module DM described above (see Figure 2 For example, the first layer LRL may be spaced apart from the display module DM (eg, in the third direction DR3) with the base layer BL interposed therebetween.

[0121] The first layer LRL may include a material having a low refractive index and high adhesion to the base layer BL. In an embodiment, the first layer LRL may include a first material, and the first material may include a material having a refractive index lower than that of a material included in the base layer BL. In an embodiment, the first material included in the first layer LRL may include, for example, silicon dioxide, fused silicon dioxide, fluorine-doped fused silicon dioxide, magnesium fluoride (MgF 2 ), calcium fluoride (CaF 2 ), aluminum fluoride (AlF 3 ), yttrium fluoride (YF 3 ), Ytterbium fluoride (YbF 3 ), aluminum oxide (Al 2 O 3 ) and magnesium oxide (MgO). For example, the first LRL layer may include magnesium fluoride (MgF 2 ) and magnesium oxide (MgO) as the first material.

[0122] In an embodiment, the first LRL layer may include magnesium fluoride (MgF 2 ). For example, the first layer LRL may be a single layer made of magnesium fluoride.

[0123] Alternatively, in addition to magnesium fluoride, the first layer LRL may further include magnesium oxide (MgO) and yttrium oxyfluoride (YOF). In an embodiment, the first layer LRL may include a solid solution containing magnesium oxide in the structure. For example, the first layer LRL may include a solid solution in which magnesium oxide, magnesium fluoride, and yttrium oxyfluoride are mixed.

[0124] The thickness d2 of the first layer LRL (e.g., the length in the third direction DR3) may be, for example, in the range of about 50 nm to about 90 nm. For example, in an embodiment, the thickness d2 of the first layer LRL may be in the range of about 60 nm to about 80 nm. In a comparative embodiment in which the thickness d2 of the first layer LRL is less than about 50 nm, the surface reflectivity of the window WM may not be sufficiently reduced. In a comparative embodiment in which the thickness d2 of the first layer LRL is greater than about 90 nm, the total thickness of the window WM may increase, so that the total thickness of the display device may be excessively increased.

[0125] In an embodiment, at a wavelength of about 550 nm, the first layer LRL may have a refractive index of about 1.5 or less. For example, at a wavelength of about 550 nm, the first layer LRL may have a refractive index in the range of about 1.3 to about 1.5. In the window WM of an embodiment, at a wavelength of about 550 nm, the first layer LRL may have a refractive index in the range of about 1.38 to about 1.40. Since the refractive index of the first layer LRL satisfies the above range at a wavelength of about 550 nm, the surface reflectivity of the window WM can be reduced.

[0126] In an embodiment, the first layer LRL may be formed by an ion-assisted deposition process. For example, in an embodiment, as described above, the first layer LRL may be formed of magnesium oxide, magnesium fluoride, and yttrium oxyfluoride. In the process of forming the first layer LRL, each of magnesium oxide, magnesium fluoride, and yttrium oxyfluoride is deposited on the surface of the base layer BL in the form of particles, while ionized argon (Ar) gas or oxygen (O) is provided together during the deposition process. 2 ) gas, so that the adhesion of the deposited film to the surface of the base layer BL can be increased. Alternatively, the first layer LRL may be formed of a single material of magnesium fluoride, and the magnesium fluoride may be deposited on the surface of the base layer BL in the form of particles while providing ionized argon (Ar) gas or oxygen (O 2 ) gas, thereby increasing the adhesion of the deposited film to the surface of the base layer BL.

[0127] In an embodiment, the first layer LRL may have a single layer structure formed of a single material. As described above, the first layer LRL may be a single layer formed of magnesium fluoride, or a single layer formed of a solid solution in which magnesium oxide, magnesium fluoride, and yttrium oxyfluoride are mixed. For example, the first layer LRL may not include a plurality of layers.

[0128] The second layer ML may be disposed on the first layer LRL (e.g., directly disposed on the first layer LRL in the third direction DR3), and may be a layer for increasing adhesion between the first layer LRL and the third layer FL. The second layer ML may have high adhesion to each of the first layer LRL and the third layer FL, and may be an adhesion promoter that increases interlayer adhesion between the first layer LRL and the third layer FL. In addition, the second layer ML may be disposed on the first layer LRL to increase chemical resistance, scratch resistance, and wear resistance of the window WM. In an embodiment, the second layer ML may be directly disposed on the first layer LRL.

[0129] The second layer ML may have high mechanical strength and may include a material for increasing adhesion. In an embodiment, the second layer ML may include silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 The aluminum oxide (Al2O3) included in the second layer ML 2 O 3 ) is greater than the content of silicon dioxide (SiO 2 In an embodiment, the silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) may be in a weight ratio of about 25:75 to about 35:65. For example, silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) may satisfy the following Expression 1 to Expression 3:

[0130] [Expression 1]

[0131] 25≤a≤35

[0132] [Expression 2]

[0133] 65≤b≤75

[0134] [Expression 3]

[0135] a+b=100

[0136] In Expression 1 to Expression 3, "a" represents silicon dioxide (SiO 2 ) by weight, and "b" represents aluminum oxide (Al 2 O 3 ) by weight. 2 ) and aluminum oxide (Al 2 O 3) in an embodiment in which the weight ratio of the window WM satisfies the above range, both the optical properties and the mechanical durability of the window WM can be increased.

