Secondary battery and electronic device

By controlling the specific electrolyte components in the secondary battery and using boehmite on the polyolefin substrate separator, the problem of taking into account both the energy density and safety of the secondary battery is solved, and the high potential life and low temperature output characteristics are significantly improved.

CN119029271APending Publication Date: 2024-11-26NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411139082.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

While improving the energy density of existing secondary batteries, it is difficult to take into account both safety performance and high potential life. How to improve the safety and high potential life of secondary batteries while maintaining high energy density is an urgent problem.

Method used

The content of 1,3-propanesulfonate, 1,3,6-hexanetrinitrile, lithium difluorophosphate and boron-containing lithium salt are controlled in the electrolyte of the secondary battery, and the polyolefin substrate is separated with the polyolefin substrate. The boehmite bond on it improves the adhesion of the diaphragm and the low-temperature output characteristics of the battery, improves the safety performance and high potential life of the battery.

Benefits of technology

It realizes that the high potential life and low temperature output characteristics of the secondary battery are significantly improved while maintaining high energy density, while improving the safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005000711250000171
    Figure BDA0005000711250000171
  • Figure BDA0005000711250000181
    Figure BDA0005000711250000181
  • Figure BDA0005000711250000221
    Figure BDA0005000711250000221
Patent Text Reader

Abstract

The invention discloses a secondary battery and an electronic device, and relates to the technical field of new energy. The secondary battery comprises a positive electrode, a negative electrode, an electrolyte and a diaphragm, the diaphragm comprises a polyolefin base material and a coating arranged on at least one surface of the polyolefin base material, and the coating comprises boehmite; the electrolyte contains specific amounts of 1, 3-propane sultone, 1, 3, 6-hexane trinitrile, lithium difluorophosphate, boron-containing lithium salt and adiponitrile, and the total amount of the 1, 3-propane sultone and the 1, 3, 6-hexane trinitrile and the total amount of the lithium difluorophosphate, the boron-containing lithium salt and the adiponitrile are all in specific ranges. Therefore, the secondary battery can keep high energy density, has good high potential life and also has good safety.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of a patent application with an application date of June 14, 2024, application number 202410770399.5, and invention name “A secondary battery and electronic device”. Technical Field

[0002] The present application relates to the field of new energy technology, and in particular to a secondary battery and an electronic device. Background Art

[0003] Secondary batteries have the advantages of high energy storage density, high open circuit voltage, low self-discharge rate, long cycle life, good safety, etc., and are widely used in various fields such as portable power storage, electronic equipment, electric vehicles, etc. However, secondary batteries also expose problems such as life and safety during use. Therefore, consumers have higher requirements for the comprehensive performance of secondary batteries, such as secondary batteries with good safety, high energy density and high potential life.

[0004] At present, the traditional methods to increase the energy density of secondary batteries include increasing the coating weight, increasing the compaction density of the electrode, and increasing the voltage. However, while the above methods increase the energy density of secondary batteries, they also reduce the safety performance and high potential life of the secondary batteries. Therefore, how to ensure the high potential life and safety of high energy density secondary batteries is an urgent problem to be solved in the battery industry. Summary of the invention

[0005] The present application provides a secondary battery and an electronic device, which can enable the secondary battery to maintain high energy density while also having a good high potential life and good safety.

[0006] In the first aspect, the present application provides a secondary battery, which includes a positive electrode, a negative electrode, an electrolyte and a separator; the separator includes a polyolefin substrate and a coating disposed on at least one surface of the polyolefin substrate, and the coating includes boehmite. Based on the total mass of the electrolyte, the electrolyte satisfies: (I) including 1,3-propane sultone with a content of 1.3wt% or more and 2.7wt% or less; (II) including lithium difluorophosphate with a content of 0.01wt% or more and 2wt% or less; (III) including 1,3,6-hexane trinitrile with a content of 1.6wt% or more and 3.9wt% or less; (IV) including a boron-containing lithium salt with a content of 0.01wt% or more and 3wt% or less. The total content of 1,3-propane sultone and 1,3,6-hexane trinitrile is 1.61wt% or more and 6wt% or less, and the total content of lithium difluorophosphate and boron-containing lithium salt is 0.02wt% or more and 5wt% or less.

[0007] Based on the secondary battery of the present application, the total content of 1,3-propane sultone and 1,3,6-hexane trinitrile, the total content of lithium difluorophosphate and boron-containing lithium salt, and the content of each of the four substances in the present application are controlled within specific ranges, and used in combination with a polyolefin-based diaphragm containing boehmite. This not only improves the adhesion of the diaphragm after electrolyte infiltration, but also improves the high potential life and low-temperature output characteristics of the secondary battery, and also has good safety performance. The boehmite in the surface coating of the polyolefin substrate can significantly improve the safety of the battery. In addition, the inventor unexpectedly discovered that the presence of 1,3-propane sultone and 1,3,6-hexane trinitrile in the electrolyte can inhibit the swelling of the polyolefin substrate in the electrolyte, but the presence of boehmite will catalyze the decomposition of 1,3-propane sultone and 1,3,6-hexane trinitrile on the negative electrode surface; the inventor then discovered that a specific amount of lithium difluorophosphate and boron-containing lithium salt can just inhibit the decomposition of 1,3-propane sultone and 1,3,6-hexane trinitrile, forming a stable coating on the negative electrode surface. By using this design, not only can the adhesion of the diaphragm after electrolyte immersion be improved, but also the high potential life and low temperature output characteristics of the secondary battery can be significantly improved.

[0008] In some embodiments, the boron-containing lithium salt includes lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium bisoxalatoborate, lithium tetracyanoborate, lithium tetrakis(trifluoromethyl)borate, lithium (trifluoromethyl) trifluoroborate, lithium bis(trifluoromethyl) difluoroborate, lithium pentafluoroethyl trifluoroborate, lithium dicyanooxalatoborate, lithium bismalonate borate, lithium (2-fluoromalonate) difluoroborate, lithium malonate oxalatoborate, lithium di(salicylate)borate, lithium di(catecholate) borate At least one of lithium borate, lithium methoxytricyanoborate, lithium ethoxytricyanoborate, lithium tetramethoxyborate, lithium tetraethoxyborate, lithium tetrakis(trifluoromethoxy)borate, lithium tetrakis(2,2,2-trifluoroethoxy)borate, polytetrakis(hydroquinone oxygen)borate, lithium di(trifluoroborate) sulfate, lithium difluoroborate, lithium methanedisulfonate difluoroborate, lithium difluorophosphoryloxy trifluoroborate, lithium di(difluorophosphoryloxy) difluoroborate or lithium tetrakis(difluorophosphoryloxy)borate. In the embodiment of the present application, when the boron-containing lithium salt includes the above materials, the safety performance, energy density, high potential life and low temperature output performance of the secondary battery are better.

[0009] In some of the embodiments, the electrolyte includes 1,3-propane sultone in an amount of 1.3 wt % or more and 2.7 wt % or less based on the total mass of the electrolyte.

