Electrochemical anti-corrosion and anti-fouling system and method for offshore wind power steel pile
Through an electrochemical anti-corrosion and anti-fouling system composed of flexible anode and reference electrode, combined with cathode protection and electrolytic anti-fouling, the electrochemical anti-corrosion and anti-fouling of offshore wind power steel piles is realized, and the corrosion of steel piles and marine organisms in seawater is solved. The problem of pollution extends the anti-fouling efficiency period and reduces the risk of corrosion.
Patent Information
- Application Number
- CN202411128035.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-29
AI Technical Summary
Corrosion and marine biological pollution problems of offshore wind power steel piles in seawater. The existing technology anti-fouling coating has a short validity period and is difficult to apply. The protective potential distribution is uneven when cathode protection and protective coating are used together, resulting in steel piles. Face high risk of corrosion.
The electrochemical anti-corrosion and anti-fouling system consisting of a flexible anode and multiple reference electrodes is used to realize long-term cathode protection and pulsed electrolytic anti-fouling through rectifiers. Combining the growth law of marine organisms and the diffusion and decomposition effect of anti-fouling agents, the output current is adjusted to achieve The uniform protection potential and antifoulant concentration distribution of the steel pile surface.
The integrated electrochemical anti-corrosion and anti-fouling control of steel piles has been realized, the anti-fouling efficiency period has been extended, the risks of corrosion and marine biological pollution of steel piles have been reduced, and the uniform protection and anti-fouling effect of the steel pile surface has been ensured.
Smart Images

Figure CN119040895A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of marine engineering corrosion protection, and in particular to an electrochemical anti-corrosion and anti-fouling system and method for offshore wind power steel piles. Background Art
[0002] Offshore wind power steel piles stand in seawater, which is a highly corrosive medium. In addition, marine microorganisms, attached organisms and their metabolites directly or indirectly accelerate the corrosion process. For offshore wind power foundations made of steel materials, "anti-corrosion and anti-fouling" has become the biggest challenge after its operation.
[0003] At present, the anti-corrosion and anti-fouling technologies commonly used in marine engineering equipment mainly include cathodic protection, electrolytic anti-fouling and anti-corrosion and anti-fouling coatings, among which cathodic protection and anti-corrosion and anti-fouling coatings are mature in the application of offshore wind power steel piles. Considering the sufficient power supply of offshore wind power and the longer service life, impressed current cathodic protection has been promoted in offshore wind power steel piles in recent years. CN217174898 U, CN 112031015A and CN 103726057 A all disclose some impressed current cathodic protection methods for offshore wind power foundations, which can effectively solve the corrosion problem of wind power steel piles. The technical principle of electrolytic anti-fouling is to pass an electrolytic current through the electrolytic electrode, and an oxidation reaction occurs on the anode surface to generate anti-fouling agents such as sodium hypochlorite. When the concentration of anti-fouling agents in seawater reaches a certain value, the anti-fouling effect can be achieved. This method is mature in closed environments such as seawater pipeline systems, and the use effect is good. Anti-corrosion and anti-fouling coatings have been widely used and verified in the fields of marine ships, marine engineering, etc., and a complete product series has been formed. When designing the protection of offshore wind power steel piles, relevant standards recommend the use of cathodic protection or a combination of cathodic protection and protective coating.
