Process for the preparation of anhydrous rare earth fluorides from rare earth reduction slags in one step

Rare earth fluoride is prepared from rare earth reduction slag by a one-step hydrothermal method, which solves the problems of complex process, serious pollution and low rare earth yield in the existing technology, and realizes the efficient recovery and recycling of rare earth and fluorine.

CN119040641BActive Publication Date: 2025-10-14JIANGXI IONIC RARE EARTH ENG RES CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411155796.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2025-10-14
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The existing technology for recovering rare earth and fluorine elements from rare earth reduction slag has the problems of long process flow, high equipment corrosion, serious pollution and low rare earth yield.

Method used

A one-step hydrothermal method is used to directly prepare rare earth fluoride from rare earth and fluorine in rare earth reduction slag. The rare earth and fluorine are recovered and recycled through steps such as crushing, ball milling, mixing, precipitation conversion, washing and roasting.

Benefits of technology

The process flow is simplified, the recovery rate of rare earth and fluorine is improved, the pollution of hydrogen fluoride gas during the high-temperature transformation process is avoided, and green and efficient resource recovery is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040641B_ABST
    Figure CN119040641B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of industrial waste residue treatment, in particular to a process for preparing anhydrous rare earth fluoride from rare earth reduction slag by one-step method.The process provided by the present application is that the rare earth reduction slag raw material is treated by crushing, ball milling, acidification, etc., the treated slag is subjected to a precipitation conversion reaction with a rare earth chloride feed liquid, and fluorinated rare earth and a filtrate are obtained by filtration, the generated fluorinated rare earth is prepared into anhydrous fluorinated rare earth after filtration, washing, drying, vacuum roasting and other processes, and the rare earth chloride in the filtrate is enriched by using P507 extractant and returned for reuse.The process provided by the present application synchronously converts rare earth and fluorine in the rare earth reduction slag by one-step hydrothermal method, realizes the recycling of rare earth and fluorine resources, and has a simple process flow and is easy to be industrialized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of industrial waste residue treatment, and in particular to a process for preparing anhydrous rare earth fluoride from rare earth reduction residue in one step while also recovering rare earth and fluorine elements. Background Art

[0002] The production of high-melting-point rare earth metals (such as Gd, Tb, Dy, Ho, Er, Y, Lu metals, Tb-Dy alloys, etc.) generally uses metallic calcium as a reducing agent and rare earth fluorides as raw materials. Rare earth metals are generated under high temperature conditions, and calcium thermal reduction slag is also produced. The main component of the slag is calcium fluoride. Some rare earth scraps and incompletely converted materials also enter the calcium fluoride slag. The rare earth content (REO) is usually 0.9-8%, mainly rare earth metals, rare earth oxides, rare earth fluorides, fluoride oxides, etc.

[0003] In recent years, invention patents have been developed for recovering valuable elements such as rare earths and fluorine from reduced slag through methods such as magnetic separation-sulfuric acid transformation, sodium silicate roasting transformation, and lithium salt vacuum roasting transformation. For example, Chinese invention patent CN 116287735A converts calcium-terbium waste slag into powder by fully air-drying. A magnetic separator then separates terbium-rare earth concentrate and calcium fluoride. Rare earth oxides are obtained through sulfuric acid acidification, oxalic acid precipitation, and calcination. Chinese invention patent CN 105177324 B calcines sodium silicate with vacuum calcium thermally reduced rare earth slag powder at high temperature, acidifies with hydrochloric acid, and separates the rare earth liquid. Chinese invention patent CN 111961872 A mixes lithium salt with calcium thermally reduced slag, vacuum-displaces it, and then vacuum distills it to obtain high-purity lithium fluoride. The distilled slag is then subjected to acid leaching, extraction, precipitation, and calcination to obtain rare earth oxides. Chinese invention patent CN 116497241B mixes lithium carbonate with terbium-calcium slag, calcines it, and immerses the calcined mixture in a leachate for leaching, followed by solid-liquid separation to obtain a mixture of terbium oxide and lithium fluoride. All of these schemes require the use of a high-temperature roasting transformation process to decompose rare earth fluoride and calcium fluoride. However, fluorine-containing compounds and high-acid treatment conditions are highly corrosive to equipment, and the generated hydrogen fluoride gas causes serious pollution to the environment. At the same time, the transformation process requires the introduction of other elements, which increases the difficulty of rare earth purification. The obtained product is mainly a rare earth chloride solution, which needs to be further extracted, precipitated, and calcined to obtain a rare earth oxide product. The process flow is long and the rare earth yield is low. Summary of the Invention

