Polyolefin composition comprising heterophasic polypropylene polymer and recycled plastic material

By rationally formulating heterophasic propylene copolymers and recycled materials in polyolefin compositions, the problem of difficult maintenance of the thermal mechanical properties of recycled polypropylene is solved, and a high-quality polyolefin composition is achieved, which is suitable for complex applications.

CN119032131APending Publication Date: 2024-11-26BOREALIS AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380034589.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-19
Filing Date
2023-04-18
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to effectively recycle and reuse high-quality polypropylene plastics, especially because the thermal mechanical properties of recycled polypropylene are difficult to maintain or improve when mixed with native polypropylene, resulting in insufficient performance in applications.

Method used

Using a polyolefin composition containing 60-95% heterophase propylene copolymer and 5-40% recycled material mixed with plastic polypropylene blends, by adjusting component ratios and additives to increase melt flow rate and impact strength, Ensure that the fatigue crack growth rate is comparable to that of the native polymer.

Benefits of technology

It is achieved to improve the quality of recovered polypropylene material while maintaining or improving the thermomechanical properties, so that it exhibits properties comparable to native polymers in applications such as pipes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119032131A_ABST
    Figure CN119032131A_ABST
Patent Text Reader

Abstract

The present invention relates to a polyolefin composition comprising: a) 60% to 95% by weight (based on the total weight of the polyolefin composition) of at least one heterophasic propylene copolymer (HECO), the at least one heterophasic propylene copolymer (HECO) has a total ethylene (C2) content (as determined according to CRYSTEX QC analysis) of from 0.5% to 4.5% by weight and a xylene cold soluble fraction (determined according to ISO 16152 at 25 DEG C) in the range of from 2% to 9% by weight, and a melt flow rate MFR2 (ISO 1133, 2.16 kg, 230 DEG C, measured according to ISO 1133) in the range of from 0.1 g / 10 to 1 g / 10, b) from 5% to 40% by weight (based on the total weight of the polyolefin composition) of a mixed plastic polypropylene blend of recycled material having an ethylene (C2) content, determined according to the CRYSTEX QC analysis, in the range of from 5% to 35% by weight, and c) optionally further additives, the sum of all the components always totaling 100% by weight, wherein the polyolefin composition is characterized by a melt flow rate MFR2 (230 DEG C, 2.16 kg, measured according to ISO 1133) of at least 0.3 g / 10 minutes; and an impact strength (ISO 179-1, Charpy 1 eA + 23 DEG C) of at least 15 kJ / m2.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a polyolefin composition comprising at least one heterophasic polypropylene copolymer and recycled plastic material, to articles comprising said polyolefin composition and to a process for the preparation of such a polyolefin composition.

[0002] describe

[0003] Polyolefins, particularly polyethylene and polypropylene, are increasingly consumed in large quantities in a wide range of applications, including packaging for food and other items, fibers, automotive components, and a variety of manufactured articles. Polyethylene-based materials are a particular problem because these materials are widely used for packaging. Given the huge amount of waste collected compared to the amount of waste recycled back into the stream, the intelligent reuse of plastic waste streams and the mechanical recycling of plastic waste still have great potential.

[0004] With their inherent versatility, plastics play a vital role in a sustainable and resource-efficient economy. However, as more and more plastics are manufactured and used in a linear economy, plastic waste is now considered a serious social problem. To this end, it is important to form a circular economy that gives plastic waste a second life (i.e., recycles it). This not only avoids leaving plastic waste in the environment, but also recovers its value.

[0005] The European Commission confirmed in 2017 that it would focus on plastic production and use. The EU’s goals are that 1) by 2025, at least 55% of all plastic packaging in the EU should be recycled; and 2) by 2030, all plastic packaging placed on the EU market should be reusable or easily recyclable. This has prompted brand owners and plastic processors to seek solutions with recycled content or virgin / recycled content blends. More recently, in 2021, the EU agreed to impose a tax on plastic packaging waste. The tax, which will be imposed from January 1, 2021, is calculated based on the weight of non-recycled plastic packaging waste and “requires a rate of €0.80 / kg, with mechanisms to avoid excessively regressive effects on national contributions.”

[0006] Therefore, there is an urgent need to find ways to recycle plastic waste. However, recycled plastic is often inferior to virgin plastic in terms of its quality due to degradation, contamination and mixing of different plastics.

[0007] A major trend in the field of polyolefins is to use recycled materials derived from a variety of sources. Durable goods streams such as those derived from yellow bags, yellow bins, community collections, waste electrical equipment (WEE) or end-of-life vehicles (ELV) contain a variety of plastics. These materials can be processed to recycle acrylonitrile-butadiene-styrene (ABS), high impact polystyrene (HIPS), polypropylene (PP) and polyethylene (PE) plastics. Density separation in water can be used and then further separation based on fluorescence, near infrared absorption or Raman fluorescence is separated. However, it is usually difficult to obtain pure recovery polypropylene or pure recovery polyethylene.

[0008] Typically, a large amount of polypropylene recycled on the market is a mixture of polypropylene (PP) and polyethylene (PE), which is especially true for post-consumer waste streams. In addition, commercial recyclates from post-consumer waste sources are routinely cross-contaminated with non-polyolefin materials (e.g., polyethylene terephthalate, polyamide, polystyrene) or non-polymer substances (such as wood, paper, glass or aluminum). These cross-contaminations greatly limit the final application of the recycling stream, leaving no useful final use. Polyolefin recycling materials, especially polyolefin recycling materials from post-consumer waste streams, are a mixture of PE and PP. The better the quality of the recycling material, the less available it is, and the more expensive it is.

[0009] The quality issues of recyclates compared to virgin ones can be overcome to some extent by mixing recyclates with virgin polymers. Compositions comprising virgin polymers (ie first-time used polymers) and recycled mixed plastics have been investigated.

[0010] EP 3715410 A1 relates to a composition comprising a recycled polymer composition (RPC) and a heterophasic propylene copolymer (HECO). The recycled polymer composition (RPC) comprises at least 80% by weight of recycled polypropylene. The heterophasic propylene copolymer (HECO) has a xylene cold soluble (XCS) fraction in the range of 5.0% to 18% by weight, and a melt flow rate MFR2 (230°C / 2.16kg) in the range of 0.05g / 10min to 1.5g / 10min.

[0011] WO2021 / 032459A1 discloses a polypropylene-polyethylene blend comprising component A): a recycled blend having a total C2 content of 12 wt% to 14.5 wt% and component B): a virgin random polypropylene having a total C2 content of 3.7 wt% and an XCS content of 6.5 wt% Copolymer .

[0012] WO2021 / 032460A1 discloses a polypropylene-polyethylene blend comprising component A): a recycled material blend, and component B): virgin random polypropylene Homopolymer .

[0013] Wang et al. (Mechanical and Processing Enhancement of a Recycled HDPE / PPR-Based Double-Wall Corrugated Pipe via a POE-g-MAH / CaCO3 / HDPE Polymer Composite; ACS Omega, 2021, 6(30), 19705-19716) used a modified maleic anhydride grafted polyethylene (POE-g-MAH) compatibilizer to increase interfacial adhesion and dispersion. POE-g-MAH / CaCO3 / HDPE polymer composites were prepared by surface modification of calcium carbonate. Such modified polymer composites can further enhance the processing performance and mechanical properties of recycled HDPE and PPR (random copolymer polypropylene) materials. The results show that with the introduction of polymer composites, significant improvements in processability, tensile strength, flexural properties and impact force can be obtained for recycled materials, and POE-g-MAH / CaCO3 / HDPE polymer composites will help achieve an impressive balance between high rigidity and toughness. In addition, the feasibility and mechanical properties of recycled HDPE-PPR-POE-g-MAH / CaCO3 / HDPE blends were studied: with the help of composite microcapsules, the mechanical property gap between recycled and non-recycled materials was further narrowed, and such blends can be commercialized in the pipeline industry.

[0014] Matias et al. (Use of recycled polypropylene / poly(ethylene terephthalate) blends to manufacture water pipes: An industrial scale study, Waste Management (Oxford, United Kingdom); 2020, 101, 250-258) explored the possibility of incorporating PP or PET from plastic solid waste (PSW) in pipe manufacturing with competitive mechanical properties compared to PP or PET made from virgin materials. To achieve this industrial solution, a method using a PP / PET 70 wt% / 30 wt% formulation was developed, and the effects of replacing virgin materials with different PSWs on the microstructure, thermal properties, and mechanical properties of the final material were analyzed. The impact of using a compatibilizer that can offset the natural immiscibility between the PP domain and the PET domain was also evaluated. The formulation developed with recycled PET is a good example of applying work developed on a laboratory scale to industrial-scale production.

[0015] As can be seen, it is generally possible to use recycled polypropylene in place of virgin polypropylene. However, when replacing virgin polymer with recycled material, there is still a need to improve or maintain thermomechanical properties, such as fatigue crack growth performance.

[0016] It is therefore an object of the present invention to provide a polyolefin composition wherein at least a portion of the virgin polyolefin is replaced by a polyolefin material recycled from waste plastic material, while the thermomechanical properties of such a polyolefin composition are at least maintained or even improved.