[0010] In some of the embodiments, the electrolyte includes 1,3-propane sultone in an amount of 2.6 wt % or more and 2.9 wt % or less based on the total mass of the electrolyte.

[0011] Based on the above embodiment, the content of 1,3-propane sultone is controlled within the above range, which can well inhibit the swelling of the polyolefin substrate, thereby improving the safety performance of the secondary battery.

[0012] In some embodiments, the electrolyte includes lithium difluorophosphate in an amount of 0.07 wt % or more and 0.91 wt % or less based on the total mass of the electrolyte.

[0013] In some embodiments, the electrolyte includes lithium difluorophosphate in an amount of 0.01 wt % or more and 0.11 wt % or less based on the total mass of the electrolyte.

[0014] In some embodiments, the electrolyte includes lithium difluorophosphate in an amount of 0.11 wt % or more and 0.59 wt % or less based on the total mass of the electrolyte.

[0015] Based on the above embodiment, the content of lithium difluorophosphate is controlled within the above range, which can effectively inhibit the decomposition of 1,3-propane sultone and 1,3,6-hexane trinitrile, thereby effectively inhibiting the swelling of the polyolefin substrate, thereby improving the safety performance of the secondary battery.

[0016] In some embodiments, the electrolyte includes 1,3,6-hexanetricarbonitrile in an amount of 1.6 wt % to 2.8 wt % based on the total mass of the electrolyte. The content of 1,3,6-hexanetricarbonitrile is controlled within the above range, which can well inhibit the swelling of the polyolefin substrate, thereby improving the safety performance of the secondary battery.

[0017] In some embodiments, the electrolyte further comprises other nitrile compounds, including at least one of succinonitrile, adiponitrile, ethylene glycol di(propionitrile) ether, 1,2,3-tri(2-cyanoethoxy)propane, and 3-methyl-1,3,5-tri(cyanoethoxy)pentane; based on the total mass of the electrolyte, the content of other nitrile compounds is 0.3wt% or more and 8wt% or less. The inventor unexpectedly discovered that other nitrile compounds can improve the stability of the formed film, thereby further improving the high potential life and low temperature output characteristics of the secondary battery.

[0018] In some embodiments, the content of succinonitrile is 1.7 wt % or more and 5.5 wt % or less based on the total mass of the electrolyte. When the electrolyte contains succinonitrile within the above range, the low-temperature output characteristics of the secondary battery can be further improved.

[0019] In some embodiments, the content of adiponitrile is 2.3 wt % or more and 4 wt % or less based on the total mass of the electrolyte. When the electrolyte contains adiponitrile within the above range, the high potential life and low temperature output characteristics of the secondary battery can be further improved.

[0020] In some embodiments, the content of ethylene glycol di(propionitrile) ether is 0.3 wt % to 0.9 wt % based on the total weight of the electrolyte. When the electrolyte contains ethylene glycol di(propionitrile) ether within the above range, the low temperature output characteristics of the secondary battery can be further improved.

[0021] In some embodiments, the content of 1,2,3-tris(2-cyanoethoxy)propane is 0.4wt% to 2.3wt% based on the total mass of the electrolyte. When the electrolyte contains 1,2,3-tris(2-cyanoethoxy)propane within the above range, the low temperature output characteristics of the secondary battery can be further improved.

[0022] In some embodiments, the electrolyte also includes other additives, including 2-ethyl-1-hexyl difluorophosphite, 4-methyl-2-pentyl difluorophosphite, pentyl difluorophosphite, fluoroethylene carbonate, vinylene carbonate, lithium fluorosulfonate, vinyl sulfate, 1,3-propylene glycol cyclic sulfate, fluorobenzene, cyclohexylbenzene, biphenyl, tris (trimethylsilane) phosphate or tris (trimethylsilane) borate; based on the total mass of the electrolyte, the content of other additives is 0.01wt% or more and 10wt% or less. The inventor unexpectedly found that other additives can inhibit the decomposition and regeneration of the aforementioned coating during the charge and discharge process, thereby further improving the high potential life and low temperature output characteristics of the secondary battery.

[0023] In some embodiments, the content of fluoroethylene carbonate is greater than or equal to 0.01 wt % and less than or equal to 3 wt % based on the total mass of the electrolyte.

[0024] In some embodiments, the content of fluoroethylene carbonate is 4.1 wt % or more and 6.9 wt % or less based on the total mass of the electrolyte.

[0025] Based on the above embodiment, when the electrolyte contains the above content of fluoroethylene carbonate, the high potential life and low temperature output characteristics of the secondary battery can be further improved.

[0026] In some embodiments, the content of vinyl sulfate is 0.01 wt % or more and 0.3 wt % or less based on the total mass of the electrolyte. When the electrolyte contains vinyl sulfate in the above content, the high potential life and low temperature output characteristics of the secondary battery can be further improved.

[0027] In some embodiments, the content of 2-ethyl-1-hexyl difluorophosphite is greater than 0.01wt% and less than 1.4wt% based on the total mass of the electrolyte. When the electrolyte contains the above content of 2-ethyl-1-hexyl difluorophosphite, the high potential life and low temperature output characteristics of the secondary battery can be further improved.

[0028] In a second aspect, an embodiment of the present application provides an electronic device, comprising any secondary battery of the first aspect. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical scheme and advantages of the present application clearer, the present application is further described in detail below in conjunction with the embodiments. The embodiments of the present application will be described in detail below. The embodiments of the present application should not be construed as limiting the present application. Unless otherwise clearly indicated, the following terms used in the present application have the meanings indicated below.

[0030] The present application uses a specific combination of a diaphragm structure and an electrolyte. This design can not only improve the adhesion of the diaphragm after being immersed in the electrolyte, but also significantly improve the high potential life and low temperature output characteristics of the secondary battery.

[0031] In one embodiment, the present application provides a secondary battery comprising the following electrolyte, a separator, a positive electrode, and a negative electrode.

[0032] I. Electrolyte

[0033] The electrolyte used in the secondary battery of the present application includes an electrolyte and a solvent for dissolving the electrolyte. In some embodiments, the electrolyte of the present application includes:

[0034] (I) 1,3-propane sultone in an amount of 1.3 wt% to 2.7 wt%;

[0035] (II) lithium difluorophosphate in an amount of 0.01 wt % to 2 wt %;

[0036] (III) 1,3,6-hexanetrinitrile in an amount of 1.6 wt % to 3.9 wt %;

[0037] (IV) A boron-containing lithium salt having a content of 0.01 wt % to 3 wt %.

[0038] The total content of 1,3-propane sultone and 1,3,6-hexanetrinitrile is 1.61 wt % or more and 6 wt % or less, and the total content of lithium difluorophosphate and boron-containing lithium salt is 0.02 wt % or more and 5 wt % or less.