[0004] In light of this, the present invention provides a one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag. This process utilizes a hydrothermal method to directly convert rare earth and fluorine from the rare earth reduction slag into rare earth fluoride, enabling the recovery and recycling of rare earth and fluorine resources. The rare earth fluoride is washed to remove impurities and then vacuum-heated to obtain anhydrous rare earth fluoride, which is then returned as raw material for calcium thermal reduction. This process allows the recycling of calcium, fluorine, and rare earth elements from the rare earth reduction slag, reducing resource waste and production costs.

[0005] The present invention proposes a one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag, comprising:

[0006] Step 1: The massive rare earth reduction slag is crushed and ball-milled into powder;

[0007] Step 2: Mix the powder obtained in step 1 with pure water, remove the generated gas under stirring, and obtain a supernatant and water-leached residue after standing. The water-leached residue is further acidified, filtered, and washed with water to obtain treated rare earth reduction residue;

[0008] Step 3: The treated rare earth reduction slag obtained in step 2 is mixed with a rare earth chloride liquid of the same type, the mixed slurry is placed in a high-pressure reactor, a sealing cover is put on, stirring is started, a precipitation conversion reaction is carried out under high temperature conditions, and the rare earth fluoride and the filtrate are obtained by filtration;

[0009] Step 4: The rare earth fluoride obtained in step 3 is washed, dried, vacuumed, and calcined to obtain anhydrous rare earth fluoride;

[0010] Step 5: The filtrate obtained in step 3 contains rare earth chloride and calcium chloride. The rare earth is enriched using P507 extractant and returned to step 3 for recycling.

[0011] Preferably, the rare earth reduction slag in step 1 includes one or more of metal terbium reduction slag, metal dysprosium reduction slag, metal yttrium reduction slag, and metal gadolinium reduction slag.

[0012] Preferably, the composition of the rare earth reduction slag in step 1 includes Ca: 45-57%, F: 40-49%, and RE: 0.6-10%.

[0013] Preferably, in step 2, the mass ratio of rare earth reduction slag powder to pure water is 1:3-10, and the stirring speed is 100-160 r / min.

[0014] Preferably, in step 2, 0.5-3 mol / L hydrochloric acid is used for acidification, and the pH of the solution after acidification is 0.5-1.5. After filtration, the solution is washed with pure water, and the acid water obtained by filtration is neutralized with the supernatant.

[0015] Preferably, in step three, the concentration of the rare earth chloride solution is 1.0 mol / L to 1.5 mol / L, the pH of the rare earth solution is adjusted to 1 to 4 using ammonium bicarbonate, the amount of rare earth reduction slag input and the amount of rare earth solution input are calculated according to the molar ratio of fluorine in the rare earth reduction slag to REO in the rare earth solution, and the molar ratio of fluorine in the rare earth reduction slag to REO in the rare earth solution is 3:1.0 to 3.0.

[0016] Preferably, in step three, the precipitation conversion reaction temperature is 90-200° C., the stirring speed is 150-300 r / min, and the reaction time is 200-300 min.

[0017] Preferably, in step 4, pure water is used for washing, and the mass ratio of rare earth fluoride to pure water is 1:50-70. The washed rare earth fluoride is dried at a drying temperature of 100-110°C and a drying time of 180-480 min. After drying, vacuum is applied to a vacuum degree of minus 50 kPa to minus 20 kPa, and the vacuum is turned off for calcination at a temperature of 600-800°C and a time of 120-360 min.

[0018] The beneficial effects achieved by the present invention are as follows:

[0019] (1) The same type of rare earth chloride liquid in the reducing slag is used to realize the transformation and decomposition of rare earth and calcium fluoride in the reducing slag under a hydrothermal system, and rare earth fluoride is prepared in one step. The process is simple and easy to operate; (2) The invention simultaneously realizes the comprehensive recovery of rare earth and fluorine resources in the reducing slag, and the recovery rate reaches more than 96%; (3) The invention process realizes the recovery of rare earth and fluorine resources in aqueous solution, avoiding the pollution of waste gas such as hydrogen fluoride and chlorine generated in the high-temperature transformation process, and at the same time does not produce fluorine-containing wastewater, thereby realizing green and efficient recovery of reducing slag. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The figure is a schematic flow chart of the process for preparing anhydrous rare earth fluoride from rare earth reduction slag in one step according to the present invention. DETAILED DESCRIPTION