[0004] However, when the offshore wind power steel piles are jointly protected by cathodic protection and protective coating, the number of anodes installed on the surface of the steel piles is limited, and the installation position is relatively concentrated. Although the steel piles can be effectively protected, the protection potential distribution is uneven, and over-protection is prone to occur around the anodes; due to the overall technical level limitations, the anti-fouling period of mainstream products at home and abroad is only 3 to 5 years, which is far lower than the design life of offshore wind power (usually more than 20 years), and the difficulty of re-coating offshore wind power steel piles is extremely great, resulting in unsatisfactory anti-fouling effect of steel piles. Therefore, offshore wind power steel piles rarely use anti-fouling coatings, and only anti-corrosion coatings are applied, which makes steel piles face extremely high risks of marine biofouling. When electrolytic anti-fouling technology is used for offshore wind power steel piles, due to the large scale of steel piles and their location in open seas, it is extremely difficult to maintain a certain concentration of anti-fouling agent on the surface of steel piles, and it has not been applied in offshore wind power. Therefore, it is necessary to develop an electrochemical protection method that can simultaneously solve the problems of steel pile corrosion and marine biofouling to solve the above problems. Summary of the invention
[0005] In order to solve the above problems, the present invention provides an electrochemical anti-corrosion and anti-fouling system and method for offshore wind power steel piles. The present invention provides the following technical solutions:
[0006] The present invention provides an electrochemical anti-corrosion and anti-fouling system for offshore wind power steel piles, the system comprising wind power steel piles, a rectifier, an anode and a plurality of reference electrodes, wherein:
[0007] The wind power steel pile and the anode are respectively connected to the negative electrode and the positive electrode of the rectifier to form a closed loop with the seawater medium;
[0008] The plurality of reference electrodes are connected to the rectifier via cables, including:
[0009] a first reference electrode mounted below the waterline and at a first distance from the anode;
[0010] A second reference electrode is mounted below the waterline at a second distance from the anode.
[0011] Specifically, the anode is a flexible anode.
[0012] Specifically, the anode includes a platinum-plated titanium anode or a titanium-based ruthenium-iridium mixed metal oxide anode.
[0013] Specifically, the anode is an anode encapsulated by an insulating material.
[0014] Specifically, the anodes are evenly distributed on the outer surface of the wind power steel pile, and the anodes do not contact the wind power steel pile.
[0015] Specifically, the anodes are evenly wound around the outer surface of the wind power steel pile below the water surface and above the mud surface, wherein the spacing between the anodes is 0-2m.
[0016] Specifically, the rectifier includes a potentiostat.
[0017] Specifically, the rectifier is installed in a wind turbine cabin on the top of a wind power steel pile, and a cathode grounding point is provided in the wind turbine cabin.
[0018] Specifically, the plurality of reference electrodes is two or more.
[0019] Specifically, the reference electrode includes an Ag / AgCl / seawater electrode, a high-purity zinc electrode or a composite double reference electrode.
[0020] Specifically, the first distance is half the distance between the low tide waterline and the anode;
[0021] The second distance is 10-50 cm.
[0022] The present invention also provides an electrochemical anti-corrosion and anti-fouling method for offshore wind power steel piles, using the above system, the method comprises:
[0023] Estimate the required cathodic protection current and electrolytic anti-fouling current according to the steel pile size and offshore environmental characteristics;
[0024] During cathodic protection, the wind power steel pile protection potential measured by the first reference electrode installed below the waterline and at a first distance away from the anode is obtained as a control signal or evaluation parameter.
[0025] Based on the wind power steel pile protection potential and the estimated cathode protection current, setting the rectifier constant potential or constant current output protection potential or constant current output protection current, and continuously running for a first predetermined time;
[0026] During electrolytic antifouling, obtaining the anode working potential measured by a second reference electrode installed at a second distance below the waterline and close to the anode;
[0027] Based on the anode working potential and the estimated electrolytic anti-fouling current, the rectifier outputs a chlorine evolution potential or an electrolytic current to perform pulsed electrolytic anti-fouling;
[0028] The cathodic protection process and the electrolytic anti-fouling process are repeated alternately to achieve electrochemical anti-corrosion and anti-fouling control of offshore wind power steel piles.
[0029] Specifically, the first predetermined time is 2 to 6 hours.
[0030] Specifically, the process of pulse electrolysis anti-fouling is:
[0031] The electrolytic anti-fouling runs for a second predetermined time, the second predetermined time being 10 to 30 minutes;
[0032] Then the output is stopped for a third predetermined time, where the third predetermined time is ≤ 10 minutes.