[0137] The second layer ML may be disposed between the first layer LRL and the third layer FL to increase the adhesive strength between the first layer LRL and the third layer FL. In addition, the second layer ML may increase the surface hardness of the window WM while increasing the wear resistance and scratch resistance.

[0138] Only silicon dioxide (SiO 2 ) is limited by its poor resistance to thermal shock and stress. However, studies have been conducted on the 2 ) and metal oxides (such as aluminum oxide (Al 2 O 3 )) is mixed to form a thin film to increase the resistance to thermal shock and stress. 2 O 3 ) and silicon dioxide (SiO 2 ) mixed, the effects of increasing the adhesion between the layers, increasing the film hardness and increasing the friction durability can be shown, but the above effects can be reduced with the increase of silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) content composition ratio varies significantly. In the embodiment of the present disclosure, the silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) is applied within the above range, thereby increasing the adhesion between the layers and maximizing the effects of hardness, wear resistance, scratch resistance, etc.

[0139] In an embodiment, the second layer ML may include silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 The second layer ML may include, for example, silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) mixed solid solution.

[0140] In an embodiment, silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) may be present as a substitutional solid solution in the second layer ML. For example, the second material included in the second layer ML may have a structure including AlSiO 5 solid solution structure.

[0141] In an embodiment, the second layer ML may have a single-layer structure formed of a single material. As described above, the second layer ML may be a single layer formed of a solid solution in which magnesium oxide and silicon dioxide are mixed, or a single layer formed of a solid solution in which aluminum oxide and silicon dioxide are mixed. The second layer ML may be a single layer formed of AlSiO 5 For example, the second layer ML may not include multiple layers.

[0142] In addition to silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ), the second layer ML may further include another component. For example, in an embodiment, the second layer ML may further include magnesium fluoride (MgF 2 ), calcium fluoride (CaF 2 ), aluminum fluoride (AlF 3 ), yttrium fluoride (YF 3 ), Ytterbium fluoride (YbF 3 ) and at least one of magnesium oxide (MgO).

[0143] Similar to the first layer LRL, the second layer ML may be formed by an ion-assisted deposition process. However, the embodiments of the present disclosure are not necessarily limited thereto, and the second layer ML may be formed by various deposition methods. For example, in an embodiment, the second layer ML may be formed by atomic layer deposition (ALD).

[0144] In an embodiment, the thickness d3 of the second layer ML (e.g., the length in the third direction DR3) may be, for example, in the range of about 10 nm to about 20 nm. In a comparative embodiment in which the thickness d3 of the second layer ML is less than about 10 nm, the adhesion between the first layer LRL and the third layer FL may not increase, and the mechanical strength of the window WM may decrease. In a comparative embodiment in which the thickness d3 of the second layer ML is greater than about 20 nm, the reflectivity of the window WM may increase, and the total thickness of the window WM may increase, so that the total thickness of the display device may be excessively increased.

[0145] In an embodiment, the refractive index of the second layer ML may be in the range of about 1.43 to about 1.50 at a wavelength of about 550 nm. Since the refractive index of the second layer ML satisfies the above range at a wavelength of about 550 nm, the surface reflectivity of the window WM may be reduced. The second layer ML may have a higher refractive index than the first layer LRL.

[0146] The third layer FL may be disposed on the second layer ML (for example, in the third direction DR3), and may be a layer that increases the anti-slip properties, scratch resistance, etc. of the surface of the window WM. In an embodiment, the third layer FL may be an anti-fingerprint layer having high fingerprint resistance and preventing surface wear. In an embodiment, the third layer FL may be disposed directly on the second layer ML (for example, in the third direction DR3). The third layer FL may be disposed on the uppermost layer of the window WM, and the upper surface of the third layer FL may define the uppermost surface of the window WM. For example, the upper surface of the third layer FL may define the outermost surface of the window WM.

[0147] The third layer FL may include a material having high scratch resistance and anti-slip properties and low refractive properties. In an embodiment, the third layer FL may include a fluorine-containing polymer. For example, the third layer FL may include, for example, a perfluoropolyether (PFPE) compound. In an embodiment, the third layer FL may include perfluoropolyether silane, perfluoroalkyl ether alkoxysilane, perfluoroalkyl ether copolymer, etc. Since the third layer FL includes the perfluoropolyether compound, the third layer FL may have increased fingerprint resistance and scratch resistance.

[0148] In an embodiment, the thickness d4 of the third layer FL (e.g., the length in the third direction DR3) may be, for example, in the range of about 5 nm to about 40 nm. In a comparative embodiment in which the thickness d4 of the third layer FL is less than about 5 nm, the fingerprint resistance and scratch resistance of the window WM may be reduced. In a comparative embodiment in which the thickness d4 of the third layer FL is greater than about 40 nm, the reflectivity of the window WM may increase, and the total thickness of the window WM may increase, so that the total thickness of the display device may be excessively increased.