[0021] The present invention provides a rare earth reduction slag recovery and treatment method, comprising the following steps:

[0022] Step 1: The massive rare earth reduction slag is crushed and ball-milled into powder;

[0023] Step 2: Mix the powder obtained in step 1 with pure water, remove the generated gas under stirring, and obtain a supernatant and water-leached residue after standing. The water-leached residue is further acidified, filtered, and washed with water to obtain treated rare earth reduction residue;

[0024] Step 3: The treated rare earth reduction slag obtained in step 2 is mixed with a rare earth chloride liquid of the same type, the mixed slurry is placed in a high-pressure reactor, a sealing cover is put on, stirring is started, a precipitation conversion reaction is carried out under high temperature conditions, and the rare earth fluoride and the filtrate are obtained by filtration;

[0025] Step 4: The rare earth fluoride obtained in step 3 is washed, dried, vacuumed, and calcined to obtain anhydrous rare earth fluoride;

[0026] Step 5: The filtrate obtained in step 3 contains rare earth chloride and calcium chloride. The rare earth is enriched using P507 extractant and returned to step 3 for recycling.

[0027] In the present invention, the mass percentage of calcium in the rare earth reduction slag is preferably 48-55%; the mass percentage of fluorine in the rare earth reduction slag is preferably 43-48%; and the mass percentage of rare earth in the rare earth reduction slag is preferably 2-8%.

[0028] In the present invention, the blocky rare earth reduction slag is crushed by a jaw crusher and ball milled by a wet rolling ball mill.

[0029] In the present invention, the powder is mixed with pure water to convert residual metallic calcium, calcium oxide, and other substances in the powder into calcium hydroxide with water molecules, releasing the generated hydrogen. In the present invention, the mass ratio of the rare earth waste to pure water is preferably 1:4-8. In the present invention, the mixing is preferably performed under stirring conditions, and the stirring speed is preferably 120-160 rpm.

[0030] After obtaining the water-leached residue, the present invention adds a hydrochloric acid solution dropwise to the water-leached residue. The molar concentration of the hydrochloric acid solution is preferably 1 to 2 mol / L. In the present invention, the pH value of the acidification is preferably 1.0 to 1.5. The acidified water-leached residue is filtered for solid-liquid separation, and the separated solid is filtered and washed with pure water. Washing is stopped when the pH value of the wash water is preferably 6 to 7, and vacuum filtration is performed.

[0031] In the present invention, the molar concentration of the rare earth solution is preferably 1.2 mol / L to 1.5 mol / L. In the present invention, the acid value of the rare earth solution is adjusted using analytically pure ammonium bicarbonate, and the adjusted pH value is preferably 2 to 3.

[0032] In the present invention, the treated rare earth reduction slag is mixed with a rare earth liquid, and the mixing molar ratio is preferably 3:1.2-2.8. The mixed slurry is placed in a high-pressure reactor, covered with a sealing cover, and stirred. The stirring speed is preferably 180-260 r / min. The reaction is carried out at a high temperature, and the reaction temperature is preferably 180-200°C for precipitation conversion reaction to generate rare earth fluoride.

[0033] In the present invention, after the precipitation conversion reaction, the precipitation conversion reaction system is preferably filtered to obtain a solid. The present invention has no special requirements for the filtration process; conventional filtration methods in the art can be employed. The filter residue obtained by filtration is preferably washed to remove surface calcium and chloride ions. In the present invention, the washing solvent is preferably pure water. In the present invention, the mass ratio of the rare earth fluoride to pure water is preferably 1:55-65.

[0034] In the present invention, the drying temperature is preferably 100-105° C.; the drying time is preferably 240-420 min.

[0035] In the present invention, the calcination temperature is preferably 700-800° C.; and the calcination time is preferably 3-6 hours.

[0036] In the present invention, the filtrate obtained by filtration contains a large amount of calcium chloride solution and a small amount of rare earth. In the present invention, the extraction is carried out using P507 extractant. The calcium ions and rare earth ions are separated, and the recovered rare earth ions can be further used as raw materials, achieving resource recycling.

[0037] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0038] Example 1

[0039] according to Figure 1 Anhydrous terbium fluoride is prepared in one step from metallic terbium reduction slag.

