Solvent-less cathode compositions and methods of making same
By using cathode active material particles and cathode electrolyte in the solvent-free mixture, combined with low-content adhesive particles, the adhesive microfibers are formed, which solves the solvent use and fiberization performance problems when manufacturing solid cathodes, and achieves high efficiency Cathode preparation.
Patent Information
- Application Number
- CN202380033471.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-21
- Filing Date
- 2023-04-21
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art is difficult to manufacture solid cathodes with good fibrosis properties without using a large amount of solvents, and there are challenges in the method of mixing active materials.
A solvent-free mixture containing cathode active material particles and cathode electrolyte, with a content of 1% w/w or less, and a binder microfiber is formed by rolling and twisting, and solid cathode sheet is deposited.
It is realized that the solid-state cathode with good fibrosis performance is manufactured without using a large amount of solvent, and the manufacturing efficiency and performance of the cathode is improved.
Smart Images

Figure CN119032432A_ABST
Abstract
Description
[0001] Cross-references
[0002] This application claims the benefit of and priority to U.S. Provisional Application No. 63 / 333,501, filed on April 21, 2022, the entire contents of which are incorporated by reference into this application for all purposes. Technical Field
[0003] The present application relates to rechargeable lithium batteries and electrodes (eg, cathodes) used in these batteries, as well as methods of making the batteries and electrodes. Background Art
[0004] Solid-state cathodes are advantageous for reasons of safety and energy density. However, solid-state cathodes are difficult to manufacture.
[0005] One process challenge is the amount of solvent used to make the cathode. Another difficulty is the method of mixing the active materials to provide the most desirable properties, such as the degree of fibrillation, in the cathode active mass.
[0006] What is needed is a process that can form cathodes with good fibrillation properties without using large amounts of solvents. This application describes a solution to this and other problems in the art to which this application relates. SUMMARY OF THE INVENTION
[0008] In one embodiment, the present application describes a method for manufacturing a solid-state cathode (SSC) sheet, comprising: providing or having provided a solvent-free mixture, the solvent-free mixture containing cathode active material particles, cathode electrolyte and binder particles; the binder particle content is 1% w / w or less; kneading the mixture into a mass to form binder fibrils; and depositing the mixture to make an SSC sheet.
[0009] In a second embodiment, the present application describes a method for making a solid cathode (SSC) sheet, comprising: providing or having provided a solvent-free mixture, the solvent-free mixture containing cathode active material particles, cathode electrolyte and binder particles; the binder particle content is 5% w / w or less; placing the mixture at a temperature of about -30°C to -5°C; kneading the mixture into a mass at a temperature of about 25°C to 200°C to form binder microfibers; depositing the mixture to form an SSC sheet; thereby providing an SSC sheet. In some embodiments, the method further comprises: mixing the cathode active material particles, cathode electrolyte and binder particles before placing the mixture. In some embodiments, the method comprises: mixing the mixture while placing the mixture at a temperature of about -30°C to -5°C.
[0010] In a third embodiment, the composition described in the present application includes: cathode active material particles; a binder content of 1% w / w or less; the binder is mixed with the cathode active material particles; the binder is in the form of microfibers; and there is no solvent in the mixture.
[0011] In a fourth embodiment, the present application relates to another composition, which is made by the following method: stabilizing the binder mixture and kneading the cathode active material into a mass under elevated temperature conditions. In some embodiments, the kneading is performed at a temperature of 35°C to 200°C. In some embodiments, the kneading is performed at a temperature of 35°C to 100°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 Shown is an example of a method of making a solid-state cathode.
[0013] Figure 2 Shown is an example of a method of making a solid-state cathode.
[0014] Figure 3 is a differential scanning calorimetry (DSC) graph of a solid-state cathode.
[0015] Figure 4 It is a graph showing the relationship between voltage (V) and cycle active mass-specific capacity (mAh / g).
[0016] Figure 5 It is a graph showing the relationship between area-specific resistance (ASR) and pulse index.
[0017] Figure 6 It is a graph of the relationship between tensile strength (stress in kPA) and strain.
[0018] Figure 7 It is a graph of sheet Young's modulus (sheet Youn's modulus / GPa) versus sheet tensile strength (sheet tensile strength / MPa) in some comparative examples.
[0019] Figure 8 It is a graph of sheet plastic elongation (sheet plastic elongation / %) versus sheet tensile strength (sheet tensile strength / MPa) in some comparative examples. DETAILED DESCRIPTION OF THE INVENTION
[0021] definition
[0022] In the present application, when a number is limited, such as about 15% weight % (w / w%), the term "about" refers to the limited value, and may also include values within the range of ±10% of the value. For example, about 15% w / w includes 15% w / w and 13.5% w / w, 14% w / w, 14.5% w / w, 15.5% w / w, 16% w / w or 16.5% w / w. For example, "about 75°C" includes 75°C and 67°C, 68°C, 69°C, 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C or 83°C.
[0023] In the present application, "selected from the group consisting of..." refers to a single member from the group, a plurality of members from the group, or a combination of members from the group. For example, the members selected from the group consisting of A, B, and C may include only A, only B, or only C, or may include A and B, A and C, B and C, and A, B, and C.
[0024] The term "cathode active material" in this application refers to a material that can intercalate lithium ions or react with lithium ions in a reversible manner. For example, LiMPO 4 (M=Fe, Ni, Co, Mn); Li x Ti y O z , where x is 0 to 8, y is 1 to 12, and z is 1 to 24; LiMn 2a Ni a O 4 , where a is 0 to 2; nickel cobalt aluminum oxide; LiNi x Mn y Co z O 2 , x+y+z=1, 0≤x≤1, 0≤y≤1, 0≤z≤1; LiNi x Co y Al z O 2 , where x+y+z=1, 0≤x≤1, 0≤y≤1, 0≤z≤1. In these chemical formulas, x, y, and z are selected so that the chemical formula is charge neutral.
[0025] The term "solid cathode" in this application refers to a cathode that does not contain a liquid electrolyte. The terms "cathode" and "anode" in this application refer to the electrodes of a battery. The cathode and anode are generally referred to as the positive electrode and the negative electrode, respectively, in the relevant field. During the charging cycle of a lithium secondary battery, lithium ions leave the cathode and reach the anode through the electrolyte; during the charging cycle, electrons leave the cathode and move to the anode through an external circuit. In the discharge cycle of a lithium secondary battery, lithium ions migrate from the anode to the cathode through the electrolyte. In the discharge cycle, electrons leave the anode and move to the cathode through an external circuit. The term "positive electrode" in this application refers to the electrode in a secondary battery where positive ions, such as Li, migrate during battery discharge. + Conduct, flow or move toward the electrode. The term "negative electrode" in this application refers to the electrode in a secondary battery that conducts, flows or moves positive ions such as Li during battery discharge. + In a system consisting of a lithium metal electrode and a conversion chemistry, an intercalation chemistry, or a combination of conversion / intercalation chemistry - including an electrode (i.e., a cathode active material such as NiF x 、LiNi x Mn y Co z O 2 [NMC] or LiNi x Al y Co z O 2 [NCA], where x+y+z=1), the electrode with conversion chemistry, embedding chemistry, or a combination of conversion / embedding chemistry is called the positive electrode. In some usages, the cathode is used instead of the positive electrode, and the anode is used instead of the negative electrode. When a lithium secondary battery is charged, lithium ions are transferred from the positive electrode (such as NiF x , NMC, NCA) to the negative electrode (such as Li-metal). When the lithium secondary battery is discharged, the lithium ions move from the negative electrode to the positive electrode.
[0026] In this application, the term "solid separator" refers to a solid separator that can conduct Li + A material that is substantially insulating to ions but electronically, for example, one whose lithium ion conductivity is at least 10 times its electronic conductivity 3 times, usually 10 6 times, and acts as a physical barrier or spacer between the positive and negative electrodes in an electrochemical cell.
[0027] In this application, "LSTPS" refers to a polysaccharide having the formula Li a MP b S c LSPS refers to a material characterized by the formula L a SiP b Sc An electrolyte material characterized by 2≤a≤8, 0.5≤b≤2.5, 4≤c≤12. LSPS refers to an electrolyte material characterized by the formula L a SiP b S c Electrolyte materials, wherein 2≤a≤8, 0.5≤b≤2.5, 4≤c≤12, d<3. Exemplary LSTPS materials are disclosed in International Patent Application PCT / US14 / 38283, entitled "Solid State Catholyte or Electrolyte for Battery Using Li A MP B S C (M=SI, GE, AND / OR SN)”, filed on May 15, 2014, and published on November 20, 2014 as WO2014 / 186634, the entirety of which is incorporated herein by reference. Exemplary LSTPS materials can be found, for example, in U.S. patent application Ser. No. 14 / 618,979 filed on February 10, 2015 (Publication No. 2015 / 0171465, June 18, 2015), the entirety of which is incorporated herein by reference. When M is Sn and Si, both are present. In this application, “LSTPSO” refers to LSTPS doped with or containing O. In one embodiment, “LSTPSO” is LSTPS with an oxygen content between 0.01% and 10% atomic. PS material. "LSPS" refers to an electrolyte material containing chemical components such as Li, Si, P, S, etc. In this application, "LSTPS" refers to an electrolyte material having the chemical components of Li, Si, P, Sn and S. In this application, "LSPSO" refers to an LSPS doped with or containing O. In one embodiment, "LSPSO" is an LSPS material with an oxygen content between 0.01% and 10% atoms. In this application, "LATP" refers to an electrolyte material having the chemical components of Li, As, Sn and P. In this application, "LAGP" refers to an electrolyte material having the chemical components of Li, As, Ge and P. The so-called "LSTPSO" in this application refers to an electrolyte having the formula Li a MP b S c O d A cathode material wherein M is Si, Ge, Sn and / or Al, and 2≤a≤8, 0.5≤b≤2.5, 4≤c≤12, d<3. LSTPSO refers to LSTPS as defined above, and oxygen doping is between 0.1% and about 10% atomic. LPSO refers to LPS as defined above, and is doped with 0.1% to about 10% atomic oxygen.
[0028] In this application, area specific resistance (ASR) is measured by electrochemical cycling using an Arbin or Biologic instrument, unless otherwise specified to the contrary.
[0029] In the present application, the ionic conductivity is measured by electrical impedance spectroscopy method known in the art.
[0030] In this application, the term "electrolyte" refers to a material that conducts ions but insulates electrons. Electrolytes can be used to electrically insulate the positive and negative electrodes of a rechargeable battery while allowing ions (such as Li + ) is conducted through the electrolyte.
[0031] In this application, the phrase "film" or "thin film" refers to a thin film having a thickness less than 1.0 mm and greater than 100 nm. The lateral dimension of the film is greater than 5 mm. The "film" or "thin film" can be produced by a continuous process, such as casting, slip casting or screen printing.
[0032] In this application, the phrase "thickness of a film" refers to the distance between the top and bottom surfaces of a film or the median of the measured distance. In this application, top and bottom refer to the sides of the film with the largest surface area. Thickness in this application is measured by cross-sectional scanning electron microscopy.
[0033] In the present application, when describing a solid cathode (SSC) sheet, "thin" means that the average cross-sectional thickness of the sheet or film is less than 1.0 mm and greater than 20 μm. In some embodiments, the thickness of the SSC sheet is 50 μm to 500 μm. In some embodiments, the thickness of the SSC sheet is 10 μm to 300 μm. In some embodiments, the thickness of the SSC sheet is 100 μm to 150 μm. In some embodiments, the thickness of the SSC sheet is 100 μm to 120 μm. In some embodiments, the thickness of the SSC sheet is 80 μm to 100 μm.
[0034] "Binder" in this application refers to a polymer having the ability to increase the adhesion and / or cohesion of a material, such as a solid in a raw tape. Suitable binders include, but are not limited to, PVDF, PVDF-HFP, SBR, and ethylene-alpha olefin copolymers. "Binder" refers to a material that can help bond another material. For example, polyvinyl butyral in this application is a binder because it can be used to bond garnet materials. Other binders include polycarbonates. Other binders include polyacrylates and polymethacrylates. These binders are merely examples and are not the full range of binders considered herein. Useful adhesives in the present application include, but are not limited to, polypropylene (PP), polyethylene, atactic polypropylene (aPP), isotactic polypropylene (iPP), ethylene-propylene rubber (EPR), ethylene-pentene copolymer (EPC), polyisobutylene (PIB), butadiene rubber (SBR), polyolefins, polyethylene-co-octene (PE-co-PO), polyethylene-co-methylene cyclopentane (PE-co-PMCP), polymethyl methacrylate (and other acrylic acids), acrylic acid, polyethylene-acetal resin, polyvinyl butyral resin, PVB, polyvinyl acetal resin, stereo block polypropylene, polypropylene polymethylpentene copolymer, polyethylene oxide (PEO), PEO block copolymer, silicone, etc. In some examples, including any of the above, the binder is a polymer selected from polyacrylonitrile (PAN), polypropylene, polyethylene, polyoxide (PEO), polymethyl methacrylate (PMMA), polyvinyl chloride (PVC), polyvinyl pyrrolidone (PVP), polyoxide poly(allyl glycidyl ester) PEO-AGE, polyoxide 2-methoxyethoxyethyl glycidyl ester (PEO-MEEGE), polyoxyethylene 2-methoxyethoxyethyl glycidyl ester poly(allyl glycidyl ether) (PEO-MEEGE-AGE), polysiloxane, polyvinylidene fluoride (PVDF), polyvinylidene fluoride hexafluoropropylene (PVDF-HFP), ethylene propylene (EPR), nitrile rubber (NPR), styrene butadiene rubber (SBR), polybutadiene polymer, polybutadiene rubber (PB), polyisobutadiene rubber (PIB), polyolefin, α-polyolefin, ethylene α-polyolefin, polyisobutadiene rubber (PI), polychloroprene rubber (CR), acrylonitrile butadiene rubber (NBR) and polyacrylate (PEA).