[0039] The diaphragm used in the secondary battery of the present application includes a polyolefin substrate and a coating on at least one surface of the polyolefin substrate, and the coating includes boehmite, which can significantly improve the safety of the battery. The inventor unexpectedly discovered that 1,3-propane sultone and 1,3,6-hexane trinitrile in the electrolyte can inhibit the swelling of the polyolefin substrate in the electrolyte, but the presence of boehmite will catalyze the decomposition of 1,3-propane sultone and 1,3,6-hexane trinitrile on the negative electrode surface, and a specific amount of lithium difluorophosphate and boron-containing lithium salt can just inhibit the decomposition of 1,3-propane sultone and 1,3,6-hexane trinitrile, forming a stable coating on the negative electrode surface. By using this design, not only can the adhesion of the diaphragm after electrolyte immersion be improved, but also the high potential life and low temperature output characteristics of the secondary battery can be significantly improved.

[0040] Specifically, from the viewpoint of improving the adhesion of the separator after immersion in the electrolyte, the content of 1,3-propane sultone is 1.3wt% or more based on the total mass of the electrolyte. In addition, as the upper limit of the mass content of 1,3-propane sultone, from the viewpoint of improving the life of the high potential region, the mass content of 1,3-propane sultone is 2.7wt% or less, preferably 2.4wt% or less, and more preferably 1.6wt% or less. When within the above range, it helps to further improve the life of the high potential region.

[0041] In some embodiments, the content of 1,3-propane sultone is set to a1wt%, and a1 is 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.08, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.4, 2.6, 2.7, 2.8, 2.9 or in the range consisting of any two of the above values. For example, 0.01 to 0.09, 0.01 to 1.3, 0.05 to 0.1, 0.1 to 0.8, 0.5 to 1.2, 0.7 to 1.9, 1.3 to 2.7, 1.1 to 2.9. When within the above ranges, it helps to further improve the life of the high potential region.

[0042] Specifically, from the viewpoint of improving the adhesion of the diaphragm after immersion in the electrolyte, based on the total mass of the electrolyte, the mass content of lithium difluorophosphate is 0.01wt% or more, preferably the mass content of lithium difluorophosphate is 0.02wt% or more, preferably 0.07wt% or more, and more preferably 0.11wt% or more. In addition, as the upper limit of the mass content of lithium difluorophosphate, from the viewpoint of improving the life of the high potential zone, the mass content of lithium difluorophosphate is 2wt% or less, preferably 1.8wt% or less, more preferably 1.6wt% or less, further preferably 1.3wt% or less, particularly preferably 1.2wt% or less, and more particularly preferably 0.91wt% or less. When within the above range, it helps to further improve the life of the high potential zone.

[0043] In some embodiments, the content of lithium difluorophosphate is set to a2wt%, and a2 is 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, or in a range consisting of any two of the above values. For example, 0.01 to 0.09, 0.01 to 0.11, 0.05 to 0.1, 0.1 to 0.8, 0.6 to 1.2, 0.8 to 1.8. When it is within the above range, it helps to further improve the life of the high potential region.

[0044] Specifically, from the viewpoint of improving the low-temperature output characteristics of the secondary battery, based on the total mass of the electrolyte, the content of 1,3,6-hexane trinitrile is 1.6wt% or more, preferably 1,3,6-hexane trinitrile is 1.8wt% or more, more preferably 2.1wt% or more, and further preferably 2.4wt% or more. In addition, as the upper limit of the mass content of 1,3,6-hexane trinitrile, from the viewpoint of improving the life of the high potential zone, the mass content of 1,3,6-hexane trinitrile is 3.9wt% or less, preferably 3.7wt% or less, more preferably 3.5wt% or less, further preferably 3.3wt% or less, and particularly preferably 3.1wt% or less. When within the above range, it helps to further improve the life of the high potential zone.

[0045] In some embodiments, the content of 1,3,6-hexanetrinitrile is set to a3wt%, and a3 is 1.6, 1.8, 2.0, 2.3, 2.6, 2.8, 3.1, 3.3, 3.5, 3.7, 3.9 or in a range consisting of any two of the above values. For example, 1.6 to 2.8, 1.8 to 3.3, 2.0 to 3.5, 2.3 to 3.7, 1.6 to 2.3. When within the above range, it helps to further improve the life of the high potential region.

[0046] In some embodiments, the boron-containing lithium salt includes lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium bisoxalatoborate, lithium tetracyanoborate, lithium tetrakis(trifluoromethyl)borate, lithium (trifluoromethyl) trifluoroborate, lithium bis(trifluoromethyl) difluoroborate, lithium pentafluoroethyl trifluoroborate, lithium dicyanooxalatoborate, lithium bismalonate borate, lithium (2-fluoromalonate) difluoroborate, lithium malonate oxalatoborate, lithium di(salicylate)borate, lithium di(catecholate)borate, lithium methoxytricyanoborate, lithium ... At least one of oxytricyanoborate, tetramethoxyborate, tetraethoxyborate, tetrakis(trifluoromethoxy)borate, tetrakis(2,2,2-trifluoroethoxy)borate, polytetrakis(hydroquinone)borate, di(trifluoroborate)dilithium sulfate, difluoroborate, methanedisulfonate difluoroborate, difluorophosphoryloxy trifluoroborate, di(difluorophosphoryloxy)difluoroborate or tetrakis(difluorophosphoryloxy)borate, in which case the formed coating has excellent stability and the battery performance is further improved. The boron-containing lithium salt may be only one, or two or more, or three or more.

[0047] In some embodiments, the boron-containing lithium salt preferably includes at least one of lithium tetrafluoroborate, lithium bis(oxalatoborate) (LiBOB), and lithium difluorooxalatoborate (LiDFOB).

[0048] Specifically, from the viewpoint of improving the low-temperature output characteristics of the secondary battery, based on the total mass of the electrolyte, the mass content of the boron-containing lithium salt is 0.01wt% or more, preferably the mass content of the boron-containing lithium salt is 0.02wt% or more, preferably 0.06wt% or more, and more preferably 0.1wt% or more. In addition, as the upper limit of the mass content of the boron-containing lithium salt, from the viewpoint of improving the life of the high potential zone, the mass content of the boron-containing lithium salt is 3wt% or less, preferably 2.3wt% or less, more preferably 1.5wt% or less, further preferably 1.1wt% or less, and particularly preferably 0.7wt% or less. When within the above range, it helps to further improve the life of the high potential zone.

[0049] In some embodiments, the content of the boron-containing lithium salt is set to a4wt%, and a4 is 0.01, 0.02, 0.06, 0.1, 0.4, 0.7, 1.1, 1.5, 2.3, 2.8, 3, or within a range consisting of any two of the above values. For example, 0.01 to 0.1, 0.1 to 0.7, 0.4 to 1.1, 0.7 to 2.3, 1.5 to 3. When within the above range, it helps to further improve the life of the high potential region.

[0050] Furthermore, from the viewpoint of improving the life of the high potential region, based on the mass of the electrolyte, the total mass content of (I) and (III) is 1.61wt% or more, preferably 1.85wt% or more. In addition, as the upper limit of the total content of (I) and (III), from the viewpoint of improving the electrochemical characteristics under low temperature environment, it is 6wt% or less, preferably 5.7wt% or less.