[0149] In an embodiment, at a wavelength of about 550 nm, the third layer FL may have a refractive index in the range of about 1.2 to about 1.5. In the window WM of an embodiment, at a wavelength of about 550 nm, the third layer FL may have a refractive index in the range of about 1.20 to about 1.35. Since the refractive index of the third layer FL satisfies the above range at a wavelength of about 550 nm, the surface reflectivity of the window WM can be reduced.

[0150] In an embodiment, the total thickness (d2+d3+d4) of the first layer LRL, the second layer ML, and the third layer FL disposed on the base layer BL may be about 160 nm or less. In the window WM of an embodiment, the total thickness of the first layer LRL, the second layer ML, and the third layer FL disposed on the base layer BL of the window WM may be formed within a range of about 160 nm or less, thereby realizing a window WM having low reflective properties and high wear resistance, chemical resistance, polishing resistance, and hardness.

[0151] In the window WM of the embodiment, the surface of the window WM may have a reflectivity of about 6.0% or less at a wavelength of about 550nm. In the window WM of the embodiment, the third layer FL may be disposed on the uppermost layer, and the upper surface of the third layer FL may have a reflectivity of about 6.0% or less at a wavelength of about 550nm. The upper surface of the third layer FL may have a reflectivity in the range of about 5.8% to about 6.0% at a wavelength of about 550nm. In the present specification, the "reflectivity" of the window WM is defined as the proportion of light reflected to the outside in the light incident from the outside in the internal direction of the window WM. The light reflected to the outside includes both specularly reflected light reflected at the same angle as the incident light and diffusely reflected light scattered and reflected in various directions. For example, in the present specification, the reflectivity is defined as including the specularly reflected light (SCI) reflectivity.

[0152] The window WM of the embodiment may have a reflection color value a* in the range of about -2 to about 2 and a reflection color value b* in the range of about -1.5 to about 0.5 at a wavelength of about 550 nm. In an embodiment in which each of the reflection color values ​​a* and b* at a wavelength of about 550 nm satisfies the above range, the reflection of external light on the surface of the window WM can be reduced, and thus the visibility of the display device DD can be increased. By having the reflection color values ​​a* and b* in the above range, the window WM of the embodiment may exhibit a reflectivity of about 6.0% or less. In this specification, the reflection color values ​​"a*" and "b*" of the window WM represent the color values ​​"a" and "b" in the CIE coordinate system, respectively. The color values ​​a and b can be obtained from the CIE coordinate system, in which the x-axis representing the a value and the y-axis representing the b value are perpendicular to each other. As the absolute value of the a value increases in the positive direction, the color becomes red. As the absolute value of the a value increases in the negative direction, the color becomes green. As the absolute value of the b value increases in the positive direction, the color becomes yellow. As the absolute value of the b value increases in the negative direction, the color becomes blue. In this specification, the reflection color value of the window WM refers to a value measured in the specular reflection light exclusion (SCE) method.

[0153] Reference together Figure 1B , Figure 3 and Figure 4A , compared to an embodiment including a polarizing layer with increased reflectivity, as in the display device DD of the embodiment, when the anti-reflection layer 300 included in the display module DM includes a plurality of color filters 320, display efficiency can be increased. In the display device DD according to the embodiment of the present disclosure, the window WM includes the first layer LRL, the second layer ML, and the third layer FL (which includes a material with a low refractive index), and thus the surface reflectivity of the window WM can be reduced. Therefore, the reflectivity of the entire display device DD can be kept relatively low.

[0154] In the window WM according to an embodiment of the present disclosure, each of the first layer LRL, the second layer ML, and the third layer FL includes a low-refractive material, and the second layer ML includes silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ). In addition, in the window WM according to the embodiment, as the silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) is adjusted to be in the range of about 25:75 to about 35:65, the adhesion between the layers can be increased, and the optical characteristics, wear resistance, and scratch resistance of the window WM can be increased. The window WM according to the embodiment includes a structure of a first layer LRL and a second layer ML that are provided as a single layer while ensuring a low refractive property, and includes silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) is adjusted to a specific range, thereby exhibiting high optical characteristics and improving wear resistance and scratch resistance. Therefore, the reliability and durability of the display device DD including the window WM can be increased.

[0155] The window WM according to an embodiment of the present disclosure may include (for example, in the third direction DR3) a second layer ML interposed between the first layer LRL and the third layer FL, and silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) content is adjusted to a specific range, so that the chemical resistance and polishing resistance of the window WM can be increased. In the window WM of the embodiment, the silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) is adjusted to be within the range of about 25:75 to about 35:65, so that the chemical resistance and polishing resistance of the window WM can be increased, and thus the durability and reliability of the display device DD including the window WM can be increased.

[0156] The silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) does not satisfy the above range, the second layer ML or the third layer FL may be worn and lost in the evaluation of chemical resistance in which friction is applied under the condition where a solvent (such as alcohol) is applied, or in the evaluation of wear resistance in which friction is applied with steel wool or the like. In the window WM of the embodiment of the present disclosure, the silicon dioxide (SiO2 ) and aluminum oxide (Al 2 O 3 ) is adjusted to a specific range so that when friction is applied under the condition of applying a solvent (such as alcohol), the second layer ML or the third layer FL can be prevented from being lost, and when friction is applied with steel wool, etc., the second layer ML or the third layer FL can be prevented from being lost. Therefore, the chemical resistance and polishing resistance of the window WM can be increased, and thus the durability and reliability of the display device DD including the window WM can be increased.