[0035] The term "electrolyte" in this application refers to a material that can conduct ions but insulate electrons. Electrolytes can be used to electrically insulate the positive and negative electrodes of a rechargeable battery while allowing ions (such as Li + ) is conducted through the electrolyte. In some electrochemical devices described in the present application, the electrolyte includes a solid film, particle or monomer capable of conducting Li +oxides, such as lithium - filled garnets. In some examples, the electrolyte further includes a gel electrolyte that is laminated to or in direct contact with a solid film, particles, or monomers.
[0036] In this application, the "solid - state thin - film or particulate separator" refers to a solid - state electrolyte in the form of a thin film or a pelletized powder. The thin film or particles may comprise sintered or unsintered Li - conducting + oxides, such as lithium - filled garnets.
[0037] In this application, the term "solid - state electrolyte" refers to an electrolyte as defined in this application, where the electrolyte is in solid form.
[0038] In this application, the terms "separator" and "Li - conducting + separator" are used interchangeably unless otherwise clearly stated; a separator is a short form of a Li - conducting + separator. A separator refers to a solid - state electrolyte that can conduct Li + ions and is substantially electron - insulating, suitable for use as a physical barrier or spacer between the positive and negative electrodes in an electrochemical cell or a rechargeable battery. The separator mentioned here is substantially electron - insulating. The lithium - ion conductivity of the separator is at least 10 3 times that of the electron conductivity of the separator, typically 10 6 times.
[0039] The term "lithium - filled garnet" in this application refers to an oxide having crystal - structure characteristics related to the garnet crystal structure. Lithium - filled garnets include compounds having the formula Li A La B Zr C O F 、Li A La B M′ CM ″ D Ta E O F or Li A La B M′ CM ″ D Nb E O F where 4 < A < 8.5, 1.5 < B < 4, 0 < C ≦ 2, 0 < D < 2, 0 < E < 2.5, 10 < F < 13, and in each instance M′ and M″ are selected from Al, Mo, W, Nb, Ga, Sb, Ca, Ba, Sr, Ce, Hf, Rb, Ta respectively; or the formula Li a La b Zr c Al d Me″ e O f, where 5 < a < 7.7, 2 < b < 4, 0 ≤ c ≤ 2.5, 0 < d < 2, 0 < e < 2, 10 < f < 13, and Me″ is a metal selected from Nb, V, W, Mo, Ta, Ga, or Sb. The garnets used in this application also include those doped with Al or Al 2 O 3 of the above garnets. In addition, the garnets used in this application include, but are not limited to, Li A La B Zr C O F +yAl 2 O 3 , where x ranges from 5.8 to 7.0 and y is 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, and 1.0; 4 < A < 8.5, 1.5 < B < 4, 0 < C ≤ 2, 0 < D < 2, 10 < F < 13. In addition, the garnets used in this application include, but are not limited to, Li x La 3 Zr 2 O 12 +yAl 2 O 3 , where x ranges from 5.8 to 7.0 and y is 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, and 1.0. The garnets in this application do not include YAG garnets (i.e., yttrium aluminum garnets or, for example, Y 3 Al 5 O 12 ). The garnets in this application do not include silicate-based garnets such as grossular, almandine, pyrope, hydrogrossular, or cinnamon stone, sandfeldspar, uvarovite, and anorthite, as well as solid solution - almandine - pyrope and uvarovite - pyrope - anorthite. The garnets in this application do not include non - silicates with the general formula X 3 Y 2 (SiO 4 ) 3 , where X is Ca, Mg, Fe, and / or Mn; Y is Al, Fe, and / or Cr.
[0040] The terms "garnet precursor chemicals" and "chemical precursors of garnet - type electrolytes" in this application refer to chemicals that can form the lithium - filled garnet materials through reaction. These chemical precursors include, but are not limited to, lithium hydroxide (e.g., LiOH), lithium oxide (e.g., Li 2 O), lithium carbonate (e.g., LiCO 3 ), zirconium oxide (e.g., ZrO 2 ), lanthanum oxide (e.g., La 2 O 3 ), aluminum oxide (e.g., Al 2 O3 ), aluminum (such as Al), aluminum nitrate (such as Al(NO 3 ) 3 ), non-hydrated aluminum nitrate, niobium oxide (such as Nb 2 O 5 ), and tantalum oxide (e.g. Ta 2 O 5 ).
[0041] In this application, the phrase " 50 "Diameter" refers to the median size in a size distribution as measured by microscopy or other particle size analysis techniques such as, but not limited to, scanning electron microscopy or dynamic light scattering. 50 A characteristic dimension comprising 50% of the particles being smaller than said dimension.
[0042] In this application, the phrase " 90 "Diameter" refers to a size within a size distribution as measured by microscopy or other particle size analysis techniques, such as, but not limited to, scanning electron microscopy or dynamic light scattering. 90 A characteristic size comprising 90% of the particles being smaller than said size.
[0043] In this application, the term "cathode electrolyte" refers to a liquid or gel electrolyte confined within the positive electrode space of an electrochemical cell. Cathodic electrolyte also refers to an electrolyte that is intimately mixed with or surrounded by the positive electrode active material, or that is in contact with the positive electrode active material and is Li + The cathode electrolyte may also be a liquid, gel, semi-liquid, semi-solid, polymer and / or solid polymer ion conductor. In some examples, the cathode electrolyte comprises a gel as described herein. In some embodiments, the gel electrolyte comprises any electrolyte as described herein, including nitrile, dinitrile, organic sulfur-containing solvent or a combination thereof as described herein.
[0044] Composition
[0045] The composition described in the present application includes: cathode active material particles; 1 w / w% or less (for example, 1, 0.95, 0.9, 0.85, 0.8, 0.75, 0.7, 0.65, 0.6, 0.55, 0.5, 0.45, 0.4, 0.35, 0.3, 0.25, 0.2, 0.15, 0.1%) of a binder; wherein the binder is mixed with the cathode active material particles; the binder is in the form of microfibers; and there is no solvent in the mixture.
[0046] In some embodiments, including any of the above, the binder content is 0.3 w / w % or less (eg, 0.25, 0.20, 0.15, 0.10, 0.075, or 0.05%).
[0047] In some embodiments, including any of the above, the binder is polytetrafluoroethylene (PTFE).
[0048] In some embodiments, including any of the above, the binder is PTFE or polyvinylpyrrolidone (PVP).
[0049] In some embodiments, including any of the above, the PTFE adhesive particle size is less than 2 mm. In some embodiments, including any of the above, the PTFE adhesive particle size is less than 1.5 mm. In some embodiments, including any of the above, the PTFE adhesive particle size is less than 1 mm. In some embodiments, including any of the above, the PTFE adhesive particle size is less than 0.75 mm. In some embodiments, including any of the above, the PTFE adhesive particle size is less than 0.5 mm.
[0050] In some embodiments, including any of the above, the binder is PTFE and at least one additional binder.
[0051] In some embodiments, including any of the above, the binder is polytetrafluoroethylene and at least one additional binder selected from the group consisting of polyvinylidene fluoride (PVDF), polyvinylidene fluoride hexafluoropropylene (PVDF-HFP), ethylene propylene (EPR), nitrile rubber (NPR), styrene-butadiene rubber (SBR), polypropylene (PP), polyethylene, atactic polypropylene (aPP), isotactic polypropylene (iPP), ethylene propylene rubber (EPR), ethylene pentene copolymer (EPC), polyisobutylene (PIB), butadiene rubber (SBR), polyolefins, polyethylene-co-l-octene (PE-co-PO), polyethylene-co-methylene cyclopentane (PE-co-PMCP), polymethyl methacrylate (PMMA), polyvinyl butyral (PVB), polyethylene-co-acetal resin, polyvinyl alcohol butyral resin, polyvinyl alcohol butyral resin, and acrylic acid. Acetal resin, stereo block polypropylene, polypropylene polymethylpentene copolymer, polyethylene oxide (PEO), PEO block copolymer, silica gel, polyacrylonitrile (PAN), polyvinyl chloride (PVC), polyvinyl pyrrolidone (PVP), polyoxide poly (allyl glycidyl ester) PEO-AGE, polyoxide 2-methoxyethoxyethyl glycidyl ester (PEO-MEEGE), polyoxyethylene 2-methoxyethoxyethyl glycidyl ester poly (allyl glycidyl ether) (PEO-MEEGE-AGE), polysiloxane, polybutadiene polymer, polybutadiene rubber (PB), polyisobutadiene rubber (PIB), polyolefin, α-polyolefin, ethylene α-polyolefin, polyisobutadiene rubber (PI), polychloroprene rubber (CR), acrylonitrile butadiene rubber (NBR) and polyacrylate (PEA) and combinations thereof.
[0052] In some embodiments, including any of the above, the cathode active material is a material described in the International Patent Application Publication No. PCT / US2021 / 049528 (filed on September 8, 2021, entitled “CATHODE COATING”, the entire contents of which are hereby incorporated by reference into this application for all purposes.
[0053] In some embodiments, including any of the above embodiments, the cathode active material is selected from: LiMPO 4 (M=Fe, Ni, Co, Mn); Li x Ti y O z , where x is 0 to 8, y is 1 to 12, and z is 1 to 24; LiMn 2a Ni a O 4 , where a is 0 to 2; nickel cobalt aluminum oxide; LiNi x Mn y Co z O 2 , where x+y+z=1, 0≤x≤1, 0≤y≤1, 0≤z≤1; and LiNi x Co y Al z O 2 , where x+y+z=1, 0≤x≤1, 0≤y≤1, 0≤z≤1.
[0054] In some embodiments, including any of the above embodiments, the cathode active material is LiNi x Mn y Co z O 2 , where x+y+z=1, 0≤x≤1, 0≤y≤1, and 0≤z≤1.
[0055] In some embodiments, including any of the above embodiments, the cathode active material is LiNi x Mn y Co z O 2 , where x is 0.8, y is 0.1, and z is 0.1.
[0056] In some embodiments, including any of the above embodiments, the cathode active material is LiNi x Mn y Co z O 2 , where x is 0.6, y is 0.2, and z is 0.2.
[0057] In some embodiments, including any of the above embodiments, the cathode active material is LiNix Mn y Co z O 2 , where x is 0.5, y is 0.3, and z is 0.2.
[0058] In some embodiments, including any of the above embodiments, the cathode active material is LiNi x Mn y Co z O 2 , where x is 1 / 3, y is 1 / 3, and z is 1 / 3.
[0059] In some embodiments, including any of the above embodiments, the cathode active material is Li(NiCoMn)O 2 .
[0060] In some embodiments, including any of the above embodiments, the cathode active material is LiFePO 4 .
[0061] In some embodiments, including any of the above embodiments, NMC has a d 50 particle size S of 0.1 μm < S < 50 μm.
[0062] In some embodiments, including any of the above embodiments, NMC has a d 50 particle size S of 0.5 μm < S < 30 μm.
[0063] In some embodiments, including any of the above embodiments, NMC has a d 50 particle size S of 1 μm < S < 20 μm.
[0064] In some embodiments, including any of the above embodiments, NMC has a d 50 particle size S of 2 μm < S < 15 μm.
[0065] In some embodiments, including any of the above embodiments, NMC has a d 50 particle size S of 3 μm < S < 12 μm.
[0066] In some embodiments, including any of the above embodiments, NMC has a d 50 particle size S of 4 μm < S < 10 μm.
[0067] In some embodiments, including any of the above embodiments, the d 50 particle size T of the cathode electrolyte is 0.005 μm < T < 20 μm.
[0068] In some embodiments, including any of the above embodiments, the d 50 particle size T of the cathode electrolyte is 0.01 μm < T < 10 μm.
[0069] In some embodiments, including any of the above embodiments, the cathode electrolyte has a 50 Particle size T is 0.02 μm <T<10μm。
[0070] In some embodiments, including any of the above embodiments, the cathode electrolyte has a 50 Particle size T is 0.05 μm <T<8μm。
[0071] In some embodiments, including any of the above embodiments, the cathode electrolyte has a 50 Particle size T is 0.02 μm <T<5μm。
[0072] In some embodiments, including any of the above embodiments, the cathode electrolyte has a 50 Particle size T is 0.05 μm <T<3μm。
[0073] In some embodiments, including any of the above embodiments, the cathode electrolyte has a 50 Particle size T is 0.1 μm <T<1.5μm。
[0074] In some embodiments, including any of the above, the density of the composition is 2-2.5 g / cm 3 , for example, about 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5 or 2.6.
[0075] In some embodiments, including any of the above embodiments, described herein are sheets comprising the compositions described herein.