[0040] The composition of the terbium metal reduction slag is shown in Table 1.

[0041] Table 1 Composition of terbium metal reduction slag

[0042] Element RE F Ca Mass percentage (%) 5.90 46.50 47.60

[0043] Take 1.0 kg of metallic terbium reduction slag and crush it with a jaw crusher. After crushing, place it in a ball mill and mix it with 3 L of pure water. After mixing, obtain the supernatant and water-leached slag. Slowly add 3 mol / L hydrochloric acid dropwise to the water-leached slag slurry. When the slurry is adjusted to a pH value of 1.0, stop adding hydrochloric acid and perform solid-liquid separation. Set the stirring speed to 130 r / min. The separated solid (calculated as fluorine in the metallic terbium reduction slag) was mixed with 1.2 mol / L terbium chloride feed solution (REO) in a molar ratio of 3:1.2. The mixed slurry was placed in a 10L high-pressure reactor, covered with a sealing cover, and stirred. A precipitation conversion reaction was carried out under high temperature conditions. The acid value of the feed solution was adjusted to a pH of 3 using ammonium bicarbonate. The reaction time was controlled to be 280 min, the stirring speed was 180 r / min, the reaction temperature was controlled to be 180° C., and solid-liquid separation was carried out by filtration. The separated fluoride was washed with pure water at a washing mass ratio of 1:55. The washed fluoride was dried at 105° C. for 240 min. After drying, vacuum was applied until the vacuum reached negative 30 kPa. The vacuum was stopped, and heating was continued. When the temperature reached 700° C., the temperature was kept at 120 min. The central particle size of the generated fluoride was 4.65 μm, O was 0.036%, Ca was 0.2%, and the fluorine conversion rate reached 99.28%. Excess terbium chloride and calcium chloride mixture is fractionated and extracted in a 2:1 organic phase P507:kerosene ratio to separate metallic terbium from calcium chloride. The enriched and separated terbium feed solution is then reused as raw material, ensuring the recovery of both the input rare earth feed solution and the rare earths in the rare earth reduction slag. The organic phase wash water reacts with the reduction slag and pure water soaking solution (i.e., the supernatant), resulting in zero wastewater discharge throughout the process.

[0044] Table 2 Particle size distribution data of anhydrous terbium fluoride crystals prepared in Example 1

[0045]

[0046]

[0047] Example 2

[0048] according to Figure 1 Anhydrous terbium fluoride is prepared in one step from metallic terbium reduction slag.

[0049] The composition of the terbium metal reduction slag is shown in Table 3.

[0050] Table 3 Composition of terbium metal reduction slag

[0051] Element RE F Ca Mass percentage (%) 0.85 43.90 55.25

[0052] Take 1.0 kg of metal terbium reduction slag with a jaw crusher for crushing, after crushing, put in the ball mill, the ball mill after the material is poured into 10 L plastic measuring cup with 5 L pure water for mixing, after mixing, get the supernatant and water immersion residue, slowly drop 2 mol / L hydrochloric acid into the water immersion residue slurry, when the slurry is adjusted to pH 1.5, stop adding hydrochloric acid, solid-liquid separation, stirring speed is set to 150 r / min. The separated solid (calculated by fluorine in metal terbium reduction slag) is mixed with 1.3 mol / L terbium chloride solution (REO) according to the molar ratio of 3:1.6, the mixed slurry is put into a 20 L high pressure reaction kettle, covered with a sealing cover, and the stirring is started. The acid value of the solution is adjusted to pH 2 with analytical pure ammonium bicarbonate, the reaction time is controlled to 290 min, the stirring speed is 200 r / min, and the reaction temperature is controlled to 190℃. The solid-liquid separation is carried out by filtration, the separated fluoride is washed with pure water, the mass ratio of washing is 1:58, the washed fluoride is dried at 103℃ for 300 min, vacuumized to negative 40 kpa, heated to 750℃ for 180 min, and the generated fluoride has a center particle size of 1.67 um, O is 0.048%, Ca is 0.27%, and the conversion rate of fluorine reaches 99.03%. The excess terbium chloride mixed with calcium chloride solution is separated by P507: kerosene-2:1 organic phase fractionation extraction, and the separated terbium solution is used as raw material for continuous use, ensuring that the rare earth in the input rare earth solution and rare earth reduction slag can be recovered. The reduction slag acidification water and organic phase washing water are neutralized with the immersion liquid of the reduction slag and pure water, and the whole process has no wastewater discharge.