[0017] This object has been solved by providing a polyolefin composition comprising:

[0018] a) 60 to 95 wt.-% (based on the total weight of the polyolefin composition) of at least one heterophasic propylene copolymer (HECO) having a total ethylene (C2) content of 0.5 to 4.5 wt.-% (as determined according to CRYSTEX QC analysis) and a xylene cold soluble fraction in the range of 2 to 9 wt.-% (determined according to ISO 16152 at 25 °C) and a melt flow rate MFR2 (ISO 1133, 2.16 kg, 230 °C, measured according to ISO 1133) in the range of 0.1 to 1 g / 10 min,

[0019] b) 5 to 40 wt% (based on the total weight of the polyolefin composition) of a mixed plastic polypropylene blend of recycled material, the mixed plastic polypropylene blend of recycled material having an ethylene (C2) content (as determined according to CRYSTEX QC analysis) in the range of 5 to 35 wt%, and

[0020] c) optionally further additives, wherein the sum of all constituents always amounts to 100% by weight, wherein the polyolefin composition has

[0021] - a melt flow rate MFR2 (230° C., 2.16 kg, measured according to ISO 1133) of at least 0.3 g / 10 min; and

[0022] - At least 15 kJ / m 2 Impact strength (ISO179-1, Charpy 1eA+23℃).

[0023] Thus, a polyolefin composition comprising recycled plastic material and virgin heterophasic polypropylene polymer is provided. This combination provides a composition wherein at least a portion of the virgin polymer is replaced by recycled material, wherein properties such as fatigue crack growth rate are nearly comparable to the virgin polymer. Such a composition is suitable for use in pipes, such as high pressure pipes.

[0024] The polyolefin composition containing recyclate of the present invention is characterized in that fatigue crack growth rate and impact strength are suitable with original heterophasic polypropylene copolymer.The performance of the combination of different types of polymer and recyclate is not easy to predict.Due to the interaction between various components, it is therefore particularly difficult to predict fatigue crack growth rate and impact strength.In addition, recycled polyolefin is usually polluted by polar polymers (for example PA, PET) or other non-PO (for example PS or filler), which makes the obvious calculation of final mechanical properties more difficult.

[0025] It is to be understood that the polyolefin composition of the present invention does not contain talc, glass fibers, compatibilizers, HDPE or rubber - except for any amounts of such components present in the recyclate.

[0026] For the purposes of this specification and the appended claims, the term "recycled" is used to indicate that the material is recovered from post-consumer waste and / or post-industrial waste. That is, post-consumer waste refers to an object that has completed at least the first use cycle (or life cycle), that is, has served its first purpose and has passed through the hands of a consumer; while post-industrial waste refers to manufacturing waste that does not usually reach a consumer. In the gist of the present invention, "recycled polymer" may also contain up to 17% by weight, preferably up to 3% by weight, more preferably up to 1% by weight, and even more preferably up to 0.1% by weight of other components derived from the first use, based on the total weight of the recycled polymer. The type and amount of these components affect the physical properties of the recycled polymer. The physical properties given below refer to the main components of the recycled polymer.

[0027] As also described further below, typical other components originating from the first use are thermoplastic polymers (such as polystyrene and PA6), talc, chalk, ink, wood, paper, limonene and fatty acids. The content of polystyrene (PS) and polyamide 6 (PA6) in the recycled polymer can be determined by Fourier transform infrared spectroscopy (FTIR), and the content of talc, chalk, wood and paper can be measured by thermogravimetric analysis (TGA).

[0028] The term "virgin" refers to newly generated materials and / or objects prior to first use and not recycled. A polymer is a "virgin" polymer when the source of the polymer is not explicitly mentioned.

[0029] According to one embodiment, the polyolefin composition of the present invention comprises

[0030] a) 70 to 90 wt.-% (based on the total weight of the polyolefin composition) of at least one heterophasic propylene copolymer (HECO) having a total ethylene (C2) content of 0.5 to 4.5 wt.-% (as determined according to CRYSTEX QC analysis) and a xylene cold soluble fraction in the range of 2 to 9 wt.-% (determined according to ISO 16152 at 25 °C) and a melt flow rate MFR2 (ISO 1133, 2.16 kg, 230 °C, measured according to ISO 1133) in the range of 0.1 to 1 g / 10 min,

[0031] b) 10 to 30 wt% (based on the total weight of the polyolefin composition) of a mixed plastic polypropylene blend of recycled material, the mixed plastic polypropylene blend of recycled material having an ethylene (C2) content in the range of 5 to 35 wt% as determined according to CRYSTEX QC analysis, and

[0032] c) optionally further additives, the sum of all constituents always adding up to 100% by weight.

[0033] It will be appreciated that the amounts of heterophasic propylene copolymer (HECO) and polypropylene recyclate are always complementary to each other. For example, in one embodiment, the composition may comprise 70 wt% heterophasic propylene copolymer (HECO) and 30 wt% polypropylene recyclate, or 80 wt% heterophasic propylene copolymer (HECO) and 20 wt% polypropylene recyclate.

[0034] In a preferred embodiment, the polyolefin composition of the present invention may comprise:

[0035] - 65 wt.% heterophasic propylene copolymer (HECO) and 35 wt.% polypropylene regrind;

[0036] - 70 wt.% heterophasic propylene copolymer (HECO) and 30 wt.% polypropylene regrind;

[0037] - 75 wt.% heterophasic propylene copolymer (HECO) and 25 wt.% polypropylene regrind;

[0038] - 80 wt.% heterophasic propylene copolymer (HECO) and 20 wt.% polypropylene regrind;

[0039] - 85 wt.% heterophasic propylene copolymer (HECO) and 15 wt.% polypropylene regrind;

[0040] - 90 wt.% heterophasic propylene copolymer (HECO) and 10 wt.% polypropylene regrind;

[0041] - 95 wt.% heterophasic propylene copolymer (HECO) and 5 wt.% polypropylene recycle.

[0042] It will be appreciated that small amounts of additives, such as antioxidants, may be present in the compositions described. The sum of all ingredients always totals 100%.

[0043] In a preferred embodiment, the polyolefin composition of the present invention has a melt flow rate MFR2 (2.16 kg, 230°C, measured according to ISO 1133) in the range of 0.3 g / 10 min to 1 g / 10 min, preferably 0.4 g / 10 min to 0.8 g / 10 min, more preferably 0.5 g / 10 min to 0.7 g / 10 min.

[0044] In another embodiment, the impact strength (ISO 179-1, Charpy 1eA+23°C) of the polyolefin composition of the present invention is at least 17 kJ / m 2 , more preferably at least 19 kJ / m 2 , still more preferably at least 20 kJ / m2 , especially at 15 kJ / m 2 Up to 25kJ / m 2 in the range of 17 kJ / m 2 Up to 23kJ / m 2 in the range of 19 kJ / m 2 Up to 21 kJ / m 2 within the range.

[0045] In case the polyolefin composition comprises 8 to 12 wt%, preferably 10 wt% of polypropylene recycled content, the impact strength is between 18 kJ / m 2 Up to 23kJ / m 2 in the range of 19 kJ / m 2 Up to 22 kJ / m 2 in the range of 20 kJ / m 2 Up to 21 kJ / m 2 within the range.

[0046] In case the polyolefin composition comprises 18 to 22 wt%, preferably 20 wt% polypropylene polyethylene recycle, the impact strength is between 17 kJ / m 2 Up to 22 kJ / m 2 in the range of 18 kJ / m 2 Up to 21 kJ / m 2 in the range of 19 kJ / m 2 Up to 20kJ / m 2 within the range.

[0047] In case the polyolefin composition comprises 28 wt% to 32 wt%, preferably 30 wt% polypropylene polyethylene recycle, the impact strength is between 15 kJ / m 2 Up to 20kJ / m 2 in the range of 16 kJ / m 2 Up to 19 kJ / m 2 in the range of 17 kJ / m 2 Up to 18kJ / m 2 within the range.

[0048] In a preferred embodiment, the polyolefin composition of the present invention has a relative humidity of greater than 0.8 MPa*m 0.5 , preferably greater than 0.9MPa*m 0.5 , more preferably greater than 0.95 MPa*m 0.5 , even more preferably greater than 1.0 MPa*m 0.5 The ΔK at 8E5 cycles I(derived from CRB testing according to ISO 18489:2015) as an indicator of fatigue crack growth resistance. ΔK at 8E5 cycles I The appropriate limit would be 1.5MPa*m 0.5 , preferably 1.3MPa*m 0.5 , more preferably 1.2 MPa*m 0.5 .

[0049] ΔK of the polyolefin composition of the present invention under 8E5 cycles I The values ​​may vary depending on the amount of polypropylene recycle added to the composition.

[0050] For example, if 8 wt% to 12 wt%, preferably 10 wt% polypropylene recycle is added, the ΔK of the final polyolefin composition at 8E5 cycles is I The value can be greater than 1.05MPa*m 0.5 , more preferably greater than 1.07MPa*m 0.5 .

[0051] If 18 wt% to 22 wt%, preferably 20 wt% polypropylene regrind is added, the ΔK of the final polyolefin composition at 8E5 cycles is I The value can be greater than 0.98MPa*m 0.5 , preferably greater than 1.00 MPa*m 0.5 , more preferably greater than 1.02MPa*m 0.5 .