[0076] In some embodiments, including any of the above embodiments, the cathode electrolyte is LSTPS.
[0077] In some embodiments, including any of the above embodiments, the cathode electrolyte is argyrodite.
[0078] In some embodiments, including any of the above embodiments, the cathode electrolyte is a sulfide that conducts lithium ions, such as Li 2 S-SiS 2 .
[0079] In some embodiments, including any of the above embodiments, the cathode electrolyte is an oxide that conducts lithium ions, such as a lithium-filled garnet.
[0080] In some embodiments, including any of the above embodiments, the cathode electrolyte is a lithium ion conducting halide, such as a perovskite.
[0081] In some embodiments, including any of the above embodiments, the cathode electrolyte is an organic polymer that conducts lithium ions, for example, LiPF in PEO. 6 .
[0082] In some embodiments, including any of the above embodiments, the cathode active loading in the cathode is between 1 and 15 mAh / cm 2 between.
[0083] In some embodiments, including any of the above embodiments, the cathode active load is at least 5 mAh / cm 2 .
[0084] In some embodiments, including any of the above embodiments, the sheet has a thickness of 120 μm.
[0085] In some embodiments, including any of the above embodiments, the sheet has a thickness of 150 μm.
[0086] In some embodiments, including any of the above embodiments, the width of the sheet is at least 5 centimeters (cm).
[0087] In some embodiments, including any of the above embodiments, the width of the sheet is at least 1 meter (m).
[0088] In some embodiments, including any of the above embodiments, the length of the sheet is at least 10 cm.
[0089] In some embodiments, including any of the above embodiments, the length of the sheet is at least 70 cm.
[0090] In some embodiments, including any of the above embodiments, the sheet is 100 mm x 2000 mm.
[0091] In some embodiments, including any of the above embodiments, the sheet is at least 150 mm x 100 m.
[0092] In some embodiments, including any of the above embodiments, the sheet is 300 mm x continuous roll.
[0093] In some embodiments, including any of the above embodiments, the length of the sheet is at least 1 meter.
[0094] In some embodiments, including any of the above embodiments, described herein is a double layer comprising a metal layer in contact with the two sheets described herein.
[0095] In some embodiments, including any of the above embodiments, described herein is a three-layer including a metal layer, wherein the metal layer is located between and in contact with the two sheets described herein.
[0096] In some embodiments, including any of the above embodiments, the metal layer is an aluminum layer.
[0097] In some embodiments, including any of the above embodiments, the metal layer is a Ni layer.
[0098] In some embodiments, including any of the above, the electrode has a porosity range of 40% to 50% prior to des, such as about 35%, 40%, 45%, 50% or 55%.
[0099] In some embodiments, including any of the above, the electrode product has a tensile strength of about 0.3 to 0.5 MPa, such as 0.28, 0.3, 0.33, 0.35, 0.38, 0.4, 0.43, 0.45, 0.48, 0.5, 0.53 or 0.55 MPa.
[0100] In some embodiments, including any of the above, the electrode product has a Young's modulus of about 0.5 to 0.8 MPa, for example, 0.48, 0.5, 0.53, 0.55, 0.58, 0.6, 0.63, 0.65, 0.68, 0.7, 0.73, 0.75, 0.78, 0.8, 0.83 or 0.85 MPa.
[0101] In some embodiments, including any of the above, the electrode product has a plastic elongation of about 5% to 15%, such as about 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15%.
[0102] In some embodiments, including any of the above embodiments, the electrode product has an elasticity of about 0.01 to 0.15 GPa, such as about 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14 or 0.15%.
[0103] In some embodiments, the compositions otherwise listed herein are prepared by a process of kneading the cathode active material at low temperature (ie, "cold kneading").
[0104] In some embodiments, the compositions listed herein are prepared by a method comprising stabilizing the binder at low temperature and kneading the cathode active material at a higher temperature. In some embodiments, kneading is performed at a temperature of 25°C to 200°C (eg, 45°C).
[0105] method
[0106] The present application discloses a method for manufacturing a solid-state cathode (SSC) sheet, which comprises: providing or having provided a solvent-free mixture, wherein the solvent-free mixture contains cathode active material particles, cathode electrolyte and binder particles; the binder particle content is 1% w / w or less, for example, 1, 0.95, 0.9, 0.85, 0.8, 0.75, 0.7, 0.65, 0.6, 0.55, 0.5, 0.45, 0.4, 0.35, 0.3, 0.25, 0.2, 0.15, 0.1%; kneading the mixture into a mass to form binder fibrils; and depositing the mixture to make an SSC sheet.
[0107] In some embodiments, including any of the above embodiments, the present application discloses a method for manufacturing a solid-state cathode (SSC) sheet, which includes: providing or having provided a solvent-free mixture, the solvent-free mixture containing cathode active material particles, cathode electrolyte and binder particles; the binder particle content is 5% w / w or less; placing the mixture at a temperature of about -30°C to -5°C; kneading the mixture into a mass at a temperature of about 25°C to 200°C to form binder microfibers; and depositing the mixture to make an SSC sheet.
[0108] In some embodiments, including any of the above, the step of kneading the mixture into a mass to form binder microfibers includes shearing the cathode active material particles and the binder particles to form binder microfibers.
[0109] In some embodiments, including any one of the above, the step of kneading the mixture into a mass to form binder microfibers further comprises: compressing the cathode active material particles and the binder particles to form a binder microfiber network in the cathode active material particles.
[0110] In some embodiments, including any of the above, the process includes rolling the cathode to form and network PTFE microfibers in the cathode. In some embodiments, the process includes using a calendar to densify the cathode at the final stage of the process.
[0111] In some embodiments, including any of the above, the mixture is kneaded using a mortar.
[0112] In some embodiments, including any of the above, the mixture is kneaded using a twin-screw co-rotating extruder. Commercial examples of such extruders include, but are not limited to, ThemoFisher's Process 11; or Buhler's 20MM twin-screw mixing line. Other manufacturers include Coperion.
[0113] In some embodiments, including any of the above, the method further comprises pretreating the adhesive. For example, pretreatment may include, but is not limited to, atomizing polytetrafluoroethylene powder. One method of atomizing polytetrafluoroethylene powder is to perform blade mixing at a cold temperature. In some embodiments, the cold temperature is below the phase transition temperature. In some embodiments, the cold temperature is 10°C. In some embodiments, the cold temperature is below the phase transition temperature. In some embodiments, the cold temperature is at the phase transition temperature. In some embodiments, the cold temperature is 11°C. In some embodiments, the cold temperature is below the phase transition temperature. In some embodiments, the cold temperature is 12°C. In some embodiments, the cold temperature is below the phase transition temperature. In some embodiments, the cold temperature is 13°C. In some embodiments, the cold temperature is below the phase transition temperature. In some embodiments, the cold temperature is 14°C. In some embodiments, the cold temperature is below the phase transition temperature. In some embodiments, the cold temperature is 15°C. In some embodiments, the cold temperature is below the phase transition temperature. In some embodiments, the cold temperature is 16°C. In some embodiments, the cold temperature is below the phase transition temperature. In some embodiments, the cold temperature is 17°C. In some embodiments, the cold temperature is below the phase transition temperature. In some embodiments, the cold temperature is 18°C. In some embodiments, the cold temperature is 19°C. In some embodiments, the cold temperature is below the phase transition temperature. In some embodiments, the cold temperature is 20°C.
[0114] In some embodiments, including any of the above, the method further comprises stabilizing the adhesive. For example, the stabilization step includes, but is not limited to, for example, placing the mixture at a low temperature; and further mixing the adhesive (e.g., polytetrafluoroethylene) powder at a cold temperature, for example, by blade mixing. In some embodiments, the cold temperature is below the phase transition temperature. In some embodiments, the cold temperature is below the phase transition temperature. In some embodiments, the cold temperature is about -40°C to 0°C. In some embodiments, the cold temperature is about -30°C to -5°C. In some embodiments, the cold temperature is -30°C. In some embodiments, the cold temperature is -29°C. In some embodiments, the cold temperature is -28°C. In some embodiments, the cold temperature is -27°C. In some embodiments, the cold temperature is -26°C. In some embodiments, the cold temperature is -25°C. In some embodiments, the cold temperature is -24°C. In some embodiments, the cold temperature is -23°C. In some embodiments, the cold temperature is -22°C. In some embodiments, the cold temperature is -21°C. In some embodiments, the cold temperature is -20°C. In some embodiments, the cold temperature is -19°C. In some embodiments, the cold temperature is -18°C. In some embodiments, the cold temperature is -17°C. In some embodiments, the cold temperature is -16°C. In some embodiments, the cold temperature is -15°C. In some embodiments, the cold temperature is -14°C. In some embodiments, the cold temperature is -13°C. In some embodiments, the cold temperature is -12°C. In some embodiments, the cold temperature is -11°C. In some embodiments, the cold temperature is -10°C. In some embodiments, the cold temperature is -9°C. In some embodiments, the cold temperature is -8°C. In some embodiments, the cold temperature is -7°C. In some embodiments, the cold temperature is -6°C. In some embodiments, the cold temperature is -5°C. In some embodiments, the cold temperature is -4°C. In some embodiments, the cold temperature is -3°C. In some embodiments, the cold temperature is -2°C. In some embodiments, the cold temperature is -1°C. In some embodiments, the cold temperature is 0°C.
[0115] In some embodiments, the stabilizing adhesive step includes leaving the mixture at low temperature for at least 1 hour. In some embodiments, stabilizing the adhesive includes leaving it this way for at least 1.5 hours. In some embodiments, stabilizing the adhesive includes leaving it this way for at least 2 hours. In some embodiments, stabilizing the adhesive includes leaving it this way for at least 2.5 hours. In some embodiments, stabilizing the adhesive includes leaving it this way for at least 3 hours. In some embodiments, stabilizing the adhesive includes leaving it this way for at least 3.5 hours. In some embodiments, stabilizing the adhesive includes leaving it this way for at least 4 hours. In some embodiments, stabilizing the adhesive includes leaving it this way for at least 5 hours. In some embodiments, stabilizing the adhesive includes leaving it this way for at least 6 hours.
[0116] In some embodiments, stabilizing the binder comprises further mixing (e.g., by a blade mixer). In some embodiments, mixing is performed at least 10 times (e.g., 20,000 rpm 10 x 2 sec) for at least one hour. In some embodiments, cooling is performed during mixing of the composition (e.g., in a cryogenic environment). In some embodiments, cooling is performed during the intervals between mixing of the composition (e.g., in a cryogenic environment).