[0033] Technical effects and advantages of the present invention:
[0034] The present invention starts from the perspective of coordinated control of steel pile anti-corrosion and anti-fouling, combines the electrochemical properties of cathodic protection and electrolytic anti-fouling, and studies the structure, installation method and output current of the anode to propose a coordinated control method of electrochemical anti-corrosion and anti-fouling. Flexible anodes are arranged on the steel piles, and the steel piles are used as cathodes. According to the cathodic protection and electrolytic anti-fouling requirements of the steel piles, combined with the growth law of marine organisms and the diffusion and decomposition effect of anti-fouling agents, and considering the hydrogen evolution problem of the steel piles, the control parameters are reasonably adjusted, and the long-term cathodic protection + pulsed electrolytic anti-fouling method is adopted. The output current is automatically adjusted periodically, and the steel piles are respectively subjected to cathodic protection and electrolytic anti-fouling, so as to realize the integrated control of electrochemical anti-corrosion and anti-fouling of the steel piles.
[0035] At the same time, based on the similarity of electrochemical properties of cathodic protection and electrolytic antifouling, the present invention invented an electrochemical anti-corrosion and anti-fouling synergistic control method. The method is designed to use flexible anodes to be evenly wound on the surface of steel piles to ensure that the protection potential and antifouling agent concentration on the surface of the steel piles are evenly distributed; when used, it is based on long-term cathodic protection output, combined with pulsed electrolytic antifouling output, and by designing reasonable output parameters, the anti-corrosion and anti-fouling synergistic control effect is achieved.
[0036] Other features and advantages of the present invention will be described in the following description, and partly become obvious from the description, or be understood by implementing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is a diagram of an electrochemical anti-corrosion and anti-fouling system for offshore wind power steel piles provided in an embodiment of the present application;
[0038] Figure 2 This is a current output characteristic diagram provided in an embodiment of the present application. DETAILED DESCRIPTION
[0039] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] In order to solve the deficiencies of the prior art, the present invention discloses an electrochemical anti-corrosion and anti-fouling system for offshore wind power steel piles, such as Figure 1 As shown, the system includes a rectifier, a flexible anode and a plurality of reference electrodes, wherein:
[0041] The wind power steel pile and the flexible anode are respectively connected to the negative electrode and the positive electrode of the rectifier, forming a closed loop with the seawater medium; the anode is evenly distributed on the outer surface of the wind power steel pile, and the anode does not contact the steel pile; multiple reference electrodes are connected to the rectifier through cables; wherein,
[0042] a reference electrode installed below the waterline and at a first distance away from the anode to measure the potential of the steel pile;
[0043] a reference electrode mounted below the waterline at a second distance from the anode to measure the working potential of the anode;
[0044] The rectifier is used to measure the potential of the steel pile according to the reference electrode and regulate the current output by the cathodic protection; it is also used to measure the potential of the anode according to the second reference electrode and regulate the current output by the electrolytic anti-fouling.
[0045] In a specific embodiment of the present invention, the anode is a flexible anode; the flexible anode can be a platinum-plated titanium anode or a titanium-based ruthenium-iridium mixed metal oxide anode. The anode can be in the form of a flat belt, a mesh belt or a wire, and the anode size is designed or selected according to the output current. The anode is installed on the outer surface of the steel pile below the water surface and above the mud surface by winding. During installation, the anode cannot be in direct contact with the steel pile. It is installed in an insulating manner, or the anode is encapsulated with insulating materials before installation. During installation, the spacing between the anodes should not exceed 2m to ensure that the surface potential of the steel pile and the concentration of the antifouling agent are evenly distributed.
[0046] In a specific embodiment of the present invention, the reference electrode used includes at least a first reference electrode and a second reference electrode. The reference electrode can be an Ag / AgCl / seawater electrode or a high-purity zinc electrode, or a composite double reference electrode. When different reference electrodes are selected, the standard electrode potential difference should be referred to for conversion. The first reference electrode is installed at a moderate distance from the anode below the waterline, and is used to measure the potential of the steel pile and is used as a basis for regulating the output of the cathodic protection; the second reference electrode is installed at a position below the waterline close to the anode, and is used to measure the working potential of the anode and is used as a basis for regulating the output of the electrolytic antifouling.
[0047] In a specific embodiment of the present invention, platinum-plated titanium and mixed metal oxide anodes can be used as electrodes for both cathodic protection and electrolytic antifouling, while other lead-silver alloys and the like cannot be used for electrolytic antifouling; existing ships and platforms usually use disc-shaped or plate-shaped anodes, and the number of installed anodes is very small, which results in a large potential distribution gradient on the hull or platform, and the potential around the anode is very negative, requiring the installation of an anode screen for protection.