[0052] If 28 wt% to 32 wt%, preferably 30 wt% polypropylene regrind is added, the ΔK of the final polyolefin composition at 8E5 cycles is I The value can be greater than 0.90MPa*m 0.5 , more preferably greater than 0.95 MPa*m 0.5 .

[0053] In another embodiment, the polyolefin composition of the present invention has a Young's modulus of 1500 MPa to 1800 MPa, preferably 1600 MPa to 1700 MPa; a yield strength of 30 MPa to 40 MPa, preferably 33 MPa to 36 MPa and a strain at break of 50% to 200%, preferably 60% to 150%, more preferably 70% to 115%.

[0054] In another embodiment, the density of the polyolefin composition of the present invention is 0.9 g / cm 3 Up to 0.95g / cm 3 , preferably 0.91 g / cm 3 Up to 0.92g / cm 3 .

[0055] In one embodiment, the polyolefin composition of the present invention has a PP enthalpy of 75 J / g to 110 J / g, preferably 95 J / g to 105 J / g, a PE enthalpy of 0.02 J / g to 3.0 J / g, preferably 0.02 J / g to 0.3 J / g, a PP T of 165° C. to 167° C. M and a PE T of 122°C to 126°C, preferably 122°C to 124°C M .

[0056] In a particularly preferred embodiment, the polyolefin composition comprises:

[0057] a) 70 to 90 wt.-% (based on the total weight of the polyolefin composition) of at least one heterophasic propylene copolymer (HECO) having a total ethylene (C2) content of 0.5 to 4.5 wt.-% (as determined according to CRYSTEX QC analysis) and a xylene cold soluble fraction in the range of 2 to 9 wt.-% (determined according to ISO 16152 at 25 °C) and a melt flow rate MFR2 (ISO 1133, 2.16 kg, 230 °C, measured according to ISO 1133) in the range of 0.1 to 1 g / 10 min,

[0058] b) 10 to 30 wt% (based on the total weight of the polyolefin composition) of a mixed plastic polypropylene blend of recycled material, the mixed plastic polypropylene blend of recycled material having an ethylene (C2) content in the range of 5 to 10 wt% as determined according to CRYSTEX QC analysis, and

[0059] c) optionally further additives, wherein the sum of all constituents always amounts to 100% by weight, wherein the polyolefin composition has

[0060] a melt flow rate MFR2 (230° C., 2.16 kg, measured according to ISO 1133) in the range of 0.3 g / 10 min to 1 g / 10 min, preferably 0.4 g / 10 min to 0.8 g / 10 min, more preferably 0.5 g / 10 min to 0.7 g / 10 min,

[0061] - at 17 kJ / m 2 Up to 23kJ / m 2 in the range of 19 kJ / m 2 Up to 21 kJ / m 2 Impact strength within the range (ISO179-1, Charpy 1eA+23℃),

[0062] -Preferably greater than 0.9 MPa*m 0.5 , preferably greater than 0.95MPa*m 0.5 , more preferably greater than 1.0 MPa*m 0.5 The ΔK at 8E5 cycles I (Derived from cracked round bar test according to ISO 18489:2015).

[0063] In a particularly preferred embodiment, the polyolefin composition comprises

[0064] a) 70 to 90 wt.-% (based on the total weight of the polyolefin composition) of at least one heterophasic propylene copolymer (HECO) having a total ethylene (C2) content of 0.5 to 4.5 wt.-% (as determined according to CRYSTEX QC analysis) and a xylene cold soluble fraction in the range of 2 to 9 wt.-% (determined according to ISO 16152 at 25 °C) and a melt flow rate MFR2 (ISO 1133, 2.16 kg, 230 °C, measured according to ISO 1133) in the range of 0.1 to 1 g / 10 min,

[0065] b) 10 to 30 wt% (based on the total weight of the polyolefin composition) of a mixed plastic polypropylene blend of recycled material, the mixed plastic polypropylene blend of recycled material having an ethylene (C2) content determined according to CRYSTEX QC analysis in the range of 5 to 10 wt% and a C2 (CF) content of the crystalline fraction as determined according to CRYSTEX QC analysis of less than 5 wt%,

[0066] c) optionally further additives, wherein the sum of all constituents always amounts to 100% by weight, wherein the polyolefin composition has

[0067] a melt flow rate MFR2 (230° C., 2.16 kg, measured according to ISO 1133) in the range of 0.3 g / 10 min to 1 g / 10 min, preferably 0.4 g / 10 min to 0.8 g / 10 min, more preferably 0.5 g / 10 min to 0.7 g / 10 min,

[0068] - at 17 kJ / m 2 Up to 23kJ / m 2 in the range of 19 kJ / m 2 Up to 21 kJ / m 2 Impact strength within the range (ISO179-1, Charpy 1eA+23℃),

[0069] -Preferably greater than 0.9 MPa*m0.5 , preferably greater than 0.95MPa*m 0.5 , more preferably greater than 1.0 MPa*m 0.5 The ΔK at 8E5 cycles I (Derived from cracked round bar test according to ISO 18489:2015).

[0070] Heterophasic Polypropylene Virgin Polymer (HECO)

[0071] The heterophasic polypropylene copolymer comprises a polypropylene matrix (M) and an elastomeric copolymer (EPC) as polymer components. In one embodiment, at least one heterophasic propylene copolymer (HECO) comprises a propylene homopolymer (PPH) as (semi-crystalline) matrix and a propylene-ethylene rubber as elastomeric propylene copolymer (EPC).

[0072] The polypropylene matrix (M) is preferably a random propylene copolymer or a propylene homopolymer, the latter being particularly preferred. The expression "propylene homopolymer" relates to a polypropylene comprising more than 99.5 wt.-%, preferably more than or at least 99.7 wt.-% propylene units. In a preferred embodiment only propylene units are detectable in the propylene homopolymer.

[0073] The elastomeric propylene copolymer (EPC) comprises units derived from propylene and ethylene and / or C4 to C20 α-olefins, more preferably derived from ethylene and / or C4 to C10 α-olefins, and most preferably derived from ethylene, C4, C6 and / or C8 α-olefins (e.g. ethylene), and optionally comprises units derived from a conjugated diene.

[0074] In a preferred embodiment the at least one heterophasic propylene copolymer (HECO) comprises a propylene homopolymer and a propylene-ethylene rubber as elastomeric propylene copolymer.

[0075] The amount of elastomeric propylene copolymer (EPC) typically corresponds to the xylene cold soluble (XCS) fraction. The heterophasic propylene copolymer (HECO-1) used in the instant invention has a xylene cold soluble fraction determined according to ISO 16152 at 25 °C in the range of 2.5 to 8.5 wt.-%, preferably in the range of 3.0 to 8.0 wt.-%, more preferably in the range of 4.0 to 7.0 wt.-%.

[0076] The heterophasic propylene copolymer (HECO) has a total ethylene (C2) content as determined according to CRYSTEX QC analysis of 1.0 to 4.0 wt.-%, preferably 1.0 to 3.0 wt.-%, more preferably 1.0 to 2.0 wt.-%.

[0077] The instant heterophasic propylene copolymer (HECO-1) has a content of soluble fraction (SF) determined according to CRYSTEX analysis in the range of 2.0 to 10.0 wt.-%, preferably 3.0 to 8.0 wt.-%, more preferably 4.0 to 7.0 wt.-%, even more preferably 5.0 to 6.0 wt.-%, based on the total weight of the heterophasic propylene copolymer.

[0078] The ethylene content (C2(SF)) of the soluble fraction (SF) of the heterophasic propylene copolymer (HECO-1) as determined according to CRYSTEX QC analysis is in the range of 10.0 to 30.0 wt.-%, preferably in the range of 15.0 to 25.0 wt.-%, more preferably in the range of 18.0 to 22.0 wt.-%.

[0079] The soluble fraction (SF) of the heterophasic propylene copolymer (HECO-1) has an intrinsic viscosity (iV(SF)) of not more than 3.0 dl / g, preferably not more than 3.5 dl / g, such as in the range of 2.0 to 4.0 dl / g, preferably in the range of 3.2 to 4.0 dl / g, e.g. 3.5 dl / g.

[0080] The ethylene content of the crystalline fraction (CF) of the heterophasic propylene copolymer (HECO-1) as determined according to CRYSTEX QC analysis (C2(CF)) is in the range of 0.1 to 2.0 wt.-%, preferably in the range of 0.2 to 1.0 wt.-%, more preferably in the range of 0.3 to 0.5 wt.-%.

[0081] The crystalline fraction (CF) of the heterophasic propylene copolymer (HECO-1) has an intrinsic viscosity (iV(CF)) of not more than 3.5 dl / g, preferably not more than 4.0 dl / g, like in the range of 3.0 to 6.0 dl / g, preferably in the range of 4.0 to 5.0 dl / g.

[0082] The at least one heterophasic propylene copolymer (HECO-1) has a melt flow rate MFR2 (ISO 1133, 2.16 kg, 230 °C, measured according to ISO 1133) in the range of 0.1 g / 10 min to 0.9 g / 10 min, preferably 0.15 g / 10 min to 0.8 g / 10 min, more preferably 0.2 g / 10 min to 0.7 g / 10 min.