[0117] In some embodiments, including any of the above embodiments, kneading is performed at a temperature of about 18°C to about 180°C. In some embodiments, kneading is performed at a temperature of about 50°C to about 80°C. In some embodiments, kneading is performed at a temperature of about 60°C to about 80°C. In some embodiments, kneading is performed at a temperature of about 70°C to about 80°C. In some embodiments, kneading is performed at a temperature of about 80°C to about 100°C. In some embodiments, kneading is performed at a temperature of about 90°C to about 100°C. In some embodiments, kneading is performed at a temperature of about 18°C. In some embodiments, kneading is performed at a temperature of about 19°C. In some embodiments, kneading is performed at a temperature of about 20°C. In some embodiments, kneading is performed at a temperature of about 21°C. In some embodiments, kneading is performed at a temperature of about 22°C. In some embodiments, kneading is performed at a temperature of about 23°C. In some embodiments, kneading is performed at a temperature of about 24°C. In some embodiments, kneading is performed at a temperature of about 25°C. In some embodiments, kneading is performed at a temperature of about 26°C. In some embodiments, kneading is performed at a temperature of about 27°C. In some embodiments, kneading is performed at a temperature of about 28°C. In some embodiments, kneading is performed at a temperature of about 29°C. In some embodiments, kneading is performed at a temperature of about 30°C. In some embodiments, kneading is performed at a temperature of about 31°C. In some embodiments, kneading is performed at a temperature of about 32°C. In some embodiments, kneading is performed at a temperature of about 33°C. In some embodiments, kneading is performed at a temperature of about 34°C. In some embodiments, kneading is performed at a temperature of about 35°C. In some embodiments, kneading is performed at a temperature of about 36°C. In some embodiments, kneading is performed at a temperature of about 37°C. In some embodiments, kneading is performed at a temperature of about 38°C. In some embodiments, kneading is performed at a temperature of about 39°C. In some embodiments, kneading is performed at a temperature of about 40°C. In some embodiments, kneading is performed at a temperature of about 41°C. In some embodiments, kneading is performed at a temperature of about 42°C. In some embodiments, kneading is performed at a temperature of about 43°C. In some embodiments, kneading is performed at a temperature of about 44°C. In some embodiments, kneading is performed at a temperature of about 45°C. In some embodiments, kneading is performed at a temperature of about 46°C. In some embodiments, kneading is performed at a temperature of about 47°C. In some embodiments, kneading is performed at a temperature of about 48°C. In some embodiments, kneading is performed at a temperature of about 49°C. In some embodiments, kneading is performed at a temperature of about 50°C. In some embodiments, kneading is performed at a temperature of about 51°C. In some embodiments, kneading is performed at a temperature of about 52°C. In some embodiments, kneading is performed at a temperature of about 53°C. In some embodiments, kneading is performed at a temperature of about 54°C.In some embodiments, kneading is performed at a temperature of about 55°C. In some embodiments, kneading is performed at a temperature of about 56°C. In some embodiments, kneading is performed at a temperature of about 57°C. In some embodiments, kneading is performed at a temperature of about 58°C. In some embodiments, kneading is performed at a temperature of about 59°C. In some embodiments, kneading is performed at a temperature of about 60°C. In some embodiments, kneading is performed at a temperature of about 61°C. In some embodiments, kneading is performed at a temperature of about 62°C. In some embodiments, kneading is performed at a temperature of about 63°C. In some embodiments, kneading is performed at a temperature of about 64°C. In some embodiments, kneading is performed at a temperature of about 65°C. In some embodiments, kneading is performed at a temperature of about 66°C. In some embodiments, kneading is performed at a temperature of about 67°C. In some embodiments, kneading is performed at a temperature of about 68°C. In some embodiments, kneading is performed at a temperature of about 69°C. In some embodiments, kneading is performed at a temperature of about 70°C. In some embodiments, kneading is performed at a temperature of about 71°C. In some embodiments, kneading is performed at a temperature of about 72°C. In some embodiments, kneading is performed at a temperature of about 73°C. In some embodiments, kneading is performed at a temperature of about 74°C. In some embodiments, kneading is performed at a temperature of about 75°C. In some embodiments, kneading is performed at a temperature of about 76°C. In some embodiments, kneading is performed at a temperature of about 77°C. In some embodiments, kneading is performed at a temperature of about 78°C. In some embodiments, kneading is performed at a temperature of about 79°C. In some embodiments, kneading is performed at a temperature of about 80°C. In some embodiments, kneading is performed at a temperature of about 81°C. In some embodiments, kneading is performed at a temperature of about 82°C. In some embodiments, kneading is performed at a temperature of about 83°C. In some embodiments, kneading is performed at a temperature of about 84°C. In some embodiments, kneading is performed at a temperature of about 85°C. In some embodiments, kneading is performed at a temperature of about 86°C. In some embodiments, kneading is performed at a temperature of about 87°C. In some embodiments, kneading is performed at a temperature of about 88°C. In some embodiments, kneading is performed at a temperature of about 89°C. In some embodiments, kneading is performed at a temperature of about 90°C. In some embodiments, the kneading is performed at a temperature of about 91°C. In some embodiments, the kneading is performed at a temperature of about 92°C. In some embodiments, the kneading is performed at a temperature of about 93°C. In some embodiments, the kneading is performed at a temperature of about 94°C. In some embodiments, the kneading is performed at a temperature of about 95°C. In some embodiments, the kneading is performed at a temperature of about 96°C. In some embodiments, the kneading is performed at a temperature of about 97°C. In some embodiments, the kneading is performed at a temperature of about 98°C. In some embodiments, the kneading is performed at a temperature of about 99°C.In some embodiments, kneading is performed at a temperature of about 100°C. In some embodiments, kneading is performed at a temperature of about 101°C. In some embodiments, kneading is performed at a temperature of about 102°C. In some embodiments, kneading is performed at a temperature of about 103°C. In some embodiments, kneading is performed at a temperature of about 104°C. In some embodiments, kneading is performed at a temperature of about 105°C. In some embodiments, kneading is performed at a temperature of about 106°C. In some embodiments, kneading is performed at a temperature of about 107°C. In some embodiments, kneading is performed at a temperature of about 108°C. In some embodiments, kneading is performed at a temperature of about 109°C. In some embodiments, kneading is performed at a temperature of about 110°C. In some embodiments, kneading is performed at a temperature of about 111°C. In some embodiments, kneading is performed at a temperature of about 112°C. In some embodiments, kneading is performed at a temperature of about 113°C. In some embodiments, kneading is performed at a temperature of about 114°C. In some embodiments, kneading is performed at a temperature of about 115°C. In some embodiments, kneading is performed at a temperature of about 116°C. In some embodiments, the kneading is performed at a temperature of about 117°C. In some embodiments, the kneading is performed at a temperature of about 118°C.
[0118] In some embodiments, kneading is performed at a temperature of about 119°C. In some embodiments, kneading is performed at a temperature of about 120°C. In some embodiments, kneading is performed at a temperature of about 121°C. In some embodiments, kneading is performed at a temperature of about 122°C. In some embodiments, kneading is performed at a temperature of about 123°C. In some embodiments, kneading is performed at a temperature of about 124°C. In some embodiments, kneading is performed at a temperature of about 125°C. In some embodiments, kneading is performed at a temperature of about 126°C. In some embodiments, kneading is performed at a temperature of about 127°C. In some embodiments, kneading is performed at a temperature of about 128°C. In some embodiments, kneading is performed at a temperature of about 129°C. In some embodiments, kneading is performed at a temperature of about 130°C. In some embodiments, kneading is performed at a temperature of about 131°C. In some embodiments, kneading is performed at a temperature of about 132°C. In some embodiments, kneading is performed at a temperature of about 133°C. In some embodiments, kneading is performed at a temperature of about 134°C. In some embodiments, kneading is performed at a temperature of about 135°C. In some embodiments, kneading is performed at a temperature of about 136°C. In some embodiments, kneading is performed at a temperature of about 137°C. In some embodiments, kneading is performed at a temperature of about 138°C. In some embodiments, kneading is performed at a temperature of about 139°C. In some embodiments, kneading is performed at a temperature of about 140°C. In some embodiments, kneading is performed at a temperature of about 141°C. In some embodiments, kneading is performed at a temperature of about 142°C. In some embodiments, kneading is performed at a temperature of about 143°C. In some embodiments, kneading is performed at a temperature of about 144°C. In some embodiments, kneading is performed at a temperature of about 145°C. In some embodiments, kneading is performed at a temperature of about 146°C. In some embodiments, kneading is performed at a temperature of about 147°C. In some embodiments, kneading is performed at a temperature of about 148°C. In some embodiments, kneading is performed at a temperature of about 149°C. In some embodiments, kneading is performed at a temperature of about 150°C. In some embodiments, kneading is performed at a temperature of about 151°C. In some embodiments, kneading is performed at a temperature of about 152°C. In some embodiments, the kneading is performed at a temperature of about 153°C. In some embodiments, the kneading is performed at a temperature of about 154°C. In some embodiments, the kneading is performed at a temperature of about 155°C. In some embodiments, the kneading is performed at a temperature of about 156°C. In some embodiments, the kneading is performed at a temperature of about 157°C. In some embodiments, the kneading is performed at a temperature of about 158°C. In some embodiments, the kneading is performed at a temperature of about 159°C. In some embodiments, the kneading is performed at a temperature of about 160°C. In some embodiments, the kneading is performed at a temperature of about 161°C.In some embodiments, kneading is performed at a temperature of about 162°C. In some embodiments, kneading is performed at a temperature of about 163°C. In some embodiments, kneading is performed at a temperature of about 164°C. In some embodiments, kneading is performed at a temperature of about 165°C. In some embodiments, kneading is performed at a temperature of about 166°C. In some embodiments, kneading is performed at a temperature of about 167°C. In some embodiments, kneading is performed at a temperature of about 168°C. In some embodiments, kneading is performed at a temperature of about 169°C. In some embodiments, kneading is performed at a temperature of about 170°C. In some embodiments, kneading is performed at a temperature of about 171°C. In some embodiments, kneading is performed at a temperature of about 172°C. In some embodiments, kneading is performed at a temperature of about 173°C. In some embodiments, kneading is performed at a temperature of about 174°C. In some embodiments, kneading is performed at a temperature of about 175°C. In some embodiments, kneading is performed at a temperature of about 176°C. In some embodiments, kneading is performed at a temperature of about 177°C. In some embodiments, kneading is performed at a temperature of about 178°C. In some embodiments, kneading is performed at a temperature of about 179°C. In some embodiments, kneading is performed at a temperature of about 180°C. In some embodiments, kneading is performed at a temperature of about 181°C. In some embodiments, kneading is performed at a temperature of about 182°C. In some embodiments, kneading is performed at a temperature of about 183°C. In some embodiments, kneading is performed at a temperature of about 184°C. In some embodiments, kneading is performed at a temperature of about 185°C. In some embodiments, kneading is performed at a temperature of about 186°C. In some embodiments, kneading is performed at a temperature of about 187°C. In some embodiments, kneading is performed at a temperature of about 188°C. In some embodiments, kneading is performed at a temperature of about 189°C. In some embodiments, kneading is performed at a temperature of about 190°C. In some embodiments, kneading is performed at a temperature of about 191°C. In some embodiments, kneading is performed at a temperature of about 192°C. In some embodiments, kneading is performed at a temperature of about 193°C. In some embodiments, kneading is performed at a temperature of about 194°C. In some embodiments, kneading is performed at a temperature of about 195°C. In some embodiments, the kneading is performed at a temperature of about 196° C. In some embodiments, the kneading is performed at a temperature of about 197° C. In some embodiments, the kneading is performed at a temperature of about 198° C. In some embodiments, the kneading is performed at a temperature of about 199° C. In some embodiments, the kneading is performed at a temperature of about 200° C.
[0119] In some embodiments, including any of the above embodiments, the kneading is performed at a temperature of about 21°C to about 31°C.
[0120] In some embodiments, including any of the above embodiments, the kneading is performed at a temperature of about 21°C to about 65°C.
[0121] In some embodiments, including any of the above embodiments, the kneading is performed at a temperature of about 31°C to about 65°C.
[0122] In some embodiments, including any of the above embodiments, the kneading is performed at a temperature of about 31°C to about 85°C.
[0123] In some embodiments, including any of the above embodiments, the kneading is performed at a temperature of about 75°C.
[0124] In some embodiments, including any of the above embodiments, kneading is performed at a temperature of about 25°C to about 200°C. In some embodiments, including any of the above embodiments, kneading is performed at a temperature of about 30°C to about 60°C. In some embodiments, including any of the above embodiments, kneading is performed at a temperature of about 40°C to about 80°C. In some embodiments, kneading is performed at a temperature of about 50°C to about 100°C. In some embodiments, kneading is performed at a temperature of about 60°C to about 120°C. In some embodiments, kneading is performed at a temperature of about 70°C to about 140°C. In some embodiments, kneading is performed at a temperature of about 80°C to about 160°C. In some embodiments, kneading is performed at a temperature of about 90°C to about 180°C. In some embodiments, including any of the above embodiments, kneading is performed at a temperature of about 45°C. In some embodiments, kneading is performed at a temperature of about 50°C. In some embodiments, kneading is performed at a temperature of about 55°C. In some embodiments, kneading is performed at a temperature of about 60°C. In some embodiments, kneading is performed at a temperature of about 65°C. In some embodiments, kneading is performed at a temperature of about 70°C. In some embodiments, kneading is performed at a temperature of about 75°C. In some embodiments, kneading is performed at a temperature of about 80°C. In some embodiments, kneading is performed at a temperature of about 85°C. In some embodiments, kneading is performed at a temperature of about 90°C. In some embodiments, kneading is performed at a temperature of about 95°C. In some embodiments, kneading is performed at a temperature of about 100°C. In some embodiments, kneading is performed at a temperature of about 105°C. In some embodiments, kneading is performed at a temperature of about 110°C. In some embodiments, kneading is performed at a temperature of about 115°C. In some embodiments, kneading is performed at a temperature of about 120°C. In some embodiments, kneading is performed at a temperature of about 125°C. In some embodiments, kneading is performed at a temperature of about 130°C. In some embodiments, kneading is performed at a temperature of about 135°C. In some embodiments, kneading is performed at a temperature of about 140°C. In some embodiments, kneading is performed at a temperature of about 145°C. In some embodiments, kneading is performed at a temperature of about 150°C. In some embodiments, kneading is performed at a temperature of about 155°C. In some embodiments, the kneading is performed at a temperature of about 160°C. In some embodiments, the kneading is performed at a temperature of about 165°C. In some embodiments, the kneading is performed at a temperature of about 170°C. In some embodiments, the kneading is performed at a temperature of about 175°C. In some embodiments, the kneading is performed at a temperature of about 180°C. In some embodiments, the kneading is performed at a temperature of about 185°C. In some embodiments, the kneading is performed at a temperature of about 190°C. In some embodiments, the kneading is performed at a temperature of about 195°C. In some embodiments, the kneading is performed at a temperature of about 200°C.
[0125] In some embodiments, including any of the above embodiments, the kneading is performed at a temperature of about 45°C.
[0126] In some embodiments, the method further comprises densifying the electrode by any method used by a skilled artisan. In some embodiments, the densification is achieved by applying high pressure with a uniaxial press. In some embodiments, the densification is achieved by applying high pressure with an isostatic press. In some embodiments, the densification is performed by calendaring the electrode.
[0127] In some embodiments, the pressure applied during densification is about 400 MPa to 1 GPa, such as 400, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, 950, or 1000 MPa.
[0128] In some embodiments, including any of the above, the binder particles are present at 0.3% w / w or less.
[0129] In some embodiments, including any of the above embodiments, the binder is PTFE.
[0130] In some embodiments, including any of the above, the binder is PTFE and at least one additional binder.