[0157] The window WM according to an embodiment of the present disclosure may include a second layer ML interposed between the first layer LRL and the third layer FL (for example, in the third direction DR3), and the silicon dioxide (SiO2) included in the second layer ML may be formed by 2 ) and aluminum oxide (Al 2 O 3 ) content is adjusted to a specific range to increase the scratch resistance of the window WM. The silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) does not satisfy the above range, the second layer ML may not be able to prevent the friction load in the evaluation of scratch resistance in which vibration friction is applied using ceramic particles or the like, and thus the first layer LRL disposed therebelow may be scratched. In the window WM of the embodiment of the present disclosure, the silicon dioxide (SiO2) included in the second layer ML 2 ) and aluminum oxide (Al 2 O 3 The content of the ceramic particles is adjusted to a specific range so that the second layer ML can be prevented from being worn or lost even when friction using ceramic particles is applied under a certain range of vibration conditions. Therefore, the scratch resistance of the window WM can be increased.

[0158] The surface reflectance, reflection color, chemical resistance, polishing resistance and vibration friction evaluation of the windows of the examples and comparative examples are shown in Table 1 below. In Table 1, the windows of the examples and comparative examples are those having Figure 4A The first to third layers shown in FIG. are sequentially stacked on the base layer. By changing the silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) were mixed to produce windows of the example and comparative examples. The example window is one in which the silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) weight ratio satisfies the range of about 25:75 to about 35:65, and the window of the comparative example is a window in which the silicon dioxide (SiO2 ) and aluminum oxide (Al 2 O 3 ) deviates from a window of the range of about 25:75 to about 35:65.

[0159] In the windows of the examples and comparative examples, the base layer is formed of a glass substrate, the first layer is formed of magnesium fluoride (MgF 2 ) is formed to have a thickness of about 70 nm, and the second layer is composed of silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) are mixed in a content ratio shown in the following Table 1 to form a solid solution to have a thickness of about 15 nm, and the third layer is formed of perfluoropolyether (PFPE) to have a thickness of about 36 nm.

[0160] In Table 1, the reflectance is measured at a wavelength of about 550 nm in a specular reflection light (SCI) mode using a CM-3700A (KONICA MINOLTA, Inc.) device. For the reflective color sense, the corresponding color shift values ​​of the color coordinates a* and b* at a wavelength of about 550 nm based on the exclusion of specular reflection light (SCE) reflection are measured using a CM-3700A (KONICA MINOLTA, Inc.) device, and the results are shown in Table 1. When the color coordinate value a* is about -2 to about 2 and the color coordinate value b* is about -1.5 to about 0.5, the effect of the embodiment of the present disclosure can be achieved. When the range of the reflective color values ​​a* and b* of the window satisfies the above range, when the window is applied to a display device, the screen quality can be high. Chemical resistance evaluation was performed by rubbing the window 3000 times with an industrial eraser at a load of 1 Kgf under the condition of applying alcohol (ethanol, purity 99.99%) and measuring the contact angle of the surface of the window, and the results are shown in Table 1. Polishing resistance evaluation was performed by rubbing the window 2500 times or 3000 times with steel wool at a load of 1 Kgf and then measuring the contact angle of the window surface, and the results are shown in Table 1. Both chemical resistance evaluation and polishing resistance evaluation were performed by measuring the contact angle of deionized water relative to the surface of the sample window. For vibration friction evaluation, a sample was placed in a container containing a surfactant solution and ceramic particles, and the sample was subjected to friction by applying a vibration of 50 Hz, and then the surface of the sample was observed with the naked eye to evaluate the occurrence of scratches, and the results are shown in Table 1. The sample was observed with the naked eye after the vibration friction experiment, and it was evaluated as "NG" when scratches appeared, and it was evaluated as "OK" when scratches did not appear. In the wear resistance evaluation, the contact angle may refer to the angle formed by the surface of the window (to which moisture adheres) and the surface of water. As the contact angle increases, the property that moisture adhered to the surface of the window is easily wiped may be exhibited.

[0161] [Table 1]

[0162]

[0163] Referring to the results of Table 1, it can be confirmed that the windows of Examples 1 to 3 exhibit low surface reflectance of 6.0% or less, and simultaneously exhibit high wear resistance and high scratch resistance, compared to the windows of Comparative Examples 1 to 3.

[0164] Referring to the examples and comparative examples, it can be confirmed that the silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 )'s total weight, reflectivity and aluminum oxide (Al 2 O 3 ) content increases in proportion. In addition, it can be confirmed that as the aluminum oxide (Al 2 O 3 ) content decreases, the wear resistance and scratch resistance decrease. For example, it can be observed that aluminum oxide (Al 2 O 3 ) affects the overall reflectivity and mechanical properties of the window.