[0048] In a specific embodiment of the present invention, the potentiostat / rectifier adopts a mature switch type or thyristor type, the potentiostat / rectifier is installed in the wind turbine cabin, and a cathode grounding point is installed in the wind turbine cabin, and the anode and reference electrode on the steel pile are connected to the potentiostat / rectifier through a cable. The potentiostat / rectifier includes timing control and rectification output functions. In the embodiment of the present invention, the wind turbine refers to the entire wind turbine unit, including steel piles, cabins, blades, etc., and the steel piles are only the foundation part. Offshore wind power is fixed by steel piles driven into the seabed, followed by the tower. The highest point is the wind turbine cabin, and the main power generation system is placed in the cabin.
[0049] The method of the present invention is based on the similarity of the electrochemical properties of cathodic protection and electrolytic antifouling. A flexible anode is designed to be evenly wound on the surface of a steel pile to ensure that the protective potential and antifouling agent concentration on the surface of the steel pile are evenly distributed. When in use, it is based on long-term cathodic protection output and combined with pulsed electrolytic antifouling output. By designing reasonable output parameters, a synergistic control effect of anti-corrosion and anti-fouling is achieved.
[0050] In the coordinated control process of anti-corrosion and anti-fouling of the present invention, the steel pile is used as the cathode and the auxiliary electrode is used as the anode for anti-corrosion and anti-fouling. However, the current required for anti-fouling is much greater than that for anti-corrosion. In order to reduce the influence of cathode hydrogen evolution on the steel pile, a pulsed output mode is firstly designed in combination with the attachment law of fouling organisms, and a long-term cathodic protection + short-time electrolytic anti-fouling mode is adopted to intermittently perform electrolytic anti-fouling, thereby realizing the anti-fouling function and reducing the risk of hydrogen evolution on the steel pile; secondly, in order to achieve a comprehensive anti-fouling effect, it is necessary to ensure that the concentration of the anti-fouling agent on the surface of the steel pile reaches an effective range. Due to the influence of waves, etc., the anti-fouling agent produced on the anode surface is easily diluted by the waves and is difficult to be evenly distributed on the surface of the steel pile. Therefore, the design adopts a method of evenly and densely distributing anodes on the surface of the steel pile, such as winding flexible anodes. On the one hand, the distribution density of the anodes is increased, that is, the output source of the anti-fouling agent is widely distributed. On the other hand, the distance between the anode and the steel pile is also reduced, so that the anti-fouling agent is more easily diffused to the surface of the steel pile, thereby ensuring the anti-fouling effect.
[0051] The present invention also provides an electrochemical anti-corrosion and anti-fouling method for offshore wind power steel piles. The method starts from the perspective of coordinated control of steel pile anti-corrosion and anti-fouling, combines the electrochemical properties of cathodic protection and electrolytic anti-fouling, and studies the structure, installation method and output current of the anode to propose an electrochemical anti-corrosion and anti-fouling coordinated control method. Flexible anodes are arranged on steel piles, and steel piles are used as cathodes. According to the cathodic protection and electrolytic anti-fouling requirements of steel piles, combined with the growth law of marine organisms and the diffusion and decomposition effect of anti-fouling agents, and considering the hydrogen evolution problem of steel piles, the control parameters are reasonably adjusted, and the long-term cathodic protection + pulsed electrolytic anti-fouling method is adopted. The output current is automatically adjusted periodically, and the steel piles are respectively subjected to cathodic protection and electrolytic anti-fouling, so as to realize the integrated control of electrochemical anti-corrosion and anti-fouling of steel piles.
[0052] The specific steps are as follows:
[0053] In engineering applications, the required cathodic protection current and electrolytic anti-pollution current are estimated according to the steel pile specifications and environmental characteristics and with reference to relevant design standards. The output current characteristic curve of the constant potential instrument is set as follows: Figure 2 When running, the constant potential or constant current output control mode can be adopted;
[0054] During cathodic protection, the steel pile protection potential measured by a reference electrode installed below the waterline and at a first distance away from the anode is obtained as a control signal or evaluation parameter.