[0053] As can be seen from examples 1 and 2, by controlling the parameters, the particle size of the generated anhydrous terbium fluoride can be adjusted to meet different particle size requirements.

[0054] Table 4 particle size distribution data of anhydrous terbium fluoride crystals prepared in example 2

[0055] project result <![CDATA[D 10 / μm]]> 0.74 <![CDATA[D 25 / μm]]> 1.04 <![CDATA[D 50 / μm]]> 1.67 <![CDATA[D 75 / μm]]> 2.67 <![CDATA[D 90 / μm]]> 3.79 <![CDATA[D 97 / μm]]> 5.10 <![CDATA[D 100 / μm]]> 11.18 D (3,2) / μm 1.38 <![CDATA[D (4,3) / μm]]> 2.01 Span 1.83 weight specific surface area / m 2 / kg 4339.03

[0056] Example 3

[0057] According to the process of Figure 1 , the metal dysprosium reduction slag is prepared by one-step method to prepare anhydrous dysprosium fluoride.

[0058] The composition of the metal dysprosium reduction slag is shown in table 5.

[0059] Table 5 composition of metal dysprosium reduction slag

[0060] Element RE F Ca Mass percentage (%) 5.97 46.80 47.23

[0061] Take 1.0 kg of metallic dysprosium reduction slag and crush it with a jaw crusher. After crushing, place it in a ball mill and mill it. Pour the ball-milled material into a 10 L plastic measuring cup and mix it with 6 L of pure water. After mixing, obtain the supernatant and water-leached slag. Slowly add 1.5 mol / L hydrochloric acid dropwise to the water-leached slag slurry. When the slurry is adjusted to a pH value of 1.0, stop adding hydrochloric acid and perform solid-liquid separation. Set the stirring speed to 120 r / min. The separated solid (calculated as fluorine in the metallic dysprosium reduction slag) was mixed with 1.3 mol / L dysprosium chloride liquid (REO) in a molar ratio of 3:1.8. The mixed slurry was placed in a 20 L high-pressure reactor, covered with a sealing cover, and stirred. A precipitation conversion reaction was carried out under high temperature conditions. The acid value of the liquid was adjusted to pH 1 using analytically pure ammonium bicarbonate. The reaction time was controlled to 260 min, the stirring speed was 230 r / min, the reaction temperature was controlled to 200° C., and filtration was used for solid-liquid separation. The separated fluoride was washed with pure water at a washing mass ratio of 1:62. The washed fluoride was dried at 102° C. for 360 min. After drying, vacuum was applied until the vacuum reached minus 40 kPa. The vacuum was stopped, and heating was continued. When the temperature reached 800° C., the temperature was kept at 120 min. The central particle size of the generated fluoride was 1.08 μm, O was 0.050%, Ca was 0.41%, and the fluorine conversion rate reached 98.5%. Excess dysprosium chloride and calcium chloride mixture is fractionated and extracted in a 2:1 ratio of P507 to kerosene in the organic phase to separate the dysprosium metal from the calcium chloride. The separated terbium solution is then reused as raw material, ensuring the recovery of both the rare earth feed solution and the rare earths in the rare earth reduction slag. The acidified slag water and organic phase wash water react with the slag and pure water soaking solution to neutralize the slag. The entire process produces no wastewater.

[0062] Table 6 Particle size distribution data of anhydrous dysprosium fluoride crystals prepared in Example 3

[0063] project result <![CDATA[D 10 / μm]]> 0.51 <![CDATA[D 25 / μm]]> 0.71 D 50 / μm 1.08 D 75 / μm 1.78 D 90 / μm 2.73 D 97 / μm 3.90 D 100 / μm 5.66 <![CDATA[D (3,2) / μm]]> 0.94 D (4,3) / μm 1.39 Span 2.06 weight specific surface area / m 2 / kg 6363.08

[0064] Example 4

[0065] according to Figure 1 Anhydrous yttrium fluoride is prepared in one step from metallic yttrium reduction slag.

[0066] The composition of the metal yttrium reduction slag is shown in Table 7.