[0083] It is to be understood that the polyolefin composition of the present invention may comprise not only one heterophasic virgin propylene copolymer but two heterophasic virgin propylene copolymers having different melt flow rates. This allows to adjust the melt flow rate of the final polyolefin composition.

[0084] The at least one heterophasic propylene copolymer (HECO-1) has an impact strength (ISO 179-1, Charpy 1eA + 23°C) of at least 20 kJ / m 2 , more preferably at least 25 kJ / m 2 , still more preferably at least 30 kJ / m 2 , especially at 20 kJ / m 2 Up to 40kJ / m 2 in the range of 25 kJ / m 2 Up to 38kJ / m 2 in the range of 30 kJ / m 2 Up to 35kJ / m 2 within the range.

[0085] The virgin heterophasic polypropylene copolymer (HECO-1) may have a tensile Young's modulus measured according to ISO 527-2 of at least 1800 MPa, preferably at least 1830 MPa, like in the range of 1800 to 2100 MPa, preferably in the range of 1830 to 2050 MPa.

[0086] The heterophasic propylene copolymer (HECO-1) may have a yield strength from 30 to 40 MPa, preferably from 33 to 37 MPa and a strain at break from 40 to 50%, preferably from 44 to 46%.

[0087] Mixed plastics polypropylene blends from recycled materials

[0088] The mixed plastic polypropylene blend is obtained from a recycled waste stream recycling post-consumer waste or post-industrial waste, such as for example from the automotive industry, or alternatively a combination of both. It is particularly preferred that the recyclate consists of recycled post-consumer waste and / or post-industrial waste.

[0089] In one aspect, the recyclate blend can be a polypropylene (PP)-rich material for recycling plastic materials, and the polypropylene (PP)-rich material includes significantly more polypropylene than polyethylene. The recycled waste stream with more polypropylene can be obtained, for example, from the automotive industry, especially because some automotive parts such as bumpers are the source of quite pure polypropylene materials in the recycling stream, or obtained by enhanced sorting. The rich PP material can be obtained by selective treatment, degassing and filtering, and / or by separation according to type and color (such as NIR or Raman sorting and VIS sorting). It can be obtained from a life waste stream (that is, it is a product of life recycling), such as the "yellow bag" recycling system organized by the "green dot" organization running in some areas of Germany.

[0090] Preferably, the polypropylene-rich recycled material is obtained from recycled waste by a plastic recycling process known in the art. Such PP-rich recyclates are commercially available from, for example, Corepla (Italian Consortium for the collection, recovery, recycling of packaging plastic wastes), Resource Plastics Corp. (Brampton, Ontario), Kruschitz GmbH, Plastics and Recycling (Austria), Vogt Plastik GmbH (Germany), MtmPlastics GmbH (Germany), etc. Non-exhaustive examples of polypropylene-rich recycled materials include: (Mtm Plastics GmbH), Recycled polypropylene pellets (Axion Ltd) and polypropylene copolymers (BSP compounds). It is believed that the present invention may be applicable to a wide range of recycled polypropylene materials or materials or compositions having a high content of recycled polypropylene. The polypropylene-rich recycled material may be in the form of pellets.

[0091] In one embodiment, the ethylene C2 content of the mixed plastic polypropylene blend of recycled material (as determined according to CRYSTEX QC analysis) is in the range of 5 wt% to 20 wt%, more preferably 5 wt% to 10 wt%. It is preferred to use propylene recyclate with a C2 content of less than 10 wt%.

[0092] The C2(SF) content of the soluble fraction of the recyclate blend as determined according to CRYSTEX QC analysis is in the range of 25 to 35 wt.-%, preferably 27 to 33 wt.-%, more preferably 29 to 31 wt.-%.

[0093] The C2(CF) content of the crystalline fraction of the recyclate blend as determined according to CRYSTEX QC analysis is in the range of 1 wt.-35 wt.-%, preferably 2 wt.-20 wt.-%, more preferably 4 wt.-10 wt.-%, in particular below 5 wt.-%, for example in the range of 1 wt.-5 wt.-%. It is particularly preferred to use a recyclate blend having a C2(CF) content below 5 wt.-%, for example 4.5 wt.-%.

[0094] In another embodiment, the melt flow rate (ISO1133, 2.16kg; 230°C) of the mixed plastic polypropylene blend of recycled materials is 5g / 10min to 30g / 10min, preferably 10g / 10min to 20g / 10min, more preferably 12g / 10min to 18g / 10min, and most preferably 13g / 10min to 17g / 10min. It is particularly preferred to use propylene recyclate with a melt flow rate of 13g / 10min to 16g / 10min.

[0095] Impact strength of recycled mixed plastic polypropylene blends (ISO179-1, Charpy 1eA + 23 ° C) is at least 4 kJ / m 2 , more preferably at least 5 kJ / m 2 , still more preferably at least 6 kJ / m 2 , especially at 4 kJ / m 2 Up to 15kJ / m 2 in the range of 5 kJ / m 2 Up to 10kJ / m 2 in the range of 6 kJ / m 2 Up to 8kJ / m 2 The use impact strength is 6kJ / m 2 Up to 7 kJ / m 2 Propylene recycle within the range of is particularly preferred.

[0096] In another embodiment, the recyclate blend has a Young's modulus of 1000 MPa to 1400 MPa, preferably 1100 MPa to 1300 MPa; a yield strength of 20 MPa to 30 MPa, preferably 25 MPa to 28 MPa, and a strain at break of 10% to 50%, preferably 30% to 50%, more preferably 35% to 45%, such as 39% or 46%.

[0097] In another embodiment, the mixed plastic polypropylene blend of recycled material comprises additional components selected from the group consisting of polystyrene, stabilizers, polyamides, talc, chalk, paper, wood, metals, limonene, fatty acids and mixtures thereof, in particular polystyrene as determined by FTIR, polyamide-6, limonene as determined by using solid phase microextraction (HS-SPME-GC-MS), chalk.

[0098] The blend may comprise organic fillers and / or inorganic fillers and / or additives in an amount of up to 10% by weight, preferably up to 3% by weight, relative to the weight of the blend, due to recycled sources.

[0099] As noted above, the recyclate blend may contain one or more additional components selected from:

[0100] - up to 3.0 wt. %, preferably up to 2.0 wt. %, of polystyrene and / or copolymers, such as ABS,

[0101] - up to 3.0% by weight of stabilizers, preferably up to 2.0% by weight of stabilizers,

[0102] - up to 4.0 wt. % polyamide, preferably up to 2.0 wt. % polyamide,

[0103] - up to 3.0% by weight of talc, preferably up to 1.0% by weight of talc,

[0104] - up to 1.0 wt. % paper, preferably up to 0.5 wt. % paper,

[0105] - up to 1.0 wt. % wood, preferably up to 0.5 wt. % wood, and

[0106] - up to 0.5% by weight of metal, preferably up to 0.1% by weight of metal,

[0107] - 0.1 ppm to 100 ppm of limonene as determined by using solid phase microextraction (HS-SPME-GC-MS), and

[0108] - 0 ppm to 200 ppm total fatty acid content as determined by using solid phase microextraction (HS-SPME-GC-MS), wherein all amounts are given relative to the total weight of the recyclate blend.

[0109] The properties of different recyclate blends that can be used are now described.

[0110] Blend A1: C2 content is 8 wt% to 9 wt%, C2 (CF) content is 7 wt% to 8 wt%, C2 (SF) content is 29 wt% to 30 wt%, intrinsic viscosity is 1.6 dL / g to 1.7 dL / g; MFR2 is 15 g / 10 min to 16 g / 10 min, Young's modulus is 1100 MPa to 1200 MPa, impact strength (Charpy test 23 ° C) is 6 kJ / m 2 Up to 7 kJ / m 2 .

[0111] Blend A2: C2 content is 7 wt% to 8 wt%, C2 (CF) content is 4 wt% to 5 wt%, C2 (SF) content is 30 wt% to 31 wt%, intrinsic viscosity is 1.7 dL / g to 1.8 dL / g; MFR2 is 13 g / 10 min to 14 g / 10 min, Young's modulus is 1300 MPa to 1400 MPa, impact strength (Charpy test 23 ° C) is 6 kJ / m 2 Up to 7 kJ / m 2 .

[0112] Blend A3: C2 content is 32 wt% to 33 wt%, C2 (CF) content is 31 wt% to 32 wt%, C2 (SF) content is 34 wt% to 35 wt%, intrinsic viscosity is 1.8 dL / g to 1.9 dL / g; MFR2 is 9 g / 10 min to 10 g / 10 min, Young's modulus is 1000 MPa to 1100 MPa, impact strength (Charpy test 23 ° C) is 5 kJ / m 2 Up to 6kJ / m 2 .

[0113] It is to be understood that Blend A1 and Blend A2 are preferred, with Blend A2 being the most preferred blend for use in the polyolefin composition of the present invention.

[0114] additive

[0115] Examples of additives for the polyolefin composition of the present invention are pigments or dyes (e.g. carbon black), stabilizers (antioxidants), antacids and / or anti-UV agents, antistatic agents, nucleating agents and utilization agents (e.g. processing aids). Preferred additives are carbon black, at least one antioxidant and / or at least one UV stabilizer.