[0165] When comparing Examples 1 to 3 with Comparative Example 1, it can be confirmed that after evaluating chemical resistance and polishing resistance, the window of Comparative Example 1 exhibits contact angle characteristics similar to those of the window of Examples, but the surface reflectance of Comparative Example 1 increases by about 0.2% or more compared to Examples 1 to 3. In addition, it can be confirmed that the window of Comparative Example 1 has a reflection color value a* deviating from the range of about -2 to about 2 and a reflection color value b* deviating from the range of about -1.5 to about 0.5 compared to Examples.

[0166] The window of Comparative Example 1 corresponds to a window in which the aluminum oxide (Al 2 O 3 ) content is higher than that of the aluminum oxide (Al 2 O 3 ) content. When Examples 1 to 3 are compared with Comparative Example 1, it can be seen that when aluminum oxide (Al 2 O 3 ) content relative to the silicon dioxide (SiO 2 ) increases, the mechanical properties of the window increase, but when the content exceeds a predetermined range, the reflective properties decrease. As in Comparative Example 1, it can be seen that when the silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) total weight, aluminum oxide (Al 2 O 3) content is greater than about 75wt%, the surface reflectivity exceeds about 6.0%. On the other hand, it can be confirmed that the aluminum oxide (Al 2 O 3 ) content is about 75 wt % or less exhibits a reflectivity of about 6.0% or less, but the example window exhibits a contact angle similar to that of Comparative Example 1 even after evaluation of chemical resistance and wear resistance, and exhibits high mechanical durability even after vibration friction evaluation because no scratches were found.

[0167] When comparing Examples 1 to 3 with Comparative Examples 2 and 3, it can be confirmed that the windows of Comparative Examples 2 and 3 exhibit low reflectivity of about 6.0% or less, but the wear resistance and scratch resistance are reduced compared to Examples 1 to 3. It can be seen that the windows based on the silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) total weight, aluminum oxide (Al 2 O 3 ) content is lower, the reflective properties are better. However, when the content is less than the predetermined range, the wear resistance and scratch resistance are reduced. As in Comparative Examples 2 and 3, when the silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) total weight, aluminum oxide (Al 2 O 3 ) content is less than about 65wt%, it can be confirmed that, in the evaluation of chemical resistance or wear resistance, the contact angle is reduced compared to Examples 1 to 3, and surface scratches are generated after performing vibration friction evaluation. On the other hand, it can be confirmed that, compared to the comparative example, in which the aluminum oxide (Al 2 O 3 The wear resistance and scratch resistance of Examples 1 to 3 in which the content of ) is about 65 wt % or more are increased.

[0168] Therefore, it can be confirmed that when the silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3) satisfies the range of about 25:75 to about 35:65, the window of the embodiment of the present disclosure has high anti-reflection properties, wear resistance and scratch resistance. The window of the display device can exhibit high mechanical properties capable of protecting the display device from external stimuli while obtaining low reflection properties capable of reducing the reflection of light incident from the outside of the display device. Specifically, since the window provided on the upper portion of the display device can receive external artificial contact, the possibility of scratches or wear is high, and therefore high resistance to vibration wear and the like may be required. However, it is difficult to simultaneously meet the mechanical properties and optical properties required for the window of the display device. The window WM according to the embodiment of the present disclosure includes a first layer LRL, a second layer ML and a third layer FL, and the silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) is adjusted to a specific range to maintain high optical properties and exhibit high mechanical properties. Therefore, when the window WM of the embodiment is applied to a display device, the reliability and durability of the display device can be increased.

[0169] refer to Figure 4B The window WM-1 of the embodiment may further include a fourth layer SML disposed between the base layer BL and the first layer LRL (eg, in the third direction DR3).

[0170] The fourth layer SML may be disposed on the base layer BL and may be a layer for increasing adhesion between the base layer BL and the first layer LRL. The fourth layer SML may be an adhesion promoter having high adhesion with respect to each of the base layer BL and the first layer LRL and increasing interlayer adhesion between the base layer BL and the first layer LRL. The fourth layer SML may be directly disposed on the base layer BL. The fourth layer SML may be in direct contact with the base layer BL and the first layer LRL.

[0171] The fourth layer SML may have a low refractive property and high mechanical strength, and include a material for increasing adhesion. In an embodiment, the fourth layer SML may include magnesium oxide (MgO). In an embodiment, the fourth layer SML may further include silicon dioxide (SiO 2 ). The fourth layer SML may include a solid solution including magnesium oxide in the structure. The fourth layer SML may include, for example, a solid solution in which magnesium oxide and silicon dioxide are mixed. The fourth layer SML includes a solid solution including magnesium oxide, and thus may increase adhesion to the first layer LRL including magnesium oxide. Similar to the first layer LRL, the fourth layer SML may be formed by an ion-assisted deposition process.

[0172] In an embodiment, the thickness of the fourth layer SML may be, for example, in a range of about 5 nm to about 25 nm. In a comparative embodiment in which the thickness of the fourth layer SML is less than about 5 nm, the effect of increasing the adhesion between the base layer BL and the first layer LRL may not be achieved. In a comparative embodiment in which the thickness of the fourth layer SML is greater than about 25 nm, the reflectivity of the window WM-1 may increase, and the total thickness of the window WM-1 may increase, so that the total thickness of the display device may be excessively increased.