[0067] Table 7 Composition of metal yttrium reduction slag

[0068] Element RE F Ca Mass percentage (%) 0.75 45.6 53.65

[0069] Take 1.0 kg of metallic yttrium reduction slag and crush it with a jaw crusher. After crushing, place it in a ball mill and mill it. Pour the ball-milled material into a 10 L plastic measuring cup and mix it with 8 L of pure water. After mixing, obtain the supernatant and water-leached slag. Slowly add 2 mol / L hydrochloric acid dropwise to the water-leached slag slurry. When the slurry is adjusted to a pH value of 1.0, stop adding hydrochloric acid and perform solid-liquid separation. Set the stirring speed to 120 r / min. The separated solid (calculated as fluorine in the metallic yttrium reduction slag) was mixed with 1.25 mol / L dysprosium chloride liquid (REO) in a molar ratio of 3:2.0. The mixed slurry was placed in a 20 L high-pressure reactor, covered with a sealing cover, and stirred. A precipitation conversion reaction was carried out under high temperature conditions. The acid value of the liquid was adjusted to a pH of 2 using analytically pure ammonium bicarbonate. The reaction time was controlled to 270 min, the stirring speed was 260 r / min, the reaction temperature was controlled to 190 ° C, and filtration was used for solid-liquid separation. The separated fluoride was washed with pure water at a washing mass ratio of 1:59. The washed fluoride was dried at 105 ° C for 300 min. After drying, vacuum was evacuated until the vacuum reached minus 20 kPa. The vacuum was stopped and heating was continued. When the temperature reached 700 ° C, the temperature was kept at 700 ° C for 240 min. The central particle size of the generated fluoride was 1.60 μm, O was 0.039%, Ca was 0.58%, and the fluorine conversion rate reached 98.59%. Excess yttrium chloride and calcium chloride mixture is fractionally extracted through a 2:1 P507:kerosene organic phase to separate the metallic yttrium from the calcium chloride. The separated terbium feed is reused as raw material, ensuring the recovery of both the rare earth feed and the rare earths in the rare earth reduction slag. The acidified slag water and organic phase wash water react with the slag and pure water soaking solution to neutralize the slag. The entire process produces no wastewater.

[0070] Table 8 Particle size distribution data of anhydrous yttrium fluoride crystals prepared in Example 4

[0071] project result D 10 / μm 0.74 D 25 / μm 1.03 <![CDATA[D 50 / μm]]> 1.60 <![CDATA[D 75 / μm]]> 2.54 <![CDATA[D 90 / μm]]> 3.50 <![CDATA[D 97 / μm]]> 4.72 <![CDATA[D 100 / μm]]> 7.17 <![CDATA[D (3,2) / μm]]> 1.36 <![CDATA[D (4,3) / μm]]> 1.91 Span 1.73 <![CDATA[重量比表面积 / m 2 / kg]]> 4427.63

[0072] Example 5

[0073] according to Figure 1 Anhydrous gadolinium fluoride is prepared in one step from metallic gadolinium reduction slag.

[0074] The composition of the gadolinium reduction slag is shown in Table 9.

[0075] Table 9 Composition of metallic gadolinium reduction slag

[0076] Element RE F Ca Mass percentage (%) 0.68 43.81 55.51

[0077] 1.0 kg of metallic gadolinium reduction slag was crushed with a jaw crusher and then ball-milled in a ball mill. The ball-milled material was poured into a 10 L plastic measuring cup and mixed with 5 L of pure water to obtain a supernatant and water-leached slag. 2 mol / L hydrochloric acid was slowly added dropwise to the water-leached slag slurry. When the slurry was adjusted to a pH of 1.2, the addition of hydrochloric acid was stopped for solid-liquid separation. The stirring speed was set to 160 r / min. The separated solid (calculated as fluorine in the metallic gadolinium reduction slag) was mixed with 1.4 mol / L dysprosium chloride liquid (REO) in a molar ratio of 3:2.6. The mixed slurry was placed in a 20 L high-pressure reactor, covered with a sealing cover, and stirred. A precipitation conversion reaction was carried out under high temperature conditions. The acid value of the liquid was adjusted to a pH of 3.5 using analytically pure ammonium bicarbonate. The reaction time was controlled to 300 min, the stirring speed was 220 r / min, the temperature was controlled to 200° C., and solid-liquid separation was carried out by filtration. The separated fluoride was washed with pure water at a washing mass ratio of 1:60. The washed fluoride was dried at 105° C. for 360 min. After drying, vacuum was applied until the vacuum reached 30 kPa. The vacuum was stopped, and heating was continued. When the temperature reached 760° C., the temperature was kept at 300 min. The central particle size of the generated fluoride was 5.12 μm, O was 0.042%, Ca was 0.25%, and the fluorine conversion rate reached 99.10%. Excess gadolinium chloride and calcium chloride mixture is fractionally extracted through a 2:1 P507:kerosene organic phase to separate the gadolinium metal from the calcium chloride. The separated terbium feed is reused as raw material, ensuring the recovery of both the rare earth feed and the rare earths in the rare earth reduction slag. The acidified slag water and organic phase wash water react with the slag soaked in pure water to neutralize the slag. The entire process produces no wastewater.