[0116] Typically, the amount of these additives ranges from 0 to 5.0 wt%, preferably from 0.01 to 3.0 wt%, more preferably from 0.01 to 2.0 wt%, based on the weight of the total polyolefin composition.

[0117] Examples of antioxidants commonly used in the art are sterically hindered phenols (e.g. CAS No. 6683-19-8, also known as Irganox 1010FF TM sold by BASF), phosphorus-based antioxidants (e.g. CAS No. 31570-04-4, also as Hostanox PAR 24 (FF) TM sold by Clariant or as Irgafos 168 (FF) TM by BASF), sulfur-based antioxidants (e.g. CAS No. 693-36-7, sold as Irganox PS-802FL TM Sold by BASF), nitrogen-based antioxidants (e.g. 4,4'-bis(1,1'-dimethylbenzyl)diphenylamine), or antioxidant blends. Preferred antioxidants may be tris(2,4-di-tert-butylphenyl)phosphite and / or octadecyl 3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate.

[0118] Antacids are also well known in the art. Examples are calcium stearate, sodium stearate, zinc stearate, magnesium oxide and zinc oxide, synthetic hydrotalcite (e.g. SHT, CAS No. 11097-59-9), lactates and lactyl esters, and calcium stearate (CAS No. 1592-23-0) and zinc stearate (CAS No. 557-05-1).

[0119] Common anti-adhesion agents are natural silicon dioxide, such as diatomaceous earth (e.g., CAS No. 60676-86-0 (SuperfFloss TM ), CAS number 60676-86-0 (SuperFloss E TM ), or CAS No. 60676-86-0 (Celite499 TM )); synthetic silica (e.g., CAS No. 7631-86-9, CAS No. 7631-86-9, CAS No. 7631-86-9, CAS No. 7631-86-9, CAS No. 7631-86-9, CAS No. 7631-86-9, CAS No. 112926-00-8, CAS No. 7631-86-9, or CAS No. 7631-86-9); silicates (e.g., aluminum silicate (kaolin )CAS No. 1318-74-7, sodium aluminum silicate CAS No. 1344-00-9, calcined kaolin CAS No. 92704-41-1, aluminum silicate CAS No. 1327-36-2, or calcium silicate CAS No. 1344-95-2); synthetic zeolite (e.g., sodium calcium aluminosilicate hydrate CAS No. 1344-01-0, CAS No. 1344-01-0, or sodium calcium aluminosilicate hydrate CAS No. 1344-01-0).

[0120] The anti-UV agent is, for example, bis-(2,2,6,6-tetramethyl-4-piperidinyl)-sebacate (CAS No. 52829-07-9, Tinuvin 770); 2-hydroxy-4-n-octyloxy-benzophenone (CAS No. 1843-05-6, Chimassorb 81). Preferred UV stabilizers can be low molecular weight UV stabilizers and / or high molecular weight UV stabilizers, such as n-hexadecyl-3,5-di-tert-butyl-4-hydroxybenzoate, a mixture of esters of 2,2,6,6-tetramethyl-4-piperidinol and higher fatty acids (mainly stearic acid), and / or poly((6-morpholino-s-triazine-2,4-diyl)(1,2,2,6,6-pentamethyl-4-piperidinyl)imino)hexamethylene(1,2,2,6,6-pentamethyl-4-piperidinyl)imino)).

[0121] Alpha nucleating agents such as sodium benzoate (CAS No. 532-32-1); 1,3:2,4-bis(3,4-dimethylbenzylidene)sorbitol (CAS 135861-56-2, Millad 3988). Suitable antistatic agents are, for example, glycerol esters (CAS No. 97593-29-8) or ethoxylated amines (CAS No. 71786-60-2 or 61791-31-9) or ethoxylated amides (CAS No. 204-393-1).

[0122] These additives are generally added in amounts of 100 ppm to 2000 ppm for each individual component of the polymer.

[0123] It will be appreciated that the present invention also relates to a process for producing the polyolefin composition as defined herein.

[0124] The method comprises the following steps:

[0125] - providing a mixture of 60 to 95 wt.-% (based on the total weight of the polyolefin composition) of at least one heterophasic propylene copolymer (HECO) having a total ethylene (C2) content (as determined according to CRYSTEX QC analysis) of 0.5 to 4.5 wt.-%, and a xylene cold soluble fraction (determined according to ISO 16152 at 25 °C) in the range of 2 to 9 wt.-%, and a melt flow rate MFR2 (ISO 1133, 2.16 kg, 230 °C, measured according to ISO 1133) in the range of 0.1 to 1 g / 10 min, and 5 to 40 wt.-% (based on the total weight of the polyolefin composition) of a mixed plastic polypropylene blend of recycled material, and optionally further additives,

[0126] - melting the mixture in an extruder, and

[0127] - Optionally pelletizing the polyolefin composition obtained.

[0128] For purposes of the present invention, mixing and melting may be performed using any suitable melting and mixing means known in the art.

[0129] However, the melting and mixing steps are preferably carried out in a mixer and / or blender, a high shear mixer or a low shear mixer, a high speed blender or a twin screw extruder. Most preferably, the melting and mixing steps are carried out in a twin screw extruder, such as a co-rotating twin screw extruder. Such twin screw extruders are well known in the art, and the skilled person will adjust the melting and mixing conditions (e.g., melt temperature, screw speed, etc.) according to the process equipment.

[0130] The polyolefin composition according to the invention can be used in a wide range of applications, for example in the manufacture of structural products, appliances, pipes, roofing applications, in particular for pipes. Therefore, another subject of the present invention is an article, in particular a pipe, comprising the polyolefin composition according to the invention.

[0131] The present invention will now be described in more detail with reference to the embodiments and the accompanying drawings.

[0132] Figure 1 The ΔK at 8E5 cycles for fatigue crack growth of the comparative example and the inventive example is shown. I [MPa*m 0.5 ] versus melt flow rate [g / 10 min].

[0133] Experimental Section

[0134] The following examples are included to illustrate certain aspects and embodiments of the present invention as described in the claims. However, it should be understood by those skilled in the art that the following description is illustrative only and should not be construed in any way as limiting the present invention.

[0135] I. Analytical Methods

[0136] Determination of the amount of "iPP", "PVC", "PA", "PET", "PS" and "PE" by transmission infrared spectroscopy

[0137] Sample preparation:

[0138] All calibration samples and samples to be analyzed were prepared in a similar manner on fused pressed plaques.

[0139] About 2 g to 3 g of the compound to be analyzed are melted at 190 ° C. Subsequently, a pressure of 60 to 80 bar is applied in a hydraulic heating press for 20 seconds. Next, the sample is cooled to room temperature in 40 seconds under the same pressure in a cold press to control the morphology of the compound. The thickness of the plate is controlled to be 100 μm to 200 μm thick (depending on the MFR from the sample) by a 2.5 cm × 2.5 cm metal calibration frame plate; two plates are produced in parallel at the same time and under the same conditions. The thickness of each plate is measured before any FTIR measurement; all plates are 100 μm to 200 μm thick.

[0140] In order to control the plate surface and avoid any disturbance during the measurements, all plates were pressed between two double-sided silicone release papers.

[0141] In case of powder samples or inhomogeneous compounds, the pressing process was repeated three times by pressing and cutting the samples under the same conditions as described before to improve homogeneity.

[0142] Spectrometer:

[0143] Use a standard transmission FTIR spectrometer such as a Bruker Vertex 70 FTIR spectrometer with the following settings:

[0144] 4000cm -1 Up to 400cm -1 The spectral range,

[0145] 6mm aperture,

[0146] 2cm -1 The spectral resolution,

[0147] ·With 16 background scans, 16 spectrum scans,

[0148] An interference pattern zero filling factor of 32,

[0149] ·Norton Beer strong change.

[0150] Spectra were recorded and analyzed in Bruker Opus software.

[0151] Calibration samples:

[0152] Since FTIR is a secondary method, several calibration standards are composited to cover the target analytical range, typically:

[0153] For PA, 0.2 wt% to 2.5 wt%

[0154] For PS, 0.1 wt% to 5 wt%

[0155] For PET, 0.2 wt% to 2.5 wt%

[0156] For PVC, 0.1 wt% to 4 wt%

[0157] For the compounds, the following commercial materials were used: Borealis HC600TF as iPP, Borealis FB3450 as HDPE; and for the target polymers, such RAMAPET N1S (Indorama Polymer) for PET, B36LN (BASF), Styrolution PS 486N (Ineos) for high impact polystyrene (HIPS), and Inovyn PVC 263B (in powder form) for PVC.

[0158] All compounds were prepared on a small scale in a Haake kneader at temperatures below 265°C and for less than 10 minutes to avoid degradation.

[0159] Additional antioxidants such as Irgafos 168 (3000 ppm) were added to minimize degradation.

[0160] calibration:

[0161] The FTIR calibration principle is the same for all components: the intensity of a particular FTIR band divided by the plate thickness is related to the amount of the component determined by 1H or 13C solution state NMR for the same plate.

[0162] Each specific FTIR absorption band was chosen because its intensity increases with the amount of component concentration and because it is separated from the remaining peaks, regardless of the composition of the calibration standards and actual samples.