[0051] In some embodiments, the total weight content of (I) and (III) is a1+a3 wt %, and a1+a3 is 1.61, 1.85, 2.18, 2.4, 2.8, 3.4, 4, 4.7, 5.2, 5.7, 6, or in the range consisting of any two of the above values. For example, 1.61 to 2.8, 1.85 to 5.2, 1.61 to 2.18, 1.85 to 3.4, 2.4 to 4.7, 2.8 to 5.7. When it is within the above range, it helps to further improve the life of the high potential region.

[0052] Furthermore, from the viewpoint of improving the life of the high potential region, based on the electrolyte mass, the total mass content of (II) and (IV) is more than 0.02wt%, preferably more than 0.14wt%. In addition, as the upper limit of the total content of (II) and (IV), from the viewpoint of improving the electrochemical characteristics under low temperature environment, it is less than 5wt%, preferably less than 4.4wt%.

[0053] In some embodiments, the total weight content of (II) and (IV) is a2+a4 wt %, and a2+a4 is 0.02, 0.04, 0.09, 0.14, 0.47, 0.66, 0.81, 1.12, 1.33, 1.56, 1.88, 2.21, 2.34, 2.56, 2.88, 3.12, 3.35, 3.78, 4.11, 4.4, 4.7, 5, or within the range consisting of any two of the above values. For example, 0.02 to 0.14, 0.09 to 0.66, 0.47 to 1.56, 1.12 to 2.88, 1.56 to 4.7. When within the above range, it helps to further improve the life of the high potential region.

[0054] In addition, the electrolyte may also include other nitrile compounds. The inventors have also unexpectedly discovered that other nitrile compounds can improve the stability of the aforementioned coating, improve lithium ion charge transfer, increase the high potential life of the secondary battery and improve low temperature output characteristics.

[0055] Other nitrile compounds include at least one of succinonitrile, adiponitrile, ethylene glycol di(propionitrile) ether, 1,2,3-tris(2-cyanoethoxy)propane, and 3-methyl-1,3,5-tris(cyanoethoxy)pentane. The other nitrile compounds may be only one or more.

[0056] Specifically, from the viewpoint of improving the low temperature output characteristics of the secondary battery, based on the total mass of the electrolyte, the content of other nitrile compounds is more than 0.3wt%, preferably the content of other nitrile compounds is more than 0.6wt%, more preferably more than 0.9wt%, and further preferably more than 1.4wt%. In addition, as the upper limit of the content of other nitrile compounds, the content of other nitrile compounds is less than 8wt%, preferably less than 7.9wt%, more preferably less than 7.1wt%, further preferably less than 6.2wt%, and particularly preferably less than 5.3wt%.

[0057] In some embodiments, the total content of other nitrile compounds is bwt%, and b is 0.3, 0.35, 0.4, 0.45, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.4, 1.5, 2, 2.5, 3, 3.1, 3.6, 3.9, 4, 4.6, 5.3, 6.2, 7.1, 7.9, 8 or in the range consisting of any two of the above values. For example, 0.3 to 5.3, 0.6 to 4.6, 0.9 to 3.1, 0.4 to 2, 0.45 to 3.6, 0.8 to 2.5, 1.4 to 3.9, 2.5 to 8, 0.9 to 6.2, 0.45 to 5.3, 0.6 to 1.4, when within the above range, it helps to further improve the low temperature output characteristics of the secondary battery. Specifically, the content of succinonitrile is 1.7 wt % to 5.5 wt %, or the content of adiponitrile is 2.3 wt % to 4 wt %, or the content of ethylene glycol di(propionitrile) ether is 0.3 wt % to 0.9 wt %, or the content of 1,2,3-tris(2-cyanoethoxy)propane is 0.4 wt % to 2.3 wt %.

[0058] In addition, the electrolyte may also include other additives. The inventors have also unexpectedly discovered that other additives can inhibit the decomposition and regeneration of the aforementioned coating during the charge and discharge process, thereby further improving the high potential life and low temperature output characteristics of the secondary battery.

[0059] Other additives include at least one of 2-ethyl-1-hexyl difluorophosphite, 4-methyl-2-pentyl difluorophosphite, pentyl difluorophosphite, fluoroethylene carbonate, vinylene carbonate, lithium fluorosulfonate, vinyl sulfate, 1,3-propylene glycol cyclosulfate, fluorobenzene, cyclohexylbenzene, biphenyl, tris(trimethylsilane)phosphate or tris(trimethylsilane)borate. The other additives may be only one or more.

[0060] Specifically, from the viewpoint of improving the low-temperature output characteristics, based on the total mass of the electrolyte, the content of other additives is 0.01wt% or more, preferably 0.1wt% or more, preferably 1.6wt% or more, and more preferably 2.8wt% or more. In addition, from the viewpoint of improving the low-temperature output characteristics, the content of other additives is 10wt% or less, preferably 9.7wt% or less, more preferably 8.2wt% or less, further preferably 7.1wt% or less, and particularly preferably 6.7wt% or less.

[0061] In some embodiments, the total content of other additives is cwt%, and c is 0.01, 0.03, 0.1, 0.3, 0.35, 0.4, 0.45, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.5, 1.6, 2, 2.5, 2.9, 3, 3.5, 3.9, 4, 4.5, 5, 5.7, 6, 6.5, 7.1, 7.5, 8.2, 8.6, 9, 9.3, 9.7, 10 or in the range consisting of any two of the above values. For example, 0.3 to 18.2, 0.45 to 7.5, 0.6 to 9.7, 5.5 to 9.7, 6 to 8.6, 2.8 to 6.5, 1 to 6.5, 0.7 to 7.1, 1.5 to 9.3, 0.45 to 3.9, 0.7 to 4.5, when within the above range, it helps to further improve the low temperature output characteristics. Specifically, the content of fluoroethylene carbonate is 4.1wt% or more and 6.9wt% or less, or the content of vinyl sulfate is 0.01wt% or more and 0.3wt% or less, or the content of 2-ethyl-1-hexyl difluorophosphite is 0.01wt% or more and 1.4wt% or less.

[0062] The lithium salt used in the electrolyte of the present application includes lithium hexafluorophosphate, and the content of lithium hexafluorophosphate is 9 to 15 wt %, preferably 9 to 13 wt %, and more preferably 9 to 12 wt % based on the total mass of the electrolyte. By setting the content in the above range, the low temperature characteristics can be improved.

[0063] The electrolyte of the present application may further include any non-aqueous solvent known in the prior art that can be used as a solvent for the electrolyte. For example, cyclic carbonates, chain carbonates, cyclic carboxylates, chain carboxylates, cyclic ethers, chain ethers, phosphorus-containing organic solvents, and sulfur-containing organic solvents. Chain carboxylates are preferred, such as ethyl acetate, ethyl fluoroacetate, ethyl propionate, and propyl propionate.

[0064] II. Diaphragm

[0065] In order to prevent short circuit, a separator is usually provided between the positive electrode and the negative electrode. In this case, the electrolyte of the present application is usually used by permeating the separator.