[0173] In an embodiment, at a wavelength of about 550 nm, the fourth layer SML may have a refractive index in the range of about 1.3 to about 1.6. In the window WM-1 of the embodiment, at a wavelength of about 550 nm, the fourth layer SML may have a refractive index in the range of about 1.45 to about 1.50. Since the refractive index of the fourth layer SML satisfies the above range at a wavelength of about 550 nm, the surface reflectivity of the window WM-1 can be reduced.

[0174] refer to Figure 4C , the window WM-2 of the embodiment may further include (for example, in the third direction DR3) a fifth layer HRL disposed between the base layer BL and the first layer LRL. The fifth layer HRL may be a layer having a higher refractive index than the other layers. In the window WM-2 of the embodiment, at a wavelength of about 550 nm, the fifth layer HRL may have a refractive index in the range of about 1.7 to about 3.0. At a wavelength of about 550 nm, the fifth layer HRL may have a refractive index in the range of about 2.0 to about 2.5. At a wavelength of about 550 nm, the fifth layer HRL may have a refractive index of about 2.33.

[0175] The fifth layer HRL may be disposed on the base layer BL and have a high refractive property, and thus the surface reflectivity of the window WM-2 may be further reduced. The window WM-2 of the embodiment may have a structure in which a first layer LRL, a second layer ML, and a third layer FL (for example, in the third direction DR3) having a low refractive property are sequentially stacked on the fifth layer HRL having a high refractive property, so that the surface reflectivity of the window WM-2 may be reduced, and the fifth layer HRL may have high adhesion relative to each of the base layer BL and the first layer LRL, so that the interlayer adhesion between the base layer BL and the first layer LRL may be maintained high. In an embodiment, the fifth layer HRL may be directly disposed on the base layer BL (for example, in the third direction DR3). The fifth layer HRL may be in direct contact with the base layer BL and the first layer LRL.

[0176] The fifth layer HRL may have high refractive properties and high mechanical strength, and include a material for increasing adhesion. In an embodiment, the fifth layer HRL may include zinc oxide (ZnO 2), hafnium oxide (HfO 2 ), Tantalum Oxide (Ta 2 O 5 ), niobium oxide (Nb 2 O 5 ), titanium oxide (TiO 2 ), Ytterbium oxide (Y 2 O 3 ), silicon nitride (Si 3 N 4 ), SrTiO 3 ), tungsten oxide (WO 3 ) and aluminum nitride (AlN). For example, the fifth HRL layer may include niobium oxide (Nb 2 O 5 Since the fifth HRL layer includes niobium oxide (Nb 2 O 5 ), the fifth layer HRL may have a high refractive index within the above range and may have high adhesion to each of the base layer BL and the first layer LRL that are in direct contact with the fifth layer HRL. Like the first layer LRL, the fifth layer HRL may be formed by an ion-assisted deposition process. In the process of forming the fifth layer HRL, a zinc oxide (ZnO 2 ), hafnium oxide (HfO 2 ), Tantalum Oxide (Ta 2 O 5 ), niobium oxide (Nb 2 O 5 ), titanium oxide (TiO 2 ), Ytterbium oxide (Y 2 O 3 ), silicon nitride (Si 3 N 4 ), SrTiO 3 ), tungsten oxide (WO 3 ) and aluminum nitride (AlN) are deposited on the surface of the base layer BL in the form of particles, and together provide ionized oxygen (O 2 ) gas, thereby increasing the adhesion of the deposited film to the surface of the base layer BL.

[0177] In an embodiment, the thickness d5 of the fifth layer HRL (e.g., the length in the third direction DR3) may be, for example, about 5 nm to about 25 nm. For example, the thickness d5 of the fifth layer HRL may be about 10 nm. In a comparative embodiment in which the thickness d5 of the fifth layer HRL is less than about 5 nm, the reflectivity of the window WM-2 may be increased, and the adhesion between the base layer BL and the first layer LRL may not be increased. In a comparative embodiment in which the thickness d5 of the fifth layer HRL is greater than about 25 nm, the total thickness of the window WM-2 may be increased, so that the total thickness of the display device may be excessively increased.

[0178] In the window WM-2 of the embodiment, the surface of the window WM-2 may have a reflectivity of about 6.0% or less at a wavelength of about 550nm. In the window WM-2 of the embodiment, the third layer FL may be disposed on the uppermost layer, and the upper surface of the third layer FL may have a reflectivity of about 6.0% or less at a wavelength of about 550nm. The upper surface of the third layer FL may have a reflectivity in the range of about 5.8% to about 6.0% at a wavelength of about 550nm. The window WM-2 according to the embodiment of the present disclosure also includes (for example, in the third direction DR3) a fifth layer HRL disposed between the first layer LRL and the base layer BL, and therefore may have a surface reflectivity lower than an embodiment in which the first layer LRL is directly disposed on the base layer BL without the fifth layer HRL. For example, in the window WM-2 according to the embodiment, the fifth layer HRL having a high refractive property may be disposed between the base layer BL and the first layer LRL (for example, in the third direction DR3), and thus, the high refractive layer and the low refractive layer may be sequentially disposed on the base layer BL, thereby realizing a structure that further reduces the surface reflectivity of the window WM-2. In the embodiment, since a material such as niobium oxide (NbO2) is deposited on the upper surface of the base layer BL by an ion-assisted deposition process, 2 O 5 ), and thus the fifth layer HRL included in the window WM-2 can have high adhesion to the base layer BL, and thus can have wear resistance, chemical resistance, and polishing resistance equivalent to those of the window in which the fifth layer HRL is omitted. Therefore, a display device including the window WM-2 can have low reflection characteristics while maintaining its durability.