[0055] Based on the steel pile protection potential and the estimated cathodic protection current, the rectifier is set to output the protection potential or protection current at a constant potential or constant current, and the protection potential or protection current is continuously operated for a time of t1 to provide cathodic protection for the steel pile, and t1 is preferably 2 to 6 hours. At this time, the set protection potential or protection current should be able to effectively protect the steel pile, and the steel pile protection potential measured by the first reference electrode is used as a control signal or evaluation parameter.
[0056] Then, pulse electrolytic antifouling is performed, and the set chlorine evolution potential or electrolytic current I2 is output, and effective chlorine antifouling agent is generated on the anode surface. The antifouling agent covers the surface of the steel pile by diffusion, and the electrolytic antifouling control of the steel pile is realized. The electrolytic antifouling operation time t2 is preferably 10 to 30 minutes. This value is related to the degree of contamination. The lossless medium in different sea areas is different, and the preferred time is different. The preferred time of the embodiment of the present invention is 15 minutes; then stop outputting t3 time, t3 is preferably ≤10 minutes, and this time period is used to make the steel pile properly depolarized, so as to avoid the polarization current reversal when the cathodic protection is performed again because the polarization potential exceeds the set protection potential. After depolarization, the process of t1, t2 and t3 is repeated, and this cycle is used to achieve continuous anti-corrosion and anti-fouling control.
[0057] The technical solution of the present invention will be further described below in conjunction with specific implementation methods.
[0058] like Figure 1 Specifically, the flexible anode in the present invention can be a platinum-plated titanium anode or a titanium-based ruthenium-iridium mixed metal oxide anode. The anode can be in the form of a flat belt, a mesh belt or a wire. The anode size is designed or selected according to the output current. Preferably, the anode in this embodiment usually has a suitable working current density range, such as an oxide anode preferably 500 to 2000A / m 2 , exceeding this range may shorten the life of the anode or make it ineffective. The anode is installed on the outer surface of the steel pile below the water surface and above the mud surface by winding. During installation, the anode cannot be in direct contact with the steel pile. It is installed by insulation or the anode is encapsulated with insulating materials before installation. During installation, the spacing between the anodes should not exceed 2m to ensure that the surface potential of the steel pile and the concentration of the antifouling agent are evenly distributed.
[0059] The reference electrode used includes at least two electrodes, the first reference electrode and the second reference electrode. The reference electrode can be Ag / AgCl / seawater electrode or high-purity zinc electrode, or a composite double reference electrode. When different reference electrodes are selected, the standard electrode potential difference should be referred to for conversion. The first reference electrode is installed below the waterline at a moderate distance from the anode (in the middle of the low-tide waterline and the anode), which is used to measure the potential of the steel pile and is used as a basis for regulating the output of the cathodic protection; the second reference electrode is installed below the waterline near the anode, preferably 10 to 50 cm around the anode, preferably 30 cm, which is used to measure the working potential of the anode and is used as a basis for regulating the output of the electrolytic antifouling.
[0060] The potentiostat / rectifier adopts mature switch type or thyristor type. The potentiostat / rectifier is installed in the cabin of the fan, and the cathode grounding point is installed in the fan. The anode and reference electrode on the steel pile are connected to the potentiostat / rectifier through cables. The potentiostat / rectifier includes timing control and rectification output functions.
[0061] In engineering applications, the required cathodic protection current and electrolytic anti-pollution current are estimated according to the steel pile specifications and environmental characteristics and with reference to relevant design standards, where cathodic protection current = steel pile protection area × protection current density; electrolytic anti-pollution current = chlorine production / 0.926;
[0062] Set the output current characteristic curve of the potentiostat as Figure 2 As shown. During operation, a constant potential or constant current output control mode can be used. First, according to the set protection potential or protection current I1 output (the protection potential is set according to the requirements of the design standard, and the protection current is set according to the calculated result), cathodic protection is provided for the steel pile, and it runs continuously for t1 hours, and t1 is preferably 2 to 6 hours. Considering the effectiveness of electrolytic antifouling, the spores of fouling organisms usually attach for about 4 to 6 hours. Therefore, it is designed that an electrolytic antifouling output is required after every 2 to 6 hours of cathodic protection operation.