[0066] In some embodiments, from the viewpoint of improving adhesion of the separator after being impregnated with an electrolyte, the separator includes a polyolefin substrate and a coating on the substrate, wherein the coating includes boehmite.

[0067] In some embodiments, the polyolefin is polyethylene or polypropylene. The separator may also be a material formed by laminating the above materials, examples of which include, but are not limited to, a three-layer separator formed by laminating polypropylene, polyethylene, and polypropylene in this order.

[0068] The form of the separator may be a thin film form, examples of which include, but are not limited to, nonwoven fabrics, woven fabrics, microporous films, etc. In the thin film form, the pore size (diameter) of the separator is 0.01 μm to 1 μm, and the thickness is 5 μm to 50 μm. In addition to the above-mentioned independent thin film separators, the following separators can also be used: a separator formed by forming a composite porous layer containing the above-mentioned inorganic particles on the surface of the positive electrode and / or the negative electrode using a resin-based adhesive, for example, a separator formed by using a fluororesin as an adhesive to form a porous layer on both sides of the positive electrode with alumina particles having a particle size (Dv90) of 90% less than 1 μm.

[0069] The thickness of the separator is arbitrary. In some embodiments, the thickness of the separator is greater than 1 μm, greater than 5 μm, or greater than 8 μm. In some embodiments, the thickness of the separator is less than 50 μm, less than 40 μm, or less than 30 μm. When the thickness of the separator is within the above range, insulation and mechanical strength can be ensured, and the rate characteristics and energy density of the secondary battery can be ensured.

[0070] III. Positive electrode

[0071] The positive electrode includes a positive electrode current collector and a positive electrode mixture layer disposed on a surface of the positive electrode current collector.

[0072] The positive electrode mixture layer contains positive electrode active material, and the positive electrode mixture layer can be one layer or multiple layers. The positive electrode active material is any material that can reversibly insert and release lithium ions.

[0073] For example, as a positive electrode active material for a secondary battery, a composite metal oxide containing one or more selected from the group consisting of cobalt, manganese, and nickel and lithium, or an olivine-type phosphate containing one or more selected from iron, cobalt, nickel, and manganese is used. These positive electrode active materials can be used alone or in combination of two or more.

[0074] As such lithium composite metal oxides, for example, LiCoO2, LiMn2O4, LiNiO2, LiCo 1-x NixO2(0.01 <x<1)、LiNi x Mn y Co zA solid solution of O2 (x + y + z = 1), Li2MnO3 and LiMO2 (M is a transition metal such as Co, Ni, Mn, Fe, etc.), LiNi 1 / 2 Mn 3 / 2 O4, LiFePO4, LiMnPO4, and LiMn 1-x Fe x PO4 (0.01 < x < 1), and more preferably two or more. A part of these composite metal oxides with lithium or olivine-type phosphates containing lithium can be replaced by other elements, or a part of cobalt, nickel, manganese, and iron can be replaced by one or two or more elements selected from Co, Mn, Ni, Mg, Al, B, Ti, V, Nb, Cu, Zn, Mo, Ca, Sr, W, and Zr, or coated with a compound containing these other elements or a carbon material.

[0075] Regarding the voltage during charging, from the perspective of increasing the voltage, the positive electrode potential is preferably 4.4 V (vs. Li / Li+) or more, more preferably 4.5 V (vs. Li / Li+) or more, and particularly preferably 4.6 V (vs. Li / Li+) or more.

[0076] The conductive agent for the positive electrode is not particularly limited as long as it is an electron-conducting material that does not cause chemical changes. Examples include natural graphite (such as flake graphite), artificial graphite, carbon blacks such as acetylene black, Ketjen black, channel black, furnace black, lamp black, or thermal cracking carbon black. In addition, graphite and carbon black can be appropriately mixed and used. The mass content of the conductive agent in the positive electrode mixture is preferably 1 to 10 wt%, and particularly preferably 1.5 to 5 wt%.

[0077] The positive electrode can be manufactured as follows: Mix the above-mentioned positive electrode active material with a conductive agent such as acetylene black and carbon black, and a binder such as polytetrafluoroethylene, polyvinylidene fluoride, polyacrylonitrile, a copolymer of styrene and butadiene, and carboxymethyl cellulose. Add a high-boiling solvent such as 1-methyl-2-pyrrolidone and knead to form a positive electrode mixture slurry, then coat it on an aluminum foil or the like of the positive electrode current collector, dry, and press to form a positive electrode mixture layer.

[0078] The density of the part of the positive electrode other than the positive electrode current collector is usually 3.5 g / cm 3 or more. To further increase the capacity of the battery, it is preferably 3.8 g / cm 3 or more, more preferably 4 g / cm 3 or more, further preferably 4.1 g / cm 3 or more. In addition, as its upper limit, it is preferably 4.6 g / cm 3 or less.

[0079] There is no particular limitation on the type of positive electrode current collector, which can be any material known to be suitable for use as a positive electrode current collector. Examples of positive electrode current collectors may include, but are not limited to, metal materials such as aluminum, stainless steel, nickel plating, titanium, and tantalum; and carbon materials such as carbon cloth and carbon paper. In some embodiments, the positive electrode current collector is a metal material. In some embodiments, the positive electrode current collector is aluminum.

[0080] In order to reduce the electronic contact resistance between the positive electrode current collector and the positive electrode mixture layer, the surface of the positive electrode current collector may include a conductive additive or a conductive coating. Examples of conductive additives may include, but are not limited to, carbon and precious metals such as gold, platinum, and silver. Examples of conductive coatings may include a mixture layer containing an inorganic oxide, a conductive agent, and a binder.

[0081] The positive electrode can be made by forming a positive electrode mixture layer containing a positive electrode active material and a binder on the positive electrode current collector. The manufacture of the positive electrode using the positive electrode active material can be carried out by conventional methods, that is, the positive electrode active material and the binder, as well as the conductive material and the thickener as needed, are dry-mixed to form a sheet, and the obtained sheet is pressed onto the positive electrode current collector; or these materials are dissolved or dispersed in a liquid medium to form a slurry, and the slurry is applied to the positive electrode current collector and dried to form a positive electrode mixture layer on the positive electrode current collector, thereby obtaining a positive electrode.

[0082] IV. Negative electrode

[0083] The negative electrode includes a negative electrode current collector and a negative electrode mixture layer disposed on the surface of the negative electrode current collector, wherein the negative electrode mixture layer contains a negative electrode active material. In some embodiments, the chargeable capacity of the negative electrode active material is greater than the discharge capacity of the positive electrode active material to prevent lithium metal from being accidentally precipitated on the negative electrode during charging.

[0084] The negative electrode active material is not particularly limited, and examples thereof include carbon-based negative electrode active materials, metal-based negative electrode active materials, and negative electrode active materials obtained by combining these.

[0085] Carbon-based negative electrode active material

[0086] Here, the carbon-based negative electrode active material refers to an active material having a carbon-based skeleton into which lithium can be inserted, and examples of the carbon-based negative electrode active material include carbonaceous materials and graphite materials.