[0179] refer to Figure 4D, the window WM-3 of the embodiment may further include a sixth layer CLRL disposed below the base layer BL. The sixth layer CLRL may be a layer having a low refractive index. In the window WM-3 of the embodiment, at a wavelength of about 550 nm, the sixth layer CLRL may have a refractive index in the range of about 1.3 to about 1.5. In an embodiment, at a wavelength of about 550 nm, the sixth layer CLRL may have a refractive index in the range of about 1.38 to about 1.40.

[0180] The sixth layer CLRL may be disposed below the base layer BL and have a low refractive property, and thus the surface reflectivity of the window WM-3 may be further reduced. In addition, the window WM-3 of the embodiment further includes a sixth layer CLRL disposed below the base layer BL, and thus may have an increased reflective color sense compared to a window not including the sixth layer CLRL. In an embodiment, the sixth layer CLRL may be disposed below the base layer BL, and may be spaced apart from the first layer LRL (for example, in a third direction DR3) with the base layer BL interposed therebetween. For example, when the window WM-3 of the embodiment is applied to a display device DD (see Figure 2 ), compared with the base layer BL, the first layer LRL, the second layer ML and the third layer FL, the sixth layer CLRL may be arranged to be consistent with the display module DM (see Figure 2 ). In an implementation, the sixth layer CLRL may be disposed directly below the base layer BL. The sixth layer CLRL may be in direct contact with a lower surface of the base layer BL.

[0181] In an embodiment, the sixth layer CLRL may include a material having a low refractive index and high adhesion to the base layer BL. The sixth layer CLRL may include a first material similar to the first layer LRL, and the first material may include a material having a refractive index lower than that of the material included in the base layer BL as described above. In an embodiment, the first material included in the sixth layer CLRL may include, for example, silicon dioxide, fused silicon dioxide, fluorine-doped fused silicon dioxide, magnesium fluoride (MgF 2 ), calcium fluoride (CaF 2 ), aluminum fluoride (AlF 3 ), yttrium fluoride (YF 3 ), Ytterbium fluoride (YbF 3 ), aluminum oxide (Al 2 O 3 ) and magnesium oxide (MgO). For example, the sixth CLRL layer may include magnesium fluoride (MgF 2 ) and magnesium oxide (MgO) as the first material.

[0182] In an embodiment, the sixth layer CLRL may include magnesium oxide (MgO). In addition to or instead of magnesium oxide, the sixth layer CLRL may also include magnesium fluoride (MgF 2 ) and yttrium oxyfluoride (YOF). The sixth layer CLRL may include a solid solution containing magnesium oxide in the structure. In an embodiment, the sixth layer CLRL may include, for example, a solid solution in which magnesium oxide, magnesium fluoride, and yttrium oxyfluoride are mixed. Alternatively, the sixth layer CLRL may include magnesium fluoride (MgF 2 The sixth CLRL layer may be made of magnesium fluoride (MgF 2 ) formed a single layer.

[0183] In an embodiment, the sixth layer CLRL may include the same material as the first layer LRL or a different material from the first layer LRL. For example, in an embodiment, each of the first layer LRL and the sixth layer CLRL may include magnesium fluoride. Each of the first layer LRL and the sixth layer CLRL may include a solid solution in which magnesium oxide, magnesium fluoride, and yttrium oxyfluoride are mixed. Alternatively, in an embodiment, one of the first layer LRL and the sixth layer CLRL may include magnesium fluoride, and the other may include a solid solution in which magnesium oxide, magnesium fluoride, and yttrium oxyfluoride are mixed.

[0184] Like the first layer LRL, the sixth layer CLRL may be formed by an ion-assisted deposition process. In the process of forming the sixth layer CLRL, at least one of materials such as magnesium oxide, magnesium fluoride, and yttrium oxyfluoride is deposited on the surface of the base layer BL in the form of particles, and ionized argon (Ar) gas or oxygen (O) is provided together during the deposition process. 2 ) gas, thereby increasing the adhesion of the deposited film to the surface of the base layer BL.

[0185] In an embodiment, the thickness d6 of the sixth layer CLRL (e.g., the length in the third direction DR3) may be, for example, in the range of about 50 nm to about 130 nm. In a comparative embodiment in which the thickness d6 of the sixth layer CLRL is less than about 50 nm, the surface reflectivity of the window WM-3 may not be sufficiently reduced. In a comparative embodiment in which the thickness d6 of the sixth layer CLRL is greater than about 130 nm, the mechanical strength of the window WM-3 may be reduced, so that the durability may be reduced, and the total thickness of the window WM-3 may be increased, so that the total thickness of the display device may be excessively increased.