[0163] The methodology is described in the publication from Signoret et al. “Alterations of plastic spectrain MIR and the potential impacts on identification towards recycling”, Resources, conservation and Recycling journal, 2020, Vol. 161, Article 104980.

[0164] The wavelengths used for each calibration band are:

[0165] For PA, 3300cm -1 ,

[0166] For PS, 1601cm -1 ,

[0167] For PET, 1410cm -1 ,

[0168] For PVC, 615cm -1 ,

[0169] For iPP, 1167cm -1 .

[0170] For each polymer component i, a linear calibration (linearity based on the Beer-Lambert law) is constructed. A typical linear correlation for such a calibration is given below:

[0171]

[0172] where x i is the fraction amount of polymer component i (in wt%)

[0173] E i is the absorption intensity (in au absorption units) of the specific bands associated with polymer component i. These specific bands are 3300 cm -1 ; For PS: 1601cm -1 ; For PET: 1410cm -1 ; For PVC: 615cm -1 ; 1167cm for iPP -1 .

[0174] d is the thickness of the sample plate

[0175] A i and B i are the two correlation coefficients determined for each calibration curve

[0176] For the C2-rich fraction, no specific isolated band could be found, and thus the C2-rich fraction was estimated indirectly,

[0177] x 富C2 =100-(x iPP +x PA +x PS +x PET +x EVA +x PVC +x 白垩 +x 滑石 )

[0178] The EVA, chalk and talc contents were estimated "semi-quantitatively". This therefore makes the C2-rich content "semi-quantitative".

[0179] The following tapes are used to estimate EVA, chalk and talc content:

[0180] EVA: 607cm -1 The center belt

[0181] Chalk: 1798cm -1 The center belt

[0182] Talc: 3676cm -1 The center belt

[0183] In addition, the presence of titanium dioxide, TiO2 and carbon black was reported. Their quantification by FTIR is not feasible.

[0184] For each calibration standard, whenever available, the amount of each component is given by 1 H or 13 C solution state NMR was determined as the primary method (except for PA). NMR measurements were performed on exactly the same FTIR plate used to construct the FTIR calibration curve.

[0185] The amount of talc and chalk was measured by thermogravimetric analysis (TGA). The experiment was performed using a Perkin Elmer TGA8000. About 10 mg to 20 mg of material was placed in a platinum pan. The temperature was balanced at 50°C for 10 minutes, then raised to 950°C at a heating rate of 20°C / min under nitrogen. The weight loss (WCO2) between about 550°C and 700°C was assigned to CO2 released from CaCO3, and the chalk content was therefore estimated as:

[0186] Chalk content = 100 / 44×WCO2

[0187] Afterwards, the temperature was lowered to 300°C at a cooling rate of 20°C / min. The gas was then switched to oxygen and the temperature was raised again to 900°C. The weight loss in this step is designated as carbon black (Wcb). Knowing the contents of carbon black and chalk, the ash content excluding chalk and carbon black is calculated as:

[0188] Ash content = (ash residue) - 56 / 44 × WCO2 - Wcb

[0189] The ash residue is in % by weight measured at 900° C. in a first step carried out under nitrogen. The ash content is estimated to be identical to the talc content of the recyclate studied.

[0190] Amount of paper and wood

[0191] Paper and wood are determined by conventional laboratory methods including grinding, flotation, microscopy and thermogravimetric analysis (TGA) or flotation techniques.

[0192] The amount of metal was determined by x-ray fluorescence (XRF).

[0193] The amount of limonene was determined by solid phase microextraction (HS-SPME-GC-MS).Additional details are given below for specific samples.

[0194] The amount of total fatty acids was determined by solid phase microextraction (HS-SPME-GC-MS).

[0195] Xylene cold solubles (XCS) are measured according to ISO 16152; First Edition; 2005-07-01 at 25°C.

[0196] Crystex analysis: crystalline and soluble fractions and their respective properties

[0197] The crystalline fraction (CF) and the soluble fraction (SF) of the polypropylene (PP) composition as well as the comonomer content and the intrinsic viscosity of each fraction were analyzed by means of CRYSTEX QC from Polymer Char (Valencia, Spain).

[0198] A schematic diagram of the CRYSTEX QC instrument is shown in Del Hierro, P.; Ortin, A.; Monrabal, B.; 'Soluble Fraction Analysis in polypropylene, The Column, February 2014, pages 18 to 23. The crystalline and amorphous fractions were separated by a temperature cycle of dissolution at 160°C, crystallization at 40°C, and redissolution in 1,2,4-trichlorobenzene (1,2,4-TCB) at 160°C. The quantification of SF and CF and the determination of the ethylene content (C2) were achieved by an infrared detector (IR4), and the intrinsic viscosity (IV) was determined using an online 2-capillary viscometer.

[0199] The IR4 detector is a multi-wavelength detector that detects IR absorbance at two different bands (CH3 and CH2) for determining the concentration and ethylene content of ethylene-propylene copolymers. The IR4 detector is calibrated with a series of EP copolymers with known ethylene contents ranging from 2 wt% to 69 wt% (determined by 13C-NMR).

[0200] The amounts of the soluble fraction (SF) and the crystalline fraction (CF) are related by means of the XS calibration to the amount of "xylene cold soluble" (XCS) and the xylene cold insoluble (XCI) fraction, respectively, determined according to the standard gravimetric method according to ISO 16152. The XS calibration was achieved by testing various EP copolymers with XS contents ranging from 2 wt% to 31 wt%.

[0201] The intrinsic viscosity (IV) of the parent EP copolymer and its soluble and crystalline fractions were determined using an online 2-capillary viscometer and correlated to the corresponding IV determined according to ISO 1628 in decalin.

[0202] Calibration was performed with several commercial EP PP copolymers with IV = 2 dL / g to 4 dL / g.

[0203] A sample of the PP composition to be analyzed was weighed out at a concentration of 10 to 20 mg / ml. After automatically filling the vial with 1,2,4-TCB containing 250 mg / l of 2,6-tert-butyl-4-methylphenol (BHT) as an antioxidant, the sample was dissolved at 160°C with constant stirring at 800 rpm until complete dissolution was achieved (usually for 60 minutes).

[0204] A defined volume of the sample solution is injected into a column filled with an inert support, where crystallization of the sample and separation of the soluble fraction from the crystalline part occurs. This process is repeated twice. During the first injection, the entire sample is measured at high temperature, and the IV [dl / g] and C2 [wt%] of the PP composition are determined. During the second injection, the soluble fraction (at low temperature) and the crystalline fraction (at high temperature) with a crystallization cycle are determined (wt% of SF, wt% of C2, IV).

[0205] II. Test Methods

[0206] Unless otherwise defined, the following definitions of terms and methods apply to the above general description of the invention as well as the following examples.

[0207] Production of Multi-Purpose Specimens (MPS) and Charpy Type 1 Specimens

[0208] All MPS were produced by injection molding on an Engel Victory 60 (Engel, Austria) according to ISO 3167 (Plastics-Multipurpose test specimens) and ISO 19069-2 (Plastics-Polypropylene (PP) molding and extrusion materials-Part 2: Preparation of test specimens and determination of properties). The specimens were conditioned at 23°C and 50% relative humidity for at least three days. After conditioning, these specimens were used for tensile testing and were subsequently cut and notched into Type 1 specimens for Charpy notched impact testing according to ISO 179-1 (see later for more information on testing).

[0209] Production of CRB specimens

[0210] The CRB specimens were produced according to ISO 18489, but with slight adjustments for different materials. Therefore, plates with dimensions of 16 mm×120 mm×150 mm were pressed in a male mold at 210°C. More specifically, a hydraulic press from Langzauner Perfectline (Langzauner, Austria) was used. In a fully automatic procedure, 270 g of granules were heated to 210°C in the mold with the weight of the mold and cylinder on top of the granules. An integrated temperature sensor allows direct measurement of the granules or the melt, respectively. When a temperature of 210°C is reached, a constant temperature is maintained for 15 minutes. Thereafter, a slow cooling with a cooling rate of 2K / min is started. Depending on the viscosity of the sample, a full pressure of 10 MPa is applied to the granules at a temperature starting from 165°C. After reaching 40°C, the pressure is released, the mold is opened, and the plate can then be removed.

[0211] The produced boards were conditioned at 23°C and 50% relative humidity for at least three days before being cut into bars on a table saw and turned on a lathe into CRB specimens according to ISO 18389. A 0.3 mm thick industrial grade razor blade was used to notch the specimens. After notching, the specimens were conditioned at 23°C and 50% relative humidity for an additional day before testing.

[0212] Melt flow rate (MFR)

[0213] According to ISO 1133-1 (Plastics-Determination of the melt mass-flowrate (MFR) and melt volume-flow rate (MVR) of thermoplastics-Part 1: Standard method), MFR measurements were performed at 230°C and with 2.16 kg on a Zwick / Roell Mflow melt flow indexer (Zwick Roell, Germany). Cuts were made every 3 mm of piston movement. The time between cuts was measured and each extrudate was weighed on an ABS220-4 electronic balance (Kern & Sohn, Germany). The MFR in g / 10 minutes for each cut was calculated by extrapolation to 10 minutes. Each material was measured once. In one measurement, 6 cuts were made and used to calculate the average and standard deviation.