[0087] As carbonaceous materials, for example, graphitizable carbon, non-graphitizable carbon with a similar amorphous structure represented by glassy carbon, etc. can be cited. Here, as graphitizable carbon, for example, carbon materials obtained from petroleum or coal using tar pitch as raw material can be cited. Specific examples can be coke, mesocarbon microbeads (MCMB), mesophase pitch-based carbon fibers, and pyrolysis vapor-grown carbon fibers. In addition, as non-graphitizable carbon, for example, phenolic resin sintered bodies, polyacrylonitrile-based carbon fibers, quasi-isotropic carbon, furfuryl alcohol resin sintered bodies (PFA), hard carbon, etc. can be cited.

[0088] Furthermore, as graphite materials, for example, natural graphite, artificial graphite, etc. can be cited. Among them, as artificial graphite, for example: artificial graphite obtained by heat-treating carbon containing graphitized carbon mainly at 2800°C or above, graphite MCMB obtained by heat-treating MCMB at 2000°C or above, graphite mesophase pitch-based carbon fiber obtained by heat-treating mesophase pitch-based carbon fiber at 2000°C or above, etc. can be cited. In addition, in the present application, as a carbon-based negative electrode active material, natural graphite (amorphous coated natural graphite) in which at least a portion of its surface is coated with amorphous carbon can be used.

[0089] In addition, the metal-based negative electrode active material is an active material containing a metal, generally referring to an active material having an element capable of inserting lithium or alloying with lithium in the structure, and a theoretical current capacity of 500 mAh / g or more per unit mass when inserting lithium or alloying with lithium. As a metal-based negative electrode active material, for example, lithium metal, a single metal that can form a lithium alloy (such as Ag, Al, Ba, Bi, Cu, Ga, Ge, In, Ni, P, Pb, Sb, Si, Sn, Sr, Zn, Ti, etc.) and its alloy, and their oxides, sulfides, nitrides, silicides, carbides, phosphides, etc. can be used. Among them, as a metal-based negative electrode active material, an active material containing silicon (silicon-based negative electrode active material) is preferably used. This is because the use of a silicon-based negative electrode active material can increase the capacity of a lithium-ion secondary battery.

[0090] Examples of the silicon-based negative electrode active material include silicon (Si), alloys containing silicon, silicon oxides, and composites of a silicon-containing material and conductive carbon in which a silicon-containing material is coated with conductive carbon or composited with conductive carbon.

[0091] From the viewpoint of improving battery capacity, a silicon-carbon material, for example, a porous carbon-supported silicon composite material is preferred.

[0092] The negative electrode active material may be used alone or in combination of two or more at any ratio.

[0093] The negative electrode mixture layer may further include a negative electrode binder. The negative electrode binder can improve the bonding between the negative electrode active material particles and the bonding between the negative electrode active material and the current collector. The type of negative electrode binder is not particularly limited, as long as it is a material that is stable to the solvent used in the electrolyte or electrode manufacturing. In some embodiments, the negative electrode binder includes a resin binder. Examples of resin binders include, but are not limited to, fluororesins, polyacrylonitrile (PAN), polyimide resins, acrylic resins, polyolefin resins, and the like. When an aqueous solvent is used to prepare the negative electrode mixture slurry, the negative electrode binder includes, but is not limited to, carboxymethyl cellulose (CMC) or its salt, styrene-butadiene rubber (SBR), polyacrylic acid (PAA) or its salt, polyvinyl alcohol, and the like.

[0094] As the negative electrode current collector for holding the negative electrode active material, any known current collector can be used. Examples of the negative electrode current collector include, but are not limited to, metal materials such as copper, nickel, stainless steel, and nickel-plated steel. In some embodiments, the negative electrode current collector is copper.

[0095] The negative electrode can be prepared by applying a negative electrode mixture slurry containing a negative electrode active material, a resin binder, etc. on a negative electrode current collector, drying it, and then rolling it to form a negative electrode mixture layer on both sides of the negative electrode current collector, thereby obtaining a negative electrode.

[0096] The present application further provides an electronic device, which includes the secondary battery according to the present application.

[0097] The use of the secondary battery of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. In some embodiments, the secondary battery of the present application can be used for, but not limited to, laptop computers, pen-input computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries and lithium-ion capacitors, etc.

[0098] The preparation of the secondary battery is described below in conjunction with specific embodiments. Those skilled in the art will understand that the preparation method described in this application is only an example, and any other suitable preparation method is within the scope of this application.

[0099] Example

[0100] Examples of the nonaqueous electrolyte solution of the present application are shown below, but the present application is not limited to these examples.

[0101] Secondary battery manufacturing

[0102] The positive electrode active material lithium cobalt oxide (97 wt%) and acetylene black (1.5 wt%) were mixed, added to a solution prepared by dissolving polyacrylonitrile (1.5 wt%) in 1-methyl-2-pyrrolidone, and mixed to prepare a positive electrode mixture paste. The positive electrode mixture paste was applied to an aluminum foil, dried, pressurized, and then cut into a specified size to prepare a positive electrode.

[0103] The negative electrode active material artificial graphite and silicon carbon (mass ratio 90:10, total 96wt%) and styrene-butadiene rubber (2wt%) were mixed and added to a solution obtained by dissolving lithium carboxymethyl cellulose (2wt%) in deionized water in advance and mixed to prepare a negative electrode mixture paste. The negative electrode mixture paste was coated on a copper foil, dried, pressurized, and then cut into a specified size to make a negative electrode.

[0104] A 5 μm polyethylene porous membrane was used as a diaphragm substrate; deionized water and boehmite were added to a double planetary mixer and dispersed at high speed at 40°C for 1 hour; then a binder, sodium carboxymethyl cellulose, was added and stirred at low speed at room temperature for 1 hour to obtain a boehmite slurry with a solid content of 3%, wherein boehmite accounted for 2% of the total weight of the slurry and sodium carboxymethyl cellulose accounted for 1% of the total weight of the slurry. The boehmite slurry was then coated on one side of the 5 μm polyethylene porous membrane by printing and coating, and dried to obtain diaphragm 1, with a boehmite layer thickness of 1.5 μm. The diaphragm substrate without a boehmite layer was recorded as diaphragm 2.

[0105] The positive electrode and negative electrode prepared as above are each connected to a wire. The layers are stacked and wound via the above-mentioned separator. In addition, LiPF6 as a supporting electrolyte is dissolved in a solution containing (I) 1,3-propane sultone, (II) lithium difluorophosphate, (III) 1,3,6-hexane trinitrile, (IV) boron-containing lithium salts, other nitrile compounds, and other additives. Based on 100 parts by weight of the total mass of the electrolyte, the contents and components of (I) to (IV), other nitrile compounds, and other additives are shown in Tables 1-1 and 1-2. The content of LiPF6 is 14%, and the rest is ethylene carbonate, propylene carbonate, propyl propionate, and ethyl propionate (mass ratio 0.8:1:2:0.5).