[0186] In the window WM-3 according to the embodiment of the present disclosure, the surface of the window WM-3 may have a reflectivity of about 6.0% or less at a wavelength of about 550nm. In the window WM-3 of the embodiment, the third layer FL may be disposed on the uppermost layer, and the upper surface of the third layer FL may have a reflectivity of about 6.0% or less at a wavelength of about 550nm. The upper surface of the third layer FL may have a reflectivity in the range of about 5.8% to about 6.0% at a wavelength of about 550nm. The window WM-3 according to the embodiment of the present disclosure also includes a sixth layer CLRL disposed below the base layer BL, and thus the window WM-3 may have a lower surface reflectivity than when there is no separate layer disposed below the base layer BL. For example, the window WM-3 according to the embodiment may have a structure in which a first layer LRL and a sixth layer CLRL having low refractive properties are respectively disposed on both sides of the base layer BL, thereby achieving a structure that further reduces the surface reflectivity of the window WM-3. Therefore, a display device including the window WM-3 may have an increased low reflection characteristic.

[0187] According to an embodiment of the present disclosure, the window includes a plurality of layers disposed on a base layer and including a specific material, and thus can have low refractive properties and high adhesion between the layers, and also has increased mechanical strength such as wear resistance, chemical resistance, and polishing resistance. Therefore, the durability and reliability of a display device including the window can be improved.

[0188] Although the present disclosure has been described with reference to non-limiting embodiments, it will be understood that the embodiments of the present disclosure should not necessarily be limited to these embodiments, but may be variously changed and modified by those skilled in the art without departing from the spirit and scope of the present disclosure. Therefore, the technical scope of the present disclosure is not intended to be limited to the described embodiments set forth in the detailed description of the specification.

Claims

1. Window, include: Base layer; A first layer, disposed on the base layer; a second layer, disposed on the first layer; as well as A third layer is provided on the second layer, wherein the second layer comprises silicon dioxide and aluminum oxide, and A weight ratio of the silicon dioxide to the aluminum oxide in the second layer is in a range of 25:75 to 35:

65.

2. The window according to claim 1, in, the second layer is disposed directly on the first layer; and The third layer is disposed directly on the second layer.

3. The window according to claim 1, in, The second layer has a thickness in the range of 10 nm to 20 nm.

4. The window according to claim 1, in, At a wavelength of 550 nm, the second layer has a refractive index in the range of 1.43 to 1.

50.

5. The window according to claim 1, in, At a wavelength of 550 nm, the first layer has a refractive index in the range of 1.3 to 1.5; and The third layer has a refractive index in the range of 1.2 to 1.5 at a wavelength of 550 nm.

6. The window according to claim 1, in, The refractive index of the first layer is less than the refractive index of the base layer; and The refractive index of the second layer is greater than the refractive index of the first layer.

7. The window according to claim 1, in, The second layer includes a solid solution in which the silicon dioxide and the aluminum oxide are mixed.

8. The window according to claim 1, in, The reflectivity on the upper surface of the third layer is 6.0% or less at a wavelength of 550 nm.

9. The window according to claim 1, in, The third layer includes a fluoropolymer.

10. The window according to claim 1, in, The base layer includes a glass substrate or a polymer film.

11. The window according to claim 1, in, The first layer has a thickness in the range of 60 nm to 80 nm; and The third layer has a thickness in the range of 5 nm to 40 nm.

12. The window according to claim 1, further comprising a fourth layer disposed between the base layer and the first layer, in, The fourth layer includes magnesium oxide. 13 . The window of claim 1 , further comprising a fifth layer disposed between the base layer and the first layer, the fifth layer having a refractive index of 1.7 to 3.0 at a wavelength of 550 nm.

14. The window according to claim 13, in, The fifth layer includes at least one compound selected from the group consisting of zinc oxide, hafnium oxide, tantalum oxide, niobium oxide, titanium oxide, ytterbium oxide, silicon nitride, strontium titanate, tungsten oxide, and aluminum nitride. 15 . The window of claim 1 , further comprising a sixth layer disposed below the base layer, the sixth layer having a refractive index in a range of 1.3 to 1.5 at a wavelength of 550 nm.

16. The window according to claim 15, in, The sixth layer includes at least one compound selected from the group consisting of magnesium oxide, magnesium fluoride, and yttrium oxyfluoride.

17. Display devices, include: Display module; as well as The window according to any one of claims 1 to 16, arranged on the display module.

18. The display device according to claim 17, in, The display module comprises: base substrate; A circuit layer is disposed on the base substrate; A light emitting element layer, disposed on the circuit layer, the light emitting element layer comprising a plurality of light emitting elements; an encapsulation layer, disposed on the light-emitting element layer; and an anti-reflection layer, disposed on the encapsulation layer, The anti-reflection layer includes a dividing layer having a plurality of dividing openings respectively overlapping the plurality of light emitting elements and a plurality of color filters respectively arranged to correspond to the plurality of dividing openings.

19. The display device according to claim 17, in, The first layer is spaced apart from the display module and the base layer is interposed between the first layer and the display module.

20. The display device according to claim 17, in, An upper surface of the third layer defines an outermost surface of the window.

Citation Information

Patent Citations

  • A device for pipe connection with a threaded fastening method with improved airtightness

    KR1020230067837A