[0214] density

[0215] Density measurements were performed according to ISO 01183-1 (Plastics-Methods for determining the density of non-cellular plastics-Part 1: Immersion method, liquid pycnometer method and titration method) using a Sartorius CPA 225D laboratory balance (Sartorius, Germany). The samples were cut from the gate-side shoulder of the multi-purpose specimen (MPS). In the first step, the corresponding samples were dry weighed and their mass in air (m S,A In the second step, the sample is immersed in deionized water with added detergent and placed under a buoyancy cage connected to a balance, enabling the measurement of the sample buoyancy (m) without the need for a sinker. S.IL A wire was used to keep the sample free of bubbles, and the temperature of the immersion liquid was recorded for calculation of its density (ρ IL ). The sample density is calculated using the measurement equipment correction variables A and B according to the following formula:

[0216]

[0217] For each material, five samples, each cut from a separate MPS, were used to calculate the mean and standard deviation.

[0218] Differential Scanning Calorimetry (DSC)

[0219] DSC test is carried out on Perkin Elmer differential scanning calorimeter DSC 8500 (Perkin Elmer, the United States). Samples are cut from the shoulder of injection molded multipurpose specimens and packaged in perforated aluminum pans. The average sample weight is about 8 mg. The program consists of a first heating, subsequent cooling, and a second heating stage with a constant heating / cooling rate of 10K / min in a temperature range of 0°C to 200°C, wherein nitrogen is used as a purge gas and the flow rate is 20ml / min. DSC measurements are completed to determine the melting peak in the second heating stage, which is a characteristic of the semi-crystallinity obtained under controlled cooling in the DSC device. In order to determine the melting enthalpy, the area of ​​the melting peak is integrated. Since the heat flux is normalized by the sample mass, the thermogram can be displayed as a normalized heat flux (W / g) over time (seconds), and the area of ​​the peak (W / g*seconds) will be calculated as W*seconds / g or J / g normalized melting enthalpy. For each material, five samples cut from separate MPS were used to calculate the average and standard deviation. Measurements were made according to ISO 11357-1 (Plastics-Differential scanning calorimetry (DSC)-Part 1: General principles) and ISO 11357-3 (Part 3: Determination of temperature and enthalpy of melting and crystallization). In short, the area of ​​the melting peak during the second heating process was integrated.

[0220] Oxidation induction temperature (T OX )

[0221] The oxidation induction temperature (dynamic OIT) was characterized using a DSC 4000 differential thermal analysis (DTA) instrument (PerkinElmer, USA) according to ISO 11357-6 (Plastics-Differential scanning calorimetry (DSC)-Part 6: Determination of oxidation induction time (isothermal OIT) and oxidation induction temperature (dynamic OIT)). The samples were cut from the injection molded MPS shoulder and packaged in a perforated aluminum pan. The average sample weight was about 8 mg. A single heating step from 23°C to 300°C was performed at a heating rate of 10 K / min, with synthetic air as the purge gas and a flow rate of 20 ml / min. The intersection of the slope before and during oxidation gives the onset of oxidation or the oxidation induction temperature in °C. For each material, five samples, each cut from a separate MPS, were used to calculate the mean and standard deviation.

[0222] Tensile properties

[0223] Mechanical properties (Young's modulus, yield strength and strain at break) were checked at 23°C using a universal testing machine Zwick AllroundLine Z020 (Zwick Roell, Germany) equipped with a multi-extensometer. Test parameters and MPS were used according to ISO 527-1 (Plastics-Determination of tensile properties-Part 1: General principles) and ISO 527-2 (Part 2: Test conditions for moulding and extrusion plastics), with a transverse speed of 1 mm / min for determining the Young's modulus until the strain was 0.25%, and then 50 mm / min until failure. For each material, five MPS were tested for calculation of the mean and standard deviation.

[0224] Charpy notched impact strength

[0225] Impact tests were performed according to ISO 179-1 (Plastics-Determination of Charpy impact properties-Part 1: Non-instrumented impact test) on a Zwick / Roell HIT25P pendulum impact tester (Zwick Roell, Germany) with injection molded specimens (see information below). After preliminary tests to determine the appropriate pendulum size, the appropriate pendulum was selected for testing each corresponding material. The notch was produced with a Leica RM2265 microtome (Leica, Germany) and measured on an Olympus SZX16 stereomicroscope (Olympus, Japan). The test conditions were 23° C., with the specimens notched along the edge having a notch radius of 0.25 mm (1 eA). For each material, ten specimens were tested for calculation of the average and standard deviation.

[0226] Cracked round bar method

[0227] For the investigation of fatigue crack growth (FCG) properties following ISO 18489:2015 (Polyethylene (PE) materials for piping systems-Determination of resistance to slow crack growth under cyclic loading-Cracked Round Bar test method), all materials were tested using an ElectroPuls E10000 electric testing machine (Instron, USA). To produce the CRB specimens, the plates were sheet molded and subsequently cut, turned and notched according to ISO 18489. A frequency of 10 Hz, an R ratio of 0.1 and an individually adjusted initial stress intensity factor range (ΔK I ) to achieve a test time of 10 to 100 hours. I The values ​​were corrected with the actual initial crack length measured after the test by an Olympus SZX16 stereo microscope (Olympus, Japan). The results are plotted as ΔK I Relative to cycles to failure. At least three measurements were performed for each material to generate a curve showing the dependence of the time to failure on load. ΔK at 8E5 cycles I Values ​​are derived from linear regression.

[0228] Different blends of recycled materials are used. The blends are characterized by the following properties:

[0229] Blend A1: C2 content is 8 wt% to 9 wt%, C2 (CF) content is 7 wt% to 8 wt%, C2 (SF) content is 29 wt% to 30 wt%, intrinsic viscosity is 1.6 dL / g to 1.7 dL / g; MFR2 is 15 g / 10 min to 16 g / 10 min, Young's modulus is 1100 MPa to 1200 MPa, impact strength (Charpy test 23 ° C) is 6 kJ / m 2 Up to 7 kJ / m 2 .

[0230] Blend A2: C2 content is 7 wt% to 8 wt%, C2 (CF) content is 4 wt% to 5 wt%, C2 (SF) content is 30 wt% to 31 wt%, intrinsic viscosity is 1.7 dL / g to 1.8 dL / g; MFR2 is 13 g / 10 min to 14 g / 10 min, Young's modulus is 1300 MPa to 1400 MPa, impact strength (Charpy test 23 ° C) is 6 kJ / m 2 Up to 7 kJ / m 2 .

[0231] Blend A3: C2 content is 32 wt% to 33 wt%, C2 (CF) content is 31 wt% to 32 wt%, C2 (SF) content is 34 wt% to 35 wt%, intrinsic viscosity is 1.8 dL / g to 1.9 dL / g; MFR2 is 9 g / 10 min to 10 g / 10 min, Young's modulus is 1000 MPa to 1100 MPa, impact strength (Charpy test 23 ° C) is 5 kJ / m 2 Up to 6kJ / m 2 .

[0232] The following additives were used: Antioxidants: AO1 (Irganox 1010FF), AO2 (IRGAFOS 168FF).

[0233] In the following Table 1 several examples (Comparative - CE; Inventive - IE) are summarized.

[0234] Table 1 relates to a polyolefin composition comprising:

[0235] a) (IE1, IE2, IE3) a heterophasic polypropylene copolymer (HECO-1, impact strength 20 kJ / m 2 ), blend A1 and additives (AO1, AO2);

[0236] b) (IE4, IE5, IE6) a heterophasic polypropylene copolymer (HECO-1, impact strength 20 kJ / m 2), blend A2 and additives (AO1, AO2);

[0237] c) (IE7) a heterophasic polypropylene copolymer (HECO-1, impact strength 20 kJ / m 2 ), blend A3 and additives (AO1, AO2);

[0238] d) (CE1, CE2, CE3) a heterophasic polypropylene copolymer (HECO-2, impact strength 55 kJ / m 2 ), blend A1 and additives (AO1, AO2);

[0239] e) (CE4) a heterophasic polypropylene copolymer (HECO-1, impact strength 33 kJ / m 2 ),

[0240] f) (CE5) a heterophasic polypropylene copolymer (HECO-2, impact strength 55 kJ / m 2 ),

[0241] g) (CE6) Blend A1 of recycled materials,

[0242] h) (CE7) Blend A2 of recycled materials,

[0243] i) (CE8) Blend A3 of recycled materials.

[0244] As can be seen in Table 1, when recycled blends A1 to A3 are added to HECO-1, the Charpy notched impact strength values ​​of the inventive polyolefin compositions (IE1 to IE7) are reduced from the virgin HECO-1 (CE4), but to a lesser extent than HECO-2. When 10% recycled blend A1 is added to HECO-1, the Charpy notched impact strength is 65% of the virgin HECO-1. ​​However, when 20% recycled blend A1 is added to HECO-1, the Charpy notched impact strength value is reduced to 60% of HECO-1, and when 30% recycled blend A1 is added to Heco-1, the Charpy notched impact strength value is only about 52% of HECO-1. ​​In particular, the fact that the Charpy notched impact strength values ​​of the inventive polyolefin compositions with up to 30% by weight recycled blends are indeed only reduced by about 48% compared to the virgin polymer is unexpected. In addition, ΔK, which is a measure of the fatigue growth rate of the inventive polyolefin compositions, is not reduced by only about 48%. I The values ​​decreased only to a small extent (8 to 15%) depending on the amount of recyclate added.