[0106] Then, the wound body and 3.2g of electrolyte were placed in an aluminum laminate case. The opening of the case was heat-sealed, and a secondary battery was made through steps such as formation and capacity measurement. The secondary battery was a pouch-shaped secondary battery with a width of 35mm, a height of 48mm, and a thickness of 5mm.

[0107] In the above-mentioned secondary battery, the characteristics of the separator 1 and the separator 2 are shown in Table 1-1, and some components of the electrolyte are shown in Table 1-2 and Table 1-3.

[0108] Table 1-1 Types of diaphragms

[0109] serial number feature Diaphragm 1 With boehmite slurry coating Diaphragm 2 Boehmite-free slurry coating

[0110] Table 1-2 Some components of electrolyte

[0111]

[0112]

[0113] In Table 1-2, a1 represents the content of (I) 1,3-propane sultone, a2 represents the content of (II) lithium difluorophosphate, a3 represents the content of (III) 1,3,6-hexane trinitrile, a4 represents the total content of (IV) boron-containing lithium salts, b represents the total content of other nitrile compounds, and c represents the total content of other additives; the code explanations are as follows:

[0114] Table 1-3 Codes of some components of electrolyte

[0115] Code Substance name Code Substance name B1 Lithium tetrafluoroborate N1 Ethylene glycol di(propionitrile) ether B2 Lithium difluorooxalate borate N2 1,2,3-Tris(2-cyanoethoxy)propane B3 Lithium bis(oxalatoborate) N3 3-Methyl-1,3,5-tri(cyanoethoxy)pentane B4 Lithium tetracyanoborate N4 Adiponitrile B5 Lithium Tetramethoxyborate N5 Succinonitrile B6 Lithium tetrakis(2,2,2-trifluoroethoxy)borate B7 Lithium bis(trifluoromethyl)difluoroborate B8 Lithium dicyanoborate B9 Dilithium bis(trifluoroborate) sulfate B10 Lithium Malonate Oxalate Borate C1 Fluoroethylene carbonate C7 2-Ethyl-1-hexyl difluorophosphite C2 Lithium difluorophosphate C8 4-Methyl-2-pentyl difluorophosphite C3 Vinyl Sulfate C9 Amyl difluorophosphite C4 Vinylene carbonate C10 Tris(trimethylsilyl)phosphate C5 1,3-Propane sultone C11 Tris(trimethylsilyl)borate C6 1,3-Propene sultone C12 Lithium Fluorosulfate

[0116] Test Method

[0117] Adhesion after electrolyte immersion (wet adhesion)

[0118] The positive electrode and separator (with boehmite layers on both sides) prepared in the examples and comparative examples were cut into pieces of 50 mm in length and 10 mm in width, respectively. Then, the cut positive electrode and separator were overlapped and stacked. Using a roller press at a temperature of 25°C and a load of 10 kN / m, the obtained laminated sheet was pressed at a pressing speed of 30 m / min to obtain a test piece. The test piece was immersed in an electrolyte at a temperature of 60°C for 72 hours. Here, as the electrolyte, a solution containing 14 wt% LiPF6 as a supporting electrolyte in ethylene carbonate, propylene carbonate, propyl propionate, and ethyl propionate (mass ratio 0.8:1:2:0.5) was used. The immersed test piece was taken out of the electrolyte and the electrolyte on the surface of the test piece was wiped. The test piece was pressed again under the conditions of 1 MPa, 80°C, and 3 minutes. The current collector side of the positive electrode of the test piece after re-pressing is facing down, and a transparent tape (transparent tape specified in JIS Z1522) is pasted on the surface of the positive electrode. In addition, the transparent tape is pre-fixed on a horizontal test bench. Then, the stress when one end of the diaphragm is stretched in the vertical direction and peeled off at a tensile speed of 50 mm / min is measured. This measurement was carried out 3 times in total. In addition, a laminate of a negative electrode and a diaphragm is obtained in the same manner as above, and the laminate is pressed to obtain a test piece. Then, the test piece after re-pressing is obtained in the same manner as the case of using the above-mentioned positive electrode, and the stress after electrolyte immersion is measured 3 times in total.

[0119] By using the above-mentioned positive electrode and negative electrode measurements, the average value of the stress obtained in total of 6 times was obtained as the peel strength (N / m), and the process adhesion between the electrode and the separator separated by the boehmite layer after electrolyte immersion was evaluated according to the following criteria. The greater the peel strength, the better the wet adhesion, the higher the separator strength, the higher the safety performance of the secondary battery, and the better the energy density can be guaranteed.

[0120] A: The peel strength is 12.0 N / m or more.

[0121] B: The peel strength is 8.0 N / m or more and less than 12.0 N / m.

[0122] C: The peel strength is 5.0 N / m or more and less than 8.0 N / m.

[0123] D: Peel strength is less than 5.0 N / m.

[0124] High potential life characteristics

[0125] For the secondary battery produced, the operation of charging to 4.7V and discharging to 3.0V at 0.2C was repeated 3 times at 25°C. Thereafter, the operation of charging to 4.7V at 1C and discharging to 3.0V at 1C was repeated 100 times at 45°C. Then, the ratio of the 100th discharge capacity to the first discharge capacity was calculated and evaluated according to the following criteria. The larger the ratio of the discharge capacity, the better the high potential life characteristics.

[0126] A: The ratio is 85% or more.

[0127] B: The ratio is 80% or more and less than 85%.

[0128] C: The ratio is 75% or more and less than 80%.

[0129] D: The ratio is 70% or more and less than 75%.

[0130] E: ratio is less than 70%.

[0131] Low temperature output characteristics

[0132] The secondary battery prepared is charged to 4.7V by constant current constant voltage (CCCV) at a temperature of 25°C to prepare a battery cell. The prepared battery cell is discharged to 3.0V by a constant current method of 0.2C and 1C at a temperature of -20°C to calculate the capacity. Then, the discharge capacity retention rate represented by the capacitance ratio (=(capacitance at 1C / capacitance at 0.2C)×100(%)) is calculated. These measurements are performed on the batteries of five battery cells, and the average value of the discharge capacity retention rate is used as the output characteristic, and evaluated according to the following criteria. The larger the value, the better the output characteristic.

[0133] A: The average value of the discharge capacity retention rate is 85% or more.

[0134] B: The average value of the discharge capacity retention rate is 80% or more and less than 85%.

[0135] C: The average value of the discharge capacity retention rate is 75% or more and less than 80%.

[0136] D: The average value of the discharge capacity retention rate is less than 75%.

[0137] The test results are shown in Table 2:

[0138] Table 2

[0139]

[0140]

[0141] As can be seen from Table 2, when the diaphragm includes a polyolefin substrate and a coating on the substrate, and the coating includes boehmite, the electrolyte contains a specific amount of 1,3-propane sultone, lithium difluorophosphate, 1,3,6-hexane trinitrile, and a boron-containing lithium salt, and the total content of 1,3-propane sultone and 1,3,6-hexane trinitrile in the above electrolyte is set to a specific range. The design can not only improve the safety of the secondary battery, but also significantly improve the high potential life and low temperature output characteristics of the secondary battery while maintaining a high energy density.