[0131] In some embodiments, including any of the above, the binder is polytetrafluoroethylene and at least one additional binder selected from the following group: polyvinylidene fluoride (PVDF), polyvinylidene fluoride hexafluoropropylene (PVDF-HFP), ethylene propylene (EPR), nitrile rubber (NPR), styrene-butadiene rubber (SBR), polypropylene (PP), polyethylene, atactic polypropylene (aPP), isotactic polypropylene (iPP), ethylene propylene rubber (EPR), ethylene pentene copolymer (EPC), polyisobutylene (PIB), butadiene rubber (SBR), polyolefins, polyethylene-co-l-octene (PE-co-PO), polyethylene-co-methylene cyclopentane (PE-co-PMCP), polymethyl methacrylate (PMMA) (and other acrylic), acrylic, polyethylene-acetal resin, polyvinyl alcohol butyral resin, PVB, poly Vinyl acetal resin, stereo block polypropylene, polypropylene polymethylpentene copolymer, polyethylene oxide (PEO), PEO block copolymer, silica gel, polyacrylonitrile (PAN), polyvinyl chloride (PVC), polyvinyl pyrrolidone (PVP), polyoxide poly (allyl glycidyl ester) PEO-AGE, polyoxide 2-methoxyethoxyethyl glycidyl ester (PEO-MEEGE), polyoxyethylene 2-methoxyethoxyethyl glycidyl ester poly (allyl glycidyl ether) (PEO-MEEGE-AGE), polysiloxane, polybutadiene polymer, polybutadiene rubber (PB), polyisobutadiene rubber (PIB), polyolefin, α-polyolefin, ethylene α-polyolefin, polyisobutadiene rubber (PI), polychloroprene rubber (CR), acrylonitrile butadiene rubber (NBR) and polyacrylate (PEA) and combinations thereof.
[0132] In some embodiments, including any of the above, the cathode active material is a material described in International Patent Application Publication No. PCT / US2021 / 049528 (filed on September 8, 2021, entitled “CATHODE COATING”, the entire contents of which are hereby incorporated by reference into this application for all purposes.
[0133] In some embodiments, including any of the above embodiments, the cathode active material is selected from: LiMPO 4 (M=Fe, Ni, Co, Mn); Li x Ti y O z , where x is 0 to 8, y is 1 to 12, and z is 1 to 24; LiMn 2a Ni a O 4 , where a is 0 to 2; nickel cobalt aluminum oxide; LiNi x Mn y Co z O2 where x + y + z = 1, 0 ≤ x ≤ 1, 0 ≤ y ≤ 1, 0 ≤ z ≤ 1; and LiNi x Co y Al z O 2 where x + y + z = 1, 0 ≤ x ≤ 1, 0 ≤ y ≤ 1, 0 ≤ z ≤ 1.
[0134] In some embodiments, including any of the above embodiments, the cathode active material is LiNi x Mn y Co z O 2 where x + y + z = 1, 0 ≤ x ≤ 1, 0 ≤ y ≤ 1, and 0 ≤ z ≤ 1.
[0135] In some embodiments, including any of the above embodiments, the cathode active material is LiNi x Mn y Co z O 2 where x is 0.8, y is 0.1, and z is 0.1.
[0136] In some embodiments, including any of the above embodiments, the cathode active material is LiNi x Mn y Co z O 2 where x is 0.6, y is 0.2, and z is 0.2.
[0137] In some embodiments, including any of the above embodiments, the cathode active material is LiNi x Mn y Co z O 2 where x is 0.5, y is 0.3, and z is 0.2.
[0138] In some embodiments, including any of the above embodiments, the cathode active material is LiNi x Mn y Co z O 2 where x is 1 / 3, y is 1 / 3, and z is 1 / 3.
[0139] In some embodiments, including any of the above embodiments, the cathode active material is LiNi x Mn y Co z O 2 .
[0140] In some embodiments, including any of the above embodiments, NMC has a d of 0.1 μm < S < 50 μm50 Particle size S.
[0141] In some embodiments, including any of the above embodiments, NMC has a d where 0.5 μm < S < 30 μm 50 Particle size S.
[0142] In some embodiments, including any of the above embodiments, NMC has a d where 1 μm < S < 20 μm 50 Particle size S.
[0143] In some embodiments, including any of the above embodiments, the cathode electrolyte is LSTPS.
[0144] In some embodiments, including any of the above embodiments, the cathode electrolyte is argentalite.
[0145] In some embodiments, including any of the above embodiments, the cathode electrolyte is a sulfide that can conduct lithium ions, such as Li 2 S - SiS 2 .
[0146] In some embodiments, including any of the above embodiments, the cathode electrolyte is an oxide that can conduct lithium ions, such as lithium - filled garnet.
[0147] In some embodiments, including any of the above embodiments, the cathode electrolyte is a halide that can conduct lithium ions, such as perovskite.
[0148] In some embodiments, including any of the above embodiments, the cathode electrolyte is an organic polymer that can conduct lithium ions, such as LiPF in PEO 6 .
[0149] In some embodiments, including any of the above embodiments, the d 50 particle size T of the cathode electrolyte is 0.005 μm < T < 20 μm.
[0150] In some embodiments, including any of the above embodiments, the d 50 particle size T of the cathode electrolyte is 0.01 μm < T < 10 μm.
[0151] In some embodiments, including any of the above embodiments, the d 50 particle size T of the cathode electrolyte is 0.02 μm < T < 5 μm.
[0152] In some embodiments, including any of the above, the density of the composition is 2 - 2.5 g / cm 3 .
[0153] In some embodiments, including any of the above embodiments, the solvent-free mixture is prepared by mixing binder particles with cathode active material particles and cathode electrolyte at a temperature below 0°C.
[0154] In some embodiments, PTFE (e.g., when PTFE is triclinic, it is in powder form) forms microfibers throughout the cathode after mixing at cold temperatures, and the PTFE forms microfibers during kneading. In some embodiments, this results in a network of PTFE fibers mixed with the cathode active material. In some embodiments, at room temperature or above, PTFE is a hexagonal / pseudo-hexagonal crystal that is sticky or viscous.
[0155] Preparation Example A
[0156] In some embodiments, a cathode active material (e.g., NMC, 18 g) and a cathode electrolyte (e.g., LSTPS, 3.01 g) are mixed to form a mixture. The resulting mixture is mixed eight times at room temperature using a blade mixer at 20,000 rpm for 20 seconds each time.
[0157] In some embodiments, a binder (eg, PTFE, 0.201 g) is added to the mixture to form a second mixture. The second mixture is mixed twice at -7°C using a blade mixer at 20,000 rpm for 10 seconds each time.
[0158] In some embodiments, the method then includes kneading at room temperature for about 30 minutes.
[0159] In some embodiments, the method includes subsequently forming the kneaded mixture into thin sheet extensions using a sheet press.
[0160] Preparation Example B
[0161] In some embodiments, a cathode active material (e.g., NMC, 18 g) and a cathode electrolyte (e.g., LSTPS, 3.01 g) are mixed to form a mixture. The resulting mixture is mixed eight times at room temperature using a blade mixer, each for 20 seconds at a speed of 20,000 rpm.
[0162] In some embodiments, a binder (eg, PTFE, 0.201 g) is added to the mixture to form a second mixture. The second mixture is mixed twice at room temperature using a blade mixer for 10 seconds each at 20,000 rpm.
[0163] In some embodiments, the method comprises subsequently kneading at -75°C for about 30 minutes.
[0164] In some embodiments, the method includes subsequently forming the kneaded mixture into thin sheet extensions using a sheet press.
[0165] Preparation Example C
[0166] In some embodiments, a cathode active material (e.g., NMC, 18 g) is mixed with a cathode electrolyte (e.g., LSTPS, 3.01 g) to form a mixture. The resulting mixture is mixed eight times at room temperature using a blade mixer for 20 seconds each at a speed of 20,000 rpm.
[0167] In some embodiments, a binder (eg, PTFE, 0.201 g) is added to the mixture to form a second mixture. The second mixture is mixed twice at -7°C using a blade mixer for 10 seconds each at 20,000 rpm.
[0168] In some embodiments, the method comprises subsequently kneading at -75°C for about 30 minutes.
[0169] In some embodiments, the method comprises subsequently kneading at -45°C for about 30 minutes.
[0170] In some embodiments, the method includes subsequently forming the kneaded mixture into thin sheet extensions using a sheet press.
[0171] Preparation Example D
[0172] Here is explained Figure 1 and Figure 2 The method shown.
[0173] exist Figure 1 In the example process shown, NMC and cathode materials are mixed with a polytetrafluoroethylene binder, followed by kneading and then formed into thin sheet extensions using a tablet press, which may also be referred to as an extruder.
[0174] Figure 1 Shown are PTFE agglomerates mixed with NMC particles.
[0175] Figure 1 The network formed by mixing PTFE agglomerates with NMC particles is shown when PTFE forms microfibers and forms a network in a kneaded dough. Figure 1 The kneading of the dough into a sheet is shown.
[0176] exist Figure 2 In another embodiment shown, NMC and cathode materials are mixed with a polytetrafluoroethylene binder, followed by kneading and then formed into thin sheet extensions using a sheet press.
[0177] Additional Embodiments
[0178] Example 1: A method for manufacturing a solid-state cathode (SSC) sheet, comprising: providing or having provided a solvent-free mixture, the solvent-free mixture containing cathode active material particles, cathode electrolyte and binder particles; the binder particle content is 5% w / w or less; placing the mixture at a temperature of about -30°C to -5°C; kneading the mixture into a mass at a temperature of about 25°C to 200°C to form binder microfibers; and depositing the mixture to make an SSC sheet.
[0179] Embodiment 2: The method according to embodiment 1, wherein the binder particles content is 1% w / w or less.
[0180] Embodiment 3: The method according to embodiment 1 or 2, wherein the binder particles content is 0.3% w / w or less.
[0181] Embodiment 4: A method according to any one of embodiments 1-3, comprising allowing the mixture to stand for 1-4 hours.
[0182] Embodiment 5: A method according to any one of embodiments 1-4, comprising allowing the mixture to stand for 2 hours.
[0183] Embodiment 6: The method according to any one of embodiments 1-5, comprising placing the mixture at -30°C to -10°C.
[0184] Embodiment 7: The method according to any one of embodiments 1-6, comprising placing the mixture at -20°C.
[0185] Embodiment 8: The method according to any one of embodiments 1-7, wherein the step of kneading the mixture to form adhesive microfibers comprises shearing the adhesive particles to form the adhesive microfibers.
[0186] Embodiment 9: The method according to any one of embodiments 1-8, wherein the temperature during kneading the mixture to form the adhesive microfibers is about 30°C to about 60°C.
[0187] Embodiment 10: The method according to any one of embodiments 1-9, wherein the temperature during kneading the mixture to form the adhesive microfibers is about 45°C.
[0188] Embodiment 11: The method according to any one of embodiments 1-10, wherein the step of kneading the mixture to form binder microfibers comprises shearing the cathode active material particles.
[0189] Embodiment 12: The method according to any one of embodiments 1-11, wherein the step of kneading the mixture to form binder microfibers includes shearing the cathode electrolyte.
[0190] Embodiment 13: The method according to any one of embodiments 1 to 12, wherein the cathode active material particles are coated with a cathode active material.
[0191] Embodiment 14: The method according to any one of embodiments 1-13, wherein the step of kneading the mixture to form binder microfibers further comprises compressing the cathode active material particles and the binder particles.
[0192] Embodiment 15: The method according to embodiment 14, further comprising forming a binder microfiber network in the cathode active material particles.
[0193] Embodiment 16: The method according to Embodiment 14 or 15, wherein the cathode active material particles and the binder particles are compressed under a pressure of 10 MPa to 30 MPa.
[0194] Embodiment 17: The method according to any one of embodiments 1-16, wherein the mixture is kneaded using a mortar.
[0195] Embodiment 18: The method according to any one of embodiments 1-17, wherein kneading the mixture comprises using a twin-screw co-rotating extruder.
[0196] Embodiment 19: The method according to any one of embodiments 1-18, further comprising pre-treating the adhesive.
[0197] Embodiment 20: The method of embodiment 19, wherein the pretreatment comprises atomizing the adhesive.
[0198] Embodiment 21: The method of embodiment 20, comprising atomizing the binder using a blade mixer.
[0199] Example 22: According to the method of Example 20 or 21, the adhesive is atomized using a blade mixer at about 15°C.
[0200] Embodiment 23: The method according to any one of embodiments 1-22, wherein the kneading is performed at a temperature of about 21°C to about 31°C.
[0201] Embodiment 24: The method according to any one of embodiments 1-22, wherein the kneading is performed at a temperature of about 21°C to about 85°C.
[0202] Embodiment 25: The method according to any one of embodiments 1-22, wherein the kneading is performed at a temperature of about 31°C to about 85°C.
[0203] Embodiment 26: A method according to any one of embodiments 1-25, wherein the binder is polytetrafluoroethylene (PTFE).
[0204] Embodiment 27: The method of any of Embodiments 1-26, wherein the binder comprises PTFE and further comprises at least one additional binder.
[0205] Embodiment 28: The method according to any one of embodiments 1-27, wherein the cathode active material is selected from: LiMPO 4 (M=Fe, Ni, Co, Mn); Li x Ti y O z , where x is 0 to 8, y is 1 to 12, and z is 1 to 24; LiMn 2a Ni a O 4 , where a is 0 to 2; nickel cobalt aluminum oxide; LiNi x Mn y Co z O 2 , x+y+z=1, 0≤x≤1, 0≤y≤1, 0≤z≤1; LiNi x Co y Al z O 2 , where x+y+z=1, 0≤x≤1, 0≤y≤1, 0≤z≤1.