[0245] In contrast, when recycled blend A1 (CE1 to CE3) is added to HECO-2, the Charpy notched impact strength value decreases rapidly compared to the virgin polymer HECO-2 (CE5). Specifically, when 10% recycled blend A1 is added to HECO-2, the Charpy notched impact strength is 91% of the virgin HECO-2; however, when 20% recycled blend A1 is added to HECO-2, the Charpy notched impact strength value decreases to 34% of HECO-2, and when 30% recycled blend A1 is added to Heco-2, the Charpy notched impact strength value is only about 23% of HECO-2.

[0246]

[0247]

[0248] Resistance to FCG

[0249] As can be seen from Table 1, the resistance to fatigue crack growth of the polyolefin composition according to the invention comprising virgin HECO-1 and a recyclate blend varies with the recyclate loading; the lower the recyclate loading, the higher the resistance to fatigue crack growth.

[0250] Figure 1 The graph shows the resistance of different compositions to fatigue crack growth ΔK under 8E5 cycles I [MPa*m 0.5 ] relative to melt flow rate [g / 10min].

[0251] ΔK at 8E5 cycles I Used to evaluate the resistance of compounds to fatigue crack growth compared to virgin polymer references. All of the compounds of the invention (HECO-1 / recycled blends) have higher ΔK at 8E5 cycles than HECO-2 based compounds I , indicating better resistance to fatigue crack growth. Most of them even show higher ΔK at 8E5 cycles than HECO-2 with similar MFR to HECO-1 I .

[0252] also, Figure 1 The graph shows that MFR has a great influence on the resistance to fatigue crack growth: the lower the MFR, the better the resistance to fatigue crack growth.

Claims

1. A polyolefin composition comprising: a) 60 to 95 wt.-% (based on the total weight of the polyolefin composition) of at least one heterophasic propylene copolymer (HECO) having a total ethylene (C2) content of 0.5 to 4.5 wt.-% (determined according to CRYSTEX QC analysis) and a xylene cold soluble fraction in the range of 2 to 9 wt.-% (determined according to ISO 16152 at 25 °C) and a melt flow rate MFR2 (ISO 1133, 2.16 kg, 230 °C, measured according to ISO 1133) in the range of 0.1 to 1 g / 10 min, b) 5 to 40 wt% (based on the total weight of the polyolefin composition) of a mixed plastic polypropylene blend of recycled material, the mixed plastic polypropylene blend of recycled material having an ethylene (C2) content in the range of 5 to 35 wt% as determined according to CRYSTEX QC analysis, and c) optionally further additives, wherein the sum of all constituents always amounts to 100% by weight, wherein the polyolefin composition is characterized by - a melt flow rate MFR2 (230° C., 2.16 kg, measured according to ISO 1133) of at least 0.3 g / 10 min; and - At least 15 kJ / m 2 Impact strength (ISO179-1, Charpy 1eA+23℃).

2. The polyolefin composition according to claim 1, characterized in that It contains: a) 70 to 90 wt.-% (based on the total weight of the polyolefin composition) of at least one heterophasic propylene copolymer (HECO) having a total ethylene (C2) content of 0.5 to 4.5 wt.-% (determined according to CRYSTEX QC analysis) and a xylene cold soluble fraction in the range of 2 to 7 wt.-% (determined according to ISO 16152 at 25 °C); b) 10 to 30 wt% (based on the total weight of the polyolefin composition) of a mixed plastic polypropylene blend of recycled material, the mixed plastic polypropylene blend of recycled material having an ethylene (C2) content in the range of 5 to 35 wt% as determined according to CRYSTEX QC analysis, and c) optionally further additives, the sum of all constituents always adding up to 100% by weight.

3. The polyolefin composition according to claim 1, characterized in that The melt flow rate MFR2 (2.16 kg, 230° C., measured according to ISO 1133) is in the range of 0.3 to 1 g / 10 min, preferably 0.4 to 0.8 g / 10 min, more preferably 0.5 to 0.7 g / 10 min.

4. The polyolefin composition according to claim 1, characterized in that Impact strength (ISO179-1, Charpy 1eA+23°C) is at least 17 kJ / m 2 , more preferably at least 19 kJ / m 2 , still more preferably at least 20 kJ / m 2 , especially at 15 kJ / m 2 Up to 25kJ / m 2 in the range of 17 kJ / m 2 Up to 23kJ / m 2 in the range of 19 kJ / m 2 Up to 21 kJ / m 2 within the range.

5. The polyolefin composition according to any one of the preceding claims, characterized in that ΔK at 8E5 cycles I (derived from crack round bar test according to ISO 18489:2015) greater than 0.8 MPa*m 0.5 , preferably greater than 0.9MPa*m 0.5 , more preferably greater than 0.95 MPa*m 0.5 , even more preferably greater than 1.0 MPa*m 0.5 .

6. The polyolefin composition according to any one of the preceding claims, characterized in that The at least one heterophasic propylene copolymer (HECO) comprises as matrix a propylene-ethylene rubber as elastomeric propylene copolymer and a propylene homopolymer.

7. A polyolefin composition according to any one of the preceding claims, characterised in that The at least one heterophasic propylene copolymer (HECO) has a melt flow rate MFR2 (ISO 1133, 2.16 kg, 230 °C, measured according to ISO 1133) in the range of 0.1 g / 10 min to 0.9 g / 10 min, preferably 0.15 g / 10 min to 0.8 g / 10 min, more preferably 0.2 g / 10 min to 0.7 g / 10 min.

8. The polyolefin composition according to claim 1, characterized in that The at least one heterophasic propylene copolymer (HECO) has an impact strength (ISO 179-1, Charpy 1eA+23°C) of at least 17 kJ / m 2 , more preferably at least 19 kJ / m 2 , still more preferably at least 20 kJ / m 2 , especially at 15 kJ / m 2 Up to 40kJ / m 2 in the range of 17 kJ / m 2 Up to 38kJ / m 2 in the range of 19 kJ / m 2 Up to 36kJ / m 2 within the range.

9. The polyolefin composition according to claim 1, characterized in that The mixed plastic polypropylene blend of recycled material has an ethylene (C2) content determined according to CRYSTEX QC analysis in the range of 5 wt.-% to 20 wt.-%, more preferably 5 wt.-% to 10 wt.-%, and a C2 (CF) content of the crystalline fraction in the range of 1 wt.-% to 35 wt.-%, preferably 2 wt.-% to 20 wt.-%, more preferably 4 wt.-% to 10 wt.-%, in particular below 5 wt.-% (as determined according to CRYSTEX QC analysis).

10. The polyolefin composition according to claim 1, characterized in that The melt flow rate (ISO 1133, 2.16 kg; 230°C) of the mixed plastic polypropylene blend of recycled material is 5 g / 10 min to 30 g / 10 min, preferably 10 g / 10 min to 20 g / 10 min, more preferably 12 g / 10 min to 18 g / 10 min, and most preferably 13 g / 10 min to 16 g / 10 min.

11. The polyolefin composition according to claim 1, characterized in that The impact strength (ISO179-1, Charpy 1eA+23°C) of the mixed plastic polypropylene blend of the recycled material is at least 4 kJ / m 2 , more preferably at least 5 kJ / m 2 , still more preferably at least 6 kJ / m 2 , especially at 4 kJ / m 2 Up to 15kJ / m 2 in the range of 5 kJ / m 2 Up to 10kJ / m 2 in the range of 6 kJ / m 2 Up to 8kJ / m 2 within the range.

12. The polyolefin composition according to claim 1, characterized in that The mixed plastic polypropylene blend of recycled material comprises one or more of the following: polystyrene as determined by FTIR, polyamide-6 and / or limonene as determined by using solid phase microextraction (HS-SPME-GC-MS).

13. Use of a polyolefin composition according to any of the preceding claims for the manufacture of structural products, in particular for pipes.

14. A process for producing a polyolefin composition according to any one of the preceding claims, wherein the process comprises the following steps: - providing a mixture of 60 to 95 wt.-% (based on the total weight of the polyolefin composition) of at least one heterophasic propylene copolymer (HECO) having a total ethylene (C2) content (as determined according to CRYSTEX QC analysis) of 0.5 to 4.5 wt.-% and a xylene cold soluble fraction (determined according to ISO 16152 at 25 °C) in the range of 2 to 9 wt.-%, and a melt flow rate MFR2 (ISO 1133, 2.16 kg, 230 °C, measured according to ISO 1133) in the range of 0.1 to 1 g / 10 min, and 5 to 40 wt.-% (based on the total weight of the polyolefin composition) of a mixed plastic polypropylene blend of recycled material, and optionally further additives, - melting the mixture in an extruder, and - Optionally pelletizing the polyolefin composition obtained.

15. An article, in particular a pipe, comprising the polyolefin composition according to any one of the preceding claims 1 to 12.