[0142] In particular, when the electrolyte further contains other nitrile compounds, the impedance of the coating can be reduced, further improving the high potential life and low temperature output characteristics of the secondary battery.

[0143] In particular, when the electrolyte also contains other additives, the inventors unexpectedly discovered that the other additives can inhibit the decomposition and regeneration of the coating during the charge and discharge process, thereby further improving the high potential life and low temperature output characteristics of the secondary battery.

[0144] References to "embodiments", "partial embodiments", "one embodiment", "another example", "example", "specific example" or "partial example" throughout the specification mean that at least one embodiment or example in the present application includes the specific features, structures, materials or characteristics described in the embodiment or example. Therefore, descriptions appearing in various places throughout the specification, such as: "in some embodiments", "in an embodiment", "in one embodiment", "in another example", "in an example", "in a specific example" or "example", do not necessarily refer to the same embodiment or example in the present application. In addition, the specific features, structures, materials or characteristics in the present application may be combined in one or more embodiments or examples in any suitable manner.

[0145] Although illustrative embodiments have been demonstrated and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions and modifications may be made to the embodiments without departing from the spirit, principles and scope of the present application.

Claims

1. A secondary battery, characterized in that: The invention comprises a positive electrode, a negative electrode, an electrolyte and a separator, wherein the separator comprises a polyolefin substrate and a coating disposed on at least one surface of the substrate, wherein the coating comprises boehmite; Based on the total mass of the electrolyte, the electrolyte satisfies: (I) comprising 1,3-propane sultone in an amount of 1.3 wt % or more and 2.7 wt % or less; (II) comprising lithium difluorophosphate in an amount of 0.01 wt % or more and 2 wt % or less; (III) comprising 1,3,6-hexanetrinitrile in an amount of 1.6 wt % or more and 3.9 wt % or less; (IV) comprising a boron-containing lithium salt in an amount of 0.01 wt % or more and 3 wt % or less; The total content of the 1,3-propane sultone and the 1,3,6-hexane trinitrile is 1.61 wt % or more and 6 wt % or less; The total content of the lithium difluorophosphate and the boron-containing lithium salt is greater than 0.02 wt % and less than 5 wt %; The electrolyte also includes succinonitrile.

2. The secondary battery according to claim 1, characterized in that: The boron-containing lithium salts include lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium bisoxalatoborate, lithium tetracyanoborate, lithium tetrakis(trifluoromethyl)borate, lithium (trifluoromethyl) trifluoroborate, lithium bis(trifluoromethyl)difluoroborate, lithium pentafluoroethyl trifluoroborate, lithium dicyanooxalatoborate, lithium bismalonate borate, lithium (2-fluoromalonate) difluoroborate, lithium malonate oxalatoborate, lithium bis(salicylate)borate, lithium bis(catecholate)borate, At least one of lithium methoxytricyanoborate, lithium ethoxytricyanoborate, lithium tetramethoxyborate, lithium tetraethoxyborate, lithium tetrakis(trifluoromethoxy)borate, lithium tetrakis(2,2,2-trifluoroethoxy)borate, lithium polytetrakis(hydroquinoneoxy)borate, lithium di(trifluoroborate) sulfate, lithium difluoroborate, lithium methanedisulfonate difluoroborate, lithium difluorophosphoryloxy trifluoroborate, lithium di(difluorophosphoryloxy)difluoroborate or lithium tetrakis(difluorophosphoryloxy)borate.

3. The secondary battery according to claim 1 or 2, characterized in that: The electrolyte includes lithium difluorophosphate in an amount of 0.01 wt % or more and 0.11 wt % or less based on the total mass of the electrolyte.

4. The secondary battery according to claim 1 or 2, characterized in that: The electrolyte includes lithium difluorophosphate in an amount of 0.11 wt % or more and 0.59 wt % or less based on the total mass of the electrolyte.

5. The secondary battery according to claim 1 or 2, characterized in that: The electrolyte includes 1,3,6-hexanetricarbonitrile in an amount of 1.6 wt % or more and 2.8 wt % or less based on the total mass of the electrolyte.

6. The secondary battery according to claim 1 or 2, characterized in that: The electrolyte also contains other nitrile compounds, which include at least one of ethylene glycol di(propionitrile) ether, 1,2,3-tris(2-cyanoethoxy)propane, and 3-methyl-1,3,5-tris(cyanoethoxy)pentane; based on the total mass of the electrolyte, the content of the other nitrile compounds is greater than 0.3wt% and less than 8wt%.

7. The secondary battery according to claim 1, characterized in that: The content of succinonitrile is 1.7 wt % or more and 5.5 wt % or less based on the total mass of the electrolyte.

8. The secondary battery according to claim 6, characterized in that: The electrolyte includes ethylene glycol di(propionitrile) ether, and the content of the ethylene glycol di(propionitrile) ether is greater than 0.3 wt % and less than 0.9 wt % based on the total mass of the electrolyte.

9. The secondary battery according to claim 6, characterized in that: The electrolyte includes 1,2,3-tris(2-cyanoethoxy)propane, and the content of the 1,2,3-tris(2-cyanoethoxy)propane is greater than or equal to 0.4 wt % and less than or equal to 2.3 wt % based on the total mass of the electrolyte.

10. The secondary battery according to claim 1 or 2, characterized in that: The electrolyte also includes other additives, which include at least one of 2-ethyl-1-hexyldifluorophosphite, 4-methyl-2-pentyldifluorophosphite, pentyldifluorophosphite, fluoroethylene carbonate, vinylene carbonate, lithium fluorosulfonate, vinyl sulfate, 1,3-propylene glycol cyclic sulfate, fluorobenzene, cyclohexylbenzene, biphenyl, tris(trimethylsilane)phosphate or tris(trimethylsilane)borate; based on the total mass of the electrolyte, the content of the other additives is greater than 0.01wt% and less than 10wt%.

11. The secondary battery according to claim 10, characterized in that: The electrolyte includes fluoroethylene carbonate, and the content of the fluoroethylene carbonate is greater than or equal to 0.01 wt % and less than or equal to 3 wt % based on the total mass of the electrolyte.

12. The secondary battery according to claim 10, characterized in that: The electrolyte includes fluoroethylene carbonate, and the content of the fluoroethylene carbonate is greater than or equal to 4.1 wt % and less than or equal to 6.9 wt % based on the total mass of the electrolyte.

13. The secondary battery according to claim 10, characterized in that: The electrolyte includes vinyl sulfate, and the content of the vinyl sulfate is greater than or equal to 0.01 wt % and less than or equal to 0.3 wt % based on the total mass of the electrolyte.

14. The secondary battery according to claim 10, characterized in that: The electrolyte includes 2-ethyl-1-hexyl difluorophosphite, and the content of the 2-ethyl-1-hexyl difluorophosphite is greater than or equal to 0.01 wt % and less than or equal to 1.4 wt % based on the total mass of the electrolyte. 15 . An electronic device comprising the secondary battery according to claim 1 .