[0206] Embodiment 29: According to any one of the methods of Embodiments 1-28, wherein the cathode active material is LiNi x Mn y Co z O 2 , x+y+z=1, 0≤x≤1, 0≤y≤1, 0≤z≤1, and x+y+z=1.
[0207] Embodiment 30: The method according to embodiment 29, wherein the cathode active material is LiNi x Mn y Co z O 2 , x is 0.8, y is 0.1, and z is 0.1.
[0208] Embodiment 31: The method according to embodiment 29, wherein the cathode active material is LiNi x Mn y Co z O 2 , x is 0.6, y is 0.2, and z is 0.2.
[0209] Embodiment 32: The method according to embodiment 29, wherein the cathode active material is LiNi x Mn y Co z O 2, x is 0.5, y is 0.3, and z is 0.2.
[0210] Embodiment 33: The method according to embodiment 29, wherein the cathode active material is LiNi x Mn y Co z O 2 , x is 1 / 3, y is 1 / 3, and z is 1 / 3.
[0211] Embodiment 34: The method according to Embodiment 29, wherein the cathode active material is Li(NiCoMn)O 2 .
[0212] Embodiment 35: The method according to any one of embodiments 29-34, wherein the cathode active material has a d value of 0.1 μm ≤ S ≤ 50 μm. 50 Particle size S.
[0213] Embodiment 36: The method according to any one of Embodiments 29-35, wherein the NMC has a d value of 0.5 μm ≤ S ≤ 30 μm. 50 Particle size S.
[0214] Embodiment 37: The method according to any one of embodiments 29-36, wherein the NMC has a d 50 Particle size S.
[0215] Embodiment 38: The method according to any one of embodiments 29-37, wherein the NMC has a d 50 Particle size S.
[0216] Embodiment 39: The method according to any one of embodiments 29-38, wherein the NMC has a d value of 1 μm ≤ S ≤ 20 μm. 50 Particle size S.
[0217] Embodiment 40: The method according to any one of Embodiments 29-39, wherein the NMC has a d 50 Particle size S.
[0218] Embodiment 41: According to any one of the methods of embodiments 1-40, wherein the cathode electrolyte has a d 50 Particle size T is 0.02 μm <T<5μm。
[0219] Embodiment 42: A method according to any one of embodiments 1-41, wherein the cathode electrolyte has a d 50 Particle size T is 0.05 μm <T<3μm。
[0220] Embodiment 43: A method according to any one of embodiments 1-42, wherein the cathode electrolyte has a d50 Particle size T is 0.1 μm <T<1.5μm。
[0221] Embodiment 44: The method according to any one of embodiments 1-43, wherein the density of the mixture after thinning into a solid cathode sheet is 2-2.5 g / cm 3 .
[0222] Embodiment 45: According to any one of the methods of Embodiments 1-44, binder particles are mixed with cathode active material particles and cathode electrolyte at a temperature below 0°C to prepare a solvent-free mixture.
[0223] Example 46: SSC was calendered using a line pressure of 0.5 to 10 tons / cm according to any of the methods of Examples 1 to 45.
[0224] Embodiment 47: A method according to any one of embodiments 1-46, wherein the adhesive microfiber length is less than 1 mm.
[0225] Embodiment 48: The method of any one of Embodiments 1-47, wherein the SSC has a porosity of 40% to 50% by volume (v / v) before compression of the cathode active material particles and the binder particles.
[0226] Embodiment 49: The method of any one of Embodiments 1-48, wherein the SSC has a porosity of less than 40% v / v before compressing the cathode active material particles and the binder particles.
[0227] Embodiment 50: The method according to any one of embodiments 1-49, wherein the SSC has a hardness of 40-80 before compressing the cathode active material particles and the binder particles.
[0228] Embodiment 51: The method according to any one of embodiments 1-50, wherein the SSC has a density of 2-2.5 g / cc after the dough is kneaded into a sheet.
[0229] Example 52: A solid cathode made according to any one of the methods of Examples 1-51.
[0230] Embodiment 53: According to Embodiment 51: According to the solid cathode of Embodiment 52, its average tensile strength is about 0.3 MPa to 0.5 MPa.
[0231] Example 54: The solid cathode according to Example 52 has an average tensile strength of about 0.45 MPa.
[0232] Embodiment 55: The solid cathode according to Embodiment 52, having an average Young's modulus of about 0.5 GPa to 0.8 GPa.
[0233] Embodiment 56: The solid cathode according to Embodiment 52, wherein the average Young's modulus is about 0.07 GPa.
[0234] Embodiment 57: The solid cathode according to Embodiment 52, having an average plastic elongation of about 5% to 15%.
[0235] Embodiment 58: The solid cathode according to Embodiment 52, having an average plastic elongation of about 10%.
[0236] Example 59: The solid cathode according to Example 52, having an average plastic elongation of about 9%.
[0237] Example 60: The solid cathode according to Example 52, having an average plastic elongation of about 8%.
[0238] Embodiment 61: According to the solid cathode of embodiment 52, its elasticity range is 0.01-0.15GPa. In these embodiments, the thickness of the solid cathode sheet is less than 1mm. In some of these embodiments, the thickness of the solid cathode sheet is at least 100nm. In some of these embodiments, the thickness of the solid cathode sheet is at least 250nm. In some of these embodiments, the thickness of the solid cathode sheet is at least 500nm. In some of these embodiments, the thickness of the solid cathode sheet is at least 1μm.
[0239] Example 62: A composition comprising: cathode active material particles; a binder content of 1% w / w or less; the binder is mixed with the cathode active material particles; the binder is in the form of microfibers; and the mixture is solvent-free.
[0240] Embodiment 63: A composition according to embodiment 62, wherein the binder content is 0.3% w / w or less.
[0241] Embodiment 64: A composition according to Embodiment 62 or 63, wherein the binder is PTFE.
[0242] Embodiment 65: According to any one of the compositions of embodiments 62-64, the adhesive comprises PTFE and further comprises at least one additional adhesive. In some embodiments, the additional adhesive is selected from the following group: polypropylene (PP), polyethylene, atactic polypropylene (aPP), isotactic polypropylene (iPP), ethylene-propylene rubber (EPR), ethylene-pentene copolymer (EPC), polyisobutylene (PIB), butadiene rubber (SBR), polyolefins, polyethylene-co-octene (PE-co-PO), polyethylene-co-methylene cyclopentane (PE-co-PMCP), polymethyl methacrylate (and other acrylic acids), acrylic acid, polyethylene-acetal resin, polyvinyl alcohol butyral resin, PVB, polyvinyl alcohol acetal resin, stereo block polypropylene, polypropylene polymethylpentene copolymer, polyethylene oxide (PEO), PEO block copolymer, silica gel, etc. In some examples, including any of the above, the binder is a polymer selected from polyacrylonitrile (PAN), polypropylene, polyethylene, polyoxide (PEO), polymethyl methacrylate (PMMA), polyvinyl chloride (PVC), polyvinyl pyrrolidone (PVP), polyoxide poly(allyl glycidyl ester) PEO-AGE, polyoxide 2-methoxyethoxyethyl glycidyl ester (PEO-MEEGE), polyoxyethylene 2-methoxyethoxyethyl glycidyl ester poly(allyl glycidyl ether) (PEO-MEEGE-AGE), polysiloxane, polyvinylidene fluoride (PVDF), polyvinylidene fluoride hexafluoropropylene (PVDF-HFP), ethylene propylene (EPR), nitrile rubber (NPR), styrene butadiene rubber (SBR), polybutadiene polymer, polybutadiene rubber (PB), polyisobutadiene rubber (PIB), polyolefin, α-polyolefin, ethylene α-polyolefin, polyisobutadiene rubber (PI), polychloroprene rubber (CR), acrylonitrile butadiene rubber (NBR) and polyacrylate (PEA).
[0243] Embodiment 66: A composition according to any one of embodiments 62-65, wherein the cathode active material is selected from LiMPO 4 (M=Fe, Ni, Co, Mn); Li x Ti y O z , where x is 0 to 8, y is 1 to 12, and z is 1 to 24; LiMn 2a Ni a O 4 , where a is 0 to 2; nickel cobalt aluminum oxide; LiNi x Mn y Co z O 2 , where x+y+z=1, 0≤x≤1, 0≤y≤1, 0≤z≤1; LiNi x Coy Al z O 2 , where x + y + z = 1, 0 ≤ x ≤ 1, 0 ≤ y ≤ 1, 0 ≤ z ≤ 1.
[0244] Example 67: According to any one of the compositions in Examples 62 - 66, wherein the cathode active material is LiNi x Mn y Co z O 2 , where x + y + z = 1, 0 ≤ x ≤ 1, 0 ≤ y ≤ 1 and 0 ≤ z ≤ 1.
[0245] Example 68: According to the composition of Example 67, wherein the cathode active material is LiNi x Mn y Co z O 2 , x is 0.8, y is 0.1, and z is 0.1.
[0246] Example 69: According to the composition of Example 67, wherein the cathode active material is LiNi x Mn y Co z O 2 , x is 0.6, y is 0.2, and z is 0.2.
[0247] Example 70: According to the composition of Example 67, wherein the cathode active material is LiNi x Mn y Co z O 2 , x is 0.5, y is 0.3, and z is 0.2.
[0248] Example 71: According to the composition of Example 67, wherein the cathode active material is LiNi x Mn y Co z O 2 , x is 1 / 3, y is 1 / 3, and z is 1 / 3.
[0249] Example 72: According to the composition of Example 67, wherein the cathode active material is Li(NiCoMn)O 2 .
[0250] Example 73: According to any one of the compositions in Examples 67 - 72, wherein NMC has a d 50 particle size S of 0.5 μm ≤ S ≤ 30 μm.
[0251] Example 74: According to any one of the compositions in Examples 67 - 73, wherein NMC has a d of 1 μm < S < 20 μm50 Particle size S.
[0252] Example 75: Any composition according to Examples 67 - 74, wherein the NMC has a d of 4 μm < S < 20 μm 50 Particle size S.
[0253] Example 76: Any composition according to Examples 67 - 75, wherein the NMC has a d of 2 μm < S < 15 μm 50 Particle size S.
[0254] Example 77: Any composition according to Examples 67 - 76, wherein the NMC has a d of 4 μm < S < 10 μm 50 Particle size S.
[0255] Example 78: Any composition according to Examples 67 - 77, wherein the cathode electrolyte has a d of 0.02 μm < T < 5 μm 50 Particle size T.
[0256] Example 79: Any composition according to Examples 67 - 78, wherein the cathode electrolyte has a d of 0.05 μm < T < 3 μm 50 Particle size T.
[0257] Example 80: Any composition according to Examples 62 - 79, which further comprises a cathode electrolyte, wherein the cathode electrolyte has a d of 0.02 μm < T < 5 μm 50 Particle size T.
[0258] Example 81: Any composition according to Examples 62 - 80, which further comprises a cathode electrolyte, wherein the cathode electrolyte has a d of 0.05 μm < T < 3 μm 50 Particle size T.
[0259] Example 82: Any composition according to Examples 62 - 81, which further comprises a cathode electrolyte, wherein the cathode electrolyte has a d of 0.1 μm < T < 1.5 μm 50 Particle size T.
[0260] Example 83: Any composition according to Examples 36 - 82, wherein the composition has a density of 2 - 2.5 g / cm 3 of density.
[0261] Example 84: A thin sheet containing any composition according to Examples 62 - 83.
[0262] Example 85: The thin sheet according to Example 84, wherein the porosity is less than 40% v / v.
[0263] Embodiment 86: A sheet according to Embodiment 84, wherein the cathode active loading is 1 to 15 mAh / cm 2 between.
[0264] Embodiment 87: The sheet according to Embodiment 84, wherein the cathode active load is at least 5mah / cm 2 .
[0265] Embodiment 88: A thin sheet according to any one of embodiments 84-87, wherein the thickness of the thin sheet is 120 μm.
[0266] Embodiment 89: A thin sheet according to any one of embodiments 84-88, wherein the thickness of the thin sheet is 150 μm.
[0267] Embodiment 90: A sheet according to any of embodiments 84-89, wherein the width of the sheet is at least 5 centimeters (cm).
[0268] Embodiment 91: A sheet according to any one of embodiments 84-90, wherein the width of the sheet is at least 1 meter (m).
[0269] Embodiment 92: A sheet according to any one of embodiments 84-91, wherein the sheet is at least 10 cm long.
[0270] Embodiment 93: A sheet according to any one of embodiments 84-92, wherein the sheet has a length of at least 70 cm.
[0271] Embodiment 94: A sheet according to any one of embodiments 84-93, wherein the length of the sheet is at least 1 meter.
[0272] Embodiment 95: A bilayer comprising a metal layer in contact with any one of the sheets of embodiments 62-94.
[0273] Embodiment 96: A three-layer, comprising a metal layer, wherein the metal layer is located between and in contact with two sheets of any of the sheets described in Embodiments 84-94.