[0063] At this time, the set protection potential or protection current should be able to effectively protect the steel pile, and the steel pile protection potential measured by the first reference electrode is used as the control signal or evaluation parameter. Then, pulse electrolytic anti-fouling is performed, and the set chlorine evolution potential or electrolytic current I2 is output according to the chlorine evolution potential specified in the standard or the calculated electrolytic current, and an effective chlorine anti-fouling agent is generated on the anode surface. The anti-fouling agent covers the surface of the steel pile by diffusion, and the electrolytic anti-fouling control of the steel pile is realized. The electrolytic anti-fouling operation time t2 is preferably 10 to 30 minutes; then the output is stopped for t3 time, t3 is preferably ≤10 minutes. This time period is used to make the steel pile properly depolarized, and the steel pile potential is preferably positive to the set cathodic protection potential, so as to avoid polarization current reversal when the cathodic protection is performed again due to the polarization potential exceeding the set protection potential. After depolarization, the process of t1, t2 and t3 is repeated, and this cycle is repeated until the wind power steel pile is no longer used, thereby achieving continuous anti-corrosion and anti-fouling control.
[0064] Embodiment 1:
[0065] The diameter of a steel pile of an offshore wind power plant is 8m, the height below the waterline and above the mud surface is 30m, and the height below the mud is 50m. Referring to the design standard of cathodic protection, the protection current required for cathodic protection of steel piles is about 50A; when electrolytic anti-fouling is performed, the water body in a 0.5m thick cylinder on the surface of the steel pile is used as the anti-fouling object, the designed effective chlorine concentration is 0.5ppm, and the required chlorine production is about 188g. According to the design standard, the output electrolytic current is about 200A.
[0066] The design uses a flat belt type mixed metal oxide anode with a specification of 6.35×0.635mm. The anode is installed on the surface of the steel pile with an insulating clip. The spiral wire spacing is 2m, and the total anode belt length is about 350m. At the same time, two reference electrodes are installed, both of which are Ag / AgCl / seawater electrodes. The steel pile is used as the cathode grounding point, and the constant potential instrument uses a switching power supply with a specification of DC500A / 30V.
[0067] During operation, a constant potential output mode is adopted. First, the steel pile potential measured by the first reference is used as a control signal, and the steel pile protection potential is set to -0.9V (vs. Ag / AgCl / seawater). The output protection current is controlled to perform cathodic protection on the steel pile. At this time, the entire steel pile (including the part under the mud) can be effectively protected. After 6 hours of continuous cathodic protection, it is automatically switched to the anode potential measured by the second reference as the control signal for electrolysis output, and the anode chlorine potential is set to 1.1V (vs. Ag / AgCl / seawater). The output current is controlled for electrolysis. The electrolysis is continued for 20 minutes, and then the output is stopped, and the steel pile is automatically depolarized. The waiting time is 10 minutes, and cathodic protection-electrolysis antifouling-depolarization is performed again, and this cycle is run.
[0068] Embodiment 2:
[0069] Similarly, the offshore wind power steel pile shown in Example 1 is used as the object, and the anode, reference electrode and constant potential instrument are installed. The constant current output mode is adopted, and the cathode protection is first performed with a current of 50A, and the protection potential of the steel pile is continuously monitored by the first reference electrode. When insufficient protection occurs, an automatic alarm is given to prompt the adjustment of the cathode protection current; after continuous operation for 6 hours, the output current is automatically adjusted to 200A to realize the electrolytic anti-fouling function, and the protection potential of the steel pile is continuously monitored by the first reference electrode, and the working potential of the anode is continuously monitored by the second reference electrode. When the potential of the steel pile is seriously over-limit or the potential of the anode chlorine evolution is insufficient, an alarm is given to prompt the adjustment of the electrolytic current; after 20 minutes of continuous electrolysis, the output is stopped to depolarize the steel pile, and the cathode protection-electrolytic anti-fouling-depolarization is performed again after 10 minutes, and the cycle is run in this way.