[0078] Table 10 Particle size distribution data of anhydrous gadolinium fluoride crystals prepared in Example 5

[0079]

[0080]

Claims

1. A one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag, characterized in that: include: Step 1: The massive rare earth reduction slag is crushed and ball-milled into powder; Step 2: Mix the powder obtained in step 1 with pure water, remove the generated gas under stirring, and obtain a supernatant and water-leached residue after standing. The water-leached residue is further acidified, filtered, and washed with water to obtain treated rare earth reduction residue; Step 3: The treated rare earth reduction slag obtained in step 2 is mixed with a rare earth chloride liquid of the same type, the mixed slurry is placed in a high-pressure reactor, a sealing cover is put on, stirring is started, a precipitation conversion reaction is carried out under high temperature conditions, and the rare earth fluoride and the filtrate are obtained by filtration; Step 4: The rare earth fluoride obtained in step 3 is washed, dried, vacuumed, and calcined to obtain anhydrous rare earth fluoride; Step 5: The filtrate obtained in step 3 contains rare earth chloride and calcium chloride. The rare earth is enriched using P507 extractant and returned to step 3 for recycling.

2. The one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag according to claim 1, characterized in that: The rare earth reduction slag in step 1 includes one or more of metal terbium reduction slag, metal dysprosium reduction slag, metal yttrium reduction slag, and metal gadolinium reduction slag.

3. The one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag according to claim 1, characterized in that: The components of the rare earth reduction slag in step 1 include Ca: 45% to 57%, F: 40% to 49%, and RE: 0.6% to 10% by mass.

4. The one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag according to claim 1, characterized in that: In step 2, the mass ratio of rare earth reduction slag powder to pure water is 1:3-10, and the stirring speed is 100-160 r / min.

5. The one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag according to claim 1, characterized in that: In step 2, 0.5-3 mol / L hydrochloric acid is used for acidification, and the pH of the solution after acidification is 0.5-1.

5. After filtration, the solution is washed with pure water, and the acid water obtained by filtration is neutralized with the supernatant.

6. The one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag according to claim 1, characterized in that: In step three, the concentration of the rare earth chloride solution is 1.0 mol / L to 1.5 mol / L, the pH of the rare earth solution is adjusted to 1 to 4 using ammonium bicarbonate, and the amount of rare earth reduction slag input and the amount of rare earth solution input are calculated according to the molar ratio of fluorine in the rare earth reduction slag to REO in the rare earth solution, and the molar ratio of fluorine in the rare earth reduction slag to REO in the rare earth solution is 3:1.0 to 3.

0.

7. The one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag according to claim 1, characterized in that: In the step 3, the precipitation conversion reaction temperature is 90-200° C., the stirring speed is 150-300 r / min, and the reaction time is 200-300 min.

8. The one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag according to claim 1, characterized in that: In the step 4, pure water is used for washing, and the mass ratio of rare earth fluoride to pure water is 1:50-70. The washed rare earth fluoride is dried at a drying temperature of 100-110° C. and a drying time of 180-480 min. After drying, vacuum is applied to a vacuum degree of minus 50 kPa to minus 20 kPa, and the vacuum is turned off, and calcination is performed at a temperature of 600-800° C. and a time of 120-360 min.

Citation Information

Patent Citations

  • A method for recovering rare earth from vacuum calcium thermal reduction rare earth slag

    CN105177324B

  • Method for extracting valuable elements in calcium thermal vacuum reduction rare earth slag

    CN111961872A

  • Recycling method of rare earth and fluorine in terbium waste residue produced by vacuum calcium thermal reduction method

    CN116287735A

  • A method for recovering terbium from terbium-calcium slag

    CN116497241B

  • Method for efficiently removing fluorine from fluorine-containing mixed rare earth chloride solution

    CN114182113A