[0274] Embodiment 97: A double layer or triple layer according to any one of embodiments 94-96, wherein the metal layer is an aluminum layer.
[0275] Embodiment 98: A double layer or triple layer according to any one of Embodiments 94-96, wherein the metal layer is a Ni layer.
[0276] Embodiment 99: A double layer or triple layer according to any one of Embodiments 94-96, wherein the metal layer is a layer of Cu, Ni, Al, Mg, Ag, Au, Pt or a combination thereof.
[0277] Embodiment 100: A double layer comprising a solid electrolyte layer, wherein the solid electrolyte layer is in contact with any of the thin sheets described in Embodiments 84-94.
[0278] Embodiment 101: A three-layer comprising a solid electrolyte layer, wherein the solid electrolyte layer is located between and in contact with two sheets of any of the sheets described in Embodiments 84-94.
[0279] Embodiment 102: A bilayer or trilayer according to any one of embodiments 100-101, wherein the solid electrolyte layer is a lithium-filled garnet layer.
[0280] In some embodiments, the present application discloses a method for manufacturing a solid-state cathode (SSC) sheet, comprising: providing or having provided a solvent-free mixture, the solvent-free mixture containing cathode active material particles, cathode electrolyte and binder particles; the binder particle content is 5% w / w or less; placing the mixture at a temperature of about -30°C to -5°C; kneading the mixture into a mass at a temperature of about 25°C to 200°C to form binder microfibers; depositing the mixture to form an SSC sheet; thereby making an SSC sheet.
[0281] In some embodiments, including any of the above, the method includes mixing cathode active material particles, cathode electrolyte, and binder particles prior to placing the mixture.
[0282] In some embodiments, including any of the above embodiments, placing the mixture at a temperature of about -30°C to -5°C includes mixing the mixture.
[0283] In some embodiments, including any of the above, the binder particles are present at 1% w / w or less.
[0284] In some embodiments, including any of the above, the method comprises allowing the mixture to stand for 1 hour to 4 hours.
[0285] In some embodiments, including any of the above, the method comprises placing the mixture at a temperature of -30°C to -10°C.
[0286] In some embodiments, including any of the above, the process of kneading the mixture into a mass to form adhesive microfibers includes shearing the adhesive particles to form adhesive microfibers.
[0287] In some embodiments, including any of the above, during the process of kneading the mixture into a mass to form the adhesive microfibers, the temperature of the mixture is from about 30°C to about 60°C.
[0288] In some embodiments, including any of the above, the process of kneading the mixture into a mass and forming binder microfibers includes shearing the cathode electrolyte.
[0289] In some embodiments, including any of the above, the cathode active material particles are coated with cathode active material particles.
[0290] In some embodiments, including any of the above, the process of kneading the mixture into a mass and forming binder microfibers further includes compressing the cathode active material particles and the binder particles.
[0291] In some embodiments, including any of the above, the cathode active material particles and the binder particles are under a pressure of 10 MPa to 30 MPa.
[0292] In some embodiments, including any of the above, the binder is polytetrafluoroethylene (PTFE).
[0293] In some embodiments, including any of the above, the binder includes PTFE and further includes at least one additional binder.
[0294] In some embodiments, including any of the above embodiments, the cathode active material is LiNi x Mn y Co z O 2 , where x + y + z = 1, 0 ≤ x ≤ 1, 0 ≤ y ≤ 1 and 0 ≤ z ≤ 1.
[0295] In some embodiments, including any of the above embodiments, the cathode active material has a d 50 particle size S of 2 μm ≤ S < 15 μm.
[0296] In some embodiments, including any of the above embodiments, the SSC further includes a cathode electrolyte, and the cathode electrolyte has a d 50 particle size T of 0.02 μm < T < 5 μm.
[0297] In some embodiments, including any of the above embodiments, the SSC sheet has a density of 2 - 2.5 g / cm 3 .
[0298] In some embodiments, including any of the above, the method includes calendering the SSC with a tube press in the range of 0.5 tons / cm to 10 tons / cm.
[0299] In some embodiments, including any of the above embodiments, the length of the binder microfibers is less than 1 mm.
[0300] In some embodiments, including any of the above, the SSC has a porosity of 40% to 50% by volume (v / v) prior to compression of the cathode active material particles and the binder particles.
[0301] In some embodiments, including any of the above, the SSC has a porosity of less than 40% v / v after compression of the cathode active material particles and the binder particles.
[0302] In some embodiments, including any of the above, the mixture forms the binder microfibers at a temperature of about 35°C to 100°C.
[0303] In some embodiments, including any of the above, the mixture forms the binder microfibers at a temperature of about 35°C to 75°C.
[0304] In some embodiments, including any of the above embodiments, the mixture is kneaded at a temperature of about 35° C. to 50° C. to form the binder microfibers.
[0305] In some embodiments, described herein are solid-state cathode sheets made according to the methods described herein.
[0306] In some embodiments, including any of the above embodiments, the solid cathode sheet has an average tensile strength of about 0.3 MPa to about 0.5 MPa.
[0307] In some embodiments, including any of the above embodiments, the solid cathode sheet has an average Young's modulus of about 0.5 GPa to about 0.8 GPa.
[0308] In some embodiments, including any of the above, the solid cathode sheet has an average plastic elongation of about 5% to about 15%.
[0309] In some embodiments, including any of the above embodiments, the solid cathode sheet has an elasticity of about 0.01 GPa to about 0.15 GPa. In some embodiments, the elasticity may be affected by the dispersion of the binder (e.g., PTFE). In some embodiments, the elasticity may be affected by the kneading process.
[0310] In some embodiments, the composition described herein includes: cathode active material particles; a binder content of 1% w / w or less; the binder is mixed with the cathode active material particles; the binder is in the form of microfibers; and the mixture is solvent-free.
[0311] In some embodiments, including any of the above, the composition further comprises a cathode electrolyte.
[0312] In some embodiments, including any of the above, the binder is polytetrafluoroethylene (PTFE).
[0313] In some embodiments, including any of the above, the binder comprises PTFE and further comprises at least one additional binder.
[0314] In some embodiments, including any of the above embodiments, the cathode active material is LiNi x Mn y Co z O 2 , where x + y + z = 1, 0 ≤ x ≤ 1, 0 ≤ y ≤ 1, and 0 ≤ z ≤ 1.
[0315] In some embodiments, including any of the above embodiments, NMC has a d 50 particle size S of 2 μm ≤ S < 15 μm.
[0316] In some embodiments, including any of the above embodiments, the cathode electrolyte has a d 50 particle size T of 0.02 μm < T < 5 μm.
[0317] In some embodiments, including any of the above, the composition has a density of 2 - 2.5 g / cm 3 after being formed into a sheet.
[0318] In some embodiments, including any of the above, the binder microfibers have a length of less than 1 mm.
[0319] In some embodiments, including any of the above embodiments, the porosity range of the SSC is less than 40% v / v.
[0320] In some embodiments, what is described in the present application is a sheet containing the composition described in the present application.
[0321] In some embodiments, what is described in the present application is a bilayer comprising a metal layer in contact with the sheet described in the present application.
[0322] In some embodiments, what is described in the present application is a trilayer comprising a metal layer between and in contact with two sheets described in the present application.
[0323] In some embodiments, including any of the above embodiments, the metal layer is a layer of Al, Ni, Cu, Ni, Al, Mg, Ag, Au, Pt, or a combination thereof.
[0324] In some embodiments, what is described in the present application is a bilayer comprising a solid electrolyte layer in contact with the sheet described in the present application.
[0325] In some embodiments, described herein is a three-layer including a solid electrolyte layer, wherein the solid electrolyte layer is located between and in contact with two sheets described herein.
[0326] In some embodiments, including any of the above embodiments, the solid electrolyte layer is a lithium-filled garnet layer. Example
[0327] Unless otherwise stated, reagents, chemicals, and materials were purchased commercially.
[0328] The pouch batteries were purchased from Showa Denko.
[0329] The electrochemical potentiostat used was an Arbin potentiostat.
[0330] Electrical impedance spectroscopy (EIS) was performed using a Biologic VMP3, VSP, VSP-300, SP-150, or SP-200.
[0331] Electron microscopy was performed on a FEI QuantaSEM, Helios600i or Helios660 FIB-SEM.
[0332] Transmission electron microscopy was performed as follows.
[0333] Sample preparation: Samples for TEM measurements were prepared using a Ga ion source focused ion beam SEM (nanoDUET NB5000, from Hitachi High-Tech Corporation). In order to protect the material surface from the Ga ion beam, multiple protective layers were deposited before sampling; first the metal layer was deposited using a plasma coater, and then the carbon protective layer and tungsten layer were deposited using high vacuum evaporation and focused ion beam, respectively. Thin section sampling was performed using a focused ion beam. The prepared samples were measured under a transmission electron microscope.
[0334] TEM measurement: A field emission electron microscope (JEM-2100F, JEOL) was used to obtain TEM images of NMC coatings. The acceleration voltage was set to 200 kV and the electron beam radius was set to 0.7-1 nm.
[0335] X-ray powder diffraction (XRD) was performed using a Bruker D8 Advance A25 at room temperature (e.g., 21-23°C) using CuK-α radiation. The Cu-Ka source was at a wavelength of X-ray 40kV and 25ma. Detector: LYNXEYE_XE PSD opening 2.843. Slit 0.6mm, anti-slit 5.0mm fixed.
[0336] Milling was performed using a Retsch PM 400 planetary ball mill. Mixing was performed using a Fisher Scientific vortex mixer, a Flaktek high-speed mixer, or a Primix thin-film homogenizer.
[0337] Casting is done on a TQC scale table. Calendering is done on an IMC calender.
[0338] Light scattering was performed on a Horiba, Model: Partica, Type: LA-950V2, Common Name: Laser Scattering Particle Size Distribution Analyzer.
[0339] The lithium nickel cobalt manganese oxide (NMC) used in the examples is LiNi 0.85 Co 0.1 Mn 0.05 O 2 , unless otherwise noted.
[0340] Example 1 Preparation of solid cathode sheet
[0341] Step 1: 18 g NMC was mixed with 3.01 g LSTPS. The resulting mixture was mixed with a blade mixer at room temperature for 8 times, each time for 20 seconds, at a speed of 20,000 rpm. 10 Si 0.5 Sn 0.5 P 2 S 12 (hereinafter referred to as LSTPS) is wet-milled to obtain LSTPS particles with a particle size of about 50 to 500 nm. See U.S. Patent Nos. 9,172,114 and 10,535,878, which are hereby incorporated by reference in their entirety into this application for all purposes.
[0342] Step 2: Add 0.201 g of PTFE to the mixture.
[0343] Step 3: The resulting mixture was mixed at room temperature using a blade mixer twice for 10 seconds each at 20,000 rpm.
[0344] Step 4: Knead the resulting mixture at room temperature.
[0345] Step 5: Use a tablet press to compress the resulting mixture into thin sheets. The tablet press and extruder described here have the same meaning.
[0346] Example 2 Analysis of solid cathode sheet
[0347] Differential scanning calorimetry was used to analyze the microfiber formation process of PTFE. Figure 3 .from Figure 3FIG. 3 shows that there are benefits to PTFE being dispersed at lower temperature than the phase transition temperature from the triclinic phase to the hexagonal phase. In this embodiment, the phase transition temperature is 15°C. Figure 3 It is shown that kneading above the phase transition temperature has benefits.
[0348] DSC measurement was performed on PTFE alone to observe the phase transition temperature. Figure 3 It shows that the mixing of PTFE needs to be carried out below the exothermic peak temperature; and kneading should be carried out after the exothermic peak appears.
[0349] Differential Scanning Calorimetry was performed using a STA449F3 Jupiter, Netzsch system, scanning between -10°C and 70°C at a scan rate of 2°C / min, using gold-coated SS pans sealed in a dry air atmosphere (dew point = -50°C).
[0350] Example 3 Cycle Test
[0351] Preparation of solid electrolyte: Lithium sulfide (Li 2 S), phosphorus pentasulfide (P 2 S 5 ) and lithium iodide (LiI) were mixed in a predetermined ratio. In one sample, lithium sulfide (Li 2 S), phosphorus pentasulfide (P 2 S 5 ) and lithium iodide (Lil). LiI: Li 2 S:P 2 S 5 The molar ratio of (3-4): (0.1-1): (0.5-1.5) was set. The mixture was placed in a 500 ml zirconia grinding jar containing 1 mm zirconia grinding media, with a grinding media: powder mass ratio of >7.5. The mixture was stirred in a planetary mill (Retsch PM400, 150 mm rotation radius, 1:2 speed ratio) for 16-32 hours.
[0352] An all-solid-state battery was manufactured using the solid cathode manufactured in Example 1 and a separator made of the solid electrolyte described above.
[0353] The cathode layer and separator are pressed at 700 MPa to form a pellet type battery. An aluminum current collector is used near the cathode layer. A nickel current collector is used near the anode layer. Finally, the pellet stack and current collector are vacuum sealed in a polyester film bag to form a battery cell. The anode layer is made of metallic lithium. When the battery is charged, the metallic lithium is embedded as the anode. The cathode layer is a solid sheet of 100μm-150μm thick. The solid separator thickness is 30μm to 50μm.
[0354] Cycle the battery and the result is Figure 4 shown.