[0070] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An electrochemical anti-corrosion and anti-fouling system for offshore wind power steel piles, characterized in that: The system includes a wind power steel pile, a rectifier, an anode and a plurality of reference electrodes, wherein: The wind power steel pile and the anode are respectively connected to the negative electrode and the positive electrode of the rectifier to form a closed loop with the seawater medium; The plurality of reference electrodes are connected to the rectifier via cables, including: a first reference electrode mounted below the waterline and at a first distance from the anode; A second reference electrode is mounted below the waterline at a second distance from the anode.
2. The electrochemical anti-corrosion and anti-fouling system for offshore wind power steel piles according to claim 1 is characterized in that: The anode is a flexible anode.
3. The electrochemical anti-corrosion and anti-fouling system for offshore wind power steel piles according to claim 1 is characterized in that: The anode includes a platinum-plated titanium anode or a titanium-based ruthenium-iridium mixed metal oxide anode.
4. The electrochemical anti-corrosion and anti-fouling system for offshore wind power steel piles according to claim 2 is characterized in that: The anode is an anode encapsulated by an insulating material.
5. The electrochemical anti-corrosion and anti-fouling system for offshore wind power steel piles according to any one of claims 1 to 3, characterized in that: The anodes are evenly distributed on the outer surface of the wind power steel pile, and the anodes do not contact the wind power steel pile.
6. The electrochemical anti-corrosion and anti-fouling system for offshore wind power steel piles according to claim 5 is characterized in that: The anodes are evenly wound around the outer surface of the wind power steel pile below the water surface and above the mud surface, wherein the spacing between the anodes is 0-2m.
7. The electrochemical anti-corrosion and anti-fouling system for offshore wind power steel piles according to claim 1 is characterized in that: The rectifier includes a potentiostat.
8. The electrochemical anti-corrosion and anti-fouling system for offshore wind power steel piles according to claim 1 is characterized in that: The rectifier is installed in a wind turbine cabin on the top of a wind power steel pile, and a cathode grounding point is arranged in the wind turbine cabin.
9. The electrochemical anti-corrosion and anti-fouling system for offshore wind power steel piles according to claim 1 is characterized in that: The number of reference electrodes is two or more.
10. The electrochemical anti-corrosion and anti-fouling system for offshore wind power steel piles according to claim 1 is characterized in that: The reference electrode includes an Ag / AgCl / seawater electrode, a high-purity zinc electrode or a composite double reference electrode.
11. The electrochemical anti-corrosion and anti-fouling system for offshore wind power steel piles according to claim 1, characterized in that: The first distance is half the distance between the low-tide waterline and the anode; The second distance is 10-50 cm.
12. An electrochemical anti-corrosion and anti-fouling method for offshore wind power steel piles, characterized in that: Using the system according to any one of claims 1 to 11, the method comprises: Estimate the required cathodic protection current and electrolytic anti-fouling current according to the steel pile size and offshore environmental characteristics; During cathodic protection, the wind power steel pile protection potential measured by the first reference electrode installed below the waterline and at a first distance away from the anode is obtained as a control signal or evaluation parameter. Based on the wind power steel pile protection potential and the estimated cathode protection current, setting the rectifier constant potential or constant current output protection potential or constant current output protection current, and continuously running for a first predetermined time; During electrolytic antifouling, obtaining the anode working potential measured by a second reference electrode installed at a second distance below the waterline and close to the anode; Based on the anode working potential and the estimated electrolytic anti-fouling current, setting the rectifier output chlorine evolution potential or electrolytic current to perform pulse electrolytic anti-fouling; The cathodic protection process and the electrolytic anti-fouling process are repeated alternately to achieve electrochemical anti-corrosion and anti-fouling control of offshore wind power steel piles.
13. The electrochemical anti-corrosion and anti-fouling method for offshore wind power steel piles according to claim 11, characterized in that: The first predetermined time is 2 to 6 hours.
14. The electrochemical anti-corrosion and anti-fouling method for offshore wind power steel piles according to claim 11, characterized in that: The process of pulse electrolysis antifouling is: The electrolytic anti-fouling runs for a second predetermined time, the second predetermined time being 10 to 30 minutes; Then the output is stopped for a third predetermined time, where the third predetermined time is ≤ 10 minutes.