[0355] Example 4 Area Specific Resistance (ASR) Test
[0356] Preparation of solid electrolyte: Lithium sulfide (Li 2 S), phosphorus pentasulfide (P 2 S 5 ) and lithium iodide (LiI) were mixed in a predetermined ratio. In one sample, lithium sulfide (Li 2 S), phosphorus pentasulfide (P 2 S 5 ) and lithium iodide (Lil). LiI: Li 2 S:P 2 S 5 The molar ratio of (3-4): (0.1-1): (0.5-1.5) was set. The mixture was placed in a 500 ml zirconia grinding jar containing 1 mm zirconia grinding media, with a grinding media: powder mass ratio of >7.5. The mixture was stirred in a planetary mill (Retsch PM400, 150 mm rotation radius, 1:2 speed ratio) for 16 to 32 hours.
[0357] An all-solid-state battery was made using the solid cathode produced in Example 1 and a separator made of the solid electrolyte prepared in the previous section. The cathode layer was a solid sheet with a thickness of 100 μm to 150 μm. The thickness of the solid separator was 30 μm to 50 μm.
[0358] The cathode layer and separator are compressed at 700 MPa to make them compact into a particle-type battery. An aluminum current collector is used near the cathode layer. A nickel current collector is used near the anode layer. Finally, the particle stack and current collector are vacuum-sealed in a polyester film bag to make a battery cell. The anode layer is composed of metallic lithium. When the battery is charged, the metallic lithium is embedded as the anode.
[0359] The cells were charged and discharged under intermittent current pulses at 30 °C with a constant current density of 0.55 mA / cm 2(C / 10 rate) with an operating voltage of 3V to 4.25V. The current pulse is applied for 9 minutes, the current is stopped, and the system is relaxed for 3 minutes. This intermittent pulse is repeated until the battery voltage reaches 4.25V during charging and 3V during discharge. The voltage drop during the relaxation step during discharge is read to obtain the area specific resistance (ASR) of the battery. The obtained ASR is named R 1 .
[0360] After cycling at 30 °C, the battery was charged again to 4.25 V with a current density of 1.7 mA / cm 2 The battery temperature was then raised to 60°C. After the temperature stabilized at 60°C, the battery was kept at 4.25V for 7 days and the battery was discharged to 3V.
[0361] The battery temperature was lowered to 30°C. Between 3V and 4.25V, the current density was 1.7mA / cm 2 The battery is charged and discharged. ASR (R 2 ).
[0362] By ΔR = R 2 –R 1 The stability was evaluated. Figure 5 shown.
[0363] Example 5 Tensile Strength Test
[0364] The all-solid cathode sheet was manufactured using an extruder according to the method in Example 1.
[0365] The tensile strength of the cathode sheets was measured as a function of strain in a series of samples. Figure 6 shown.
[0366] Tensile tests were performed using an Instron mechanical tester with a 100N load cell and pneumatic side-action grips. The test rate was 1m / min. The difference between the two groups of samples was the kneading process. The results show that cold dispersion and warm kneading of PTFE are important to obtain higher strength and ductility.
[0367] Example 6 Preparation of solid cathode sheet
[0368] Step 1: Mix 18 g NMC with 3.01 g Li 10 Si 0.5 Sn 0.5 P 2 S 12 The obtained mixture was mixed with a blade mixer at room temperature for 8 times, each time for 20 seconds, at a rotation speed of 20,000 rpm. LSTPS was wet-milled according to the method of Example 1 to obtain LSTPS particles with a particle size of about 50 to 500 nm.
[0369] Step 2: Add 0.201 g of polytetrafluoroethylene to the mixture. The polytetrafluoroethylene powder size is 1 μm and the polytetrafluoroethylene particles are smaller than 1 μm.
[0370] Step 3: The resulting mixture was stabilized at -20°C for at least 2 hours. The stabilized mixture was then mixed 10 times with a blade mixer for 2 seconds each time at 20,000 rpm. Between each mixing, the mixture was returned to a -20°C environment and stabilized for 2 minutes.
[0371] Step 4: The resulting mixture was removed from the -20°C environment and then microfibrillated in a kneader at 45°C.
[0372] Step 5: The resulting mixture is compressed into thin sheets using a tablet press. A tablet press is also called an extruder.
[0373] Step 6: Densify the sheet under high pressure by calendering. Calender with a pipeline press between 0.5 tons / cm and 10 tons / cm.
[0374] Comparison of cathode preparation in Example 7
[0375] Three sets of exemplary cathodes were prepared by the method of Example 6, with the following differences. Three sets of exemplary cathodes were prepared by changing the conditions in steps 3 and 4 of Example 6 as shown below.
[0376] Group 1: The stabilized mixture was mixed 10 times at -30°C using a blade mixer, 2 seconds / time, and 20,000 rpm. The sample was frequently stabilized during the mixing process. After mixing at -30°C, microfibrillation was performed in a kneader at 160°C.
[0377] The second group: The stabilized mixture was mixed 10 times at -20°C to 0°C using a blade mixer, 2 seconds per time, and a rotation speed of 20,000 rpm. After mixing at -20°C to 0°C, microfibrillation was performed in a kneader at 45°C.
[0378] The third group: The stabilized mixture was mixed 10 times at room temperature using a blade mixer, 2 seconds per time, and a rotation speed of 20,000 rpm. After mixing at -20°C to 0°C, microfibrillation was performed in a kneader at room temperature.
[0379] The performance of the three groups of solid cathode sheet samples prepared in Example 6 is described in detail as follows:
[0380] The average tensile strength of each group: Group 1 = 0.84 MPa; Group 2 = 0.44 MPa; Group 3 = 0.18 MPa.
[0381] The average modulus of each group: Group 1 = 0.10 GPa, Group 2 = 0.07 GPa, Group 3 = 0.02 GPa.
[0382] The average plastic elongation of each group: Group 1 = 18%, Group 2 = 8.7%, Group 3 = 1.7%.
[0383] The performance of the samples is as follows Figure 7 and 8 shown.
[0384] The tensile strength was measured using an Instron mechanical tester with a 100 N load cell and a pneumatic side-actuated grip. The test rate was 1 m / min.
[0385] The lack of PTFE dispersion / kneading temperature control results in SSC sheets that are soft, weak and brittle and difficult to handle.
[0386] Cold dispersion of PTFE and hot rolling of SSC resulted in significantly stronger, harder and tougher SSC sheets. This is shown by the cluster 2 in the middle of Figures 9 and 10. As mentioned above, cluster 2 has surprising advantages in its average tensile strength, average modulus and average plastic elongation.
[0387] In some cases, when the sheet is too hard and strong, such as group 3, it will cause difficulties in the sheet thinning process. When the sheet is brittle and weak like group 1, there are also difficulties.
[0388] The results show that plastic elongation is an important characteristic because the most undesirable product would be a brittle SSC rolled sheet. This is related to low plastic elongation. If the tensile strength and modulus of the material are too high, the SSC thinning process will be more difficult. For example, the rolled dough may be too rigid or too hard.
[0389] The embodiments and examples described above are merely illustrative and non-restrictive. Those skilled in the art will be able to identify or determine many equivalents of specific compounds, materials and processes using routine experimental methods. All of these equivalents are within the scope of this application and are included in the scope of the appended claims.
Claims
1. A method for manufacturing a solid state cathode (SSC) sheet, comprising: A solvent-free mixture is provided or has been provided, the solvent-free mixture comprising cathode active material particles, cathode electrolyte and binder particles; the binder particles are contained in an amount of 5% w / w or less; placing the mixture at a temperature of about -30°C to -5°C; kneading the mixture into a mass at a temperature of about 25° C. to 200° C. to form adhesive microfibers; depositing the mixture to form a SSC sheet; Thus, an SSC sheet is produced. 2 . The method according to claim 1 , further comprising mixing the cathode active material particles, cathode electrolyte and binder particles before placing the mixture.
3. The method of claim 1 or 2, further comprising mixing the mixture while placing the mixture at a temperature of about -30°C to -5°C.
4. The method according to any one of claims 1 to 3, wherein the binder content is 1% w / w or less.
5. The method according to any one of claims 1 to 4, wherein the mixture is allowed to stand for 1 to 4 hours.
6. The method of any one of claims 1 to 5, wherein the mixture is placed at a temperature of about -30°C to -10°C.
7. The method according to any one of claims 1 to 6, wherein the step of kneading the mixture into a mass to form adhesive microfibers comprises shearing adhesive particles to form adhesive microfibers.
8. The method of any one of claims 1-7, wherein the temperature during kneading the mixture to form the binder microfibers is from about 30°C to about 60°C.
9. The method of any one of claims 1-8, wherein the step of kneading the mixture into a mass to form binder microfibers comprises shearing the cathode electrolyte. 10 . The method according to claim 1 , wherein the cathode active material particles are coated with cathode active material particles.
11. The method according to any one of claims 1 to 10, wherein the step of kneading the mixture to form binder microfibers further comprises compressing cathode active material particles and binder particles. 12 . The method according to claim 11 , wherein the compressing of the cathode active material particles and the binder particles is performed under a pressure of 10 MPa to 30 MPa.
13. The method of any one of claims 1-12, wherein the binder is polytetrafluoroethylene (PTFE).
14. The method of any one of claims 1-13, wherein the binder comprises PTFE and further comprises at least one additional binder.
15. The method according to any one of claims 1 to 14, wherein the cathode active material is LiNi x Mn y Co z O2, x+y+z=1, 0≤x≤1, 0≤y≤1, 0≤z≤1, and x+y+z=1.
16. The method according to any one of claims 1 to 15, wherein the cathode active material has a d value of 2 μm ≤ S < 15 μm. 50 Particle size S.
17. The method according to any one of claims 1 to 16, wherein the SSC further comprises a cathode electrolyte having a d 50 Particle size T is 0.02 μm <T<5μm。 18. The method according to any one of claims 1 to 17, wherein the density of the SSC sheet is 2 to 2.5 g / cm 3 .
19. The method according to any one of claims 1 to 18, comprising calendaring the SSC using a pipe press at 0.5 to 10 ton / cm.
20. The method of any one of claims 1-19, wherein the adhesive microfibers are less than 1 mm in length.
21. The method according to any one of claims 1 to 20, wherein the SSC has a porosity of 40 to 50% by volume (v / v) before the compressing of cathode active material particles and binder particles.
22. The method of any one of claims 1-21, said SSC having a porosity of less than 40% v / v after said compressing cathode active material particles and binder particles.
23. The method of claim 1, kneading the mixture at a temperature of about 35°C to about 100°C to form adhesive microfibers.
24. The method of claim 1, kneading the mixture at a temperature of about 35°C to about 75°C to form adhesive microfibers.
25. The method of claim 1, kneading the mixture at a temperature of about 35°C to about 50°C to form adhesive microfibers.
26. A solid cathode sheet prepared by the method according to any one of claims 1 to 25.
27. The solid cathode sheet according to claim 26, having an average tensile strength of about 0.3-0.5 MPa.
28. The solid cathode sheet according to claim 26 or 27, wherein the average Young's modulus is about 0.5 to 0.8 GPa.
29. The solid cathode sheet according to claims 26-28, having an average plastic elongation of about 5-15%.
30. The solid cathode sheet according to any one of claims 26 to 29, having an elasticity of about 0.01 to 0.15 GPa.
31. A composition comprising: cathode active material particles; a binder in an amount of 1% w / w or less; the binder being mixed with the cathode active material particles; the binder being in the form of microfibers; and the composition being solvent-free.
32. The composition of claim 31 further comprising a cathode electrolyte.
33. The composition of any one of claims 31-33, wherein the binder is polytetrafluoroethylene (PTFE).
34. The composition of any one of claims 31-33, wherein the binder comprises PTFE and further comprises at least one additional binder.
35. The composition according to any one of claims 31-34, wherein the cathode active material is LiNi x Mn y Co z O2, x+y+z=1, 0≤x≤1, 0≤y≤1, 0≤z≤1, and x+y+z=1.
36. The composition according to any one of claims 31 to 33, wherein the NMC has a d value of 2 μm ≤ S < 15 μm. 50 Particle size S.
37. The composition according to any one of claims 31-36, wherein the cathode electrolyte has a d 50 Particle size T is 0.02 μm <T<5μm。 38. A composition according to any one of claims 31 to 37 having a density of 2 to 2.5 g / cm 3 .
39. The composition of any one of claims 31-38, wherein the adhesive microfibers are less than 1 mm in length.
40. The composition of any one of claims 31-39, wherein the SSC has a porosity of less than 40% v / v.
41. A sheet comprising the composition of any one of claims 31-40.
42. A bilayer comprising a metal layer in contact with the sheet of claim 41.
43. A three-layer comprising a metal layer, said metal layer being located between and in contact with two sheets of the sheet of claim 41.
44. The bilayer of claim 41 or the trilayer of claim 43, the metal layer being a layer of Al, Ni, Cu, Mg, Ag, Au, Pt or a combination thereof.
45. A bilayer comprising a solid electrolyte layer in contact with the sheet of claim 41.
46. A three-layer comprising a solid electrolyte layer, the solid electrolyte layer being located between and in contact with two sheets of the sheet of claim 41.
47. The bilayer of claim 45 or the trilayer of claim 46, the solid electrolyte layer being a lithium filled garnet layer.